An aqueous primer composition and a method for producing thereof

The aqueous primer composition with styrene-acrylate copolymers and calcium acetate addresses adhesion issues on low surface energy substrates, improving print quality and durability by enhancing substrate interaction.

WO2026235543A1PCT designated stage Publication Date: 2026-11-12TOYOCHEM SPECIALTY CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/MY2026/050030
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-03-31
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Inkjet printing on low surface energy non-absorbent substrates faces challenges such as poor adhesion, intercolor bleeding, line sharpness issues, and high costs due to the need for offline coatings, which current primer compositions fail to adequately address.

Method used

An aqueous primer composition comprising styrene-acrylate copolymers, calcium acetate, and additives like high-density polyethylene wax and defoaming agents, which enhance adhesion and surface energy, forming a uniform film on non-absorbent substrates.

Benefits of technology

Improves ink adhesion, reduces defects like peeling and scratching, and maintains print quality on non-absorbent substrates, enhancing durability and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure MY2026050030_12112026_PF_FP_ABST
    Figure MY2026050030_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an aqueous primer composition for use in industrial inkjet printing on low surface energy non-absorbent substrates, the composition comprising an emulsion of styrene-acrylate copolymers, an aqueous dispersion of styrene-based and acrylate-based polymer resin particles, calcium acetate present in an amount ranging from 0.1% by weight to 10% by weight of the total composition and water. The present invention also relates to a method for producing thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[0001]

[0002] AN AQUEOUS PRIMER COMPOSITION AND A METHOD FOR PRODUCING THEREOF

[0003] FIEED OF INVENTION

[0004] The present invention relates to an aqueous primer composition for use in inkjet printing on non-absorbent substrates, more particularly to an aqueous primer composition for use in industrial inkjet printing on low surface energy non-absorbent substrates. The present invention also relates to a method for producing thereof.

[0005] BACKGROUND OF THE INVENTION

[0006] The industrial inkjet printing industry has rapidly converted from conventional analogue printing techniques like offset lithography and roto-gravure to digital inkjet printing techniques such as continuous inkjet or drop-on-demand. Industrial inkjet printing refers to the use of inkjet technology to print or deposit materials onto various substrates — a process that is similar to standard home or office inkjet printer. Industrial inkjet printers are not just limited to printing or marking; they can also apply coatings, deposit precise amounts of functional materials, and even build micro or macro structures. Generally, inkjet printers eject patterns of tiny drops onto various materials without physically making contact with the surface of the object. These patterns of dots are comprised of different coloured inks, which, when combined, can create photoquality images.

[0007] Modem inkjet printing techniques are useful for printing on a variety of substrates. Inkjet printing allows application of ink to discrete locations by jetting drops of ink on the substrate. Inkjet printing efficiently provides a high degree of printing control with almost effortless and endless colour control and selection. The differences in interaction of the ink and the substrate that occur with ink jet printing may not allow for a simple

[0008]

[0009] and direct transition from a traditional printing technique, such as flexography or lithograph techniques, to an inkjet process, particularly with regard to printing on nonabsorbent substrates.

[0010] Inkjet printing onto non-ab sorptive or low-absorptive substrates such as polymeric fdms, foils, coated papers, ceramics, glass is critical due to the low viscosity of inkjet inks and the resulting print artefacts like intercolor bleeding, line sharpness issues, dot spreading, and coalescence. Furthermore, the adhesion of inkjet inks to such non-adsorptive substrates can be critical if there is no binder in the inks. In order to overcome these issues, it is known to apply inkjet coatings to the non-absorptive substrate. Inkjet coatings such as microporous inkjet coatings are able to absorb the ink in a short time which leads to a fast fixation of the ink droplets. As these inkjet coatings generally need to have a coat weight of at least 15 g / m2to handle the ink laydown they are coated offline before printing and are adding high costs to the substrate material and the final print. For commercial presses with single pass printing such as in packaging or decor applications, these costs are not acceptable. Primer coatings which are applied in lower coat weights and which are therefore less expensive have also been described, particularly in combination with appropriate inks. Inkjet primer compositions often contain coagulants, such as dissolved multivalent metal cations, which play an important role in precipitating anionically charged dispersed ink ingredients, mainly the dispersed anionic colour pigments and optionally anionic binders.

