Positive electrode active material, positive electrode comprising same and rechargeable lithium batteries
A lithium nickel-based composite oxide cathode active material with controlled single crystallinity and angle of repose addresses the challenges of high capacity, energy density, and long lifespan in lithium secondary batteries, optimizing performance and stability.
Patent Information
- Application Number
- PCT/KR2026/096650
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing lithium secondary batteries face challenges in achieving high capacity, high energy density, and long lifespan while maintaining stability and efficiency, particularly at high voltages.
A cathode active material composed of a lithium nickel-based composite oxide is formulated as single particles with controlled single crystallinity, specific surface area, and angle of repose to optimize capacity, energy density, and lifespan.
The cathode active material enhances battery capacity, energy density, and lifespan by ensuring uniform distribution and preventing degradation, while maintaining high-temperature storage characteristics.
Smart Images

Figure KR2026096650_12112026_PF_FP_ABST
Abstract
Description
Cathode active material, a cathode including the same, and a lithium secondary battery
[0001] The invention relates to a positive electrode active material, a positive electrode containing the same, and a lithium secondary battery.
[0002] Lithium-ion batteries, which offer high energy density and portability, are primarily used as the power source for mobile information terminals such as mobile phones, laptops, and smartphones. Recently, active research is being conducted to utilize high-energy-density lithium-ion batteries as power sources for driving or energy storage in hybrid and electric vehicles.
[0003] Various cathode active materials are being examined to realize lithium secondary batteries suitable for these applications. With the recent surge in demand for large, high-capacity, or high-energy-density lithium secondary batteries, there is a need to develop cathode active materials that ensure stability while increasing capacity, enabling operation at high voltages, and offering high electrode density and improved capacity per unit volume.
[0004] We provide a cathode active material capable of realizing high density, high capacity, long lifespan characteristics, and high energy density, as well as a cathode and a lithium secondary battery applying the same.
[0005] In one embodiment, the positive electrode active material contains a lithium nickel-based composite oxide and is in the form of a single particle, the degree of single crystallization according to Formula 1 below of the positive electrode active material is 0.4 to 0.7, and the BET specific surface area of the positive electrode active material is 1.0 m² 2 A positive active material is provided having a value of 0.8 to 1.2 according to Equation 2 below, and a difference in the angle of repose according to Equation 3 below, which is 5° to 20°.
[0006] [Equation 1]
[0007] Single crystal degree = (BET specific surface area) / (span)
[0008] [Equation 2]
[0009] Span = (D 90 -D 10 ) / D 50
[0010] In the above Equation 2, D 10 is the particle diameter of the particle with a cumulative volume of 10 volume% in the particle size distribution, D 50 D is the particle size of the particle with a cumulative volume of 50 volume% in the particle size distribution. 90 represents the particle size of the particle whose cumulative volume is 90 volume% in the particle size distribution, and
[0011] [Equation 3]
[0012] The difference in angle of repose means = (maximum angle formed by the free surface of the powder deposition layer with the horizontal when the anode active material powder is stacked) - (minimum angle formed by the free surface of the powder deposition layer with the horizontal when the anode active material powder is stacked).
[0013] In another embodiment, a current collector; and a positive active material layer located on the current collector; wherein the positive active material layer provides a positive electrode comprising the positive active material.
[0014] In another embodiment, a lithium secondary battery comprising a positive electrode; a negative electrode; and an electrolyte is provided.
[0015] The cathode active material according to one embodiment maximizes capacity while minimizing production costs, ensuring long lifespan characteristics and improving high-temperature storage characteristics. A lithium secondary battery applying the cathode active material can exhibit high initial charge / discharge capacity and efficiency, and can achieve long lifespan characteristics.
[0016] FIG. 1 is a schematic perspective view showing a portion of a cylindrical lithium secondary battery cut off.
[0017] Figure 2 is a cross-sectional view schematically illustrating a prismatic lithium secondary battery.
[0018] Figures 3 and 4 are schematic exploded perspective views of a pouch-type lithium secondary battery.
[0019] Figure 5 is a figure showing the minimum and maximum angles that the free surface of the powder deposition layer makes with the horizontal when the positive active material powder prepared according to Example 1 is stacked.
[0020] Figure 6 is a figure showing the minimum and maximum angles that the free surface of the powder deposition layer makes with the horizontal when the positive active material powder prepared according to Comparative Example 1 is stacked.
[0021] Specific embodiments are described below in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0022] The terms used herein are for describing exemplary embodiments only and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise.
[0023] Here, "combinations of these" refers to mixtures of components, laminates, composites, copolymers, alloys, blends, reaction products, etc.
[0024] The terms "include," "equip," or "have" used herein are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should not be understood as precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0025] In the drawings, thicknesses have been enlarged to clearly represent various layers and regions, and the same reference numerals have been used for similar parts throughout the specification. When a part such as a layer, film, region, or plate is described as being "on" or "on" another part, this includes not only cases where it is "immediately on" another part, but also cases where there is another part in between. Conversely, when a part is described as being "immediately on" another part, it means that there is no other part in between.
[0026] In addition, the term “layer” here includes not only the shape formed on the entire surface when viewed in a plan view, but also the shape formed on some surfaces.
[0027] The average particle size can be measured by methods widely known to those skilled in the art, for example, by measuring with a particle size analyzer, or by using transmission electron microscope or scanning electron microscope images. Alternatively, the average particle size value can be obtained by measuring using dynamic light scattering, performing data analysis to count the number of particles for each particle size range, and then calculating from this. Unless otherwise defined, the average particle size is the diameter (D) of the particle at which the cumulative volume in the particle size distribution is 50 volume%. 50 It may mean ). In addition, unless otherwise defined, the average particle size is obtained by measuring the size (diameter or length of the major axis) of approximately 20 randomly selected particles from scanning electron microscope images to obtain a particle size distribution, and the diameter (D) of the particle with a cumulative volume of 50% in the said particle size distribution. 50 It may be that ) was taken as the average particle size.
