Positive electrode active material for lithium secondary battery, method for preparing same, positive electrode including same, and lithium secondary battery including same
A lithium secondary battery with a controlled nickel ratio in the positive electrode active material addresses surface residual lithium issues, enhancing capacity and retention rates through controlled manufacturing processes.
Patent Information
- Application Number
- PCT/KR2026/001631
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-01-28
- Publication Date
- 2026-11-12
AI Technical Summary
Existing lithium secondary battery cathode active materials with high nickel content face issues of residual lithium on the surface, leading to reactions with the electrolyte and decreased capacity and capacity retention rates due to cleaning and coating processes.
A positive electrode active material with a nickel content of 70-98 mol% and a controlled nickel ratio of 0.05 < [Ni (0nm)]/[Ni (50nm)] < 0.3, achieved through stepwise heat treatment and controlled mixing, cleaning, and coating processes, is developed.
The solution provides a lithium secondary battery with high capacity and excellent capacity retention rate by minimizing surface residual lithium effects.
Smart Images

Figure KR2026001631_12112026_PF_FP_ABST
Abstract
Description
A positive electrode active material for a lithium secondary battery, a method for manufacturing the same, a positive electrode including the same, and a lithium secondary battery including the same
[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for manufacturing the same, a positive electrode including the same, and a lithium secondary battery including the same. More specifically, the invention relates to a positive electrode active material for a lithium secondary battery with excellent capacity and capacity retention rate, a method for manufacturing the same, a positive electrode including the same, and a lithium secondary battery including the same, which improves the problem of residual lithium on the surface of the positive electrode active material by controlling the ratio of nickel content on the surface of the positive electrode active material and at a position 50 nm from the surface into the interior.
[0002] Various cathode active materials are used in lithium secondary batteries applied in fields such as electric vehicles (EVs) and energy storage systems (ESS). Among these cathode active materials for lithium secondary batteries, lithium composite metal oxides containing nickel as a main component and one or more components from cobalt, manganese, and aluminum are widely used as cathode active materials.
[0003] When the nickel content is increased to increase the capacity of the cathode active material, a larger amount of residual lithium forms on the surface of the cathode active material, and this residual lithium causes various problems, such as reactions with the electrolyte in the battery.
[0004] Although cleaning and coating processes are applied to resolve the aforementioned problems caused by residual lithium, the cleaning process removes not only residual lithium on the surface of the cathode active material but also lithium present within the cathode active material, which may lead to a decrease in battery capacity. In the coating process, while the coating material is effective in suppressing the reactivity of residual lithium on the surface of the cathode active material, the reduction in relative nickel content and increased resistance to lithium ion movement caused by the coating material may result in a decrease in battery capacity and capacity retention rate.
[0005] Therefore, there is a need to develop cathode active materials with excellent capacity and capacity retention rates that address the problem caused by residual lithium on the surface of the cathode active material.
[0006] (Prior Art Literature)
[0007] (Patent Document 1) Published Patent Application No. 10-2019-0142156 (December 26, 2019)
[0008] (Patent Document 2) Published Patent Application No. 10-2019-0142147 (December 26, 2019)
[0009] The problem that the present invention aims to solve is to provide a positive electrode active material for a lithium secondary battery having high capacity and excellent capacity retention rate, a method for manufacturing the same, a positive electrode including the same, and a lithium secondary battery including the same.
[0010] A first aspect of the present invention for solving the above problem provides a positive electrode active material for a lithium secondary battery. The positive electrode active material has a nickel content of more than 70 mol% and less than 98 mol% among the remaining components excluding lithium and oxygen, and satisfies the following mathematical formula 1.
[0011] [Mathematical Formula 1] 0.05 < [Ni (0nm) ] / [Ni (50nm) ] < 0.3.
[0012] Here, [Ni (0nm) ] is the atomic percent (at%) of nickel among the remaining components excluding oxygen on the surface of the cathode active material, and [Ni (50nm) ] is the atomic percentage of nickel among the remaining components excluding oxygen at 50 nm from the surface of the positive active material to the interior.
[0013] In one embodiment, Ni (0nm) It may be greater than 2.0 at% and less than 10.0 at%.
[0014] In one embodiment, the nickel content may be greater than 80 mol% and less than 98 mol%.
[0015] In one embodiment, the nickel content may be greater than 90 mol% and less than 98 mol%.
[0016] In one embodiment, the positive electrode active material may include a lithium complex transition metal oxide having nickel as a main component and containing one or more components among cobalt, manganese, and aluminum.
[0017] A second aspect of the present invention provides a method for manufacturing a positive electrode active material for a lithium secondary battery. The method may be a method for manufacturing a positive electrode active material for a lithium secondary battery comprising the steps of: a) manufacturing a primary positive electrode active material by first heat treating a material containing a precursor for the positive electrode active material; and b) manufacturing a secondary positive electrode active material by second heat treating a material containing the primary positive electrode active material.
[0018] In one embodiment, after step b), c) optionally, a step of preparing a third positive active material by heat-treating a material containing a second positive active material may be further included.
[0019] A third aspect of the present invention may provide a positive electrode for a lithium secondary battery comprising the positive electrode active material of the first aspect.
[0020] A fourth aspect of the present invention may provide a lithium secondary battery comprising a positive electrode of the third aspect.
[0021] According to embodiments of the present invention, by controlling the ratio of nickel content at 50 nm from the surface of the positive active material to the interior, a positive active material for a lithium secondary battery with high capacity and excellent capacity retention rate can be provided, which improves the problem of residual lithium on the surface of the positive active material.
[0022] In addition, a method for manufacturing a positive electrode active material for a lithium secondary battery can be provided, wherein the ratio of nickel content at the surface of the positive electrode active material and from the surface to the interior at 50 nm is controlled through stepwise heat treatment.
[0023] In addition, a positive electrode for a lithium secondary battery comprising the above-mentioned positive electrode active material can be provided.
[0024] In addition, a lithium secondary battery with high capacity and excellent capacity retention rate including the above-mentioned positive electrode can be provided.
[0025] Figure 1 is a graph of the XPS analysis results for the cathode active materials of Example 1-1 to Comparative Example 1-2.
[0026] Figure 2 is a graph of the XPS analysis results for the cathode active materials of Examples 4-1 to Comparative Examples 4-2.
[0027] FIG. 3 shows the [Ni of the examples and comparative examples. (0nm) ] / [Ni (50nm) This is a graph showing the correlation between ] and discharge capacity (mAh / g, @100cycle).
[0028] Preferred embodiments of the present invention will be described below with reference to the attached drawings. Embodiments of the present invention may be modified in various different forms, and the scope of the present invention is not limited to the embodiments described below. Embodiments of the present invention are provided to more fully explain the present invention to those with average knowledge in the art. Accordingly, the shapes and sizes of elements in the drawings may be exaggerated for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements. In the present invention, the expressions "first" or "second" do not imply order or importance, but are merely for distinguishing components.
[0029] A first aspect of the present invention for solving the above problem provides a positive electrode active material for a lithium secondary battery. The positive electrode active material has a nickel content of more than 70 mol% and less than 98 mol% among the remaining components excluding lithium and oxygen, and satisfies the following mathematical formula 1.
[0030] [Mathematical Formula 1] 0.05 < [Ni (0nm) ] / [Ni (50nm) ] < 0.3.
