Thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties, and method for preparing same
A ternary blend of polypropylene copolymers and a polyolefin elastomer addresses flexibility and high-temperature insulation issues in cable insulation, enhancing tensile strength and electrical properties through controlled elastic modulus and compatibility.
Patent Information
- Application Number
- PCT/KR2025/015031
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2025-09-25
- Publication Date
- 2026-11-12
AI Technical Summary
Existing thermoplastic polymer compositions for high-voltage cable insulation face challenges in achieving both high flexibility and high-temperature insulation performance due to issues like phase separation, reduced mechanical strength, and inadequate electrical insulation at varying temperatures, particularly in sub-zero and high-temperature environments.
A thermoplastic polymer composition comprising a ternary blend of a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer, with specific weight ratios and elastic moduli, is developed to enhance compatibility and control elastic modulus, resulting in improved tensile strength and high-temperature insulation.
The composition achieves a low elastic modulus with high tensile strength and excellent electrical insulation properties at high temperatures, suitable for high-voltage cable applications, maintaining mechanical flexibility and reducing interfacial defects.
Smart Images

Figure KR2025015031_12112026_PF_FP_ABST
Abstract
Description
Thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties and method for manufacturing the same
[0001] The present invention relates to a thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties, and a method for manufacturing the same.
[0002] Thermoplastic polymers (TP) are a general term for polymers that can be molded by heat. They are characterized by being very easy to mold from a process perspective, as well as being remoldable by heat and thus recyclable. Polyethylene (PE) and polypropylene (PP) are among the thermoplastic polymers that are inexpensive and possess excellent properties such as mechanical and chemical resistance, so they are widely used in various fields such as packaging materials, films, containers, pipes, and the electrical and electronic industries.
[0003] For example, while crosslinked polyethylene (XLPE) has been widely used in conventional power cables, there has recently been active technological development aimed at utilizing polypropylene-based materials. This is because polypropylene-based materials have a higher melting temperature compared to crosslinked polyethylene, which not only meets the need for increased heat resistance due to the trend of increasing power capacity, but also significantly reduce the burden of the process by eliminating the crosslinking and crosslinking byproduct removal processes, and furthermore, secure eco-friendliness through recyclability, which is difficult to obtain from conventional crosslinked polyethylene.
[0004] However, polypropylene itself is unsuitable for use as an insulation material for cables requiring flexibility due to its inherently high rigidity, or elastic modulus. Therefore, to improve flexibility and consequently impact strength, technology is being developed to manufacture thermoplastic elastomers (TPEs) using polypropylene-based copolymers or blends, which are thermoplastic and possess rubber-like elasticity.
[0005] In this regard, as disclosed in 'Ternary composition for cable insulation layer, method of manufacturing the same, cable insulation layer including the same, power cable (Korean Patent Publication No. 10-2021-0052962)', a representative flexible rubbery material used in the manufacture of polypropylene-based thermoplastic elastomers by blending is a polyolefin elastomer (POE) containing alpha olefins. Although the flexibility and impact resistance of such polypropylene-based thermoplastic elastomers can be improved depending on the content of the polyolefin elastomer, it is difficult to improve impact resistance in sub-zero low-temperature environments. Furthermore, if the content of the polyolefin elastomer in the thermoplastic elastomer is excessively high, it also presents the problem of actually degrading mechanical strength, electrical insulation, and heat resistance at room temperature and high temperatures.
[0006] To address these drawbacks, a method for improving low-temperature impact resistance is disclosed in 'Ternary insulating composition containing an organic hard modifier, method for manufacturing the same, and insulating material using the same (Korean Patent Publication No. 10-2023-0041346)' by appropriately using a material having an elastic modulus between that of polypropylene and an elastomer. However, due to the difference in crystal phase between the polypropylene resin matrix and the dispersed polyolefin elastomer phase, phase separation and a micro-non-uniform structure occur at high temperatures, resulting in reduced high-temperature heat resistance and insulation properties. Consequently, there are limitations to its application as an eco-friendly insulating material for high-voltage cables, which require not only mechanical properties but also high-temperature stability.
[0007] Generally, when polymer materials have a low elastic modulus, there is a high risk that their high-temperature insulation performance will deteriorate and their tensile strength, which corresponds to fracture strength, will be low. Conversely, as the elastic modulus increases, they possess high-temperature insulation performance. Therefore, to control the elastic modulus and high-temperature insulation performance, additives such as inorganic fillers, antioxidants, flame retardants, heat stabilizers, and compatibilizers are sometimes included in polymer materials. However, depending on the type and composition of these additives, shape stability at high temperatures may deteriorate. Accordingly, there is an urgent need to develop technology that simultaneously possesses high flexibility and high-temperature insulation performance through the control of thermoplastic elastomer compositions.