[0028] Here, “or” is not interpreted in an exclusive sense; for example, “A or B” is interpreted to include A, B, A+B, etc.
[0029] The term “metal” is interpreted as a concept that includes common metals, transition metals, and metalloids (semimetals).
[0030] positive electrode active material
[0031] In one embodiment, the positive electrode active material contains a lithium nickel-based composite oxide and is in the form of a single particle, the degree of single crystallization according to Formula 1 below of the positive electrode active material is 0.4 to 0.7, and the BET specific surface area of the positive electrode active material is 1.0 g / m² 2 The present invention provides a positive active material having the following span according to Equation 2 below, which is 0.8 to 1.2, and the difference in the angle of repose according to Equation 3 below, which is 5° to 20°.
[0032] [Equation 1]
[0033] Single crystal degree = BET specific surface area / span
[0034] [Equation 2]
[0035] Span = (D 90 -D 10 ) / D 50
[0036] In the above Equation 2, D 10 is the particle diameter of the particle with a cumulative volume of 10 volume% in the particle size distribution, D 50 D is the particle size of the particle with a cumulative volume of 50 volume% in the particle size distribution. 90 represents the particle size of the particle whose cumulative volume is 90 volume% in the particle size distribution, and
[0037] [Equation 3]
[0038] The difference in angle of repose means: the maximum angle that the free surface of the powder deposition layer makes with the horizontal when the positive active material powder is stacked minus the minimum angle that the free surface of the powder deposition layer makes with the horizontal when the positive active material powder is stacked.
[0039] Designs have been proposed to maximize capacity and energy density and realize long lifespan characteristics by controlling the physical properties of a cathode active material containing a lithium nickel-based composite oxide. Accordingly, in one embodiment, D according to the particle size distribution of a cathode active material containing a lithium nickel-based composite oxide 10, D 50 and D 90 By controlling the span and the specific surface area of the positive electrode active material, the degree of single crystallinity can be calculated to maximize the capacity and energy density of the battery and achieve long life characteristics.
[0040] A positive electrode active material according to one embodiment contains a lithium nickel-based composite oxide, and the lithium nickel-based composite oxide can be represented by the following chemical formula 1.
[0041] [Chemical Formula 1]
[0042] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1
[0043] In Chemical Formula 1, 0.9≤a1≤1.8, 0.3≤x1≤1, 0≤y1≤0.7, 0≤z1≤0.7, 0.9≤x1+y1+z1≤1.1 and 0≤b1≤0.1, and M 1 and M 2 may be different elements and each independently is one or more of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more of F, P, and S.
[0044] In Chemical Formula 1, 0.6≤x1≤1, 0≤y1≤0.4 and 0≤z1≤0.4, or 0.8≤x1≤1, 0≤y1≤0.2 and 0≤z1≤0.2, or 0.9≤x1<1, 0 <y1≤0.1 및 0≤z1≤0.1일 수 있다.
[0045] The above lithium nickel-based composite oxide can be represented by the following chemical formula 2 or chemical formula 3 as a specific example.
[0046] [Chemical Formula 2]
[0047] Li a2 Ni x2 Coy2 M 3 z2 O 2-b2 X b2
[0048] In the above chemical formula 2, 0.9≤a2≤1.2, 0.8≤x2<1, 0 <y2≤0.2, 0≤z2≤0.2, 0.9≤x2+y2+z2≤1.1 및 0≤b2≤0.1이고 M 3 is one or more of the elements Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more of the elements F, P, and S.
[0049] In the above chemical formula 2, 0.9≤x2≤0.99, 0.01≤y2≤0.1 and 0≤z2≤0.1 may be used.
[0050] [Chemical Formula 3]
[0051] Li a3 Ni x3 Co y3 M 4 z3 M 5 w3 O 2-b3 X b3
[0052] In the above chemical formula 3, 0.9≤a3≤1.2, 0.8≤x3≤0.98, 0.01≤y3≤0.19, 0.01≤z3≤0.19, 0≤w3≤0.19, 0.9≤x3+y3+z3+w3≤1.1 and 0≤b3≤0.1, and M 4 is one or more elements of Al and Mn, and M 5 is one or more of the elements B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more of the elements F, P, and S.
[0053] In the above chemical formula 3, 0.9≤x3≤0.98, 0.01≤y3≤0.09, 0.01≤z3≤0.09 and 0≤w3≤0.09 may be used.
[0054] For example, the lithium nickel-based composite oxide may be a high-nickel cathode active material in which the nickel content relative to 100 mol% of the total metal excluding lithium in the lithium nickel-based composite oxide is 80 mol% or more, 85 mol% or more, 90 mol% or more, 91 mol% or more, or 94 mol% or more, and 99 mol% or less. The high-nickel cathode active material can achieve high capacity and can be applied to high-capacity, high-density lithium secondary batteries.
[0055] The cathode active material containing the above lithium nickel-based composite oxide is in the form of a single particle. The single particle refers to a particle that exists alone without grain boundaries within the particle and consists of a single particle. Morphologically, it may refer to a single particle, a monolith structure, a monolithic structure, or a non-aggregated particle existing in an independent phase where the particles are not mutually aggregated, and as an example, it may be a single crystal. The single particle may exist alone, or the single particles may be clustered together. For example, 2 to 10 single particles may be clustered together and in contact with each other.
[0056] In one embodiment, the degree of single crystallization according to Formula 1 of the anode active material is 0.4 to 0.7, and may be, for example, 0.45 to 0.7, 0.45 to 0.65, 0.45 to 0.6, 0.4 to 0.65, 0.4 to 0.6, or 0.5 to 0.6. The degree of single crystallization is a numerical value that can represent the degree of single crystallization of the anode active material in the form of a single particle, and can be expressed as the ratio of the BET specific surface area to the span of the anode active material in the form of a single particle. When the degree of single crystallization of the anode active material in the form of a single particle falls within the above range, improved lifespan characteristics can be exhibited while realizing high capacity and high energy density.