[0031] Here, [Ni (0nm) ] is the atomic percentage of nickel on the surface of the positive electrode active material, and [Ni (50nm) ] is the atomic percentage of nickel at 50 nm from the surface of the positive active material into the interior.
[0032] The atomic percentage of nickel can be expressed based on the remaining components (main component, lithium, doping component, coating component, and other additive materials) excluding oxygen in the cathode active material composition.
[0033] The positive electrode active material of this aspect may be a lithium composite metal oxide having nickel as a main component and containing one or more components among cobalt, manganese, and aluminum.
[0034] The positive electrode active material may have a nickel content of more than 70 mol% and less than 98 mol% among the remaining components excluding lithium and oxygen. In other words, among the remaining components excluding lithium and oxygen, the nickel content may be more than 70 mol% and less than 98 mol% among the total components including the main component (e.g., one or more components among nickel, cobalt, manganese, and aluminum), the doping material, the coating material, and other additive materials.
[0035] Furthermore, for a higher capacity in the cathode active material, preferably the nickel content may be greater than 80 mol% and less than 98 mol%, and more preferably the nickel content may be greater than 90 mol% and less than 98 mol%.
[0036] Nickel content at 50 nm on the surface and inside the cathode active material
[0037] In this specification, the term "positive active material surface" refers to a single-crystal or polycrystalline lithium composite metal oxide surface having a layered structure; if there are no other components on the surface, it refers to the surface itself; if residual lithium is present on the surface, it refers to the surface containing residual lithium; and if a coating material is present on the surface, it refers to the surface containing the coating material.
[0038] The nickel content on the surface of the positive electrode active material and from the surface to the interior at 50 nm may be an atomic percentage measured using XPS (X-ray Photoelectron Spectroscopy) analysis.
[0039] In addition, 50 nm from the surface of the positive active material to the interior refers to a point 50 nm away from the surface of the positive active material in the interior direction, and the nickel content at this location may be an atomic percentage measured using XPS analysis after etching from the surface of the positive active material to 50 nm inward using an ion beam.
[0040] In addition, considering that the detection area depth of XPS analysis is several nm, the nickel content at the surface of the positive active material and at 50 nm from the surface into the interior as described in the present invention may be the average content of nickel existing up to a depth of several nm in the interior at the surface of the positive active material and at 50 nm from the surface into the interior, respectively.
[0041] In addition, considering the detection area of the XPS analysis, the nickel content at the surface of the positive active material and at 50 nm from the surface into the interior as described in the present invention may be the average nickel content in numerous positive active materials, rather than in a single positive active material.
[0042] In addition, 50 nm from the surface of the positive electrode active material into the interior can be an etching reference by the ion beam of XPS analysis.
[0043] [Ni (0nm) ] / [Ni (50nm) Key factors affecting ]
[0044] In mathematical formula 1, [Ni (0nm) ] / [Ni (50nm) That ] is greater than 0.05 and less than 0.3 indicates that the atomic percentage of nickel on the surface of the positive active material is small compared to the atomic percentage of nickel at 50 nm from the surface to the interior of the positive active material.
[0045] Such Ni (0nm) / Ni (50nm)The major factors affecting it may be the following cases.
[0046] 1) Mixing conditions of lithium compound relative to precursor in the primary cathode active material manufacturing process,
[0047] 2) Cleaning conditions in the primary cathode active material manufacturing process,
[0048] 3) Mixing conditions of the coating material relative to the primary cathode active material in the manufacturing process of the secondary cathode active material (or tertiary cathode active material if necessary),
[0049] 4) Heat treatment conditions in the manufacturing process of secondary cathode active material (tertiary cathode active material if necessary)
[0050] To explain 4) above in more detail, during the heat treatment process of manufacturing the secondary cathode active material (or tertiary cathode active material if necessary), residual lithium and surface coating materials present on the surface of the cathode active material penetrate from the surface into the interior. The degree of penetration varies depending on the heat treatment conditions, and consequently, [Ni (0nm) ] / [Ni (50nm) ] may be affected.
[0051] In summary, [Ni (0nm) ] / [Ni (50nm) By controlling the major factors of 1) to 4) above that can affect ] [Ni (0nm) ] / [Ni (50nm) The main content of the present invention is to manufacture a positive electrode active material such that ] is greater than 0.05 and less than 0.3.
[0052] Detailed explanation of Mathematical Formula 1
[0053] [Mathematical Formula 1] 0.05 < [Ni (0nm) ] / [Ni (50nm) ] < 0.3.
[0054] [Ni (0nm) ] / [Ni (50nm)When ] is greater than 0.05 and less than 0.3, a cathode active material for a secondary battery with high capacity and excellent capacity retention rate can be provided, which improves the problem caused by residual lithium.
[0055] In mathematical formula 1, [Ni (0nm) ] / [Ni (50nm) The tendency for ] to become smaller is,
[0056] ① If the mixing ratio of the lithium compound relative to the precursor in the primary cathode active material manufacturing process is excessive compared to the appropriate level,
[0057] ② If the cleaning of the cathode active material in the primary cathode active material manufacturing process is insufficient compared to the appropriate level,
[0058] ③ If the content of the coating material relative to the primary cathode active material is excessive compared to the appropriate level during the manufacturing process of the secondary cathode active material (or tertiary cathode active material if necessary),
[0059] ④ This may occur when the heat treatment conditions (temperature and time) are insufficient compared to the appropriate level during the manufacturing process of the secondary cathode active material (or tertiary cathode active material if necessary).
[0060] [Ni in Mathematical Formula 1 due to one or more causes among ① to ④ above (0nm) ] / [Ni (50nm) If ] becomes 0.05 or less,
[0061] a) Gelation of the electrode coating slurry due to residual lithium in the electrode manufacturing process,
[0062] b) Gas generation due to side reactions between residual lithium and electrolyte in the battery,
[0063] c) A decrease in capacity and capacity retention rate in the battery may occur.
[0064] In mathematical formula 1, [Ni (0nm) ] / [Ni (50nm) The tendency for ] to increase is,
[0065] ① If the mixing ratio of the lithium compound relative to the precursor in the primary cathode active material manufacturing process is insufficient compared to the appropriate level,
[0066] ② If the cleaning of the cathode active material in the primary cathode active material manufacturing process is excessive compared to the appropriate level,
[0067] ③ If the content of the coating material relative to the primary cathode active material is insufficient compared to the appropriate level during the manufacturing process of the secondary cathode active material (or tertiary cathode active material if necessary),
[0068] ④ This may occur when the heat treatment conditions (temperature and time) are excessive compared to the appropriate level during the manufacturing process of the secondary cathode active material (or tertiary cathode active material if necessary).
[0069] [Ni in Mathematical Formula 1 due to one or more causes among ①' to ④' above (0nm) ] / [Ni (50nm) If ] becomes 0.3 or higher,
[0070] a') Capacity degradation due to lithium loss in the positive electrode active material,
[0071] b') Increase in lithium ion movement resistance within the positive electrode active material due to changes in the crystal structure of the positive electrode active material (changes in charge / discharge potential),
[0072] c') A decrease in capacity and capacity retention rate may occur in the battery.