[0008] Accordingly, the inventors of the present invention have completed the present invention by controlling the compositional ratio of a composition comprising two types of polypropylene copolymers and a polyolefin elastomer with different elastic moduli in a thermoplastic polymer composition for voltage cable insulation, thereby developing a thermoplastic polymer composition that has a low elastic modulus but high tensile strength, possessing mechanical flexibility and high strength, while simultaneously having excellent high-temperature insulation properties.
[0009] Accordingly, the present invention aims to provide a thermoplastic polymer insulating composition having a low elastic modulus at room temperature, high tensile strength, and excellent electrical insulation properties at high temperatures, as well as a method for manufacturing the same, as a technical problem.
[0010] To solve the above technical problem, the present invention provides a thermoplastic polymer composition for insulating high-voltage cables having high flexibility and high-temperature insulation, characterized in that the composition comprises a ternary composition comprising 40 to 70 parts by weight of a first polypropylene copolymer; 30 to 60 parts by weight of a polyolefin elastomer; and 1 to 20 parts by weight of a second polypropylene copolymer, wherein the elastic modulus of the first polypropylene copolymer is 500 to 800 MPa, the elastic modulus of the polyolefin elastomer is 100 MPa at most, and the elastic modulus of the second polypropylene copolymer is 100 to 500 MPa, thereby having high flexibility with an elastic modulus of 300 MPa at most, and the second polypropylene copolymer has compatibility with the first polypropylene copolymer and the polyolefin elastomer, thereby strengthening the interface of the ternary system and having high-temperature insulation.
[0011] In the present invention, the composition is characterized by having a high-temperature insulation strength of at least 160 kV / mm.
[0012] In the present invention, the first polypropylene copolymer is characterized by being one or more of a propylene random copolymer, a propylene block copolymer, and a reactor-made thermoplastic olefin (RTPO).
[0013] In the present invention, the polyolefin elastomer is characterized by being manufactured by copolymerizing ethylene with an alpha olefin (α-olefin) having 4 to 20 carbon atoms.
[0014] In the present invention, the second polypropylene copolymer is characterized by being one or more of a propylene random copolymer, a propylene block copolymer, and a reactor-made thermoplastic olefin (RTPO).
[0015] To solve the other technical problems mentioned above, the present invention provides a method for manufacturing a ternary insulating composition, characterized by comprising: a step of preparing a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer; and a step of melt-mixing 40 to 70 parts by weight of the first polypropylene copolymer, 30 to 60 parts by weight of the polyolefin elastomer, and 1 to 20 parts by weight of the second polypropylene copolymer at 180 to 250°C to produce a ternary insulating composition.
[0016] To solve the above-mentioned other technical problem, the present invention provides an insulating material characterized by being formed by coating a conductor with the above composition.
[0017] According to the thermoplastic polymer insulating composition of the present invention as a means for solving the above problem, when a polyolefin elastomer is blended and dispersed in a polypropylene resin matrix, the first and second polypropylene copolymers blended with the polyolefin elastomer have mutually similar molecular structures, thereby increasing the compatibility between the materials compared to the existing polypropylene (homo polypropylene, hPP)-polyolefin elastomer system and reducing interfacial defects; furthermore, there is an effect of appropriately controlling flexibility and strength by controlling the elastic modulus of the first and second polypropylenes.
[0018] Accordingly, compared to existing polypropylene-polyolefin elastomer-based compositions, it maintains a low room-temperature elastic modulus while exhibiting excellent tensile fracture strength and improved electrical insulation properties at high temperatures, thus offering the potential for widespread use in fields requiring insulation properties, such as insulation materials for high-voltage cables.
[0019] FIG. 1 is a graph showing the elastic modulus and tensile fracture strength (Fig. 1A) and high-temperature DC insulation strength (Fig. 1B) according to Test Example 1 (ref: Comparative Example 2, S0: Example 1C, S1: Example 2A, S2: Example 2B, S3: Example 2C).
[0020] FIG. 2 is an SEM image observing the fracture surface of the insulating composition according to Test Example 1 (Fig. 2A: Comparative Example 2, Fig. 2B: Example 2B).
[0021] FIG. 3 is a graph comparing mechanical properties after accelerated degradation according to Test Example 2 (Fig. 3A: Tensile fracture strength at the beginning and after accelerated degradation, Fig. 3B: Comparison of the reduction rate of tensile fracture strength and maximum elongation at the beginning and after accelerated degradation, S0: Example 1C, S1: Example 2A, S2: Example 2B, S3: Example 2C)
[0022] The present invention will be described in detail below.