[0057] [Equation 1]
[0058] Degree of single crystallinity = (BET specific surface area) / span
[0059] The BET specific surface area in Equation 1 above can be measured by the nitrogen gas adsorption method, and the span can be measured using a particle size analyzer with laser diffraction, as described specifically below.
[0060] In one embodiment, the BET specific surface area of the positive electrode active material is 1.0 m 2 / g or less, for example, 0.5 m 2 / g to 0.9 m 2 / g, 0.5 m 2 / g to 0.8 m 2 / g, 0.55 m 2 / g to 0.75 m 2 / g, 0.55 m 2 / g to 0.7 m 2 / g, or 0.55 m 2 / g to 0.65 m 2 It may be / g. The above BET specific surface area may be measured by the nitrogen gas adsorption method using, for example, a specific surface area measuring device HM model-1208 manufactured by MOUNTECH. Specifically, the cathode active material is heated in a pretreatment device, then further pretreated in a specific surface area measuring device, cooled to the temperature of liquid nitrogen, and saturated adsorbed with a gas consisting of 30% nitrogen and 70% He. Afterward, it is heated to room temperature to measure the amount of desorbed gas, and the specific surface area can be calculated from the obtained result by the conventional BET method.
[0061] In one embodiment, the span of the positive active material is 0.8 to 1.2, and may be, for example, 0.9 to 1.2, 1.0 to 1.2, 1.07 to 1.2, or 1.07 to 1.17. In this case, the span can be calculated using Equation 2 below. When the span of the positive active material falls within the above range, the density of the positive active material layer containing the positive active material increases, thereby enabling high energy density and exhibiting high initial charge / discharge capacity and efficiency even under high voltage driving conditions.
[0062] [Equation 2]
[0063] Span = (D 90 -D 10 ) / D 50
[0064] Average particle size (D of the single particle of the above positive active material) 50 ) can be 1 μm to 8 μm, and, for example, 1.5 μm to 7 μm, 2 μm to 6 μm, or 3.6 μm to 4.5 μm. Here, the average particle size (D 50 ) may be obtained by obtaining a particle size distribution for the positive electrode active material using a particle size analyzer and taking the diameter of the particle with a cumulative volume of 50 volume% from the particle size distribution as the average particle size.
[0065] Particle size analysis of the above-mentioned cathode active material may, for example, be performed using a particle size analyzer utilizing laser diffraction, such as the LS13320 (Beckmann Coulter). As for the particle size analysis conditions, the pump speed is 55%, ultrasonic dispersion is performed at 40 KHz for 30 seconds, the run length is 60 seconds, the refractive index is 1.6, the e-factor is 1.00, the sample amount is 0.20g, and the dispersant added to the sample may be 1 ml of 10% sodium hexametaphosphate.
[0066] D of the above positive active material 10... may be 0.5 μm to 3.0 μm, and, for example, may be 1.0 μm to 3.0 μm, 1.0 μm to 2.5 μm, 1.5 μm to 2.5 μm, 2.0 μm to 2.5 μm, 2.1 μm to 2.5 μm, or 2.2 μm to 2.5 μm. Here, D 10 It may be possible to obtain a particle size distribution using a particle size analyzer and take the diameter of a particle with a cumulative volume of 10% of the particle size distribution as the average particle size.
[0067] D of the above positive active material 90 ... may be 6.0 μm to 9.0 μm, for example, 6.0 μm to 8.0 μm, 6.0 μm to 7.0 μm, or 6.3 μm to 6.9 μm. Here, D 90 It may be obtained by using a particle size analyzer to obtain a particle size distribution and taking the diameter of the particle with a cumulative volume of 90% of the particle size distribution as the average particle size. D for the anode active material 50 , D 10 , D 90 If the above range is satisfied, the density of the positive active material layer can be maximized, and accordingly, the capacity of the lithium secondary battery can be increased while simultaneously improving energy density and lifespan characteristics.
[0068] In one embodiment, the difference in the angle of repose of the positive active material may be 5° to 20°, and for example, 7° to 19°, 9° to 18°, or 11° to 17°. In this case, the difference in the angle of repose refers to the average of the difference between the maximum angle formed by the free surface of the powder deposit layer with the horizontal when the positive active material powder is stacked and the minimum angle formed by the free surface of the powder deposit layer with the horizontal when the positive active material powder is stacked. When the difference in the angle of repose falls within the above range, the positive slurry containing the positive active material is evenly delivered to the current collector without the phenomenon of separation or sedimentation of the positive active material, thereby preventing the delamination of the positive active material slurry and simultaneously suppressing the partial concentration of the electrode reaction, so the degradation of the output and lifespan of the lithium secondary battery can be suppressed.
[0069] In this case, the angle of repose refers to the inclination when stacking the positive active material powder, and the roughness of the positive active material powder can be indicated through this inclination. That is, the angle of repose refers to the angle formed by the free surface of a stationary deposit of positive active material powder with the horizontal. The larger the particle size of the particles constituting the positive active material powder, the more angular they are, the higher the moisture content, the greater the cohesiveness, and the less fine particles there are, the larger the angle of repose; conversely, a smaller angle of repose indicates good flowability of the powder. The above angle of repose can be measured, for example, by directly measuring the positive active material after pouring it out from the funnel onto a petri dish with radius r, or by measuring the height of the deposit layer and using the height of the deposit layer. In this case, the angle of repose may be 55° or less, for example, between 15° and 55°. If the above angle of repose is 55° or less, the wetting properties of the positive active material can be optimized when the positive active material slurry is delivered to the current collector. For this reason, the positive active material slurry can be uniformly distributed without the phenomenon of separation or sedimentation of the positive active material. In addition, since the peeling of the positive active material slurry is prevented and the local concentration of the electrode reaction is suppressed, the degradation of the output and lifespan of the lithium secondary battery can be suppressed. Furthermore, when the angle of repose is 15° or greater, the problem of output degradation caused by the low cohesion between the positive active material, the conductive material, and the binder during the preparation of the positive active material slurry, which prevents the positive active material and the conductive material from mixing evenly, can be prevented.
