Positive electrode active material, and positive electrode and lithium secondary battery comprising same

Tungsten-doped layered lithium transition metal oxides with optimized structural parameters address the degradation issue in nickel-cobalt-manganese-based cathode materials, enhancing battery performance and stability in high-temperature conditions.

WO2026235365A1PCT designated stage Publication Date: 2026-11-12LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/005901
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional multi-particle nickel-cobalt-manganese-based cathode materials experience rapid capacity degradation due to oxygen escape and crystal structure collapse during high-temperature charge-discharge cycles, necessitating a stable structure capable of maintaining performance in high-temperature environments.

Method used

Development of tungsten-doped layered lithium transition metal oxides with specific structural and compositional parameters, including interslab thickness, particle size, and tungsten content, to enhance structural stability and lithium ion mobility.

Benefits of technology

Improves long-term performance, capacity retention, and resistance characteristics of lithium secondary batteries by stabilizing the lattice structure and facilitating lithium ion migration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026005901_12112026_PF_FP_ABST
    Figure KR2026005901_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present specification relates to: a positive electrode active material comprising a tungsten-doped layered lithium transition metal oxide and having a value calculated by equation 1 of 33 or more and 42 or less; and a positive electrode and a lithium secondary battery comprising same.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode active material, a cathode including the same, and a lithium secondary battery

[0001] Cross-citation with related application(s)

[0002] This specification claims the benefit of the filing date of Patent No. 10-2025-0059290 filed with the Korean Intellectual Property Office on May 7, 2025, the contents of which are incorporated herein.

[0003] This specification relates to a positive electrode active material, a positive electrode containing the same, and a lithium secondary battery.

[0004] With the advancement of lithium-ion batteries, cathode active materials used in electric vehicles require high energy density. In particular, nickel-cobalt-manganese cathode materials containing nickel, cobalt, and manganese are required to possess both high capacity and stability. Specifically, to extend the driving range of electric vehicles, the development of high-voltage cathode materials with high energy density is necessary.

[0005] However, conventional multi-particle nickel-cobalt-manganese-based cathode materials suffer from a problem where a rapid decrease in capacity occurs due to degradation during repeated charge-discharge cycles at high temperatures. This degradation is caused by the escape of oxygen or the collapse of the crystal structure resulting from redox reactions on the cathode surface. Therefore, technology capable of maintaining a stable structure even in high-temperature environments is required.

[0006] To address this, the development of single-particle nickel-cobalt-manganese-based cathode materials is attracting attention. Single-particle structures have fewer grain boundaries compared to multi-particle structures, which reduces surface degradation during charging and discharging and significantly improves structural stability. Furthermore, these single-particle nickel-cobalt-manganese-based cathode materials require further optimization through elemental doping and coating technologies to ensure that electrochemical reactions can occur efficiently.

[0007] The present specification provides a positive electrode active material capable of improving long-term performance when applied to a lithium secondary battery, a method for manufacturing the same, a positive electrode including the same, and a lithium secondary battery.

[0008] The first embodiment of the present specification comprises a tungsten-doped layered lithium transition metal oxide, and

[0009] A positive active material is provided having a value calculated by the following Equation 1 that is 33 or higher and 42 or lower.

[0010] [Equation 1]

[0011] T IS / L FWHM

[0012] In the above Equation 1,

[0013] T IS is the interslab thickness (unit: Å) measured by X-ray diffraction analysis, and

[0014] L FWHM is the full width at half maximum (in degrees) of the (003) plane peak measured by X-ray diffraction analysis.

[0015] A second embodiment of the present specification provides a positive electrode active material having a value calculated by the following formula 2 of 0.58 or higher and 0.65 or lower.

[0016] [Equation 2]

[0017] D SEM / D 50

[0018] In Equation 2,

[0019] D SEM is the average particle size (unit: μm) of the smallest unit particles distinguishable in scanning electron microscope images of lithium transition metal oxides, and

[0020] D 50 is the particle size (unit: μm) at the 50% point of the volume-based cumulative particle size distribution of the above lithium transition metal oxide measured by laser diffraction particle size analysis.

[0021] The third embodiment of the present specification provides a positive active material in which, in the first or second embodiment, the value calculated by the following formula 3 is 22 or more and 27 or less.

[0022] [Equation 3]

[0023] (T IS ×D SEM ) / (L FWHM ×D 50 )

[0024] In the above Equation 3,

[0025] T IS and L FWHM is equal to the definition in Equation 1, and

[0026] D SEM is the average particle size (unit: μm) of the smallest unit particles distinguishable in scanning electron microscope images of lithium transition metal oxides, and

[0027] D 50 is the particle size (unit: μm) at the 50% point of the volume-based cumulative particle size distribution of the above lithium transition metal oxide measured by laser diffraction particle size analysis.

[0028] The fourth embodiment of the present specification provides a positive active material in any one of the first to third embodiments, wherein the inter-slab thickness measured by the X-ray diffraction analysis method is 2.69 Å or more and 3 Å or less.

[0029] The fifth embodiment of the present specification provides a positive electrode active material in any one of the first to fourth embodiments, wherein the full width at half maximum of the (003) plane peak measured by the X-ray diffraction analysis method is 0.062 or greater and 0.08 or less.

[0030] The sixth embodiment of the present specification is, in any one of the first to fifth embodiments, an average particle size (D 50 ) provides a positive electrode active material having a thickness of 1㎛ to 20㎛.

[0031] The seventh embodiment of the present specification provides a positive electrode active material in any one of the first to sixth embodiments, wherein part or all of the tungsten exists in the form of hexavalent ions.

[0032] The eighth embodiment of the present specification provides a positive electrode active material in which, in any one of the first to seventh embodiments, the tungsten content is 600 ppm or more and 1,800 ppm or less based on the total weight of the lithium transition metal oxide.

[0033] The ninth embodiment of the present specification is, in any one of the first to eighth embodiments, the temperature of the peak (T) at the position where the heat flow is maximum during thermal analysis of the positive active material by differential scanning calorimetry. MAX Provides a positive electrode active material having a temperature of 225°C or higher.

[0034] The 10th embodiment of the present specification provides a positive electrode active material in which the lithium transition metal oxide is in the form of a single particle, in any one of the 1st to 9th embodiments.

[0035] The 11th embodiment of the present specification provides a positive electrode active material in any one of the 1st to 10th embodiments, wherein the lithium transition metal oxide comprises nickel (Ni), cobalt (Co), and manganese (Mn).

[0036] The 12th embodiment of the present specification provides a positive electrode active material in which, in any one of the 1st to 11th embodiments, the nickel content is 50 mol% or more based on the total molar amount of transition metal.

[0037] The 13th embodiment of the present specification provides a positive electrode active material in any one of the 1st to 12th embodiments, wherein the lithium transition metal oxide is represented by the following chemical formula 1.

[0038] [Chemical Formula 1]

[0039] Li1+t1 Ni x Co y Mn z W w1 M 1 m1 O2

[0040] In the above chemical formula 1,

[0041] -0.2≤t1<1, 0.5≤x<1, 0 <y≤0.4, 0<z≤0.4, 0<w1≤0.1, 0≤m1≤0.1, x+y+z+w1+m1=1이고,

[0042] M 1 It is one or a combination thereof from the group consisting of Cu, Fe, V, Cr, Ti, Zr, Zn, Al, Ta, Y, In, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo.

[0043] The 14th embodiment of the present specification provides a positive electrode comprising a positive electrode active material according to any one of the 1st to 13th embodiments.

[0044] The 15th embodiment of the present specification provides a lithium secondary battery comprising a positive electrode active material according to the 14th embodiment.

[0045] The positive active material of the present invention has the effect of improving initial charge / discharge performance when applied to a lithium secondary battery.

[0046] The positive active material of the present invention has the effect of improving long-term charge / discharge performance when applied to a lithium secondary battery.

[0047] The positive active material of the present invention has the effect of improving long-term resistance characteristics when applied to a lithium secondary battery.

[0048] Figure 1 is an X-ray diffraction pattern according to Experimental Example 1.

[0049] The present specification will be described in detail below.

[0050] Unless otherwise defined in this specification, all technical and scientific terms are used merely to describe exemplary embodiments and are not intended to limit this specification. Singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, terms such as 'comprising,' 'comprising,' or 'having' are intended to specify the presence of the described features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0051] The present invention is capable of various modifications and may take various forms, and specific embodiments are illustrated and described in detail below. However, this is not intended to limit the invention to the specific disclosed forms, and it should be understood that the invention includes all modifications, equivalents, and substitutions that fall within the spirit and scope of the invention.

[0052] The technical terms used in this specification are intended merely to refer to specific embodiments and are not intended to limit the invention. Furthermore, the singular forms used herein include plural forms unless the phrases clearly indicate otherwise.

[0053] In this specification, the 'positive active material' may be a composition comprising one or more tungsten-doped layered lithium transition metal oxides. Additionally, the positive active material may further comprise a tungsten-undoped layered lithium transition metal oxide in addition to the tungsten-doped layered lithium transition metal oxide.

[0054] In this specification, the 'layered lithium transition metal oxide' may have a structure in which a transition metal-oxygen layer (TM-O) and a lithium-oxygen layer (Li-O) are alternately stacked in LiMO2 (R-3m space group).

[0055] In this specification, 'doping' means that a foreign element is substituted and inserted at a specific location in the parent crystal lattice. Specifically, the foreign element may be substituted at the transition metal site or the lithium site of the parent crystal lattice. A tungsten-doped layered lithium transition metal oxide may be one in which tungsten is substituted at the transition metal site of the lithium transition metal oxide.

[0056] In this specification, 'inter slab thickness' may refer to the thickness of a lithium-oxygen layer located between transition metal-oxygen layers (TM-O). That is, the inter slab thickness may refer to the thickness of the lithium-oxygen layer (hereinafter, the thickness of the lithium layer). Meanwhile, it may refer to the average thickness at two or more points of the lithium layer.