[0023] In one embodiment, the present invention relates to a thermoplastic polymer composition for insulating high-voltage cables having high flexibility and high-temperature insulation properties, and provides a ternary insulating composition obtained by simultaneously adding a first polypropylene copolymer, a second polypropylene copolymer, and a polyolefin elastomer during the preparation of a thermoplastic polymer by melt blending.
[0024] The ternary insulating composition of the present invention comprises 40 to 70 parts by weight of a first polypropylene copolymer, 30 to 60 parts by weight of a polyolefin elastomer, and 1 to 20 parts by weight of a second polypropylene copolymer, wherein the room temperature elastic modulus of the first polypropylene copolymer is 500 to 800 MPa, the room temperature elastic modulus of the polyolefin elastomer is at most 100 MPa, and the room temperature elastic modulus of the second polypropylene copolymer is 100 to 500 MPa.
[0025] In the present invention, the first polypropylene copolymer forms the matrix of the ternary insulating composition, and one or more of a polypropylene-based propylene random copolymer, a propylene block copolymer, and a reactor-made thermoplastic olefin (RTPO) may be selected. Specifically, the first polypropylene copolymer is characterized as a copolymer based on propylene that includes ethylene, butylene, or octene, and has a room temperature elastic modulus of 500 to 800 MPa.
[0026] The above-mentioned first polypropylene copolymer is a material forming the matrix of the insulating composition and is a copolymer containing a small amount of flexible monomer compared to pure polypropylene; it plays a role in stabilizing the elastomer core interface formed when subsequently blended with a polyolefin elastomer, thereby having the effect of obtaining high tensile fracture strength even at a low elastic modulus.
[0027] When the elastic modulus of the first polypropylene copolymer is greater than 800 MPa, it is difficult to reduce the vulnerability to brittleness, and because the content of the flexible monomer is low, the role of stabilizing the elastic core as described above is minimal, and thus the role of increasing tensile fracture strength is minimal. On the other hand, when the elastic modulus is 500 MPa or less, the vulnerability to brittleness can be reduced and the tensile fracture strength can be further increased, but the high-temperature insulation strength may decrease, so it is desirable to make the room temperature elastic modulus 500 to 800 MPa.
[0028] If the first polypropylene copolymer is added in an amount of less than 40 parts by weight, mechanical flexibility may increase, but high-temperature insulation performance is reduced, making it unsuitable for use as an insulating material for a high-voltage cable insulation layer. On the other hand, if the first polypropylene copolymer exceeds 70 parts by weight, flexibility cannot be imparted to the insulating material, which has the disadvantage that failure due to bending of the cable may occur. Accordingly, it is desirable to include the first polypropylene copolymer in an amount of 40 to 70 parts by weight to form the matrix of the ternary insulating composition, thereby securing high-temperature insulation performance while reducing vulnerability to brittleness and securing tensile fracture strength.
[0029] In the present invention, the polyolefin elastomer (POE) is derived from a polyolefin structure and has rubbery properties, and can form an elastomer core dispersion phase on a polypropylene copolymer matrix.
[0030] Polyolefin elastomers can be prepared by copolymerizing ethylene having 2 carbon atoms with alpha-olefins having 4 to 20 carbon atoms, and may be polyethylene-based copolymers such as ethylene-butene copolymer and ethylene-octene copolymer, or ethylene-propylene-based copolymers such as ethylene-propylene rubber (EPR) and ethylene-propylene diene monomer (EPDM). Additionally, styrene-ethylene-styrene copolymer (SBS) or styrene-ethylene-butadiene-styrene copolymer (SEBS) may be used.
[0031] In the case of a polyolefin elastomer, it is characterized by having a room temperature elastic modulus of 100 MPa or less to compensate for the brittleness of the insulating composition and to impart flexibility. Since a room temperature elastic modulus exceeding 100 MPa prevents the first polypropylene copolymer, which is the main matrix resin, from becoming flexible, it is preferable that the elastic modulus of the polyolefin elastomer be 100 MPa or less.
[0032] Polyolefin elastomers with an elastic modulus of 100 MPa or less may be included in a range of 30 to 60 parts by weight. At this time, if the polyolefin elastomer is less than 30 parts by weight, even if the polyolefin elastomer is dispersed on a matrix made of a first polypropylene copolymer, there is a disadvantage of having a high elastic modulus and insufficient flexibility. If it exceeds 60 parts by weight, high-temperature insulation performance may be reduced due to the inclusion of an excessive amount of polyolefin elastomers with relatively low heat resistance. Additionally, since the polyolefin elastomer does not form a dispersed phase but becomes a continuous phase and is exposed to the outer surface, it may cause a deterioration of properties such as external mechanical friction, and thus it is not desirable to use it as a cable insulation material.