[0070] The bulk density of the above-mentioned cathode active material may be 0.1 g / cc to 1.2 g / cc, for example, 0.3 g / cc to 1.1 g / cc, or 0.6 g / cc to 1.0 g / cc. The cathode according to one embodiment can achieve such a bulk density and, accordingly, can achieve high capacity and energy density. The above-mentioned bulk density refers to the density when simply placed in a container without applying external pressure, and may also be referred to as apparent density. The above-mentioned bulk density can be measured, for example, using a bulk density meter (BT-101, YIMA), and specifically, can be measured using the method of Evaluation Example 4 below.
[0071] anode
[0072] In one embodiment, a positive electrode is provided that includes a current collector and a positive active material layer located on the current collector, wherein the positive active material layer comprises the aforementioned positive active material. The positive active material layer may further include other types of positive active materials in addition to the aforementioned positive active material. Additionally, the positive active material layer may optionally further include a binder, a conductive material, or a combination thereof.
[0073] According to one embodiment, the loading level of the positive active material layer is 5 mg / cm² 2 to 40 mg / cm² 2 It could be, for example, 10 mg / cm² 2 to 35 mg / cm² 2 or 15 mg / cm² 2 to 30 mg / cm² 2In addition, the density of the positive active material layer in the rolled final positive electrode may be 2.8 g / cc to 4.0 g / cc, for example, 3.0 g / cc to 3.8 g / cc or 3.2 g / cc to 3.6 g / cc. When applying the positive active material according to one embodiment, it is advantageous to achieve such loading levels and positive active material layer densities, and a positive electrode satisfying the loading levels and composite densities within the above ranges is suitable for realizing a high-capacity, high-energy-density lithium secondary battery.
[0074] The above loading level may refer to the ratio of weight to the area of the positive active material layer. The loading level may be one of the conditions designed during the process of applying the electrode active material slurry to the current collector. For example, the loading level may be calculated as the ratio of weight to the cross-sectional area of the electrode active material layer when the electrode slurry is applied to the current collector before drying and rolling the electrode plate.
[0075] The density of the above-mentioned positive active material layer refers to the ratio of weight to volume of the positive active material layer in the rolled positive electrode. The density of the above-mentioned positive active material layer can be measured by measuring the cross-sectional area, thickness, and weight of the positive active material layer excluding the positive current collector, calculating the volume by multiplying the cross-sectional area and thickness, and dividing the weight by the volume.
[0076] The thickness of the positive active material layer may be 5 μm to 200 μm, for example, 5 μm to 180 μm, or 10 μm to 150 μm. When the thickness of the positive active material layer satisfies the above range, a battery with high capacity and high energy density can be realized. The thickness of the positive active material layer may be measured using a scanning electron microscope on a cross- section of the positive electrode.
[0077] bookbinder
[0078] The binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples of binders include, but are not limited to, polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylic resin, polyester resin, nylon, etc.
[0079] Challenge
[0080] A conductive material is used to impart conductivity to an electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, and carbon nanotube; metal-based materials containing copper, nickel, aluminum, silver, etc., in the form of metal powder or metal fibers; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0081] The content of the binder and the conductive material may be 0.5% to 5% by weight each with respect to 100% by weight of the positive active material layer.
[0082] Al thin films can be used as the current collector, but are not limited to this.
[0083] lithium secondary battery
[0084] In one embodiment, a lithium secondary battery comprising the aforementioned positive electrode, negative electrode, and electrolyte is provided. As an example, the lithium secondary battery may include a positive electrode, a negative electrode, a separator located between the positive electrode and the negative electrode, and an electrolyte.
[0085] Lithium secondary batteries can be classified into cylindrical, prismatic, pouch, coin, etc., depending on their shape. FIGS. 1 to 4 are schematic diagrams illustrating a lithium secondary battery according to one embodiment, where FIG. 1 is a cylindrical battery, FIG. 2 is a prismatic battery, and FIGS. 3 and 4 are pouch-type batteries. Referring to FIGS. 1 to 4, the lithium secondary battery (100) may include an electrode assembly (40) having a separator (30) interposed between a positive electrode (10) and a negative electrode (20), and a case (50) in which the electrode assembly (40) is housed. The positive electrode (10), the negative electrode (20), and the separator (30) may be impregnated with an electrolyte (not shown). The lithium secondary battery (100) may include a sealing member (60) that seals the case (50) as in FIG. 1. In addition, in FIG. 2, the lithium secondary battery (100) may include a positive lead tab (11) and a positive terminal (12), a negative lead tab (21) and a negative terminal (22). As shown in FIG. 3 and FIG. 4, the lithium secondary battery (100) may include an electrode tab (70), namely a positive tab (71) and a negative tab (72), which serve as an electrical path to guide the current formed in the electrode assembly (40) to the outside.
[0086] cathode
[0087] The cathode may include a current collector and a cathode active material layer located on the current collector, and the cathode active material layer may include a cathode active material and may further include a binder, a conductive material, or a combination thereof.
[0088] cathode active material
[0089] The negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0090] A material capable of reversibly intercalating / deintercalating the above lithium ions may include a carbon-based negative electrode active material, for example, crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0091] As the above lithium metal alloy, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.
[0092] As the material capable of doping and undoping the above lithium, a Si-based negative electrode active material or a Sn-based negative electrode active material may be used. The above Si-based negative electrode active material may include silicon, silicon-carbon composites, and SiO₂. x (0 <x≤2), Si-Q 합금(상기 Q는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소(Si를 제외함), 15족 원소, 16족 원소, 전이금속, 희토류 원소 및 이들의 조합에서 선택되는 원소이며, 예컨대 Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, 및 이들의 조합에서 선택됨), 또는 이들의 조합일 수 있다. 상기 Sn계 음극 활물질로는 Sn, SnO2, Sn 합금 또는 이들의 조합일 수 있다.