[0057] In this specification, 'Single Particle' refers to a form of secondary particle in which the number of primary particles constituting the secondary particle is small, and it may be a single particle form consisting of one primary particle, or a secondary particle form in which several primary particles are aggregated. That is, it is a concept distinguished from a secondary particle formed by the aggregation of hundreds of primary particles. Specifically, it may refer to a form in which the secondary particle consists of primary particles fewer than the number described below.

[0058] In this specification, a 'Primary Particle' is a basic unit that forms a 'Secondary Particle,' which is an aggregate of particles, and the Primary Particle and the Secondary Particle are distinguished by the presence or absence of particle aggregation. When multiple Primary Particles aggregate to form a Secondary Particle, a particle interface existing between the Primary Particles may exist within the Secondary Particle. The Primary Particle may refer to the smallest unit demarcated by the particle interface when observing the positive electrode active material using a Scanning Electron Microscope (SEM). Additionally, the Primary Particle may refer to a particle in a state where the positive electrode active material containing the Secondary Particle has been sufficiently crushed in a grinder or disperser.

[0059] In this specification, 'single crystal' refers to a particle form having a single crystal grain inside the particle. Alternatively, it may be a form that does not contain a crystal boundary inside the particle. Since the single crystal is distinguished by the number of crystals inside the particle, it is distinguished from the concept of a single particle defined based on the number of primary particles forming the particle, regardless of the type and number of crystals inside. When the positive electrode active material is of the single crystal type, structural stability is improved compared to the polycrystalline type, and high-speed charging characteristics are excellent due to improved lithium ion conductivity.

[0060] In this specification, the content of the components of the cathode active material can be quantified by known methods. For example, the Inductively Coupled Plasma Method (ICP) may be used. Specifically, Inductively Coupled Plasma-Optical Emission Spectroscopy (ICP-OES) or Inductively Coupled Plasma-Mass Spectrometry (ICP-MS) methods may be used.

[0061] In this specification, 'particle diameter' may be the diameter assuming the particle is spherical. In this case, the spherical shape may be the smallest circle among perfect circles that can contain the entire cross-section of the particle.

[0062] In this specification, 'grain' refers to a region in which atoms within a sample are arranged continuously and periodically in one direction. The grain can be analyzed using an Electron Backscatter Diffraction (EBSD) analyzer. Electron backscatter diffraction is a crystal orientation analysis method that is positioned between X-Ray Diffraction Analysis (XRD) and Transmission Electron Microscopy (TEM), and is a method for confirming the orientation of grains that form the microstructure of a material.

[0063] In this specification, 'grain size' refers to the size of a region having an aligned atomic arrangement. This region is named as a single grain and forms a boundary with other grains. The average grain size can be quantitatively analyzed using X-ray diffraction analysis (XRD) by Cu Kα X-rays. Specifically, X-ray diffraction analysis data of the synthesized cathode active material is obtained using a Bruker D8 XRD instrument (Cu-target, voltage: 45kV, current: 40mA, 2θ: 10° to 100°), and structural analysis of the obtained data can be performed using the Rietveld refining method, a general structural analysis method, using Malvern Panalytical's Highscore software. The Rietveld refining method is a method in which a diffraction pattern is calculated from an initial structural model that the crystal structure of the materials may have, and this is compared with the measured diffraction pattern of the actual synthesized material. Various structure-related factors are introduced and their values ​​are changed to gradually and iteratively adjust the pattern until the two patterns match well. This method adopts a method of repeating until the difference between the two patterns is minimized, while determining validity based on the difference between the calculation pattern and the measurement pattern. Among the structure-related factors that can be introduced in this process, the crystal size can be derived using the Full Width at Half Maximum (FWHM) of each crystal plane peak appearing in the measurement diffraction pattern.

[0064] In this specification, 'Dn' refers to the particle size at the n% point of the cumulative volume distribution according to particle size. For example, in a cumulative particle size distribution curve based on volume, it may be the particle size of a lithium transition metal oxide at which the cumulative volume ratio becomes n%. That is, D 50 is the particle size at the 50% point of the cumulative volume distribution according to particle size, and D 90 is the particle size at the 90% point of the cumulative volume distribution according to particle size, and D 10Dn is the particle size at the 10% point of the cumulative volume distribution according to particle size. The above Dn can be measured using the Laser Diffraction Method. Specifically, after dispersing the powder to be measured in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) to calculate the particle size distribution by measuring the difference in diffraction patterns according to particle size as the particles pass through the laser beam. By calculating the particle diameters at the points corresponding to 10%, 50%, and 90% of the cumulative volume distribution according to particle size in the measuring device, D 10 , D 50 and D 90 It can measure.

[0065] The present invention comprises a tungsten-doped layered lithium transition metal oxide, and

[0066] A positive active material is provided having a value calculated by the following Equation 1 that is 33 or higher and 42 or lower.

[0067] [Equation 1]

[0068] T IS / L FWHM

[0069] In the above Equation 1,

[0070] T IS is the interslab thickness (unit: Å) measured by X-ray diffraction analysis, and

[0071] L FWHM is the full width at half maximum (in degrees) of the (003) plane peak measured by X-ray diffraction analysis.

[0072] The cathode active material of the present invention comprises a tungsten-doped layered lithium transition metal oxide. In this case, tungsten diffused into the lithium transition metal oxide substitutes the transition metal sites, thereby stabilizing the lattice structure, improving high-temperature lifespan and capacity retention rate, and preventing an increase in internal resistance. Specifically, tungsten is an element with a high melting point (approx. 3,422°C), and when tungsten substitutes the lattice structure, the structure can be maintained at high temperatures. Furthermore, since tungsten has a high oxidation state (+6), it has excellent bonding affinity with oxygen. By strongly attracting oxygen ions within the lattice structure and causing the oxygen layer to attract adjacent metal layers, it has the effect of increasing the inter-slab distance between metal layers. At this time, the movement path of lithium ions is expanded within the space of the inter-slab, and the diffusion of lithium ions is facilitated, resulting in improved charge / discharge performance.

[0073] The inventors have developed a positive electrode active material with an improved long lifespan by doping tungsten into a layered lithium transition metal oxide, thereby enhancing structural stability and electrochemical performance through tungsten while maintaining excellent lithium ion mobility, and have completed the present invention.

[0074] In the present invention, the molecule T of Formula 1 above. IS represents the inter-slab thickness. Meanwhile, the denominator L FWHM (003) is the full width at half maximum of the peak corresponding to the diffraction plane, representing the crystallinity and the degree of growth into single particles of lithium transition metal oxide.

[0075] In the present invention, the value calculated by Equation 1 may be 33 or higher and 42 or lower. Preferably, it may be 34 or higher, 35 or higher, 36 or higher, 37 or higher, 38 or higher, or 39 or higher. Additionally, it may be 41.5 or lower, 41 or lower, 40.5 or lower, or 40 or lower. Within the above numerical range, the lithium layer is expanded to an appropriate level by the lattice oxygen-metal layer attraction caused by tungsten doping, thereby sufficiently securing a lithium ion migration path, while the particles grow sufficiently to minimize crystal defects. As a result, lithium ion mobility and lattice structure stability are simultaneously secured during charging and discharging, thereby improving the high-temperature lifespan capacity retention rate and suppressing the increase in resistance.

[0076] In the present invention, the value calculated by the following formula 2 may be 0.58 or higher and 0.65 or lower.

[0077] [Equation 2]

[0078] D SEM / D 50

[0079] D SEM is the average particle size (unit: μm) of the smallest unit particles distinguishable in scanning electron microscope images of lithium transition metal oxides, and

[0080] D 50 is the particle size (unit: μm) at the 50% point of the volume-based cumulative particle size distribution of the above lithium transition metal oxide measured by laser diffraction particle size analysis.

[0081] In the present invention, the value calculated by Equation 2 may be 0.59 or higher, 0.6 or higher, 0.61 or higher, 0.62 or higher, or 0.625 or higher. Additionally, it may be 0.64 or lower, 0.63 or lower, 0.62 or lower, 0.61 or lower, or 0.6 or lower. Within the above numerical range, as the particles grow sufficiently and approach a single-particle form, grain boundary cracking during charging and discharging is suppressed, gas generation is reduced, and particle strength and structural stability can be improved. If the value falls below the above numerical range, the particles are in a state where they have not grown sufficiently, resulting in many grain boundaries. Consequently, microcracks may occur at the grain boundaries during repeated cycles, accelerating side reactions in the electrolyte and potentially reducing lifespan. On the other hand, if the value exceeds the above numerical range, hypertrophic growth of the particles or abnormal single-particle development may occur, leading to an increase in surface defects and an increase in lithium ion diffusion distance, which may result in reduced rate characteristics and cycle stability.

[0082] In the present invention, the above D SEM represents the average particle size of the smallest unit particles distinguishable in a scanning electron microscope image. The said smallest unit particle refers to a single particle independently distinguished by a particle boundary. In this case, the particle boundary may be distinguished by contrast or facet edges. For example, a single smallest unit particle may be demarcated by a continuous facet edge. A straight line connecting any two points on a facet edge demarcating the smallest unit particle may not overlap with other facet edges. The said D SEM can refer to the average particle size of the primary particles.

[0083] The above scanning electron microscope image can be converted into a segmentation image to more clearly define the boundaries between particles. At this time, the scanning electron microscope image can be converted into a segmentation image using an artificial intelligence model. Specifically, after acquiring a scanning electron microscope image of the cathode active material to be measured, the acquired scanning electron microscope image is input into a UNET structure to generate a binary image, the binary image is converted into a distance-converted image based on a distance-converted algorithm, the binary image is filtered using a threshold set based on the distance-converted image, multiple objects included in the filtered binary image are identified, and the scanning electron microscope image is segmented into the smallest particle unit based on the multiple objects. Alternatively, a segmentation image can be obtained using the LG Chem DX program.