[0073] In the above, "the mixing ratio of the lithium compound relative to the precursor is at an appropriate level" means that, based on the molar ratio, the lithium compound is greater than 1.00 and less than 1.07 relative to the precursor 1.00; "the cleaning conditions are at an appropriate level" means that the content of lithium hydroxide and lithium carbonate, which are residual lithium components present on the surface of the cathode active material after cleaning, is 2,000 to 7,000 ppm and 1,000 to 5,000 ppm, respectively, according to the titration method; "the content of the coating material relative to the primary cathode active material is at an appropriate level" means that the coating material content is 0.2 mol% to 3.0 mol% based on the remaining components excluding lithium and oxygen in the cathode active material; and "the heat treatment conditions in the secondary (or tertiary if necessary) heat treatment process are at an appropriate level" means that the maximum heat treatment temperature is 250℃ to 550℃ and the holding time at the maximum temperature is 5 to 30 hours.
[0074] [Ni, the nickel content on the surface of the positive electrode active material in Mathematical Formula 1 (0nm) ] is preferably greater than 2.0at% and less than 10.0at%. [Ni (0nm) If ] is 2.0 at% or less, it indicates that the content of lithium and / or coating material on the surface of the cathode active material is excessive, which can cause residual lithium problems due to the excess lithium and / or a decrease in capacity and capacity retention rate due to the excess coating material. On the other hand, [Ni (0nm) If ] is 10.0 at% or more, it indicates that the content of lithium and / or coating material on the surface of the positive electrode active material is insufficient, which may cause problems such as reduced capacity and capacity retention rate due to insufficient lithium and / or residual lithium due to insufficient coating material.
[0075] In mathematical formula 1, the nickel content position within the cathode active material is preferably 50 nm. At a nickel content position less than 50 nm, the variability of nickel content is large, which poses a problem in determining the correlation between the capacity retention rate in the battery and the ratio of nickel content between the surface and the interior of the cathode active material. At a nickel content position greater than 50 nm, the nickel content and nickel content variability do not differ significantly compared to the 50 nm position; that is, since there is no problem in determining the correlation between the capacity retention rate in the battery and the ratio of nickel content between the surface and the interior of the cathode active material, the 50 nm position is preferable when considering time and cost.
[0076] Physical properties of the positive electrode active material
[0077] The crystallinity of the positive electrode active material is not particularly limited and may include single crystals, polycrystalline materials, and intermediate states between single and polycrystalline materials, that is, materials possessing both single and polycrystalline crystallinity. Additionally, a mixture of a single-crystal positive electrode active material and a polycrystalline positive electrode active material in a predetermined ratio may be included.
[0078] The particle size of the positive active material is the particle size of the anode (average particle size (D 50 )<7μm), medium particle (7μm≤average particle size (D 50 )≤13μm), coarse-sized particles (average particle size (D 50 )>13μm) and mixtures thereof may be included. However, they are not limited thereto.
[0079] The particle size distribution of the cathode active material may include narrow (Span value < 0.8), normal (0.8 ≤ Span value ≤ 1.5), wide (Span value > 1.5), and a mixture of these in a predetermined ratio (Span value is [(D 90 -D 10 ) / D 50 ] value). However, it is not limited to this.
[0080] When the positive electrode active material is a single crystal, the shape of the positive electrode active material may include spherical, elliptical, rhomboidal, rectangular, cuboidal, random, and mixtures thereof. However, it is not limited thereto.
[0081] In the case where the positive active material is a polycrystalline material having a secondary particle shape formed by aggregating multiple primary particles, the shapes of the primary particles and secondary particles may include spherical, elliptical, rhombus-shaped, rectangular, cubic, random shapes, and mixtures thereof. However, it is not limited thereto.
[0082] A second aspect of the present invention provides a method for manufacturing a positive electrode active material. The method may include: 1) a step of manufacturing a primary positive electrode active material by first heat treating a material containing a precursor and a lithium compound; 2) a step of manufacturing a secondary positive electrode active material by second heat treating a material containing the primary positive electrode active material; and 3) optionally, a step of manufacturing a tertiary positive electrode active material by third heat treating a material containing the secondary positive electrode active material.
[0083] Preparation of positive electrode active material
[0084] The following describes a process for manufacturing a positive electrode active material through stepwise heat treatment.
[0085] 1) Preparation of primary cathode active material
[0086] A material prepared by mixing a precursor and a lithium compound or a precursor and a lithium compound and a doping material, performing a primary heat treatment, and then undergoing grinding, classification, washing, filtration, drying, classification, and iron removal processes, can be called a primary cathode active material.
[0087] Since the mixing molar ratio of the lithium compound to the precursor, heat treatment conditions, and cleaning conditions affect the diffusion of the lithium compound into the precursor particles and the residual lithium content on the surface of the primary cathode active material, consequently, [Ni in Equation 1 (0nm) ] / [Ni (50nm) It can affect ]
[0088] Mixing ratio of precursor and lithium compound
[0089] The mixing ratio of the lithium compound to the precursor is preferably greater than 1.00 and less than 1.07 relative to the precursor in terms of molar ratio. If it is 1.00 or less, the lithium content inside the surface of the positive electrode active material is insufficient, which may lead to a decrease in capacity, whereas if it is 1.07 or more, problems may occur due to residual lithium on the surface of the positive electrode active material.
[0090] doping substances
[0091] In the primary cathode active material manufacturing process, components that can be used as doping materials may include at least one selected from the group consisting of Mg, Ca, Sr, Ba, Ti, V, Cr, Fe, Cu, Zn, B, Al, Si, Sn, P, Sb, Bi, S, F, Zr, Nb, Mo, Hf, Ta, W, Sc, Y, La, and Ce.
[0092] The content of the doping material is preferably 0.2 mol% to 3.0 mol% among the remaining components of the positive electrode active material excluding lithium and oxygen. If the content of the doping material is less than 0.2 mol%, it may be insufficient to contribute to the structural stability of the positive electrode active material, and if the content of the doping material exceeds 3.0 mol%, the nickel content becomes relatively low and the doping material hinders the movement of lithium ions, which may result in a decrease in capacity and capacity retention rate in the battery.
[0093] 1st heat treatment conditions
[0094] In the first heat treatment process, the maximum temperature may preferably be between 550°C and 1,000°C. If the maximum temperature is below 550°C, the sintering of the positive active material may be insufficient, which may result in reduced thermal structural stability of the positive active material; on the other hand, if the maximum temperature exceeds 1,000°C, the sintering of the positive active material may be excessive, which may cause the crystal structure of the positive active material to collapse.
[0095] In the first heat treatment process, the holding time at the maximum temperature may be 10 to 30 hours. If it is less than 10 hours, the sintering of the positive active material is insufficient, which may reduce the thermal structural stability of the positive active material, whereas if it exceeds 30 hours, the sintering of the positive active material is excessive, which may cause the crystal structure of the positive active material to collapse.
[0096] Cleaning conditions
[0097] The cleaning time is the factor that has the greatest influence on the lithium content on the surface and inside the surface of the cathode active material under cleaning conditions. It is desirable to adjust the cleaning time appropriately so that the content of lithium hydroxide and lithium carbonate, which are residual lithium components present on the surface of the cathode active material after cleaning, are 2,000 to 7,000 ppm and 1,000 to 5,000 ppm, respectively, according to the titration method. If the content of lithium hydroxide and lithium carbonate, respectively, after cleaning is less than 2,000 ppm and 1,000 ppm according to the titration method, the lithium content inside the surface of the cathode active material is insufficient, which may lead to a decrease in capacity; on the other hand, if the content of lithium hydroxide and lithium carbonate, respectively, after cleaning exceeds 7,000 ppm and 5,000 ppm according to the titration method, problems may occur due to residual lithium on the surface of the cathode active material.