[0093] The above silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle size (D) of the silicon-carbon composite particles 50 The thickness may be, for example, 0.5 μm to 20 μm. According to one embodiment, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surface of the silicon particles. For example, it may include a secondary particle (core) assembled from silicon primary particles and an amorphous carbon coating layer (shell) located on the surface of the secondary particle. The amorphous carbon may also be located between the silicon primary particles, so that, for example, the silicon primary particles may be coated with amorphous carbon. The secondary particles may be dispersed in an amorphous carbon matrix.
[0094] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core comprising crystalline carbon and silicon particles and an amorphous carbon coating layer located on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. Examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0095] When the silicon-carbon composite comprises silicon and amorphous carbon, the silicon content may be 10% to 50% by weight with respect to 100% by weight of the silicon-carbon composite, and the amorphous carbon content may be 50% to 90% by weight. Additionally, when the composite comprises silicon, amorphous carbon, and crystalline carbon, the silicon content may be 10% to 50% by weight with respect to 100% by weight of the silicon-carbon composite, the crystalline carbon content may be 10% to 70% by weight, and the amorphous carbon content may be 20% to 40% by weight.
[0096] In addition, the thickness of the amorphous carbon coating layer may be 5 nm to 100 nm. The average particle size (D) of the silicon particles (primary particles) 50 ) can be 10 nm to 1 µm, or 10 nm to 200 nm. The silicon particles may exist as silicon alone, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon is SiO x (0 <x≤2)로 표시될 수 있다. 이때, 산화 정도를 나타내는 Si:O의 원자 함량 비율은 99:1 내지 33:67일 수 있다. 본 명세서에서, 별도의 정의가 없는 한, 평균 입경(D 50 ) refers to the diameter of the particle with a cumulative volume of 50 volume% in the particle size distribution.
[0097] The above Si-based negative electrode active material or Sn-based negative electrode active material may be used in combination with a carbon-based negative electrode active material. When the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material are mixed and used, the mixing ratio may be 1:99 to 90:10 by weight.
[0098] bookbinder
[0099] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof may be used.
[0100] Examples of non-aqueous binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide imide, polyimide, or combinations thereof.
[0101] The water-based binder may be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylenepropylenediene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0102] When a water-based binder is used as the cathode binder, a cellulose-based compound capable of imparting viscosity may be further included. As this cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. Na, K, or Li may be used as the alkali metal.
[0103] The dry binder is a polymer material capable of fiberization, and may be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or a combination thereof.
[0104] Challenge
[0105] A conductive material is used to impart conductivity to an electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Specific examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjenblack, carbon fiber, carbon nanofiber, and carbon nanotube; metal-based materials in the form of metal powder or metal fibers including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0106] The content of the negative electrode active material may be 95% to 99.5% by weight with respect to 100% by weight of the negative electrode active material layer, and the content of the binder may be 0.5% to 5% by weight with respect to 100% by weight of the negative electrode active material layer. For example, the negative electrode active material layer may contain 90% to 99% by weight of the negative electrode active material, 0.5% to 5% by weight of the binder, and 0.5% to 5% by weight of the conductive material.
[0107] The whole house
[0108] The current collector may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or alloys thereof, and may be in the form of a foil, sheet, or foam. The thickness of the current collector may be, for example, 1 μm to 20 μm, 5 μm to 15 μm, or 7 μm to 10 μm.
[0109] electrolytes
[0110] The electrolyte for a lithium secondary battery may be, for example, an electrolyte solution, which may include a non-aqueous organic solvent and a lithium salt.
[0111] Non-aqueous organic solvents serve as a medium through which ions involved in the electrochemical reaction of a cell can move. Non-aqueous organic solvents may be carbonate-based, ester-based, ether-based, ketone-based, or alcohol-based solvents, aprotic solvents, or a combination thereof.
[0112] Carbonate-based solvents that may be used include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester-based solvents that may be used include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methylpropionate, ethylpropionate, decanolide, mevalonolactone, valerolactone, caprolactone, etc. As ether-based solvents, dibutyl ether, tetraglame, diglame, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. may be used. Additionally, as ketone-based solvents, cyclohexanone, etc. may be used. As alcohol-based solvents, ethyl alcohol, isopropyl alcohol, etc. may be used, and as aprotic solvents, nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, an aromatic ring, or an ether group); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane, 1,4-dioxolane; sulfolanes, etc. may be used.
[0113] Non-aqueous organic solvents may be used alone or in a mixture of two or more types, and when two or more types are mixed, the mixing ratio can be appropriately adjusted according to the desired battery performance, which is widely understood by those working in the field.
[0114] When using a carbonate-based solvent, a mixture of cyclic carbonates and chain carbonates can be used, and the cyclic carbonates and chain carbonates can be mixed in a volume ratio of 1:1 to 1:9.
[0115] The non-aqueous organic solvent may further include an aromatic hydrocarbon-based organic solvent. For example, a carbonate-based solvent and an aromatic hydrocarbon-based organic solvent may be mixed and used in a volume ratio of 1:1 to 30:1.
[0116] The electrolyte may further include vinylethylene carbonate, vinylene carbonate, or ethylene carbonate-based compounds to improve battery life.
[0117] Representative examples of the above ethylene carbonate compounds include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.
[0118] Lithium salts are substances that dissolve in organic solvents and act as a source of lithium ions within the battery, enabling the basic operation of rechargeable lithium batteries and facilitating the movement of lithium ions between the anode and cathode. Representative examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, and LiN(C x F 2x+1 SO2)(C y F 2y+1 It may include one or more selected from SO2)(x and y are integers from 1 to 20), lithium trifluoromethane sulfonate, lithium tetrafluoroethane sulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium bis(oxalate)borate (LiBOB).
[0119] It is preferable to use a lithium salt concentration within the range of 0.1M to 2.0M. When the lithium salt concentration falls within the above range, the electrolyte has appropriate ionic conductivity and viscosity, so it can exhibit excellent performance and lithium ions can move effectively.
[0120] separator
[0121] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or multilayer films of two or more layers thereof may be used, and of course, mixed multilayer films such as polyethylene / polypropylene two-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, and polypropylene / polyethylene / polypropylene three-layer separators may be used.