[0084] The average particle size of the minimum unit particle may be the equivalent circle diameter (ECD), which is the diameter of a circle having the same area as the minimum unit particle, the ferret diameter, the average value of the major and minor axis lengths, etc. Meanwhile, unless otherwise defined, the average particle size of the minimum unit particle refers to the equivalent circle diameter.

[0085] In the present invention, the value calculated by the following Equation 3 may be 22 or more and 27 or less.

[0086] [Equation 3]

[0087] (T IS ×D SEM ) / (L FWHM ×D 50 )

[0088] In the above Equation 3,

[0089] T IS and L FWHM is equal to the definition in Equation 1, and

[0090] D SEMis the average particle size (unit: μm) of the smallest unit particles distinguishable in scanning electron microscope images of lithium transition metal oxides, and

[0091] D 50 is the particle size (unit: μm) at the 50% point of the volume-based cumulative particle size distribution of the above lithium transition metal oxide measured by laser diffraction particle size analysis.

[0092] (T of Equation 3 above IS ×D SEM ) represents the 'product of the lithium migration path width and the primary particle size,' and is a lithium ion transport index that comprehensively reflects the width of the channels through which lithium ions pass within the cathode active material and the size of the primary particles. In addition, (L FWHM ×D 50 ) is 'L FWHM Crystallinity represented by and D 50 It represents the product of the overall average particle size of the lithium transition metal oxide indicated by, and indicates the degree of single particle growth. That is, the above Equation 3 is an indicator representing the balance between the lithium migration pathway and the degree of single particle growth.

[0093] In the present invention, the value calculated by Equation 3 may be 22.5 or higher, 23 or higher, 23.5 or higher, 24 or higher, or 24.5 or higher. Additionally, it may be 26.5 or lower, 26 or lower, or 25.5 or lower. Within the above numerical range, lattice expansion and single particle growth by tungsten doping proceed simultaneously to an appropriate level, thereby improving the lithium ion migration path and particle strength during charging and discharging.

[0094] In the present invention, the above Equations 1 to 3 can be achieved by controlling the tungsten doping amount, controlling the content of the lithium raw material, controlling the primary calcination temperature, or performing calcination two or more times. Specifically, the thickness of the lithium layer can be controlled by utilizing the strong oxygen bonding force of tungsten having a high oxidation state of +6, and the growth of crystal grains or single particles can be controlled during the primary and secondary calcination processes to satisfy the numerical ranges of Equations 1 to 3 described above.

[0095] In the present invention, the full width at half maximum of the (003) plane peak measured by the X-ray diffraction analysis method may be the full width at half maximum of the peak appearing at a 2θ angle of 18 to 19 degrees. The peak appearing at a 2θ angle of 18 to 19 degrees is a peak corresponding to the (003) plane of the positive electrode active material. The lithium transition metal oxide has a layered structure in which a transition metal-oxygen layer and a lithium layer are alternately stacked, and lithium ion insertion and extraction phenomena occur therein. The (003) plane peak represents the interlayer distance between the transition metal-oxygen layer and the lithium layer of the lithium transition metal oxide.

[0096] In the present invention, the interslab thickness measured by the X-ray diffraction analysis method may be 2.69 Å or more and 3 Å or less. Preferably, it may be 2.692 Å or more, 2.694 Å or more, 2.696 Å or more, 2.698 Å or more, 2.7 Å or more, or 2.702 Å or more. Additionally, it may be 2.9 Å or less, 2.8 Å or less, 2.76 Å or less, 2.75 Å or less, 2.74 Å or less, 2.73 Å or less, or 2.72 Å or less. The interslab thickness may represent the thickness of the lithium layer in the crystal structure. When the above numerical range is satisfied, sufficient space within the interslab is secured, expanding the movement path of lithium ions and facilitating the diffusion of lithium ions, thereby improving charge / discharge performance. On the other hand, when the above numerical range is exceeded, the interlayer bonding is weakened, leading to reduced structural stability and a decrease in cycle life. The above interslab thickness can be calculated as the interslab size (Inter Slab, unit: Å) by performing Rietveld refinement with the space group R-3m applied as the crystal structure model to the X-ray diffraction pattern.

[0097] In the present invention, the full width at half maximum of the (003) plane peak measured by the X-ray diffraction analysis method may be 0.062 or more and 0.08 or less. Preferably, it may be 0.063 or more, 0.064 or more, 0.065 or more, 0.066 or more, or 0.067 or more. Additionally, it may be 0.078 or less, 0.076 or less, 0.074 or less, 0.072 or less, or 0.071 or less. The (003) plane peak is a peak representing the interlayer distance between the transition metal-oxygen layer and the lithium layer of the lithium transition metal oxide, and its full width at half maximum corresponds to a crystallinity indicator reflecting the crystallite size and the degree of crystal defects. Within the above numerical range, the layered structure is stable, the growth of single particles is smooth, and lithium ion diffusion is smooth, thereby improving charge / discharge characteristics.

[0098] In the present invention, the above D SEMThe size may be 1㎛ or larger and 8㎛ or smaller. Preferably, it may be 2㎛ or larger, 2.1㎛ or larger, 2.14㎛ or larger, 2.16㎛ or larger, or 2.18㎛ or larger. Additionally, it may be 7㎛ or smaller, 6㎛ or smaller, 5㎛ or smaller, 4㎛ or smaller, 3㎛ or smaller, 2.8㎛ or smaller, 2.6㎛ or smaller, or 2.4㎛ or smaller. When the above numerical range is satisfied, the intergranular interface characteristics are excellent, resulting in excellent capacity development and preventing easy degradation during repeated battery cycles.

[0099] In the present invention, the average particle size (D) of the positive electrode active material 50 The particle size may be 1㎛ to 20㎛. Preferably, it may be 1.2㎛ or more, 1.4㎛ or more, 1.6㎛ or more, 1.8㎛ or more, 2㎛ or more, 2.2㎛ or more, 2.4㎛ or more, 2.6㎛ or more, 2.8㎛ or more, 3㎛ or more, 3.2㎛ or more, 3.4㎛ or more, or 3.6㎛ or more. Or, it may be 18㎛ or less, 16㎛ or less, 14㎛ or less, 12㎛ or less, 10㎛ or less, 8㎛ or less, 6㎛ or less, 4㎛ or less, 3.9㎛ or less, or 3.8㎛ or less. Within the above numerical range, electrode density and reaction rate can be improved, and a balance between structural stability and reaction rate can be maintained. When it falls below the above numerical range, cycle stability may be reduced due to accelerated side reactions in the electrolyte resulting from the increase in particle surface area. In addition, if the above numerical range is exceeded, the lithium ion diffusion distance increases, which may degrade the rate characteristics.

[0100] In the present invention, some or all of the tungsten may exist in the form of hexavalent ions. When the tungsten element exists in the form of hexavalent ions, it is substituted into the internal lattice of the lithium transition metal oxide, thereby stabilizing the lattice and improving lithium ion mobility. The fact that the tungsten element exists in the form of hexavalent ions means that it exists almost entirely in the form of tungsten oxide. Specifically, 80 mol% or more, 85 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more of the total tungsten may exist in the form of hexavalent ions.

[0101] In the present invention, the content of tungsten may be 600 ppm or more and 1,800 ppm or less based on the total weight of the lithium transition metal oxide. Preferably, it may be 700 ppm or more, 800 ppm or more, 900 ppm or more, 950 ppm or more, or 1,000 ppm or more. Additionally, it may be 1,700 ppm or less, 1,600 ppm or less, 1,550 ppm or less, or 1,500 ppm or less. Specifically, tungsten has a strong bonding force with oxygen, which stabilizes the crystal structure but simultaneously possesses a retardant effect that inhibits particle growth. In the present invention, by controlling the content of the tungsten element to the above numerical range, the structural stability effect provided by tungsten is secured, while allowing single particles to grow sufficiently.

[0102] In the present invention, when the anode active material is thermally analyzed by differential scanning calorimetry, the temperature of the peak at the position where the heat flow is maximum (T MAX ) may be 225°C or higher. Preferably, it may be 226°C or higher, 227°C or higher, 228°C or higher, 229°C or higher, or 230°C or higher. Additionally, it may be 300°C or lower. The peak temperature (T) at the position where the heat flow rate is maximum is MAX) refers to the temperature at which oxygen is released or the crystal structure begins to collapse when the charged anode is heated. Satisfying the above numerical range means that the oxygen-metal layer bond is strengthened by tungsten doping, so that a stable state is maintained without oxygen release or structural collapse even under high-temperature environments.

[0103] In the present invention, the lithium transition metal oxide may be in the form of a single particle. The single particle form is a concept contrasted with the secondary particle form formed by the aggregation of tens to hundreds of primary particles, and refers to a form composed of 10 or fewer primary particles. Specifically, it may be a form in which 1 to 10 or 1 to 5 primary particles are aggregated. When the lithium transition metal oxide is in the form of a single particle, phenomena occurring when it is in the form of multiple particles can be improved. That is, it is possible to prevent phenomena in which microcracks occur at grain boundaries during charging and discharging, causing side reactions or gas generation by the electrolyte penetrating into the grain boundaries, and the crystal structure collapses due to surface oxygen desorption.

[0104] In the present invention, the lithium transition metal oxide may include nickel (Ni), cobalt (Co), and manganese (Mn). The ternary lithium transition metal oxide can simultaneously secure high capacity characteristics and stability by balancing the effects of capacity enhancement, rate characteristic enhancement, structural stability enhancement, and thermal stability enhancement by each element.

[0105] In the present invention, the nickel content may be 50 mol% or more based on the total molar amount of the transition metal. Preferably, it may be 55 mol% or more, 60 mol% or more, 70 mol% or more, or 80 mol% or more. The upper limit may be 95 mol% or less or 90 mol% or less. The transition metal in the total molar amount of the transition metal may be the sum of the molar amounts of nickel, cobalt, and manganese. Within the above numerical range, the energy density and charge / discharge efficiency of the positive electrode active material may be improved.

[0106] In the present invention, the lithium transition metal oxide can be represented by the following chemical formula 1.