[0033] In particular, when a ternary insulating composition is used as an insulating material, a low elastic modulus of 300 MPa or less is required to prevent failure due to bending, taking into account the bending of cables. As the first polypropylene copolymer is included in an amount of 40 to 70 parts by weight and the polyolefin elastomer is dispersed in an amount of 30 to 60 parts by weight, the elastic modulus of the final insulating composition can be controlled to 300 MPa or less. Accordingly, the polyolefin elastomer can maintain a structure in the form of an elastic core within the matrix rather than a continuous phase, and due to the compatibility between the first polypropylene copolymer and the polyolefin elastomer, excellent tensile fracture strength and high-temperature electrical insulation properties can be maintained.
[0034] In the present invention, the second polypropylene copolymer is a material that serves as an interface reinforcing agent for a ternary insulating composition, and one or more of a polypropylene-based propylene random copolymer, a propylene block copolymer, and a reactor-made thermoplastic olefin (RTPO) may be selected. Specifically, the second polypropylene copolymer is characterized as a copolymer based on propylene containing ethylene, butylene, or octene, and having a room temperature elastic modulus of 100 to 500 MPa.
[0035] The second polypropylene copolymer has increased compatibility due to its chemical structure being similar to that of the first propylene copolymer, which is the matrix material. Additionally, because the copolymer monomer ratio is relatively higher than that of the first polypropylene copolymer, it can have some degree of compatibility with polyolefin elastomers. Overall, this allows it to play a role in stabilizing the interface of the ternary composition, thereby enabling further improvement in mechanical and electrical properties. In particular, the present invention has the advantage of achieving improved insulation strength and increased mechanical stability at high temperatures. In this regard, according to one embodiment of the present invention, it can be confirmed that changes in mechanical properties are reduced even after accelerated degradation at high temperatures (accelerated degradation in an oven at 150°C for 240 hours) (see Fig. 3). That is, when the second polypropylene copolymer is not included, the decrease in tensile fracture strength and maximum strain after accelerated degradation at high temperatures is close to 50%, whereas when the second polypropylene copolymer is included, the decrease in tensile fracture strength and maximum strain can each be up to 30%. This is because the addition of the second polypropylene copolymer can reduce interfacial defects between the first polypropylene copolymer and the polyolefin elastomer, thereby improving the high-temperature thermal stability of the composition.
[0036] At this time, if the elastic modulus of the second polypropylene copolymer is less than 100 MPa, it becomes similar to the elastic modulus of the polyolefin elastomer, so while there may be an effect of increasing mechanical flexibility, it results in a deterioration of electrical insulation properties at high temperatures. On the other hand, if the elastic modulus of the second polypropylene copolymer exceeds 500 MPa, it approaches the elastic modulus range of the first polypropylene copolymer, which reduces mechanical flexibility and makes it difficult to compensate for the brittleness of the insulation composition; therefore, it is desirable to make the room temperature elastic modulus 100 to 500 MPa.
[0037] The second polypropylene copolymer can be added in a range of 1 to 20 parts by weight. If mixed in less than 1 part by weight, it is an insufficient amount for controlling the mechanical properties of the insulating composition and improving high-temperature insulation, and if it exceeds 20 parts by weight, the amount existing in the bulk phase other than the interface between the first polypropylene copolymer matrix and the polyolefin elastomer dispersed phase becomes excessive, making it difficult to obtain improvements in electrical and mechanical properties through interface reinforcement.
[0038] Accordingly, the elastic modulus of the second polypropylene copolymer has a value between that of the first polypropylene copolymer and the polyolefin elastomer, and by including it in the ternary insulating composition in an amount of 1 to 20 parts by weight, it can not only play a role in controlling the mechanical flexibility of the ternary composition but also reduce interfacial defects due to a similar chemical structure, thereby improving additional electrical insulation properties.
[0039] In another aspect, the present invention relates to a method for manufacturing a thermoplastic polymer insulating composition having high insulation properties, high flexibility, and high strength, comprising the steps of: preparing a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer (S10); and melt-mixing 40 to 70 parts by weight of the first polypropylene copolymer, 30 to 60 parts by weight of the polyolefin elastomer, and 1 to 20 parts by weight of the second polypropylene copolymer at 180 to 250°C to produce a ternary insulating composition (S20).
[0040] According to the above-described manufacturing method, first, a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer are prepared (S10).
[0041] Each material prepared here may be a particle of 10 mm or less, and the first polypropylene copolymer, polyolefin elastomer, and first polypropylene copolymer are described above, so a description here will be omitted.