[0122] The above separator may include a porous substrate and a coating layer comprising an organic material, an inorganic material, or a combination thereof located on one or both sides of the porous substrate.
[0123] The porous substrate may be a polymer membrane formed from any one of the following: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyacetal; polyamide; polyimide; polycarbonate; polyetherketone; polyaryletherketone; polyetherimide; polyamideimide; polybenzimidazole; polyethersulfone; polyphenylene oxide; cyclic olefin copolymer; polyphenylene sulfide; polyethylene naphthalate; glass fiber; Teflon; and polytetrafluoroethylene, or a copolymer or mixture of two or more of these.
[0124] The porous substrate may have a thickness of about 1 μm to 40 μm, and may have a thickness of, for example, 1 μm to 30 μm, 1 μm to 20 μm, 5 μm to 15 μm, or 10 μm to 15 μm.
[0125] The above organic material may include a (meth)acrylic copolymer comprising a first structural unit derived from (meth)acrylamide, and a second structural unit comprising at least one of a structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamideidosulfonic acid or its salt.
[0126] The above inorganic materials are Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, It may include inorganic particles selected from SrTiO3, BaTiO3, Mg(OH)2, boehmite, and combinations thereof, but is not limited thereto. The average particle size (D) of the inorganic particles. 50 ) can be 1 nm to 2000 nm, and, for example, 100 nm to 1000 nm, or 100 nm to 700 nm.
[0127] The above organic and inorganic materials may exist mixed in a single coating layer, or may exist in a stacked form with a coating layer containing organic materials and a coating layer containing inorganic materials.
[0128] The thickness of the coating layer may be 0.5 μm to 20 μm, for example, 1 μm to 10 μm, or 1 μm to 5 μm.
[0129] Examples and comparative examples of the present invention are described below. The following examples are merely illustrative of the present invention, and the present invention is not limited to the following examples.
[0130] Example 1
[0131] 1. Preparation of positive electrode active material
[0132] (1) Preparation of a nickel-based composite oxide containing zirconium
[0133] First, a nickel-based composite oxide containing zirconium was prepared through the following co-precipitation method.
[0134] Nickel sulfate, cobalt sulfate, and manganese sulfate were dissolved in distilled water as a solvent, and then mixed with Zr(SO4)2·4H2O, a zirconium raw material, to prepare a metal raw material mixed solution. At this time, nickel sulfate, cobalt sulfate, manganese sulfate, and the zirconium raw material were mixed in a molar ratio of Ni:Co:Mn:Zr = 94.8:4:1:0.2.
[0135] A diluted solution of ammonia water (NH4OH) was prepared as a complexing agent, and sodium hydroxide (NaOH) was prepared as a pH adjuster. The concentration of the ammonia water was 10 wt%, and the concentration of the sodium hydroxide was 20 wt%. The prepared metal raw material mixed solution, the diluted ammonia water, and the sodium hydroxide were each introduced into the reactor.
[0136] After stirring for 10 hours with the pH inside the reactor set to 11.75 (Step 1), the pH was lowered to 11.55 and stirred for 22 hours (Step 2) to create a difference in synthesis rate between the inside and outside of the particles, thereby synthesizing a nickel-based complex hydroxide containing zirconium.
[0137] Next, the above-mentioned nickel-based composite hydroxide containing zirconium was subjected to a first heat treatment at 400°C for 6 hours in an oxygen atmosphere to produce a nickel-based composite oxide containing zirconium (hereinafter referred to as a 'Zr pre-placing oxide precursor').
[0138] (2) Preparation of the first preliminary positive active material
[0139] The prepared zirconium-containing nickel-based composite oxide was mixed with anhydrous lithium hydroxide, and the mixture was subjected to a secondary heat treatment at 810°C for 12 hours in an oxygen atmosphere. The zirconium-containing lithium nickel-based composite oxide prepared by heat treatment has a composition of LiNi 0.948 Co 0.04 Mn 0.01 Zr 0.002It is O2 and was confirmed in the form of secondary particles.
[0140] Next, the lithium nickel-based composite oxide containing zirconium, which is the secondary particle form, was ground using a jet mill (processing 5 kg per minute) with a bed weight of 300 kg, a classification wheel rotation speed of 1740 rpm, a blower rotation speed of 3000 rpm, a pulse pressure of 0.5 bar, a gap pressure of 0.4 bar, and a G / A of 6.3 bar to obtain a first preliminary cathode active material in the form of single particles.
[0141] The average particle size (D) of the first preliminary positive active material in the form of a single particle obtained above 50 ) is 3.58 µm, D 10 The particle size is 2.08 µm and D 90 The particle size was confirmed to be 6.32 µm.
[0142] (3) Preparation of the second preliminary positive active material and the positive active material
[0143] The first pre-positive active material in the form of single particles and cobalt hydroxide (Co(OH)2) were dry-mixed, and a second pre-positive active material was prepared by performing a third heat treatment and disintegration at 730°C for 8 hours in an oxygen atmosphere. At this time, disintegration was performed using a jet mill (processing 5 kg per minute) with a bed weight of 300 kg, a classifier wheel rotation speed of 1740 rpm, a blower rotation speed of 3000 rpm, a pulse pressure of 0.5 bar, a gap pressure of 0.4 bar, and a G / A of 6.3 bar, and the cobalt content in the cobalt hydroxide was designed to be 2.0 mol% relative to 100 mol% of the total metal excluding lithium in the positive active material.
[0144] The prepared second preliminary cathode active material and boronic acid (H3BO3) were dry-mixed, and a fourth heat treatment and disintegration were performed at 310°C for 5 hours in an oxygen atmosphere to obtain the cathode active material (LiNi 0.948 Co 0.04 Mn 0.01 Zr 0.002O2) was manufactured. At this time, disintegration was performed through a classification process using a filter mesh (325-mesh), and the boron content in the boronic acid was designed to be 0.5 mol% relative to 100 mol% of the total metal excluding lithium in the cathode active material.