[0107] [Chemical Formula 1]

[0108] Li 1+t1 Ni x Co y Mn z W w1 M 1 m1 O2

[0109] In the above chemical formula 1,

[0110] -0.2≤t1<1, 0.5≤x<1, 0 <y≤0.4, 0<z≤0.4, 0<w1≤0.1, 0≤m1≤0.1, x+y+z+w1+m1=1이고,

[0111] M 1 It is one or a combination thereof from the group consisting of Cu, Fe, V, Cr, Ti, Zr, Zn, Al, Ta, Y, In, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo.

[0112] In the present invention, t1 may be -0.1 or greater, 0 or greater, 0.01 or greater, 0.02 or greater, 0.03 or greater, or 0.05 or greater. Additionally, it may be 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, or 0.1 or less. When the above numerical range is satisfied, energy density, charge / discharge efficiency, and structural stability may be improved.

[0113] In the present invention, x is the mole fraction of nickel (Ni) among transition metals and may be 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.85 or more, 0.88 or more, 0.90 or more, 0.91 or more, 0.92 or more, 0.93 or more, 0.94 or more, 0.95 or more, or 0.96 or more. Additionally, it may be less than 1.0, 0.99 or less, 0.98 or less, 0.97 or less, or 0.96 or less. Battery capacity can be improved within the above numerical range. Meanwhile, as the operating voltage increases, there is an effect of improving energy density.

[0114] In the present invention, y is the mole fraction of cobalt (Co) among transition metals and may be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more. Additionally, it may be 0.4 or less, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less.

[0115] In the present invention, z is the mole fraction of manganese (Mn) among the transition metals and may be greater than 0, 0.01 or more, or 0.05 or more. Additionally, it may be 0.4 or less, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less.

[0116] In the present invention, w1 is the mole fraction of element W among transition metals, 1×10 -4 Above, 2×10 -4 That is, 3×10 -4 That is, 4×10 -4 5×10 -4 It may be more than 1×10 -2 Below, 5×10 -3 Below, 1×10 -3 It may be less than or equal to. Meanwhile, w1 may be adjusted within a range that satisfies the tungsten content unit described above.

[0117] In the present invention, m1 is an element M among transition metals. 1 1×10 as a mole fraction -5 Above, 1×10 -4 Above, 2×10 -4 That is, 3×10 -4 That is, 4×10 -4 5×10 -4 It may be more than 1×10 -2 Below, 5×10 -3 Below, 1×10 -3 It may be less than.

[0118] In the present invention, the lithium transition metal oxide may further include a coating portion comprising cobalt (Co) on part or all of its surface. The coating portion may further include Al, Zr, or a combination thereof. When the positive electrode active material further includes the coating portion, the amount of residual lithium byproducts may be reduced, structural stability may be increased to improve battery life and resistance performance, and gas generation may also be reduced. In this case, the coating portion may have the form of a thin film and may be formed over the entire lithium composite transition metal oxide or locally.

[0119] In the present invention, the Co present in the coating portion may be included in an amount of 0.5 mol% to 3 mol% relative to the total molar amount of transition metals excluding lithium included in the lithium composite transition metal oxide. In this case, residual lithium byproducts may be further reduced, and lifespan and resistance performance may be further improved.

[0120] The present invention comprises the step of preparing a first mixture by mixing a positive electrode active material precursor and a first lithium-containing raw material;

[0121] A step of manufacturing a primary fired product by primary firing the above first mixture;

[0122] A step of preparing a second mixture by mixing a second lithium-containing raw material with the first calcined product; and

[0123] The method includes the step of manufacturing a secondary fired product by secondarily firing the second mixture,

[0124] The first mixture, the second mixture, or a combination thereof comprises a tungsten-containing raw material including tungsten, and

[0125] A method for manufacturing the above-described positive electrode active material is provided, wherein the content of the above-described positive electrode active material is 600 ppm or more and 1,800 ppm or less based on the total weight of the above-described positive electrode active material precursor.

[0126] The inventors completed the present invention by confirming that the above-described Equation 1 is satisfied by adjusting the tungsten content to be 600 ppm or more and 1,800 ppm or less based on the total weight of the cathode active material precursor. Meanwhile, by dividing and adding the lithium-containing raw material into the first and second calcination processes and controlling the calcination temperature, the effect of controlling the tungsten content could be more easily manifested.

[0127] In the present invention, the positive active material precursor may be represented by the following chemical formula 2 or chemical formula 3.

[0128] [Chemical Formula 2]

[0129] Ni x2 Co y2 Mn z2 M 1 m2 (OH)2

[0130] [Chemical Formula 3]

[0131] Ni x3 Co y3 Mn z3 M 1 m3 OOH

[0132] In the above chemical formulas 2 and 3,

[0133] The definitions of x2 and x3 are the same as the above-described x, the definitions of y2 and y3 are the same as the above-described y, the definitions of z2 and z3 are the same as the above-described z, the definitions of m2 and m3 are the same as the above-described m1, x2+y2+z2+m2=1, and x3+y3+z3+m3=1.

[0134] In the present invention, the anode active material precursor may include nickel (Ni), cobalt (Co), and manganese (Mn). Specifically, it may be a co-precipitated compound in which these transition metals are co-precipitated.

[0135] In the present invention, the average particle size (D) of the positive electrode active material precursor is 50 The particle size may be 1㎛ or more and 10㎛ or less, preferably 2㎛ or more, 2.5㎛ or more, or 3㎛ or more. Additionally, it may be 6㎛ or less or 5㎛ or less. Within the above numerical range, the behavior of primary particles aggregating and growing into single-particle forms during primary calcination can proceed to an appropriate level. If the average particle size of the precursor is too small, particle growth may proceed excessively during primary calcination, leading to hypertrophic growth, and if it is too large, aggregation into single-particle forms may not occur sufficiently.

[0136] In the present invention, the first lithium-containing raw material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and specifically may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, or Li3C6H5O7, and any one or more of these may be used.

[0137] Preferably, the first lithium raw material may be lithium carbonate (Li2CO3). Lithium carbonate decomposes in the high-temperature region (800°C or higher) of the primary calcination described later, causing lithium to be slowly inserted into the precursor, which has the advantage of effectively inducing the behavior of primary particles to aggregate and grow into single particles.

[0138] In the present invention, the ratio (Me:Li) of the total moles of transition metal (Me) included in the positive electrode active material precursor and the Li of the first lithium raw material may be 1:0.98 or higher and 1:1.1 or lower. Preferably, it may be 1:1.01 or higher, 1:1.02 or higher, or 1:1.03 or higher. Additionally, it may be 1:1.06 or lower, 1:1.05 or lower, or 1:1.04 or lower. Within the above numerical range, lithium is inserted into the precursor lattice to an appropriate level during the first calcination, thereby forming a first calcined product with a stable layered structure, and suppressing the generation of residual lithium byproducts.

[0139] In the present invention, the tungsten-containing raw material may be a hydroxide, oxide, chloride, nitrate, sulfur oxide, sulfide, etc. containing tungsten. Preferably, it may be tungsten oxide. During the first calcination, the tungsten oxide diffuses into the lattice and substitutes the transition metal sites in the form of +6 valence ions, thereby having the effect of strengthening the bonding strength of the lattice oxygen-metal layer and expanding the interslab.

[0140] In the present invention, the content of the tungsten-containing raw material may be 600 ppm or more and 1,800 ppm or less based on the total weight of the cathode active material precursor. Preferably, it may be 700 ppm or more, 800 ppm or more, 900 ppm or more, 950 ppm or more, or 1,000 ppm or more. Additionally, it may be 1,700 ppm or less, 1,600 ppm or less, 1,550 ppm or less, or 1,500 ppm or less. Within the above numerical range, while sufficiently securing the lattice stabilization effect by tungsten, the primary particle growth inhibition effect (retardant effect) due to the strong WO bonding force of tungsten is not excessively expressed, allowing single particles to grow to an appropriate level.

[0141] In the present invention, it is preferable that 90 wt% or more of the tungsten-containing raw material used in the manufacturing process be added to the primary mixture. In this case, tungsten can sufficiently diffuse into the lattice in the high-temperature region of the primary calcination, thereby improving the uniformity of lattice substitution and doping efficiency.

[0142] In the present invention, the first mixture, the second mixture, or a combination thereof may include a tungsten-containing raw material containing tungsten. Preferably, 90 wt% or more of the tungsten-containing raw material included in the first mixture and the second mixture may be included in the first mixture. Specifically, 95 wt% or more, 98 wt% or more, or 100% may be included in the first mixture. In this case, tungsten can sufficiently diffuse into the lattice in the high-temperature region of the first calcination, thereby improving the uniformity of lattice substitution and doping efficiency.

[0143] In the present invention, the first mixture, the second mixture, or a combination thereof is M 1 M containing 1 It may include contained raw materials. The above M 1 The contained raw materials may be hydroxides, oxides, chlorides, nitrogen oxides, sulfur oxides, sulfides, etc.

[0144] In the present invention, the above M 1 In the case of yttrium (Y), the yttrium (Y)-containing raw material may be one or more selected from YCl3, Y2O3, Y(NO3)3, Y(OH)3, YSZ, Y2(SO4)3, and Y2S3, specifically one or more selected from Y2O3 and Y(OH)3, and more specifically, Y2O3. The content of the yttrium-containing raw material may be 100 ppm or more and 2,000 ppm or less with respect to the total weight of the cathode active material precursor. Specifically, it may be 100 ppm or more, 200 ppm or more, 300 ppm or more, 400 ppm or more, 500 ppm or more, 600 ppm or more, 700 ppm or more, 800 ppm or more, or 900 ppm or more. In addition, it may be 2,000 ppm or less. In this case, yttrium promotes grain growth, increasing the grain size and thereby improving single-grain properties, and consequently, the capacity and lifespan performance of the battery can be further improved.