[0098] 2) Manufacturing of secondary cathode active material
[0099] A material prepared by mixing a material containing a primary positive active material and a coping material, performing a secondary heat treatment, and then undergoing grinding, classification, and iron removal processes can be called a secondary positive active material.
[0100] Since the mixing ratio of the primary cathode active material and the coping material, the composition of the coating material, and the heat treatment conditions affect the content of lithium and coating components on the surface of the secondary cathode active material and from the surface to the interior, consequently, [Ni in Equation 1 (0nm) ] / [Ni (50nm) It can affect ]
[0101] coating material
[0102] In the manufacturing process of the secondary cathode active material, the components that can be used as coating materials may include at least one selected from the group consisting of Li, N, Mg, Ca, Sr, Ba, Ti, V, Cr, Mn, Fe, Co, Cu, Zn, B, Al, Si, Sn, P, Sb, Bi, S, F, Zr, Nb, Mo, Hf, Ta, W, Sc, Y, La, and Ce.
[0103] The content of the coating material is preferably 0.2 mol% to 3.0 mol% among the remaining components of the positive electrode active material excluding lithium and oxygen. If the content of the coating material is less than 0.2 mol%, it may be insufficient to suppress problems caused by residual lithium on the surface of the positive electrode active material, and if it exceeds 3.0 mol%, the nickel content of the positive electrode active material becomes relatively low and the movement of lithium ions is hindered, which may result in a decrease in capacity, capacity retention rate, and output characteristics.
[0104] 3) Manufacturing of tertiary cathode active material
[0105] A material obtained by performing a third heat treatment on a second positive active material can be called a third positive active material. The third heat treatment can be performed selectively if necessary. That is, the second positive active material may not satisfy the conditions of the positive active material of the present invention, in which case a positive active material satisfying the present invention can be manufactured through a third heat treatment.
[0106] For example, if the secondary cathode active material does not satisfy the range of Equation 1, a tertiary cathode active material that satisfies the range of Equation 1 can be manufactured by performing a tertiary heat treatment.
[0107] In addition, when using two or more coating materials, the two or more coating materials may be manufactured by applying them together in a secondary heat treatment process, but in some cases, the coating materials may be manufactured by applying them separately in secondary and tertiary heat treatments.
[0108] Second (or third if necessary) heat treatment conditions
[0109] In the second (or third if necessary) heat treatment process, the maximum temperature may preferably be between 250°C and 550°C. If the maximum temperature is below 250°C, a problem may occur where residual lithium and coating material on the surface of the positive active material do not properly penetrate into the positive active material, whereas if it exceeds 550°C, a problem may occur where residual lithium and coating material on the surface of the positive active material penetrate excessively into the positive active material.
[0110] In the second (or third if necessary) heat treatment process, the holding time at the maximum temperature may be 5 to 30 hours. If the holding time is less than 5 hours, a problem may occur where residual lithium and coating material on the surface of the positive active material do not properly penetrate into the positive active material, whereas if the holding time exceeds 30 hours, a problem may occur where residual lithium and coating material on the surface of the positive active material penetrate excessively into the positive active material.
[0111] A third aspect of the present invention may be a positive electrode for a lithium secondary battery comprising a positive electrode active material of the front side. The positive electrode of this aspect may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode active material layer may include a positive electrode active material on the front side of the positive electrode.
[0112] Aluminum thin films may be used as the positive current collector, but are not limited thereto. The positive active material layer may include a positive active material, a binder, and a conductive material. The positive active material layer may include a positive active material according to the present invention. The binder may include a polymer having a fluorine (F) component, for example, polyvinyl fluoride (PVF), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), and modifications thereof. The conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes in the battery may be used. For example, natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, etc. may be used.
[0113] A fourth aspect of the present invention may be a lithium secondary battery comprising a positive electrode on the front side.
[0114] The lithium secondary battery of this aspect may include a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte on the front side.
[0115] The cathode may include a cathode current collector and a cathode active material layer formed on the current collector. A copper thin film may be used as the cathode current collector, but is not limited thereto. The cathode active material layer may include a cathode active material, a binder composition, and / or a conductive material.
[0116] The separator is inserted between the anode and the cathode to separate them, and may be one that has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. For example, it may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene, or combinations thereof, and may be in the form of a nonwoven or woven fabric.
[0117] The electrolyte can be prepared by dissolving a lithium salt in an organic solvent. Any organic solvent and lithium salt that can be generally used as an organic solvent in the relevant technical field may be used. In addition, solid electrolytes such as organic solid electrolytes and inorganic solid electrolytes may be used as the electrolyte. When a solid electrolyte is used, the solid electrolyte may also serve as a separator.
[0118] Hereinafter, the present invention will be described in detail with reference to examples to specifically explain the invention. However, the embodiments according to the present invention may be modified in various different forms, and the scope of the present invention should not be interpreted as being limited to the embodiments described below. The embodiments of the present invention are provided to more completely explain the invention to those with average knowledge in the art.
[0119] 1. Preparation of positive electrode active material
[0120] In the preparation of the following positive electrode active material, the mixing molar ratios for the materials are based on the metal (or main component), and the results of the mixing molar ratios are shown in the experimental formulas in "Table 1 of 2. Evaluation" below.
[0121] 1) Example 1-1: Preparation of Cathode Active Material 1-1
[0122] Composition Ni manufactured by the continuous co-precipitation method 0.94 Co 0.01 Mn 0.05 A positive electrode active material 1-1 was prepared as follows using a (OH)2 precursor with an average particle size of 9.4 μm.
[0123] ① The above precursor, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.005 and mixed uniformly.
[0124] ② The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.
[0125] - Atmosphere gas: Oxygen
[0126] - Heating rate: Heating from room temperature to 720℃ at a rate of 2℃ / min
[0127] - Holding time: Maintain at 720℃ for 24 hours
[0128] - Cooling method: Natural cooling
[0129] ③ The primary heat-treated material of ② was crushed and classified, then washed for 15 minutes, and subsequently underwent filtration, drying, classification, and iron removal processes.
[0130] ④ The primary positive active material obtained in ③ above and boric acid as a coating material were added to a mixing container in a molar ratio of 1.00 to 0.01 and mixed uniformly.
[0131] ⑤ The mixed powder of ④ was subjected to secondary heat treatment in a box kiln under the following conditions.
[0132] - Atmosphere gas: Air
[0133] - Heating rate: Heating from room temperature to 400℃ at a rate of 2℃ / min
[0134] - Holding time: Hold at 400℃ for 12 hours
[0135] - Cooling method: Natural cooling
[0136] ⑥ The secondary heat-treated material of ⑤ was crushed and classified, and then subjected to a deironing process to produce the cathode active material 1-1.
[0137] 2) Example 1-2: Preparation of Cathode Active Material 1-2
[0138] Anode active material 1-2 was prepared by keeping the rest the same except that the mixing ratio of ① in Example 1-1 was changed as in ①' below.
[0139] ① The above precursor, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.01 to 0.005 and mixed uniformly.
[0140] 3) Examples 1-3: Preparation of Cathode Active Material 1-3
[0141] Anode active material 1-3 was prepared by keeping the rest the same except that the mixing ratio of ① in Example 1-1 was changed as in ①' below.
[0142] ① The above precursor, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.05 to 0.005 and mixed uniformly.