[0042] Next, a ternary insulating composition is prepared by melt-blending 40 to 70 parts by weight of a first polypropylene copolymer, 30 to 60 parts by weight of a polyolefin elastomer, and 1 to 20 parts by weight of a second polypropylene copolymer at 180 to 250°C (S20).
[0043] Generally, when polypropylene resin and polyolefin elastomer are melt-mixed, phase separation occurs, and the polyolefin elastomer forms a dispersed phase within the polypropylene resin matrix. However, as in the present invention, by using two types of polypropylene copolymers having different elastic moduli, the flexible monomers within the two types of polypropylene copolymers stabilize the interface with the polyolefin elastomer, thereby creating a finer dispersed elastomer phase, which can improve ternary mechanical and electrical properties.
[0044] In this case, melt mixing can be applied in various ways, such as internal mixers, extrusion, and injection molding, as long as the method is used in the process of molding thermoplastic polymers. Although melt mixing is usually determined by the melting point of the thermoplastic resin, it can be performed in a preheated state at a temperature of 160°C or higher, which is the melting point of polypropylene-based polymers, i.e., in the range of 180 to 250°C. If the temperature during melt mixing is below 180°C, the polypropylene copolymer does not melt sufficiently, making it difficult to expect uniform dispersion of the blend composition. On the other hand, if the temperature during melt mixing exceeds 250°C, degradation of each material may occur, which leads to a decrease in the physical properties of the final composition; therefore, it is desirable to perform the process at 250°C or lower.
[0045] In the process of simultaneously melt-mixing 40 to 70 parts by weight of the first polypropylene copolymer, 30 to 60 parts by weight of the polyolefin elastomer, and 1 to 20 parts by weight of the second polypropylene copolymer, an antioxidant may be added for the purpose of preventing thermal oxidation at high temperatures, and as long as the antioxidant is one that can be used in the melt-mixing process, it may be used in various ways within a range that does not impair the physical properties of the ternary insulating composition of the present invention.
[0046] The ternary insulating composition of a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer, manufactured by the method described above, utilizes the first polypropylene copolymer instead of the conventionally used polypropylene resin as a matrix material, uses the second polypropylene copolymer to enhance compatibility with the polyolefin elastomer, and controls the elastic modulus of each material to the range described above. This allows for the expression of effects that include high flexibility, high tensile fracture strength, and excellent high-temperature insulation. Therefore, it has the advantage of being usable as an insulating material in various electrical and electronic fields, including materials for high-voltage cable insulation.
[0047] In another aspect, the present invention relates to an insulating material and is characterized by providing an insulating material manufactured from an insulating composition manufactured according to the method described above.
[0048] Preferably, as described above, the highly flexible and high-temperature insulating thermoplastic polymer composition according to the present invention can be utilized as an insulating material for forming an insulating layer that surrounds the conductor of a wire-shaped power cable, or as an insulating material for various electrical and electronic fields.
[0049] The embodiments of the present invention will be described in more detail below. However, the following embodiments are provided merely to aid in understanding the present invention and do not limit the scope of the present invention.
[0050] <Example 1> A binary insulating composition comprising a first polypropylene copolymer and a polyolefin elastomer
[0051] In Example 1, a binary insulating composition was prepared using a propylene-ethylene copolymer (PPC-1) as the first component as the first polypropylene copolymer forming the matrix material, and an ethylene-octene copolymer (EOC) as the second component as the polyolefin elastomer. As shown in Table 2, the binary insulating composition was prepared by melt blending 40 to 70 parts by weight of the first propylene copolymer and 30 to 60 parts by weight of the polyolefin elastomer using an internal mixer at 200°C for 10 minutes at 60 rpm. Subsequently, a specimen was prepared by pressing with a hot press at 200°C for 10 minutes and then cooling at 10°C.
[0052] <Example 2> Ternary insulating composition comprising a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer
[0053] In Example 2, a ternary insulating composition was prepared in which a propylene-ethylene copolymer (PPC-1) was used as the first component as the first polypropylene copolymer forming the matrix material, an ethylene-octene copolymer (EOC) was used as the second component as the polyolefin elastomer, and a propylene-ethylene copolymer (PPC-2) was used as the third component as the second propylene copolymer. The composition was designed to observe the effect of the content of the second propylene copolymer, the third component, while maintaining the ratio of the first component to the second component at approximately 60:40, as shown in Table 3. The following specimens were prepared using an internal mixer and a press in the same process as in Example 1.
[0054] <Example 3> Ternary insulating composition comprising a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer
[0055] In Comparative Example 1, a ternary insulating composition was prepared using propylene-ethylene copolymer (PPC-1) as the first component, ethylene-octene copolymer (EOC) as the second component, and RTPO (PPC-3), a reactive PP-EPR (ethylene-propylene rubber) copolymer, as the third component, as the first component, which is the first polypropylene copolymer forming the matrix material. The composition was designed to observe the effect of the RTPO content as the third component while maintaining the ratio of the first component to the second component at approximately 60:40, as shown in Table 4. The following specimens were prepared using the same process as in Example 1.