[0145] In the present invention, the above M 1 In the case of this zirconium (Zr), the zirconium-containing raw materials are Zr(OH)4, ZrO2, Zr(NO3)4, ZrCl4, ZrS2, Zr(SO4)2, and C8H 12 It may be one or more selected from O8Zr, specifically one or more selected from Zr(OH)4 and ZrO2, and more specifically, ZrO2. The content of the zirconium-containing raw material may be 500 ppm or more and 5,000 ppm or less with respect to the total weight of the cathode active material precursor. Preferably, it may be 1,000 ppm or more and 1,500 ppm or more. Additionally, it may be 5,000 ppm or less, 4,500 ppm or less, or 4,000 ppm or less. In this case, Zr is stably doped into the lithium layer, which has the advantage of further improving structural stability during lithium insertion and extraction, and also improving particle strength.

[0146] In the present invention, in the step of producing a primary calcined product by primary calcining the first mixture, primary particles of the positive electrode active material precursor may aggregate to produce a primary calcined product in the form of single particles. The primary calcination may be performed in an alumina crucible. An alumina crucible is chemically stable at high temperatures and does not have side reactions with lithium and tungsten, so it can prevent the inflow of impurities from the crucible during calcination.

[0147] In the present invention, the step of producing a primary sintered product by primary sintering the first mixture may be performed in an oxygen atmosphere. By performing sintering in an oxygen atmosphere, Ni generated in the high nickel composition 2+ Suppresses the residual of and Ni 2+ ul Ni 3+ By sufficiently oxidizing, the lithium transition metal oxide can be prevented from degenerating into a rock salt structure. In addition, tungsten can be substituted into the lattice while stably maintaining a +6 oxidation state.

[0148] In the present invention, the primary calcination temperature of the step of manufacturing a primary calcined product by primary calcining the first mixture may be 800°C or higher and 980°C or lower. Specifically, it may be 820°C or higher, 840°C or higher, 860°C or higher, 880°C or higher, 900°C or higher, 910°C or higher, or 920°C or higher. Additionally, it may be 980°C or lower, 970°C or lower, 960°C or lower, 950°C or lower, 940°C or lower, or 930°C or lower. Within the above numerical range, a primary calcined product in the form of a structurally stable single particle can be formed as the primary particles of the cathode active material precursor sufficiently aggregate. If the value falls below the above numerical range, the aggregation and growth of the primary particles may not proceed sufficiently, resulting in a multi-particle form with many grain boundaries. In addition, if the above numerical range is exceeded, primary particles grow hypertrophically or crystal defects increase, making it difficult to satisfy the numerical range of Equation 1.

[0149] In the present invention, the first calcination time of the step of first calcining the first mixture to produce a first calcined product may be 3 hours or more and 12 hours or less. Preferably, it may be 4 hours or more, 5 hours or more, 6 hours or more, or 7 hours or more. Additionally, it may be 11 hours or less, 10 hours or less, or 9 hours or less. Within the above numerical range, the primary particles of the anode active material precursor are sufficiently aggregated, and the diffusion into the tungsten lattice proceeds uniformly, so that a structurally stable first calcined product in the form of a single particle can be formed.

[0150] In the present invention, the method may include a step of grinding the primary calcined product before mixing it with a second lithium raw material. The grinding step loosens the aggregated particles of the primary calcined product to increase the particle surface area, thereby enabling the second lithium raw material to uniformly contact and react with the primary calcined product during subsequent secondary calcination. Additionally, since the particle size is homogenized by grinding, the lithium insertion behavior during secondary calcination is homogeneous, which has the effect of preventing the initial resistance of the final cathode active material from increasing.

[0151] In the present invention, the average particle size (D) of the crushed primary calcined product 50 ) may be 1 μm or more and 20 μm or less. Preferably, it may be 2 μm or more and 8 μm or less, and more preferably 3 μm or more and 5 μm or less.

[0152] In the present invention, the grinding can be performed using a pin mill, an ACM, a jet mill, etc., and preferably using a jet mill. Since the jet mill performs grinding through collisions between particles caused by high-pressure air jets, it has the effect of precisely controlling the particle size without damaging the crystal structure of the primary sintered product.

[0153] In the present invention, in the step of manufacturing a secondary sintered product by secondarily sintering the second mixture, the secondary sintered product is manufactured by inserting lithium into the primary sintered product. At this time, the secondary sintered product may be a lithium complex transition metal oxide in the form of a single particle.

[0154] In the present invention, the secondary calcination temperature of the step of manufacturing a secondary calcined product by secondary calcining the second mixture may be 680°C or higher and 900°C or lower. Specifically, it may be 700°C or higher, 720°C or higher, 740°C or higher, 760°C or higher, 780°C or higher, or 790°C or higher. Additionally, it may be 880°C or lower, 860°C or lower, 840°C or lower, 820°C or lower, or 810°C or lower. Within the above numerical range, as lithium is inserted into the rock salt structure, the layered structure is restored, and the generation of lithium byproducts can be prevented.

[0155] In the present invention, the second calcination time of the step of producing a second calcined product by second calcining the second mixture may be 3 hours or more and 12 hours or less. Preferably, it may be 4 hours or more, 5 hours or more, 6 hours or more, or 7 hours or more. Additionally, it may be 11 hours or less, 10 hours or less, or 9 hours or less. Within the above numerical range, as lithium is inserted into the rock salt structure, the layered structure is restored, and the generation of lithium byproducts can be prevented.

[0156] In the present invention, the step of producing a first sintered product by first sintering the first mixture and the step of producing a second sintered product by second sintering the second mixture can each be performed in an oxygen atmosphere. In this case, the degradation of the lithium transition metal oxide into a rock salt structure can be prevented.

[0157] In the present invention, a step of crushing the primary fired product may be included. In this case, there is an effect of preventing the initial resistance from increasing. At this time, the average particle size (D) of the crushed primary fired product 50The ) may be 1㎛ to 20㎛. Preferably, it may be 2㎛ or more or 3㎛ or more. Additionally, it may be 10㎛ or less, 8㎛ or less, 6㎛ or less, or 4㎛ or less. The step of grinding the primary fired product may be performed prior to the step of manufacturing the secondary fired product.

[0158] In the present invention, a step of crushing the secondary fired product may be included. In this case, there is an effect of preventing the initial resistance from increasing. At this time, the average particle size (D) of the crushed secondary fired product 50 ) is the average particle size (D) of the aforementioned lithium transition metal oxide. 50 ) can be applied.

[0159] In the present invention, the step of grinding the primary calcined product and the step of grinding the secondary calcined product can each be performed using a pin mill, an ACM, a jet mill, etc. Meanwhile, the pin mill can be performed under conditions of 18,000 rpm, the ACM can be performed using a machine from Hosokawa under conditions of classification at 6,000 rpm and main grinding at 12,000 rpm, and the jet mill can be performed using a machine from ZM Solution under conditions of a grinding pressure of 6 bar and classification at 3,500 rpm. In this case, the desired average particle size (D 50 A positive electrode active material having ) can be easily obtained.

[0160] In the present invention, the method for manufacturing the cathode active material is characterized by dividing the lithium-containing raw material into a first lithium-containing raw material and a second lithium-containing raw material and adding them in two separate steps. Specifically, the first lithium-containing raw material is added before the first calcination product, and the second lithium-containing raw material is added before the second calcination product. In this case, there is an advantage in that lithium is inserted into the rock salt structure that may be formed on the surface, thereby facilitating recovery to a layered structure. Specifically, the problem of increased lithium by-products caused by adding an excessive amount of the lithium-containing raw material only once can be resolved, and the reaction rate can be increased by adding the lithium-containing raw material during the second calcination step.

[0161] In the present invention, the first lithium-containing raw material and the second lithium-containing raw material may be of the same type. Specifically, they may be lithium hydroxide (LiOH). Since lithium hydroxide has a low melting point of 500°C or lower, it melts rapidly even at a low secondary calcination temperature, allowing it to uniformly penetrate and react with the crushed primary calcined product. That is, by using lithium hydroxide as the second lithium raw material, the layered recovery of the surface rock salt structure and the lithium insertion reaction can be carried out.

[0162] In the present invention, the ratio (Me:Li1) of the total moles of transition metal (Me) included in the positive electrode active material precursor and the Li of the first lithium-containing raw material may be 1:0.98 or higher and 1:1.1 or lower. Preferably, it may be 1:0.99 or higher, 1:1 or higher, 1:1.01 or higher, or 1:1.02 or higher. Additionally, it may be 1:1.09 or lower, 1:1.08 or lower, 1:1.06 or lower, or 1:1.04 or lower.

[0163] In the present invention, the ratio (Me:Li2) of the total moles of transition metal (Me) included in the positive electrode active material precursor and the Li of the second lithium-containing raw material may be 1:0.01 or higher and 1:0.1 or lower. Preferably, it may be 1:0.02 or higher or 1:0.03 or higher. Additionally, it may be 1:0.08 or lower, 1:0.06 or lower, or 1:0.05 or lower. Within the above numerical range, the lithium sites of the final positive electrode active material are sufficiently filled to ensure excellent charge / discharge capacity, while preventing excessive generation of residual lithium byproducts.

[0164] In the present invention, the total moles (Me) of the transition metal included in the positive electrode active material precursor and the ratio of Li of the first lithium-containing raw material and the second lithium-containing raw material (Me:Li total The ratio may be 1:0.99 or higher and 1:1.2 or lower. Preferably, it may be 1:1 or higher, 1:1.01 or higher, 1:1.02 or higher, 1:1.03 or higher, 1:1.04 or higher, or 1:1.05 or higher. Additionally, it may be 1:1.15 or lower, 1:1.12 or lower, 1:1.09 or lower, 1:1.08 or lower, 1:1.07 or lower, or 1:1.06 or lower. Within the above numerical range, excellent charge / discharge capacity is secured while residual lithium byproducts are not excessively generated.

[0165] In the present invention, the second mixture may include a cobalt-containing raw material. In this case, a coating portion containing cobalt may be formed on the secondary sintered product, or cobalt may be doped.