[0143] 4) Comparative Example 1-1: Preparation of Comparative Anode Active Material 1-1
[0144] Comparative cathode active material 1-1 was prepared by keeping the rest the same except that the mixing ratio of ① in Example 1-1 was changed as in ①' below.
[0145] ① The above precursor, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 0.97 to 0.005 and mixed uniformly.
[0146] 5) Comparative Example 1-2: Preparation of Comparative Anode Active Material 1-2
[0147] Comparative cathode active material 1-2 was prepared by keeping the rest the same except that the mixing ratio of ① in Example 1-1 was changed as in ①' below.
[0148] ① The above precursor, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.09 to 0.005 and mixed uniformly.
[0149] 6) Example 2-1: Preparation of Cathode Active Material 2-1
[0150] Composition Ni manufactured by the continuous co-precipitation method 0.95 Mn 0.05 A positive electrode active material 2-1 was prepared as follows using a (OH)2 precursor with an average particle size of 9.6 μm.
[0151] ① The above precursor, lithium hydroxide, magnesium oxide as doping material 1, and zirconium oxide as doping material 2 were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.005 to 0.005 and mixed uniformly.
[0152] ② The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.
[0153] - Atmosphere gas: Oxygen
[0154] - Heating rate: Heating from room temperature to 700℃ at a rate of 2℃ / min
[0155] - Holding time: Maintain at 700℃ for 24 hours
[0156] - Cooling method: Natural cooling
[0157] ③ The primary heat-treated material of ② was crushed and classified, then washed for 15 minutes, and subsequently underwent filtration, drying, classification, and iron removal processes.
[0158] ④ The primary positive active material obtained in ③ above and aluminum phosphate as a coating material were added to a mixing container in a molar ratio of 1.00 to 0.005 and mixed uniformly.
[0159] ⑤ The mixed powder of ④ was subjected to secondary heat treatment in a box kiln under the following conditions.
[0160] - Atmosphere gas: Air
[0161] - Heating rate: Heating from room temperature to 400℃ at a rate of 2℃ / min
[0162] - Holding time: Hold at 400℃ for 12 hours
[0163] - Cooling method: Natural cooling
[0164] ⑥ The secondary heat-treated material of ⑤ was crushed and classified, and then subjected to a deironing process to produce the cathode active material 2-1.
[0165] 7) Example 2-2: Preparation of Cathode Active Material 2-2
[0166] Anode active material 2-2 was prepared by keeping the rest the same, except that the cleaning time in ③ of Example 2-1 was changed as in ③' below.
[0167] ③' The primary heat-treated material of ② was crushed and classified, then washed for 10 minutes, and subsequently underwent filtration, drying, classification, and iron removal processes.
[0168] 8) Example 2-3: Preparation of Cathode Active Material 2-3
[0169] Anode active material 2-3 was prepared by keeping the rest the same, except that the cleaning time in ③ of Example 2-1 was changed as in ③' below.
[0170] ③' The primary heat-treated material of ② was crushed and classified, then washed for 20 minutes, and subsequently underwent filtration, drying, classification, and iron removal processes.
[0171] 9) Comparative Example 2-1: Preparation of Comparative Anode Active Material 2-1
[0172] Comparative cathode active material 2-1 was prepared by keeping the rest the same, except that the cleaning time in ③ of Example 2-1 was changed as in ③' below.
[0173] ③' The primary heat-treated material of ② was crushed and classified, then washed for 5 minutes, and subsequently underwent filtration, drying, classification, and iron removal processes.
[0174] 10) Comparative Example 2-2: Preparation of Comparative Anode Active Material 2-2
[0175] Comparative cathode active material 2-2 was prepared by keeping the rest the same, except that the cleaning time in ③ of Example 2-1 was changed as in ③' below.
[0176] ③' The primary heat-treated material of ② was crushed and classified, then washed for 30 minutes, and subsequently underwent filtration, drying, classification, and iron removal processes.
[0177] 11) Example 3-1: Preparation of Cathode Active Material 3-1
[0178] Composition Ni manufactured by the continuous co-precipitation method 0.95 Co 0.05 A positive electrode active material 3-1 was prepared as follows using a (OH)2 precursor with an average particle size of 9.4 μm.
[0179] ① A precursor, lithium hydroxide, aluminum oxide as doping material 1, and zirconium oxide as doping material 2 were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.005 to 0.005 and mixed uniformly.
[0180] ② The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.
[0181] - Atmosphere gas: Oxygen
[0182] - Heating rate: Heating from room temperature to 700℃ at a rate of 2℃ / min
[0183] - Holding time: Maintain at 700℃ for 24 hours
[0184] - Cooling method: Natural cooling
[0185] ③ The primary heat-treated material of ② was crushed and classified, then washed for 15 minutes, and subsequently underwent filtration, drying, classification, and iron removal processes.
[0186] ④ The primary positive active material obtained in ③ above and magnesium oxide as a coating material were added to a mixing container in a molar ratio of 1.00 to 0.01 and mixed uniformly.
[0187] ⑤ The mixed powder of ④ was subjected to secondary heat treatment in a box kiln under the following conditions.
[0188] - Atmosphere gas: Air
[0189] - Heating rate: Heating from room temperature to 400℃ at a rate of 2℃ / min
[0190] - Holding time: Hold at 400℃ for 12 hours
[0191] - Cooling method: Natural cooling
[0192] ⑥ The secondary heat-treated material of ⑤ was crushed and classified, and then subjected to a deironing process to produce the cathode active material 3-1.
[0193] 12) Example 3-2: Preparation of Cathode Active Material 3-2
[0194] Anode active material 3-2 was prepared by keeping the rest the same, except that the mixing ratio of ④ in Example 3-1 was changed as in ④' below.
[0195] ④ The primary positive active material obtained in ③ above and magnesium oxide as a coating material were added to a mixing container in a molar ratio of 1.00 to 0.005 and mixed uniformly.
[0196] 13) Example 3-3: Preparation of Cathode Active Material 3-3
[0197] Anode active material 3-3 was prepared by keeping the rest the same, except that the mixing ratio of ④ in Example 3-1 was changed as in the following ④'.
[0198] ④ The primary positive active material obtained in ③ above and magnesium oxide as a coating material were added to a mixing container in a molar ratio of 1.00 to 0.02 and mixed uniformly.
[0199] 14) Comparative Example 3-1: Preparation of Comparative Anode Active Material 3-1
[0200] Comparative cathode active material 3-1 was prepared by keeping the rest the same except that the mixing ratio of ④ in Example 3-1 was changed as in ④' below.
[0201] ④' The primary positive active material obtained in ③ above and magnesium oxide as a coating material were added to a mixing container in a molar ratio of 1.00 to 0.001 and mixed uniformly.
[0202] 15) Comparative Example 3-2: Preparation of Comparative Anode Active Material 3-2
[0203] Comparative cathode active material 3-2 was prepared by keeping the rest the same, except that the mixing ratio of ④ in Example 3-1 was changed as in ④' below.
[0204] ④ The primary positive active material obtained in ③ above and magnesium oxide as a coating material were added to a mixing container in a molar ratio of 1.00 to 0.04 and mixed uniformly.
[0205] 16) Example 4-1: Preparation of single-crystal cathode active material 4-1
[0206] Composition Ni manufactured by batch co-precipitation method 0.93 Co 0.02 Mn 0.05 A single-crystal cathode active material 4-1 was prepared as follows using a (OH)2 precursor with an average particle size of 3.5 μm.