[0145] 2. Manufacture of lithium secondary batteries
[0146] A cathode active material layer slurry was prepared by mixing 98.5 wt% of the manufactured cathode active material, 1.0 wt% of a polyvinylidene fluoride binder, and 0.5 wt% of a carbon nanotube conductive material, and the slurry was coated onto an aluminum foil current collector, dried, and rolled to manufacture a cathode. The manufactured cathode contains cathode active material in the form of crushed single particles.
[0147] A negative electrode active material layer slurry was prepared by mixing 97.5 wt% of graphite negative electrode active material, 1.5 wt% of carboxymethyl cellulose, and 1 wt% of styrene butadiene rubber in a water solvent. A negative electrode was prepared by coating the negative electrode active material layer slurry onto a copper foil current collector, drying, and rolling.
[0148] A lithium secondary battery was manufactured by a conventional method using a polytetrafluoroethylene separator and an electrolyte in which 1M LiPF6 was dissolved in a solvent mixed with ethylene carbonate and dimethyl carbonate in a volume ratio of 3:7.
[0149] Example 2
[0150] In the preparation of the positive active material, the positive active material and the lithium secondary battery were prepared in substantially the same manner as in Example 1, except that the secondary heat treatment was performed at 840°C instead of 810°C.
[0151] Example 3
[0152] In the manufacture of the cathode active material, nickel sulfate, cobalt sulfate, manganese sulfate, and zirconium raw materials are mixed in a molar ratio of Ni:Co:Mn:Zr = 94.5:4:1:0.5 so that the composition is (LiNi 0.945 Co0.04 Mn 0.01 Zr 0.005 A positive electrode active material and a lithium secondary battery were manufactured in substantially the same manner as in Example 1, except that a positive electrode active material (O2) was manufactured.
[0153] Comparative Example 1
[0154] A positive electrode active material and a lithium secondary battery were manufactured in substantially the same manner as in Example 1, except that in the manufacture of the positive electrode active material, a lithium nickel-based composite oxide containing zirconium in the form of secondary particles was ground with a jet mill having a rotation speed of 1580 rpm and a G / A of 4.3 bar to obtain a first preliminary positive electrode active material in the form of single particles.
[0155] Comparative Example 2
[0156] In the preparation of the positive active material, the positive active material and the lithium secondary battery were prepared in substantially the same manner as in Example 1, except that the zirconium raw material Zr(SO4)2·4H2O was not mixed into the metal raw material mixed solution.
[0157] Comparative Example 3
[0158] In the preparation of the positive active material, the positive active material and the lithium secondary battery were prepared in substantially the same manner as in Example 1, except that the secondary heat treatment was performed at 760°C instead of 810°C.
[0159]
[0160] Evaluation Example 1: D 10 , D 50 , D 90 and span
[0161] D of the positive electrode active material prepared according to the examples and comparative examples 10 , D 50 , D 90 and span were measured and calculated and are shown in Table 1 below.
[0162] At this time, D 10 , D 50 and D 90The measurement was performed using an LS13320 (Beckmann Coulter) Particle Size Analyzer (PSA) with laser diffraction, under conditions of pump speed 55%, 40 KHz ultrasonic dispersion 30s, run length 60s, refractive index (RI) 1.6, e-factor 1.00, sample volume 0.20g, and 1 ml of 10% sodium hexametaphosphate as the sample dispersant.
[0163] Evaluation Example 2: BET Specific Surface Area and Degree of Single Crystallinity
[0164] The BET specific surface area and single crystallinity of the cathode active materials prepared according to the examples and comparative examples were measured and calculated and are shown in Table 1 below.
[0165] At this time, the BET specific surface area was measured by the nitrogen gas adsorption method using the HM model-1208 specific surface area measuring device manufactured by MOUNTECH. Specifically, 0.3g of the cathode active material prepared according to the examples and comparative examples was heated in a pretreatment device in a nitrogen atmosphere at 300°C for 1 hour, then further pretreated at 300°C for 15 minutes in the specific surface area measuring device, and cooled to the temperature of liquid nitrogen to saturately adsorb a gas consisting of 30% nitrogen and 70% He. Afterward, the amount of desorbed gas was measured by heating to room temperature, and the specific surface area was calculated from the obtained results by the conventional BET method.
[0166] Subsequently, the degree of single crystallinity was calculated according to Equation 1 using the span according to Evaluation Example 1 and the BET specific surface area.
[0167] Evaluation Example 3: Angle of repose
[0168] The angle of repose and the difference in the angle of repose of the positive electrode active materials prepared according to the examples and comparative examples were measured and are shown in Figures 5 and 6 and Table 1 below.
[0169] At this time, the angle of repose was measured by depositing the anode active material from the funnel onto a petri dish and then measuring the angle formed with the height and horizontal of the deposited layer.
[0170] Referring to Fig. 5, for the positive active material prepared according to Example 1, when the positive active material powder is stacked, the lowest angle (typically the angle with the sample stage) that the free surface of the powder deposition layer forms with the horizontal (angle ①) is about 45°, and the maximum angle (angle ②) that the free surface of the powder deposition layer forms with the horizontal is about 57°, showing a difference in angle of repose of about 12°.
[0171] In contrast, referring to Fig. 6, in the case of the positive active material prepared according to Comparative Example 1, the lowest angle formed by the free surface of the powder deposit layer with the horizontal when the positive active material powder is stacked and the maximum angle formed by the free surface of the powder deposit layer with the horizontal when the positive active material powder is stacked are measured to be approximately 43° each, confirming that there is no difference in the angle of repose.
[0172] Evaluation Example 4: Bulk Density
[0173] The bulk density of the cathode active material prepared according to the examples and comparative examples was measured and expressed as density in Table 1 below.
[0174] Prepare at least 100g of cathode active material (volume 50cm² or more) for analysis using a bulk density analyzer (BT-101). Pass through a tube equipped with baffles to a cathode active material container (25cm 3 The powder is added to the container so that it can be evenly and uniformly deposited. Care is taken not to vibrate the container in which the positive electrode active material is obtained, and the sample accumulated above the top surface of the container is removed to make it flat, and the weight of the container is measured. The bulk density can be obtained by dividing the final weight by the volume of the container.