[0166] In the present invention, the cobalt content of the cobalt-containing raw material may be mixed such that the molar amount of cobalt relative to the total molar amount of metals excluding lithium included in the secondary mixture is 1 mol% or more and 10 mol% or more. Specifically, it may be 1.5 mol% or more or 2 mol% or more. Additionally, it may be 5 mol% or less or 4 mol% or less. In this case, residual lithium byproducts can be effectively controlled without including a separate washing process, and a coating layer of appropriate thickness or a surface cobalt-rich layer can be formed, thereby improving surface structural stability.

[0167] In the present invention, the cobalt-containing raw material may be one or more selected from Co(OH)2, Co3O4, CoO, (CH3CO2)2Co, CoCl2, and CoSO4·xH2O, and specifically, may be Co(OH)2. In this case, it may decompose in the secondary calcination temperature range and be converted into active cobalt oxide, and may be uniformly coated on the surface of the primary calcined product or doped into the surface layer.

[0168] In the present invention, in the step of manufacturing a secondary sintered product by secondary sintering of the second mixture, lithium supplied from the second lithium raw material is additionally inserted into the crushed primary sintered product, and at the same time, a cobalt coating portion is formed on the surface. At this time, the secondary sintered product may be a lithium composite transition metal oxide in the form of a single particle.

[0169] In the present invention, the secondary calcination temperature may be 680°C or higher and 900°C or lower. Preferably, it may be 740°C or higher or 780°C or higher. Additionally, it may be 860°C or lower or 820°C or lower. Within the above numerical range, as lithium is inserted into the surface rock salt structure, it recovers into a layered structure, the cobalt-containing raw material is decomposed and activated to form a uniform coating on the surface, and the generation of residual lithium byproducts can be prevented.

[0170] In the present invention, it is preferable that the secondary calcination temperature be lower than the primary calcination temperature. While a high temperature is required in the primary calcination step for aggregation and growth into a single particle form, a relatively low temperature is suitable in the secondary calcination step because only lithium insertion in the surface region and formation of a coating part should occur while maintaining the already formed single particle structure.

[0171] In the present invention, the secondary firing time may be 3 hours or more and 12 hours or less. Preferably, it may be 5 hours or more or 7 hours or more. Additionally, it may be 10 hours or less or 9 hours or less.

[0172] In the present invention, the step of crushing the secondary calcined product to obtain a final positive active material may be included. After secondary calcination, the particles may be in a partially aggregated state, but by crushing, the aggregation can be resolved to obtain a positive active material with a uniform particle size, and the effect of not increasing the initial resistance is achieved.

[0173] In the present invention, the degree of grinding of the secondary sintered product can be performed using a pin mill, ACM, jet mill, etc., and preferably, can be performed using a jet mill.

[0174] The present invention provides a positive electrode comprising the positive electrode active material described above.

[0175] In the present invention, the anode comprises an anode active material layer comprising the anode active material described above. Specifically, the anode comprises an anode current collector; and an anode active material layer provided on the anode current collector. At this time, the anode active material layer may include the anode active material described above. Since the anode active material has been described above, a detailed description is omitted, and only the remaining components are described in detail below.

[0176] In the present invention, the positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive current collector may typically have a thickness of 3 μm to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the bonding strength of the positive active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0177] In the present invention, the positive active material layer may comprise a positive active material, a conductive material, and a binder. At this time, the content of the positive active material may be 80 wt% to 99 wt% based on the total weight of the positive active material layer. Specifically, it may be 85 wt% or more or 90 wt% or more. Additionally, it may be 98.5 wt% or less or 98 wt% or less. Within the above numerical range, excellent capacity characteristics may be exhibited.

[0178] In the present invention, the conductive material is used to impart conductivity to the electrode, and can be used without special limitations as long as it has conductivity without causing chemical changes in the battery. Specific examples include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fibers such as carbon fibers or metal fibers; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The content of the conductive material may be 0.1 wt% to 15 wt% based on the total weight of the positive electrode active material layer.

[0179] In the present invention, the binder serves to improve the adhesion between positive active material particles and the bonding strength between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The content of the binder may be 0.1 wt% to 15 wt% based on the total weight of the positive active material layer.

[0180] In the present invention, the anode may be manufactured according to a conventional method for manufacturing anodes, except for using the anode active material. Specifically, the anode may be manufactured by applying a composition for forming an anode active material layer to an anode current collector, followed by drying and rolling. Specifically, the composition for forming an anode active material layer may be one in which an anode active material, a binder, and a conductive material are dissolved or dispersed in a solvent. In this case, the types and contents of the anode active material, binder, and conductive material are as described above. Alternatively, the anode may be manufactured by casting the composition for forming an anode active material layer onto a separate support, and then laminating the film obtained by peeling from the support onto an anode current collector.

[0181] In the present invention, the solvent may be a solvent generally used in the relevant technical field, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of solvent used is sufficient if it has a viscosity that dissolves or disperses the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.

[0182] The present invention provides an electrochemical device comprising the anode described above. Specifically, the electrochemical device may be a battery, a capacitor, etc., and more specifically, may be a lithium secondary battery.

[0183] The present invention provides a lithium secondary battery comprising the anode described above.

[0184] In the present invention, the lithium secondary battery comprises a positive electrode and a negative electrode positioned opposite to the positive electrode. Additionally, it comprises a separator and an electrolyte provided between the positive electrode and the negative electrode. Since the positive electrode is identical to the one previously described, a detailed description is omitted, and only the remaining components are described in detail below.

[0185] In the present invention, the lithium secondary battery may optionally further include a battery container housing an electrode assembly comprising the positive electrode, the negative electrode, and a separator, and a sealing member sealing the battery container.

[0186] In the present invention, the cathode comprises a cathode current collector and a cathode active material layer provided on the cathode current collector.

[0187] In the present invention, the negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the negative electrode current collector may typically have a thickness of 3 μm to 500 μm, and, similar to the positive electrode current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0188] In the present invention, the negative electrode active material layer may include a negative electrode active material, a binder, and a conductive material.

[0189] In the present invention, the negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples include carbonaceous materials; metallic compounds; metal oxides; composites thereof; or mixtures thereof. The carbonaceous materials include artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, etc. The metallic compounds include metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys. The metal oxides include metal oxides capable of doping and dedoping lithium, such as vanadium oxide and lithium vanadium oxide. The composites include composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites.

[0190] In the present invention, the carbonaceous material may include both low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived coke.

[0191] In the present invention, a metal lithium thin film may be used as the negative electrode active material.

[0192] In the present invention, the content of the negative electrode active material may be 80 wt% to 99 wt% based on the total weight of the negative electrode active material layer.

[0193] In the present invention, the binder is a component that assists in the bonding between the conductive material, the active material, and the current collector, and can typically be added in an amount of 0.1 wt% to 10 wt% relative to the total weight of the negative active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0194] In the present invention, the conductive material may be 10 wt% or less with respect to the total weight of the negative electrode active material layer as a component for further improving the conductivity of the negative electrode active material. Specifically, it may be added in an amount of 5 wt% or less. Such a conductive material is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; metal powders such as carbon fluoride, aluminum, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives may be used.

[0195] In the present invention, the cathode may be manufactured according to a conventional method for manufacturing a cathode, except for using the cathode active material. Specifically, it may be manufactured by applying a composition for forming a cathode active material layer to a cathode current collector, followed by drying and rolling. Specifically, the composition for forming a cathode active material layer may be one in which a cathode active material, a binder, and a conductive material are dissolved or dispersed in a solvent. At this time, the types and contents of the cathode active material, binder, and conductive material are as described above. Alternatively, the cathode may be manufactured by casting the composition for forming a cathode active material layer onto a separate support, and then laminating the film obtained by peeling from the support onto a cathode current collector.

[0196] In the present invention, the separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. Any separator commonly used in lithium secondary batteries may be used without special limitations, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte moisture retention capacity. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fibers or polyethylene terephthalate fibers, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.

[0197] In the present invention, the electrolyte may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc., which can be used in the manufacture of a lithium secondary battery, but is not limited to these.

[0198] In the present invention, the electrolyte may include an organic solvent and a lithium salt.

[0199] In the present invention, the organic solvent may be used without special limitations as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester-based solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether-based solvent such as dibutyl ether or tetrahydrofuran; a ketone-based solvent such as cyclohexanone; or an aromatic hydrocarbon-based solvent such as benzene or fluorobenzene. Carbonate-based solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include an aromatic ring or ether bond of double bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge and discharge performance of the battery and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, the performance of the electrolyte can be improved by mixing cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9.

[0200] In the present invention, the lithium salt can be used without special limitations as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO2, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt may be 0.1 to 5.0 M. Specifically, it is preferable to use it within the range of 0.1 to 3.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0201] In the present invention, the electrolyte may further include additives in addition to the electrolyte components. These additives are intended to improve the lifespan characteristics of the battery, suppress the reduction of battery capacity, and improve the discharge capacity of the battery. The additives may include haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyce, hexamethylphosphoric triamide (HMPA), nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, or combinations thereof. In this case, the total content of the additives may be 0.1 wt% to 10 wt% based on the total weight of the electrolyte. Specifically, it may be 0.2 wt% or more or 1 wt% or more, and 8 wt% or less or 5 wt% or less.

[0202] The positive electrode active material of the present invention has the effect of improving lifespan characteristics or capacity characteristics when applied to a lithium secondary battery. In this case, the lithium secondary battery is useful in fields such as portable devices like mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0203] The present invention can provide a battery module including the above-described lithium secondary battery as a unit cell and a battery pack including the same.

[0204] In the present invention, the battery module or battery pack may be used as a power source for one or more medium-to-large devices, including a power tool; an electric vehicle (EV), a hybrid electric vehicle and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0205] In the present invention, the external shape of the lithium secondary battery is not particularly limited, but can be a cylindrical shape using a can, a prismatic shape, a pouch shape, or a coin shape.