[0207] ① The above precursor, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.005 and mixed uniformly.
[0208] ② The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.
[0209] - Atmosphere gas: Oxygen
[0210] - Pre-heat treatment: Increase temperature from room temperature to 450℃ at a rate of 2℃ / min, and maintain at 450℃ for 10 hours.
[0211] - Heating rate: Heating from 450 to 870℃ at a rate of 2℃ / min
[0212] - Holding time: Maintain at 870℃ for 24 hours
[0213] - Cooling method: Natural cooling
[0214] ③ The primary heat-treated material of ② was crushed and classified, then washed for 15 minutes, and subsequently underwent filtration, drying, classification, and iron removal processes.
[0215] ④ Vanadium pentoxide was added to a mixing container in a molar ratio of 1.00 to 0.005 with the primary positive active material obtained in ③ above and coating material 1, and mixed uniformly.
[0216] ⑤ The mixed powder of ④ was subjected to secondary heat treatment in a box kiln under the following conditions.
[0217] - Atmosphere gas: Air
[0218] - Heating rate: Heating from room temperature to 400℃ at a rate of 2℃ / min
[0219] - Holding time: Hold at 400℃ for 12 hours
[0220] - Cooling method: Natural cooling
[0221] ⑥ The secondary heat-treated material of ⑤ was crushed and classified, and then subjected to a deironing process.
[0222] ⑦ The secondary positive active material obtained in ⑥ above and aluminum oxide as coating material 2 were added to a mixing container in a molar ratio of 1.00 to 0.005 and mixed uniformly.
[0223] ⑧ The mixed powder of ⑦ was subjected to a third heat treatment in a box kiln under the following conditions.
[0224] - Atmosphere gas: Air
[0225] - Heating rate: Heating from room temperature to 400℃ at a rate of 2℃ / min
[0226] - Holding time: Hold at 400℃ for 12 hours
[0227] - Cooling method: Natural cooling
[0228] The single-crystal cathode active material 4-1 was prepared by crushing and classifying the 3rd heat-treated material of ⑨ and ⑧, followed by a deironing process.
[0229] 17) Example 4-2: Preparation of single-crystal cathode active material 4-2
[0230] A single-crystal positive active material 4-2 was prepared by keeping the rest the same except that the secondary and tertiary heat treatment conditions of ⑤ and ⑧ in Example 4-1 were changed as follows.
[0231] - Atmosphere gas: Air
[0232] - Heating rate: Heating from room temperature to 300℃ at a rate of 2℃ / min
[0233] - Holding time: Maintain at 300℃ for 12 hours
[0234] - Cooling method: Natural cooling
[0235] 18) Example 4-3: Preparation of single-crystal cathode active material 4-3
[0236] A single-crystal positive active material 4-3 was prepared by keeping the rest the same except that the secondary and tertiary heat treatment conditions of ⑤ and ⑧ in Example 4-1 were changed as follows.
[0237] - Atmosphere gas: Air
[0238] - Heating rate: Heating from room temperature to 500℃ at a rate of 2℃ / min
[0239] - Holding time: Hold at 500℃ for 12 hours
[0240] - Cooling method: Natural cooling
[0241] 19) Comparative Example 4-1: Preparation of Single Crystal Comparative Anode Active Material 4-1
[0242] Comparative cathode active material 4-1 of single crystals was prepared by keeping the rest the same except that the secondary and tertiary heat treatment conditions of ⑤ and ⑧ in Example 4-1 were changed as follows.
[0243] - Atmosphere gas: Air
[0244] - Heating rate: Heating from room temperature to 200℃ at a rate of 2℃ / min
[0245] - Holding time: Maintain at 200℃ for 12 hours
[0246] - Cooling method: Natural cooling
[0247] 20) Comparative Example 4-4: Preparation of Single Crystal Comparative Anode Active Material 4-2
[0248] Comparative cathode active material 4-2 of single crystals was prepared by keeping the rest the same except that the secondary and tertiary heat treatment conditions of ⑤ and ⑧ in Example 4-1 were changed as follows.
[0249] - Atmosphere gas: Air
[0250] - Heating rate: Heating from room temperature to 600℃ at a rate of 2℃ / min
[0251] - Holding time: Hold at 600℃ for 12 hours
[0252] - Cooling method: Natural cooling
[0253] 2. Evaluation
[0254] 1) Composition of the positive electrode active material
[0255] Elemental analysis of the cathode active materials of the examples and comparative examples was performed using an ICP-OES analyzer. In the ICP-OES analysis, the analysis of major components was performed using an Agilent 5800 (RF power 1200W) analyzer, and trace elements such as doping and coating materials were analyzed using a Perkin Elmer Avio550 (RF power 1300W).
[0256] Table 1 shows the experimental chemical formulas for the positive electrode active materials of the above examples and comparative examples, and the analytical chemical formulas obtained using ICP-OES.
[0257] Experimental Chemical Formula Analysis Chemical Formula Example 1-1Li 1.03 [(Ni 0.94 Co 0.01 Mn 0.05 )-(Zr 0.005 )-(B 0.01 )]O( >2 )Li 1.005 [(Ni 0.925 Co 0.010 Mn 0.050 Zr 0.005 B0.010 )]O( >2 )Examples 1-2Li 1.01 [(Ni 0.94 Co 0.01 Mn 0.05 )-(Zr 0.01 )-(B 0.01 )]O( >2 )Li 0.993 [(Ni 0.924 Co 0.011 Mn 0.049 Zr 0.005 B 0.011 )]O( <2 )Examples 1-3Li 1.05 [(Ni 0.94 Co 0.01 Mn 0.05 )-(Zr 0.01 )-(B 0.01 )]O( >2 )Li 1.011 [(Ni 0.924 Co 0.010 Mn 0.050 Zr 0.005 B 0.011 )]O( >2 )Comparative Example 1-1Li 0.97 [(Ni 0.94 Co 0.01 Mn 0.05 )-(Zr 0.01 )-(B 0.01 )]O( >2 )Li 0.948 [(Ni 0.926 Co 0.009 Mn 0.049 Zr 0.005 B 0.011 )]O( <2 )Comparative Example 1-2Li 1.09 [(Ni 0.94 Co 0.01 Mn 0.05 )-(Zr 0.01 )-(B 0.01 )]O( >2 )Li 1.024 [(Ni 0.926 Co 0.010 Mn 0.050 Zr 0.004 B 0.010 )]O( >2 Example 2-1Li 1.03 [(Ni 0.95 Mn0.05 )-(Mg 0.005 Zr 0.005 )-(Al 0.005 P 0.005 )]O( >2 )Li 1.006 [(Ni 0.930 Mn 0.050 Mg 0.005 Zr 0.005 Al 0.005 P 0.005 )]O( >2 Example 2-2Li 1.014 [(Ni 0.932 Mn 0.049 Mg 0.005 Zr 0.005 Al 0.004 P 0.005 )]O( >2 )Examples 2-3Li 1.001 [(Ni 0.932 Mn 0.050 Mg 0.004 Zr 0.004 Al 0.005 P 0.005 )]O( >2 )Comparative Example 2-1Li 1.021 [(Ni 0.929 Mn 0.049 Mg 0.006 Zr 0.006 Al 0.004 P 0.006 )]O( >2 )Comparative Example 2-2Li 0.954 [(Ni 0.930 Mn 0.050 Mg 0.006 Zr 0.004 Al 0.005 P 0.005 )]O( <2 Example 3-1Li 1.03 [(Ni 0.95 Co 0.05 )-(Al 0.005 Zr 0.005 )-(Mg 0.01 )]O( >2 )Li 1.006 [(Ni 0.932 Co 0.048 Al 0.005 Zr 0.005 Mg 0.010 )]O( >2 Example 3-2Li 1.03 [(Ni0.95 Co 0.05 )-(Al 0.005 Zr 0.005 )-(Mg 0.005 )]O( >2 )Li 1.005 [(Ni 0.935 Co 0.050 Al 0.005 Zr 0.006 Mg 0.004 )]O( >2 Example 3-3Li 1.03 [(Ni 0.95 Co 0.05 )-(Al 0.005 Zr 0.005 )-(Mg 0.02 )]O( >2 )Li 1.006 [(Ni 0.921 Co 0.050 Al 0.005 Zr 0.005 Mg 0.019 )]O( >2 )Comparative Example 3-1Li 1.03 [(Ni 0.95 Co 0.05 )-(Al 0.005 Zr 0.005 )-(Mg 0.001 )]O( >2 )Li 1.008 [(Ni 0.941 Co 0.049 Al 0.005 Zr 0.004 Mg 0.001 )]O( >2 )Comparative Example 3-2Li 1.03 [(Ni 0.95 Co 0.05 )-(Al 0.005 Zr 0.005 )-(Mg 0.04 )]O( >2 )Li 1.003 [(Ni 0.906 Co 0.048 Al 0.004 Zr 0.004 Mg 0.038 )]O( >2 Example 4-1Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 )-(Zr 0.005 )-(V0.005 )-(Al 0.005 )]O( >2 )Li 1.005 [(Ni 0.915 Co 0.021 Mn 0.050 Zr 0.005 V 0.004 Al 0.005 )]O( >2 Example 4-2Li 1.006 [(Ni 0.917 Co 0.019 Mn 0.050 Zr 0.005 V 0.004 Al 0.005 )]O( >2 Example 4-3Li 1.006 [(Ni 0.916 Co 0.021 Mn 0.048 Zr 0.005 V 0.005 Al 0.005 )]O( >2 )Comparative Example 4-1Li 1.008 [(Ni 0.914 Co 0.021 Mn 0.051 Zr 0.005 V 0.004 Al 0.005 )]O( >2 )Comparative Example 4-2Li 1.003 [(Ni 0.916 Co 0.020 Mn 0.051 Zr 0.004 V 0.004 Al 0.005 )]O( >2 )