[0056] <Comparative Example> Two-component and ternary insulating compositions composed of pure polypropylene-polyolefin elastomers
[0057] In the comparative example, a binary insulating composition was prepared using pure polypropylene (homo PP) instead of polypropylene copolymer as the first component material forming the matrix material, and a polyolefin elastomer as the second component. In comparative examples 2 and 3, a ternary insulating composition was prepared using pure polypropylene as the first component material, a polyolefin elastomer as the second component material, and a polypropylene copolymer (PPC-3, RTPO) as the third component material, in order to compare the physical properties with those of the above example.
[0058] <Test Example 1>
[0059] In this test example, the mechanical and electrical properties of specimens prepared according to the methods of the above examples and comparative examples were analyzed.
[0060] That is, the mechanical properties of the specimens prepared according to the method described above were measured in tensile mode using a universal testing machine (UTM) in accordance with IEC 60811-1, and the modulus, tensile strength, and ultimate elongation were analyzed through the stress-strain curve obtained while stretching the dumbbell-shaped specimens. Each measurement was taken for at least five specimens, and the average value was calculated.
[0061] In addition, the high-temperature electrical insulation properties of the specimens prepared according to the above method were measured in accordance with IEC 60243-1. The specimens were placed between stainless steel balls (diameter 25 mm) in silicone oil insulating oil heated to 110°C in a bath, and a voltage of 2.0 kV / s was applied. The maximum voltage at the point where the specimen finally broke and leakage current occurred was measured, and the high-temperature insulation strength (kV / mm) was analyzed by dividing this value by the specimen thickness. Each measurement was taken for at least 8 specimens, and the scale parameter obtained through the Weibull plot was compared and analyzed as the average value.
[0062] First, the mechanical properties of the raw materials used in the present invention are shown in Table 1 below.
[0063] Raw Material Tensile Test Elastic Modulus (MPa) Strength (MPa) Maximum Strain (%) PPC-1 Polypropylene Copolymer (propylene-ethylene random copolymer) 6 14 37.0 100 2 PPC-2 Polypropylene Copolymer (propylene-ethylene random copolymer) 30 226.4 3 PPC-3 Polypropylene Copolymer (PP-EPR RTPO) 42 91 2.3 8 7 POE Polyolefin Elastomer (ethylene-octene copolymer, EOC) 5.8 25.6 11 2 hPP Homo Polypropylene (isotactic PP, iPP) 95 325 60
[0064] That is, a polypropylene copolymer PPC-1 having an elastic modulus of 614 MPa was used as the first component material (a polypropylene copolymer with an elastic modulus of 500 to 800 MPa) which is the matrix component of the present invention, a polyolefin (POE) which is an ethylene-octene copolymer material was used as the second material forming the rubber dispersion phase, and polypropylene copolymers PPC-2 (302 MPa) and PPC-3 (429 MPa) having elastic modulus of 100 to 500 MPa were used as the third component materials as interface reinforcing agents. In addition, the effect on the first component material was also to be compared by using pure polypropylene (hPP, elastic modulus of 950 MPa) as the first component material.
[0065]
[0066] First, referring to Table 2 which shows the properties of the first polypropylene copolymer-polyolefin elastomer binary insulating composition prepared in Example 1, it can be seen that the elastic modulus decreases as the ratio of the first polypropylene copolymer decreases and the ratio of the polyolefin elastomer increases.
[0067] Classification Composition Tensile Test High-Temperature Insulation Test Component 1 (PPC-1) Component 2 (EOC) Component 3 Elastic Modulus (MPa) Tensile Breakdown Strength (MPa) Maximum Strain (%) DC Dielectric Breakdown Strength (110℃) Example 1A 40 60-86.4 37.2 129 224.5 Example 1B 50 50-14 63.1 124 584.7 Example 1C 60 40-23 73.7 1229 137.0 Example 1D 70 30-27 229.0 101 8117.1
[0068] However, it can be confirmed that when the polyolefin elastomer content is higher than approximately 50 parts by weight, the high-temperature insulation performance is significantly reduced. Therefore, it was confirmed that for the material used in the present invention, the appropriate condition to satisfy mechanical flexibility at room temperature and high-temperature insulation performance is a ratio of the first propylene copolymer to the polyolefin elastomer in the range of 60:40.