[0175] Evaluation Example 5: Initial Charge / Discharge Capacity and Efficiency
[0176] The lithium secondary batteries (half-cells) prepared in the examples and comparative examples were charged at 25°C with a constant current of 0.2C to an upper voltage limit of 4.3V and with a constant voltage of 0.05C, and then discharged at 0.2C to a cutoff voltage of 3.0V to perform initial charging and discharging. Table 1 below shows the initial charging capacity, initial discharging capacity, and the ratio of the latter to the former as efficiency.
[0177] Evaluation Example 6: High-temperature life
[0178] Following the initial charge and discharge of Evaluation Example 5, a cycle of charging at 1.0C and discharging at 1.0C in a voltage range of 3.0 V to 4.3 V at 45℃ was repeated 50 times or more, and the ratio of the 50-cycle discharge capacity to the initial discharge capacity was calculated and shown as the lifespan in Table 1 below.
[0179] D 10 (㎛)D 50 (㎛)D 90 (㎛)SpanBET(m 2 / g) Single Crystal Design Etching Difference (°) Density (g / cc) Charge Capacity (mAh / g) Discharge Capacity (mAh / g) Efficiency (%) Lifetime (%) Example 1 2.1 3.6 6.3 1.1 70.6 50.5 61 20.8 24 5.6 21 8.8 89.1 97.2 Example 2 2.2 3.8 6.5 1.1 30.6 0.5 31 50.8 24 6.8 21 8.3 88.5 96.8 Example 3 2.5 4.1 6.9 1.0 70.5 80.5 41 70.7 24 7.3 21 9.4 88.7 96.5 Comparative Example 1 2.0 5.0 9.0 1.4 0.5 20.3 721 223 4.5 193.2 82.4 92.6 Comparative Example 22.13.55.61.00.750.7531.4245.2206.584.289.8 Comparative Example 32.13.55.20.890.80.921.4246.3213.086.591.4
[0180] Referring to Table 1, it can be seen that Examples 1 to 3 achieve higher charging capacity, discharging capacity, charge / discharge efficiency, and high-temperature life characteristics compared to Comparative Examples 1 to 3. In particular, it can be confirmed that Example 1 achieves the highest efficiency and high-temperature life characteristics.
[0181] Although preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concepts defined in the following claims are also included within the scope of the present invention.
[0182] [Explanation of the symbol]
[0183] 100: Lithium secondary battery 10: Positive electrode
[0184] 11: Positive lead tab 12: Positive terminal
[0185] 20: Cathode 21: Cathode lead tab
[0186] 22: Negative terminal 30: Separator
[0187] 40: Electrode assembly 50: Case
[0188] 60: Sealing member 70: Electrode tab
[0189] 71: Positive tab 72: Negative tab
Claims
1. It is a positive electrode active material containing a lithium nickel-based complex oxide and in the form of a single particle, and The degree of single crystallization of the above positive active material according to Equation 1 below is 0.4 to 0.7, and The BET specific surface area of the above positive active material is 1.0 m 2 / g or less, and The span of the above positive active material according to Equation 2 below is 0.8 to 1.2, and A positive active material having a difference in angle of repose according to Equation 3 below of the above positive active material from 5° to 20°. [Equation 1] Degree of single crystallinity = (BET specific surface area) / (span) [Equation 2] Span = (D 90 -D 10 ) / D 50 In the above Equation 2, D 10 is the particle diameter of the particle with a cumulative volume of 10 volume% in the particle size distribution, D 50 D is the particle size of the particle with a cumulative volume of 50 volume% in the particle size distribution. 90 represents the particle size of the particle whose cumulative volume is 90 volume% in the particle size distribution, and [Equation 3] Difference in angle of repose = (Maximum angle formed by the free surface of the powder deposit layer with the horizontal when the anode active material powder is stacked) - (Minimum angle formed by the free surface of the powder deposit layer with the horizontal when the anode active material powder is stacked) 2. In Paragraph 1, The above lithium nickel-based composite oxide is a positive active material represented by the following chemical formula 1: [Chemical Formula 1] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1 In the above chemical formula 1, 0.9≤a1≤1.8, 0.3≤x1≤1, 0≤y1≤0.7, 0≤z1≤0.7, 0.9≤x1+y1+z1≤1.1 and 0≤b1≤0.1, and M 1 and M 2 are different elements and each independently is one or more of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more of F, P, and S.
3. In Paragraph 1, A positive active material having a single crystallinity of 0.5 to 0.6 according to Formula 1 of the above positive active material.
4. In Paragraph 1, The BET specific surface area of the above positive active material is 0.55 m² 2 / g to 0.7 m 2 Anode active material in g.
5. In Paragraph 1, A positive active material having a span of 1.07 to 1.2 according to Formula 2 of the above positive active material.
6. In Paragraph 1, Average particle size (D of the above positive active material) 50 ) is a positive active material having a thickness of 3.6 μm to 4.5 μm.
7. In Paragraph 1, D of the above positive active material 10 A positive electrode active material having a thickness of 2.1 μm to 2.5 μm.
8. In Paragraph 1, D of the above positive active material 90 A positive electrode active material having a thickness of 6.0 μm to 8.0 μm.
9. In Paragraph 1, A positive active material having a difference in angle of repose according to Equation 3 of the above positive active material from 11° to 17°.
10. In Paragraph 1, The above positive active material has a bulk density of 0.1 g / cc to 1.2 g / cc.
11. The whole house; and A positive active material layer located on the above current collector; comprising, The above positive active material layer is a positive electrode comprising a positive active material according to any one of claims 1 to 10.
12. In Paragraph 11, A positive electrode having a density of the positive electrode active material layer of 2.8 g / cc to 4.0 g / cc.
13. In Paragraph 11, The loading level of the above positive active material layer is 5 mg / cm² 2 to 40 mg / cm² 2 Phosphorus anode.
14. In Paragraph 11, A positive electrode having a positive electrode active material layer thickness of 5 μm to 200 μm.