[0206] In the present invention, the lithium secondary battery can be used not only as a battery cell used as a power source for a small device, but can also preferably be used as a unit cell in a medium-to-large battery module comprising a plurality of battery cells.

[0207] The present invention will be explained below through examples.

[0208] <Examples and Comparative Examples>

[0209] <Example 1>

[0210] Cathode active material precursor {Composition: Ni 0.7 Co 0.07 Mn 0.23 (OH)2, average particle size (D 50 ): 4㎛} and the first lithium-containing raw material (Li2CO3) were mixed such that the ratio of the total number of moles of transition metals (Me=Ni+Co+Mn) included in the cathode active material precursor to the number of moles of lithium (Li) included in the lithium-containing raw material (Me:Li=1:1.03).

[0211] Subsequently, a yttrium-containing raw material (manufacturer: Sigma Aldrich, chemical formula: Y2O3) was added so that the yttrium content was 1,000 ppm based on the total weight of the final manufactured cathode active material, and a tungsten-containing raw material (manufacturer: Sigma Aldrich, chemical formula: WO3) was added so that the tungsten content was 1,000 ppm based on the total weight of the final manufactured cathode active material to prepare a first mixture.

[0212] The above first mixture was placed in an alumina crucible and first fired at 925°C for 8 hours under an oxygen (O2) atmosphere to obtain a first fired product.

[0213] The above sintered product is processed using a jet mill to obtain an average particle size (D 50 It was ground to 3.9㎛.

[0214] The crushed calcined product is mixed with the second lithium-containing raw material (LiOH) and the cobalt-containing raw material {Co(OH)2}, and calcined at 800°C for 8 hours under an oxygen (O2) atmosphere to obtain a secondary calcined product, and the average particle size (D 50 A positive electrode active material was prepared by grinding the material to a size of 3.75㎛.

[0215] At this time, the total moles of transition metals in the positive electrode active material precursor (Ni+Co+Mn=Me) and the total moles of lithium included in the first lithium-containing raw material and the second lithium-containing raw material (Li total The rain of ) [Me:Li total =1:1.05], and the moles of cobalt were 3 mol% based on the total moles of transition metals. At this time, the tungsten content was 1,000 ppm based on the total weight of the anode active material.

[0216] <Example 2>

[0217] A positive electrode active material was prepared in the same manner as in Example 1, except that when preparing the first mixture, an yttrium-containing raw material (manufacturer: Sigma Aldrich, chemical formula: Y2O3) was added so that the yttrium content was 1,000 ppm based on the total weight of the final positive electrode active material, and a tungsten-containing raw material (manufacturer: Sigma Aldrich, chemical formula: WO3) was added so that the tungsten content was 1,500 ppm based on the total weight of the final positive electrode active material.

[0218] <Comparative Example 1>

[0219] A positive electrode active material was prepared in the same manner as in Example 1, except that when preparing the first mixture, an yttrium-containing raw material (manufacturer: Sigma Aldrich, chemical formula: Y2O3) was added so that the yttrium content was 1,000 ppm based on the total weight of the final positive electrode active material, and a tungsten-containing raw material (manufacturer: Sigma Aldrich, chemical formula: WO3) was added so that the tungsten content was 500 ppm based on the total weight of the final positive electrode active material.

[0220] <Comparative Example 2>

[0221] A positive electrode active material was prepared in the same manner as in Example 1, except that when preparing the first mixture, an yttrium-containing raw material (manufacturer: Sigma Aldrich, chemical formula: Y2O3) was added so that the yttrium content was 1,000 ppm based on the total weight of the final positive electrode active material, and a tungsten-containing raw material (manufacturer: Sigma Aldrich, chemical formula: WO3) was added so that the tungsten content was 2,000 ppm based on the total weight of the final positive electrode active material.

[0222] <Comparative Example 3>

[0223] When preparing the first mixture, the positive active material precursor {Composition: Ni 0.7 Co 0.07 Mn 0.23 (OH)2, average particle size (D 50): 4㎛} and the first lithium-containing raw material (Li2CO3) were mixed such that the ratio of the total number of moles of transition metals (Me=Ni+Co+Mn) included in the cathode active material precursor to the number of moles of lithium (Li) included in the lithium-containing raw material [Me:Li=1:1.05].

[0224] Subsequently, a yttrium-containing raw material (manufacturer: Sigma Aldrich, chemical formula: Y2O3) was added so that the yttrium content was 1,000 ppm based on the total weight of the final manufactured cathode active material, and a tungsten-containing raw material (manufacturer: Sigma Aldrich, chemical formula: WO3) was added so that the tungsten content was 1,500 ppm based on the total weight of the final manufactured cathode active material to prepare a first mixture.

[0225] The above first mixture was placed in an alumina crucible and first fired at 925°C for 8 hours under an oxygen (O2) atmosphere to obtain a first fired product.

[0226] The anode active material was prepared by grinding the above-mentioned calcined product using a jet mill. That is, secondary calcination as in Example 1 was not performed.

[0227] <Comparative Example 4>

[0228] The first mixture was prepared in the same manner as in Example 1, except that when preparing the first mixture, an yttrium-containing raw material (manufacturer: Sigma Aldrich, chemical formula: Y2O3) was added so that the yttrium content was 1,000 ppm based on the total weight of the final manufactured cathode active material, and a tungsten-containing raw material (manufacturer: Sigma Aldrich, chemical formula: WO3) was added so that the tungsten content was 1,500 ppm based on the total weight of the final manufactured cathode active material.

[0229] A first-stage fired product was prepared in the same manner as in Example 1, except that the firing temperature was changed to 910℃ during the first firing.

[0230] The remaining manufacturing process was performed in the same manner as in Example 1 to produce the positive active material.

[0231] <Comparative Example 5>

[0232] The first mixture was prepared in the same manner as in Example 1, except that when preparing the first mixture, an yttrium-containing raw material (manufacturer: Sigma Aldrich, chemical formula: Y2O3) was added so that the yttrium content was 1,000 ppm based on the total weight of the final manufactured cathode active material, and a zirconium-containing raw material (chemical formula: ZrO2, average particle size: 2 μm) was added so that the zirconium content was 1,500 ppm based on the total weight of the final manufactured cathode active material.

[0233] A first-stage fired product was prepared in the same manner as in Example 1, except that the firing temperature was changed to 920℃ during the first firing.

[0234] The remaining manufacturing process was performed in the same manner as in Example 1 to produce the positive active material.

[0235] <Experimental Example>

[0236] <Experimental Example 1: X-ray Diffraction Analysis>

[0237] For the positive electrode active materials prepared in the examples and comparative examples, X-ray diffraction analysis was performed to obtain the interslab thickness (T IS ) and (003) plane peak full width at half maximum (L FWHM ) was measured.

[0238] The positive electrode active material prepared in the examples and comparative examples was mounted on an X-ray diffraction analysis device, and an X-ray diffraction pattern was obtained by scanning at an angle 2θ. The X-ray diffraction pattern analysis was performed using a Bruker D8 Endeavor (light source: Cu-Kα, λ=1.54Å) equipped with a LynxEye XE-T-position sensitive detector. The sample was placed in a groove of a general powder holder, the surface of the sample was smoothed using a slide glass, and the sample was filled so that its height matched the edge of the holder. Then, measurements were taken for the FDS 0.5°, 2θ=15° to 90° region under conditions of Step Size=0.02° and Total Scan Time=20 minutes. The X-ray diffraction pattern is illustrated in Fig. 1.

[0239] At this time, Figure 1 (a) is the measurement result of the positive electrode active material of Example 1, (b) is Example 2, (c) is Comparative Example 1, and (d) is Comparative Example 2.

[0240] For the X-ray diffraction pattern, by performing Rietveld refinement with the space group R-3m applied as the crystal structure model, the interslab thickness (T IS ) was produced.

[0241] Peak fitting was performed on the (003) plane peak appearing at 2θ angles of 18 to 19 degrees for the X-ray diffraction pattern. From the fitted function, the angle at which the peak reaches maximum intensity and the two left and right angles at which it reaches half intensity were calculated, and the difference between them was used as the full width at half maximum (L) of the (003) plane peak. FWHM ...did it as ).

[0242] <Experimental Example 2: DSEM Measurement>

[0243] Scanning electron microscope (SEM) images (5K magnification) of the cathode active materials prepared in the examples and comparative examples were obtained using a scanning electron microscope device (FEI, Inspect F), and an image was obtained by dividing the boundaries of the primary particles present in the SEM images and displaying them in random colors using an image processing program (LG Chem, DX Program). Using the image with the boundaries of the primary particles divided and displayed in random colors, the total area of ​​n primary particles was calculated, and the average area of ​​the primary particles was calculated by dividing by n. Assuming a perfect circle having an area equal to the average area of ​​the primary particles, the diameter of the circle is D SEM It was calculated as (unit: μm).

[0244] <Experimental Example 3: D50 Measurement>

[0245] After dispersing the cathode active materials prepared in the examples and comparative examples in a dispersion medium, they are introduced into a laser diffraction particle size measuring device (Microtrac S3500, Microtrac) to measure the difference in diffraction patterns according to particle size as the particles pass through a laser beam, thereby calculating the particle size distribution, and the particle diameter D at the point where the cumulative volume distribution according to particle size in the measuring device reaches 50%. 50 (Unit: μm) was calculated.

[0246] <Experimental Example 4: Calculation of Equations 1 to 3>

[0247] Using the physical property values ​​derived from Experimental Examples 1 to 3, the values ​​calculated by the following Equations 1 to 3 were each derived.

[0248] [Equation 1]

[0249] T IS / L FWHM

[0250] In the above Equation 1,

[0251] [Equation 2]

[0252] D SEM / D 50

[0253] [Equation 3]

[0254] (T IS ×D SEM ) / (L FWHM ×D 50 )

[0255] In the above Equations 1 to 3,

[0256] T IS is the interslab thickness (unit: Å) measured by X-ray diffraction analysis, and

[0257] L FWHM is the full width at half maximum (in degrees) of the (003) plane peak measured by X-ray diffraction analysis, and

[0258] D SEM is the average particle size (unit: μm) of the smallest unit particles distinguishable in scanning electron microscope images of lithium transition metal oxides, and

[0259] D 50 is the particle size (unit: μm) at the 50% point of the volume-based cumulative particle size distribution of the above lithium transition metal oxide measured by laser diffraction particle size analysis.