[0069] Based on the results of Example 1 above, the results obtained by maintaining the ratio of the first polypropylene copolymer to the polyolefin elastomer at 60:40 and using polypropylene-ethylene copolymer PPC-2 as the third component material as the second polypropylene copolymer material are shown in Table 3 below.
[0070] Classification Composition Tensile Test High-Temperature Insulation Test Component 1 (PPC-1) Component 2 (EOC) Component 3 (PPC-2) Elastic Modulus (MPa) Tensile Breakdown Strength (MPa) Maximum Strain (%) DC Dielectric Breakdown Strength (110℃) Example 1 C 6040-23736.71229137.0 Example 2A 59.739.80.525335.31101153.6 Example 2B 59.439.61.025836.11134165.8 Example 2C 57.138.14.824237.21182170.7
[0071] As shown in Table 3 above, when the second polypropylene copolymer, which is the third component material, is added, it can be seen that the high-temperature insulation performance is significantly increased while maintaining flexibility with the elastic modulus still being 300 MPa or less.
[0072] Next, the results obtained when RTPO was added as the third component second polypropylene copolymer material are shown in Table 4 below.
[0073] Classification Composition Tensile Test High-Temperature Insulation Test Component 1 (PPC-1) Component 2 (EOC) Component 3 (PPC-3) Elastic Modulus (MPa) Tensile Breakdown Strength (MPa) Maximum Strain (%) DC Dielectric Breakdown Strength (110℃) Example 1 C 6040-23736.71229137.0 Example 3A 59.739.80.522328.51044125.4 Example 3B 59.439.61.024428.01196135.7 Example 3C 57.138.14.823625.3984158.4
[0074] As shown in the table above, although the addition of RTPO resulted in some increase in high-temperature insulation, the overall tensile fracture strength was significantly reduced. In other words, in the present invention, it was confirmed that PPC-2, a polypropylene-ethylene copolymer, is more effective in maintaining mechanical properties and improving high-temperature insulation than RTPO, which is a reactive PP-EPR copolymer, as the third component material.
[0075] Next, in order to further compare the role of the first polypropylene copolymer, which is the first matrix component, an insulating composition was prepared using pure polypropylene (hPP) instead of the first polypropylene copolymer, and the results obtained are shown in Table 5 below.
[0076] Classification Composition Tensile Test (25 mm / min) High Temperature Insulation Test Component 1 (hPP) Component 2 (EOC) Component 3 (PPC-2) Elastic Modulus (MPa) Strength (MPa) Maximum Strain (%) DC Dielectric Breakdown Strength (110℃) Comparative Example 1 40 600 44 26.3 100 3- Comparative Example 2 40 50 10 27 7 23.8 100 130.4 Comparative Example 3 50 30 20 5 22 17.9 40 6-
[0077] As shown in Table 5 above, when pure hPP is used as the first matrix material, the elastic modulus of hPP itself (950 MPa) is greater than that of PPC-1 (614 MPa). Therefore, in order for the elastic modulus of the final blending composition to be at a level similar to ~300 MPa, a larger amount of polyolefin elastomer is required. As shown in the table above, the ratio of the first component (hPP): second component (POE): third component (PPC-2) is around 40:50:10, and the elastic modulus exhibited characteristics similar to those of Example 2 and Comparative Example 1.
[0078] Looking at the results of Comparative Example 2 in Table 5 and the Example in Table 3, and the graph in Fig. 1 summarizing them, first, when the first component matrix material is a first polypropylene copolymer (PPC-1) instead of pure polypropylene, the elastic modulus is maintained similarly, but the tensile fracture strength is significantly increased (Fig. 1A), and second, when the second polypropylene copolymer (PPC-2) is used as the third component interfacial reinforcing material, it can be confirmed that there is an additional effect of significantly increasing high-temperature insulation (Fig. 1B).
[0079] Figure 2 shows SEM images observing representative specimen fracture surfaces for the comparative example and the example. It can be seen that compared to Comparative Example 2 (Figure 2A), which is a pure polypropylene-based insulating composition, the polyolefin elastomer dispersed phase core in the polypropylene copolymer-based composition (Figure 2B, Example 2B) appears much smaller and more uniform. Generally, it is known that in different polymer blends, the better the compatibility between them, the smaller the dispersed phase appears. In the present invention, the excellent mechanical and electrical properties shown in the example using a polypropylene copolymer can also be explained as being related to this small and uniform dispersed phase.
[0080] <Test Example 2>
[0081] In this test example, to evaluate the additional high-temperature mechanical stability of the specimens, the specimens prepared in Example 1C and Example 2 were subjected to accelerated aging in an oven at 150°C for 240 hours, removed, and their mechanical properties were measured again. After accelerated aging, the specimens were analyzed for elastic modulus, tensile fracture strength, and maximum elongation using a UTM in the same manner as described in Test Example 1.