[0258] In Table 1, the "Experimental" chemical formulas apply the molar ratio values used in the manufacturing method as is, while the "Analytical" chemical formulas represent the remaining components (components indicated in the formulas), excluding lithium and oxygen, based on a 1.0 molar standard. However, trace impurities were not included in Table 1. Referring to Table 1, it can be confirmed that the experimental and analytical values match well for the components other than lithium. In the case of lithium, it indicates that it varies depending on the mixing molar ratio of the lithium compound relative to the precursor and the washing time during the primary cathode active material manufacturing process.
[0259] 2) Particle size analysis of cathode active material
[0260] Particle size analysis of the cathode active materials prepared in the examples and comparative examples was performed using a particle size analyzer (Master Sizer 3000), and the results are shown in Table 2.
[0261] D 50 (μm)Span Example 1-110.11.26 Example 1-210.21.28 Example 1-310.41.27 Comparative Example 1-110.21.26 Comparative Example 1-210.21.25 Example 2-110.61.29 Example 2-210.51.29 Example 2-310.81.27 Comparative Example 2-110.51.26 Comparative Example 2-210.71.28 Example 3-110.11.26 Example 3-210.01.29 Example 3-310.31.28 Comparative Example 3-110.21.27 Comparative Example 3-210.41.26 Example 4-13.91.35 Example 4-24.11.34 Example 4-34.01.36 Comparative Example 4-14.31.37 Comparative Example 4-24.21.36
[0262] Referring to Table 2, it can be confirmed that there is no difference in average particle size and particle size distribution according to the examples and comparative examples.3) Amount of residual lithium on the surface of the positive electrode active material
[0263] The content of residual lithium (lithium hydroxide and lithium carbonate) present on the surface of the cathode active material prepared in the examples and comparative examples was evaluated as follows by titration using a 905 Titrado instrument. Specifically, 10 g of the cathode active material was dispersed in 100 mL of water and then titrated with 0.1 M HCl to obtain a pH titration result, and the content of lithium hydroxide and lithium carbonate present on the surface of the cathode active material was measured using the result, and the results are shown in Table 3.
[0264] LiOH(ppm)Li2CO3(ppm)Example 1-143242553Example 1-234372287Example 1-347783024Comparative Example 1-11431796Comparative Example 1-281696338Example 2-141842456Example 2-250863176Example 2-336323125Comparative Example 2-182246521Comparative Example 2-21473814Example 3-140572955Example 3-243353342Example 3-337732845Comparative Example 3-145823533Comparative Example 3-232222542Example 4-142732491 Example 4-245832642 Example 4-340432327 Comparative Example 4-153623176 Comparative Example 4-234722082
[0265] Referring to Table 3, it indicates that the amounts of residual lithium in the cathode active material, namely lithium hydroxide and lithium carbonate, are influenced by the mixing ratio of the precursor and lithium compound and the cleaning conditions during the manufacture of the primary cathode active material.4) Component analysis of the surface and interior of the cathode active material
[0266] Component analysis of the surface and from the surface to the interior of the cathode active materials of the examples and comparative examples was performed using an XPS analysis instrument (Shimadzu AXIS Supra+). After XPS analysis of the cathode active material surface, argon ions (Ar +The cathode active material was etched using a ) beam at a rate of 5 nm / min (standard sample - Ta2O5), and elemental analysis was performed by XPS at 10 nm intervals up to 50 nm. In the XPS analysis, the nickel content was calculated based on the elements excluding oxygen in the analytical formulas in Table 1, and [Ni (0nm) ] and [Ni (50nm) The results are shown in Table 4. In addition, to aid in understanding the XPS analysis results, [Ni (0nm) ] and [Ni (50nm) The results are shown in Figures 1 and 2, respectively.
[0267] [Ni (0nm) ][Ni (50nm) ][Ni (0nm) ] / [Ni (50nm) Example 1-16.541.30.16 Example 1-28.741.70.21 Example 1-34.840.70.12 Comparative Example 1-113.242.10.31 Comparative Example 1-21.740.20.04 Example 2-14.441.70.11 Example 2-22.440.90.06 Example 2-36.842.20.16 Comparative Example 2-11.840.50.04 Comparative Example 2-213.943.10.32 Example 3-15.440.90.13 Example 3-211.541.40.28 Example 3-32.740.20.07 Comparative Example 3-114.941.50.36 Comparative Example 3-21.239.70.03 Example 4-17.841.40.19 Example 4-25.242.20.12 Example 4-311.740.10.29 Comparative Example 4-11.743.50.04 Comparative Example 4-214.238.90.37
[0268] Referring to Table 4, in the case of the positive electrode active material of the example, [Ni (0nm) ] / [Ni (50nm) While ] is within the range of greater than 0.05 and less than 0.3, in the case of the comparative example cathode active material, [Ni (0nm) ] / [Ni (50nm)] indicates that it is 0.05 or less or 0.3 or more. Referring to Table 4, [Ni of the Examples and Comparative Examples (0nm) ] and [Ni (50nm) ] indicates that the mixing ratio of lithium compound to precursor and cleaning conditions during the manufacture of the primary cathode active material, and the heat treatment temperature conditions during the manufacture of the secondary cathode active material are significantly affected.