[0260] <Experimental Example 5: Differential Scanning Calorimetry Analysis>

[0261] In the examples and comparative examples, the positive active material, carbon black conductive material, and polyvinylidene fluoride (PVdF) binder prepared in each example were mixed in a weight ratio of 95:2:3 in an N-methylpyrrolidone solvent to prepare a positive composite material, which was then coated on one side of an aluminum current collector, dried at 130°C, and rolled to produce a positive electrode.

[0262] Lithium metal was prepared as the cathode.

[0263] An electrode assembly was manufactured by interposing a porous polyethylene separator between the manufactured positive and negative electrodes, and the electrode assembly was placed inside a case, after which an electrolyte was injected into the case to manufacture a lithium secondary battery. At this time, the electrolyte was prepared by dissolving 1M concentration lithium hexafluorophosphate (LiPF6) in an organic solvent composed of ethylene carbonate / ethyl methyl carbonate / diethyl carbonate (mixed volume ratio of EC / EMC / DEC = 3 / 4 / 3).

[0264] Thermal analysis was performed on each manufactured lithium secondary battery half-cell using a Differential Scanning Calorimetry (SETARAM Instrumentation, Sensys evo DSC) to identify the main peak at which the heat flow was maximum. Specifically, for each manufactured half-cell, the battery was charged in CCCV mode (Constant Current, Constant Voltage) at 25°C with a constant current of 0.1C to 4.45V (termination current: 0.05C). Subsequently, the battery was disassembled while the cathode was washed with dimethyl carbonate (DMC) solvent, and the heat flow was measured using the DSC device while increasing the temperature at a rate of 10°C / min. At this time, the temperature of the peak at the location where the heat flow was maximum (T MAX : ℃) was recorded.

[0265] <Experimental Example 6: Battery Performance Evaluation>

[0266] For each lithium secondary battery half cell manufactured in the same manner as in Experimental Example 5, the 'initial charge capacity' and 'initial discharge capacity' were measured by charging at 25°C in CCCV mode (Constant Current, Constant Voltage) until the voltage reached 4.45V, and then discharging at a constant current of 0.1C until the voltage reached 2.5V after a rest of 20 minutes.

[0267] For each lithium secondary battery half-cell, the discharge capacity (discharge capacity after high-temperature cycle) was measured after performing 100 cycles each of 4.4 V, 1C, 0.05C cut-off CC / CV charging and 2.5 V, 0.5C CC discharging at high temperature (45℃).

[0268] For each lithium secondary battery half-cell, formation was performed at a rate of 0.1C, and then the gas inside the battery was removed (Degas process). After the gas-removed lithium secondary battery was transferred to a charge / discharger at room temperature (25℃), charging was performed at a rate of 0.33C to 4.4V under constant current / constant voltage conditions, followed by a 0.05C cut-off charge, and then discharging at 0.33C 2.5V. After performing the above charge / discharge cycles three times each, the State of Charge (SOC) was set to 50% based on the discharge capacity. At this time, the DC internal resistance was measured using a PNE-0506 charge / discharger (Manufacturer: PNE Solution Co., Ltd., 5V, 6A) through the voltage drop that occurred when a discharge pulse was applied at 2.5C for 10 seconds, and this resistance was set as the 'initial resistance'.

[0269] For each lithium secondary battery half cell, 100 cycles of 4.4 V, 1C, 0.05C cut-off CC / CV charging and 2.5 V, 0.5C CC discharging were performed at high temperature (45℃), then the lithium secondary battery was moved to a charging / discharging device at room temperature (25℃), the State of Charge (SOC) was set to 50%, and the DC internal resistance was measured using a PNE-0506 charging / discharging device (Manufacturer: PNE Solution Co., Ltd., 5V, 6A) through the voltage drop that appeared when a discharge pulse of 2.5C was applied for 10 seconds, and recorded as 'resistance after high-temperature cycle'.

[0270] Based on the above measurements, values ​​calculated using the following Equations 4 and 5 were derived and recorded in Table 1.

[0271] [Equation 4]

[0272] Initial Efficiency = {(Initial Discharge Capacity) / (Initial Charge Capacity)} × 100 (%)

[0273] [Equation 5]

[0274] High-temperature life capacity retention rate (%) = {(Discharge capacity after high-temperature cycle) / (Initial discharge capacity)} × 100 (%)

[0275] [Equation 6]

[0276] High-temperature life resistance increase rate (%) = {(Resistance after high-temperature cycle - Initial resistance) / (Initial resistance)} × 100 (%)

[0277] Classification Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Experimental Example 1T IS (Unit: Å) 2.7025 2.7153 2.6802 2.7312 2.662 12.742 12.6505L FWHM (Unit: degrees) 0.068 0.07 0.061 0.084 0.062 0.086 0.06 Experimental Example 2D SEM (Unit: ㎛) 2.3 2.2 2.3 2.1 2.5 2.0 2 2.4 3 Experimental Example 3D 50 (Unit: μm) 3.65 3.7 3.72 3.6 3.7 3.65 3.68 Experimental Example 4 Formula 1 39.7 38.8 43.9 32.5 42.9 31.9 44.2 Formula 2 20.6 30.5 90.6 20.5 80.6 80.5 50.66 Formula 3 25.0 23.1 27.2 18.8 29.0 17.6 29.2 Experimental Example 5 (T MAX : ℃) 225 or higher 225 or higher 225 or higher 225 or higher Unmeasured Unmeasured Unmeasured Experiment Example 6 Initial Efficiency (%) 91.4 91.2 91 91 90.6 90.7 91 High-temperature Life Capacity Retention Rate (%) 97 96.8 96.6 96.5 92.3 95.5 96.4 High-temperature Life Resistance Increase Rate (%) 29.2 30.2 34.3 32.1 42.1 36.3 33.2

[0278] From the above results, it was confirmed that the positive electrode active material with a value calculated by Equation 1 of 33 or higher and 42 or lower has a high high-temperature life capacity retention rate and a low high-temperature life resistance increase rate (Examples 1 and 2).

[0279] On the other hand, it was confirmed that positive electrode active materials with a value calculated by Equation 1 that is less than 33 or exceeds 42 have a low high-temperature life capacity retention rate or a high high-temperature life resistance increase rate (Comparative Examples 1 to 5).

Claims

1. Includes a tungsten-doped layered lithium transition metal oxide, and Anode active material having a value calculated by Formula 1 below of 33 or more and 42 or less: [Equation 1] T IS / L FWHM In the above Equation 1, T IS is the interslab thickness (unit: Å) measured by X-ray diffraction analysis, and L FWHM is the full width at half maximum (in degrees) of the (003) plane peak measured by X-ray diffraction analysis.

2. In Claim 1, A positive active material having a value calculated by Equation 2 below of 0.58 or higher and 0.65 or lower: [Equation 2] D SEM / D 50 In Equation 2, D SEM is the average particle size (unit: μm) of the smallest unit particles distinguishable in scanning electron microscope images of lithium transition metal oxides, and D 50 is the particle size (unit: μm) at the 50% point of the volume-based cumulative particle size distribution of the above lithium transition metal oxide measured by laser diffraction particle size analysis.

3. In Claim 1, Anode active material having a value calculated by Equation 3 below of 22 or more and 27 or less: [Equation 3] (T IS ×D SEM ) / (L FWHM ×D 50 ) In the above Equation 3, T IS and L FWHM is equal to the definition in Equation 1, and D SEM is the average particle size (unit: μm) of the smallest unit particles distinguishable in scanning electron microscope images of lithium transition metal oxides, and D 50 is the particle size (unit: μm) at the 50% point of the volume-based cumulative particle size distribution of the above lithium transition metal oxide measured by laser diffraction particle size analysis.

4. In Claim 1, A positive active material having an interslab thickness of 2.69 Å or more and 3 Å or less as measured by the above X-ray diffraction analysis method.

5. In Claim 1, A positive active material having a full width at half maximum of the (003) plane peak measured by the above X-ray diffraction analysis method of 0.062 or more and 0.08 or less.

6. In Claim 1, Average particle size (D 50 A positive electrode active material having a thickness of 1㎛ to 20㎛.

7. In Claim 1, A positive active material in which part or all of the above tungsten exists in the form of hexavalent ions.

8. In Claim 1, A positive electrode active material having a tungsten content of 600 ppm or more and 1,800 ppm or less based on the total weight of the lithium transition metal oxide.

9. In Claim 1, When the above-mentioned positive active material is thermally analyzed by differential scanning calorimetry, the temperature of the peak at the position where the heat flow is maximum (T MAX A positive active material having a temperature of 225°C or higher.

10. In Claim 1, The above lithium transition metal oxide is a positive electrode active material in the form of a single particle.

11. In Claim 1, The above lithium transition metal oxide is a positive active material comprising nickel (Ni), cobalt (Co), and manganese (Mn).

12. In Claim 1, A positive electrode active material having a nickel content of 50 mol% or more based on the total molar amount of transition metals.

13. In Claim 1, A positive active material in which the above lithium transition metal oxide is represented by the following chemical formula 1: [Chemical Formula 1] Li 1+t1 Ni x Co y Mr z W w1 M 1 m1 O2 In the above chemical formula 1, -0.2≤t1<1, 0.5≤x<1, 0 <y≤0.4, 0<z≤0.4, 0<w1≤0.1, 0≤m1≤0.1, x+y+z+w1+m1=1이고, M 1 It is one or a combination thereof from the group consisting of Cu, Fe, V, Cr, Ti, Zr, Zn, Al, Ta, Y, In, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo.

14. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 13.

15. A lithium secondary battery comprising a positive electrode according to claim 14.