[0082] Classification Composition Decrease from Initial Tensile Test Value Component 1 (PPC-1) Component 2 (EOC) Component 3 (PPC-2) Elastic Modulus (MPa) Tensile Breaking Strength (MPa) Maximum Strain (%) Tensile Breaking Strength (%) Maximum Strain (%) Example 1 C 60 40-290 19.365 447.446.8 Example 2 A 59.73 9.80.53 323 0.49 48 13.913.9 Example 2 B 59.43 9.61.03 0426.88 7725.822.7 Example 2 C 57.13 8.14.83 0726.68 7828.525.7
[0083] Referring to Table 6 and Figures 3A and 3B, which show mechanical properties after accelerated degradation, it can be seen that the range of change in mechanical properties after accelerated degradation at high temperatures is significantly reduced as a third component material is added. Specifically, in the case of Example 1C, the reduction range of tensile fracture strength and maximum strain was 47.4% and 46.8%, respectively; however, Examples 2A, 2B, and 2C, in which 0.5, 1.0, and 4.8 parts by weight of the second polypropylene copolymer, which is the third component, were added, showed a maximum reduction range of 30% in tensile fracture strength and maximum strain after accelerated degradation at high temperatures. This means that the addition of the third component can improve the high-temperature thermal stability of the composition by reducing interfacial defects between the first and second components.
[0084] From the results of the examples and test examples described above, the ternary insulating composition of the present invention, composed of a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer, has the advantage of simultaneously achieving high flexibility and high strength by maintaining a similar elastic modulus and mechanical flexibility compared to a conventional polypropylene-polyolefin elastomer-based insulating composition, while significantly increasing the tensile fracture strength. Furthermore, the second propylene copolymer provides the effect of simultaneously improving high-temperature insulation and mechanical stability at high temperatures.
[0085] Due to these characteristics of high flexibility, high strength, and high-temperature insulation, it is expected to be actively utilized in various industrial fields, including as an insulating material coated on cables.
[0086] The foregoing description is merely an illustrative explanation of the technical concept of the present invention, and those skilled in the art to which the present invention pertains will be able to make various modifications and variations within the scope of the essential characteristics of the present invention. Accordingly, the embodiments disclosed in the present invention are intended to explain, not to limit, the technical concept of the present invention, and the scope of the technical concept of the present invention is not limited by such embodiments. The scope of protection of the present invention shall be interpreted by the claims, and all technical concepts within an equivalent scope shall be interpreted as being included within the scope of rights of the present invention.
Claims
1. 40 to 70 parts by weight of the first polypropylene copolymer; 30 to 60 parts by weight of a polyolefin elastomer; and A ternary composition comprising 1 to 20 parts by weight of a second polypropylene copolymer; and The elastic modulus of the first polypropylene copolymer is 500 to 800 MPa, the elastic modulus of the polyolefin elastomer is up to 100 MPa, and the elastic modulus of the second polypropylene copolymer is 100 to 500 MPa, thereby having high flexibility with an elastic modulus of up to 300 MPa of the composition. Characterized by the fact that the second polypropylene copolymer has compatibility with the first polypropylene copolymer and the polyolefin elastomer, thereby strengthening the interface of the ternary system and having high-temperature insulation properties. Thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties.
2. In Paragraph 1, A thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties, characterized by having a high-temperature insulation strength of at least 160 kV / mm.
3. In Paragraph 1, A thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties, characterized in that the first polypropylene copolymer is one or more of a propylene random copolymer, a propylene block copolymer, and a reactor-made thermoplastic olefin (RTPO).
4. In Paragraph 1, A thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties, characterized in that the above polyolefin elastomer is manufactured by copolymerizing ethylene with an alpha olefin (α-olefin) having 4 to 20 carbon atoms.
5. In Paragraph 1, A thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties, characterized in that the second polypropylene copolymer is one or more of a propylene random copolymer, a propylene block copolymer, and a reactor-made thermoplastic olefin (RTPO).
6. A step of preparing a first polypropylene copolymer, a polyolefin elastomer, and a second polypropylene copolymer; The method comprises the step of preparing a ternary insulating composition by melt-mixing 40 to 70 parts by weight of the first polypropylene copolymer, 30 to 60 parts by weight of the polyolefin elastomer, and 1 to 20 parts by weight of the second polypropylene copolymer at 180 to 250°C. A method for manufacturing a thermoplastic polymer composition for high-voltage cable insulation having high flexibility and high-temperature insulation properties, characterized in that the above ternary insulating composition is a composition according to any one of claims 1 to 5.
7. An insulating material characterized by being formed by coating a conductor with a composition according to any one of claims 1 to 5.