[0269] 5) Evaluation of high-temperature life characteristics
[0270] To evaluate the battery performance of the cathode active materials of the examples and comparative examples, a cathode and a lithium battery (coin half-cell) were manufactured using the following method.
[0271] A positive electrode was prepared in which a positive electrode active material layer composed of the respective positive electrode active material of the example and comparative example, carbon conductive material (Super P), and PVDF binder in a weight ratio of 97:1.5:1.5 was formed on an aluminum thin film current collector.
[0272] A coin half-cell was manufactured using the above anode, a lithium metal cathode, a polyethylene separator, and an electrolyte (composed of a mixed solution of ethylene carbonate (EC), dimethyl carbonate (DMC), ethylmethyl carbonate (EMC), and lithium hexafluorophosphate (LiPF6)).
[0273] Lifetime characteristics were evaluated as follows using each of the above-manufactured coin half-cells.
[0274] The coin half-cell was initially charged to 4.3V with a constant current of 0.2C and a cut-off of 0.01C at 45℃, and initially discharged to 3.0V with a constant current of 0.2C. Subsequently, the coin half-cell was charged to 4.3V with a constant current of 0.5C and a cut-off of 0.05C at 45℃, and discharged to 3.0V with a constant current of 1.0C. This was repeated 100 times, with this as one cycle. The results are shown in Table 5.
[0275] Initial Charge Capacity (mAh / g) Initial Discharge Capacity (mAh / g) Efficiency (%) Discharge Capacity (mAh / g, @100 cycles) Capacity Retention Rate (%, @100 cycles) Example 1-1 232.3 212.2 91.3 204.5 96.4 Example 1-2 29.4 208.4 90.8 199.1 95.5 Example 1-3 26.6 204.2 90.1 193.4 94.7 Comparative Example 1-1 221.0 196.7 89.0 176.2 89.6 Comparative Example 1-2 217.2 190.5 87.7 168.5 88.5 Example 2-1 233.0 212.2 91.1 202.6 95.5 Example Example 2-2229.1207.190.4194.193.7 Example 2-3231.4210.490.9198.694.4 Comparative Example 2-1213.4185.586.9162.687.6 Comparative Example 2-2216.9191.688.3170.789.1 Example 3-1233.2212.691.2203.895.9 Example 3-2233.6213.691.5203.195.1 Example 3-3229.8208.190.6196.794.5 Comparative Example 3-1227.0203.089.4181.089.2 Comparative Example 3-2220.2194.288.2169.187.1 Example 4-1226.7207.791.6202.497.5 Example 4-2226.8206.791.1198.796.1 Example 4-3222.7201.290.4192.495.6 Comparative Example 4-1214.1190.188.8168.388.5 Comparative Example 4-2218.5196.189.7175.389.4
[0276] [Ni in Table 4 (0nm) ] / [Ni (50nm) The correlation between ] and the discharge capacity (mAh / g, @100cycle) in Table 5 is illustrated in Fig. 3. Referring to Fig. 3, [Ni (0nm) ] / [Ni (50nm) In the case of the positive active material of the example where ] is within the range of greater than 0.05 and less than 0.30, [Ni (0nm) ] / [Ni (50nm) It indicates that the discharge capacity at 100 cycles is superior compared to the comparative example positive active material in which ] is 0.05 or less or 0.30 or more.
[0277] Referring to Tables 4 and 5, the [Ni of the cathode active materials (0nm) In the case of the positive electrode active materials of the examples where ] is greater than 2.0 at% and less than 10.0 at%, [Ni (0nm) It shows excellent results in capacity and capacity retention rate compared to comparative example cathode active materials in which ] is 2.0 at% or less or 10.0 at% or more. This is because the [Ni of the cathode active materials (0nm) It indicates that it is possible to provide a positive electrode active material with excellent capacity and capacity retention rate in a battery, in which the problem caused by residual lithium in the positive electrode active material is improved through control.
[0278] In conclusion, through the method for manufacturing a positive electrode active material presented in the present invention, a positive electrode active material can be manufactured in which the ratio of nickel content at the surface of the positive electrode active material and at a position 50 nm from the surface into the interior is controlled, and such a positive electrode active material can exhibit characteristics that improve the problem caused by residual lithium on the surface of the positive electrode active material, and furthermore, a lithium secondary battery with excellent capacity and capacity retention rate can be manufactured using a positive electrode active material having such characteristics.
[0279] The terms used in this invention are intended to describe specific embodiments and are not intended to limit the invention. Unless otherwise evident from the context, singular expressions should be understood to include a plural meaning. Terms such as "comprising" or "having" mean that the features, numbers, steps, actions, components, or combinations thereof described in the specification exist, not that they are excluded.
[0280] The present invention is not limited by the embodiments described above and the attached drawings, but is intended to be limited by the attached claims. Accordingly, various substitutions, modifications, and changes may be made by those skilled in the art within the scope of the technical concept of the present invention as described in the claims, and such should also be considered to fall within the scope of the present invention.
Claims
1. A positive electrode active material for a lithium secondary battery, wherein the nickel content among the remaining components excluding lithium and oxygen is greater than 70 mol% and less than 98 mol%, and satisfies the following mathematical formula 1: [Mathematical Formula 1] 0.05 < [Ni (0nm) ] / [Ni (50nm) ] < 0.3, Here, [Ni (0nm) ] is the atomic percent (at%) of nickel among the remaining components excluding oxygen on the surface of the cathode active material, and [Ni (50nm) ] is the atomic percentage of nickel among the remaining components excluding oxygen at 50 nm from the surface of the positive active material into the interior.
2. In Paragraph 1, [Ni (0nm) ] is a positive electrode active material for a lithium secondary battery, greater than 2.0 at% and less than 10.0 at%.
3. In Paragraph 1, A positive electrode active material for a lithium secondary battery having a nickel content of more than 80 mol% and less than 98 mol%.
4. In Paragraph 1, A positive electrode active material for a lithium secondary battery having a nickel content of more than 90 mol% and less than 98 mol%.
5. In Paragraph 1, The above positive active material is a positive active material for a lithium secondary battery comprising nickel and one or more selected from the group consisting of cobalt, manganese, and aluminum.
6. A method for manufacturing the positive electrode active material of any one of claims 1 to 5, a) a precursor manufacturing step for manufacturing a precursor for a positive electrode active material; b) a step of producing a primary positive active material by performing a primary heat treatment on a material containing the manufactured precursor; and c) a step of manufacturing a secondary positive active material by performing a secondary heat treatment on a material containing the primary positive active material; A method for manufacturing a positive electrode active material for a lithium secondary battery, comprising 7. In Paragraph 6, c) After step, d) a step of manufacturing a tertiary cathode active material by performing a tertiary heat treatment on a material containing the above secondary cathode active material; A method for manufacturing a positive electrode active material for a lithium secondary battery, further comprising 8. A positive electrode for a lithium secondary battery comprising the positive electrode active material of any one of paragraphs 1 to 5.
9. A lithium secondary battery comprising the positive electrode of paragraph 8.