[0011] Several technologies related to inkjet printing primer coatings are known in the art. For example, European Patent No. EP4324890B1 discusses an aqueous coating composition for forming an inkjet-printable primer layer on non-absorptive substrates which comprises a dispersed polymeric binder, aluminium hydroxide oxide particles of boehmite particles, pseudoboehmite particles, and combinations thereof, dissolved multivalent metal cations selected from Ca2+, Mg2+, Zn2+, Al3+, Fe2+, Fe3+, Ti4+, Zr4+, and combinations thereof, and inorganic and / or organic counteranions of the metal

[0012]

[0013] cations selected from chloride, bromide, borate, nitrate, hydrogensulfate, sulfate, hydrogencarbonate, acetate, formate, propionate, sulfamate, succinate, citrate, lactate, glycerate, p-toluolsufonate, and combinations thereof. Another example is shown in United States of America Patent Publication No. US2024376334A1 discusses a primer composition for inkjet printing which comprises a resin emulsion containing polyolefin and urethane, a surfactant which may include acetylene-based surfactants and silicone-based surfactants, nonionic surfactants, and a cohesion promoter for promoting cohesion of the primer composition including water-soluble multivalent metal salts, organic acids, cationic polymers. International Patent Publication No. WO2018225701A1 also discloses an aqueous primer composition containing an acrylic resin and / or a vinyl acetate resin and a calcium salt with calcium salts of hydrochloric acid (calcium chloride) and nitric acid (calcium nitrate) being more preferred.

[0014] A direct transition using current methods results in inferior ink lay, poor print quality, and excessive immobility of the inkjet ink that can cause such defects as cratering or pinholing. Attempts to adapt inkjet methods without sacrificing ink lay and print quality have led to the production of various basecoat formulas or ink chemistry modifications which only maiginally improve the final product. Current modifications of inkjet printing techniques are inadequate because of a lack of parameters that ensures appropriate ink jet application in particular on non-absorbent substrates having low surface energy. The present invention provides a solution to solve the aforementioned problems.

[0015] SUMMARY OF INVENTION

[0016] One object of the invention is to provide an aqueous primer composition for use in industrial inkjet printing on low surface energy non-absorbent substrates. Advantageously, the aqueous primer composition comprises an alkaline earth metal salt incorporated therein to enhance adhesion of inkjet ink on the surface of non-absorbent

[0017]

[0018] substrates by introducing cross-links therebetween and increase surface eneigy of the substrates.

[0019] Another object of the invention is to provide an aqueous primer for use in industrial inkjet printing on low surface energy non -absorbent substrates produced from the composition abovementioned.

[0020] Still, one object of the invention is to provide a method for producing the aqueous primer for use in industrial inkjet printing on low surface energy non -absorbent substrates.

[0021] At least one of the preceding objects is met, in whole or in part, in which the embodiment of the present invention describes an aqueous primer composition for use in industrial inkjet printing on low surface energy non-absorbent substrates, the composition comprising an emulsion of styrene-acrylate copolymers, an aqueous dispersion of styrene-based and acrylate-based polymer resin particles, calcium acetate present in an amount ranging from 0.1% by weight to 10% by weight of the total composition, an aqueous wax dispersion of a high-density polyethylene wax present in an amount ranging from 0.5% by weight to 25% by weight of the total composition and water.

[0022] In a preferred embodiment of the present invention, it is disclosed that the emulsion of styrene-acrylate copolymers is present in an amount ranging from 5% by weight to 90% by weight of the total composition.

[0023] Preferably, the emulsion of styrene-acrylate copolymers has a total solid content ranging from 35% to 55%.

[0024] Preferably, the particle size of the solids in the emulsion of styrene -acrylate copolymers

[0025]

[0026] is less than 40 microns.

[0027] In another preferred embodiment of the present invention, it is disclosed that the aqueous dispersion of styrene-based and acrylate-based polymer resin particles is present in an amount ranging from 2% by weight to 45% by weight of the total composition.

[0028] Preferably, the aqueous dispersion of styrene-based and acrylate-based polymer resin particles has a total solid content ranging from 35% to 50%.

[0029] Preferably, the particle size of the solids in the aqueous dispersion of styrene-based and acrylate-based polymer resin particles is less than 40 microns.

[0030] Further embodiment of the present invention discloses that the composition further comprises a mixture of additives selected from a humectant, a coalescing agent, a first defoaming agent and a second defoaming agent.

[0031] It is preferred that the humectant used in the mixture of additives is monopropylene glycol present in an amount ranging from 1% by weight to 10% by weight of the total composition.

[0032] It is preferred that the coalescing agent used in the mixture of additives is dipropylene glycol methyl ether present in an amount ranging from 0.5% by weight to 10% by weight of the total composition.

[0033] It is preferred that the first defoaming agent used in the mixture of additives is a polyether siloxane copolymer emulsion present in an amount ranging from 0.1% by weight to 1% by weight of the total composition.

[0034]

[0035] It is preferred that the second defoaming agent used in the mixture of additives is an organo-modified polysiloxane emulsion present in an amount ranging from 0.05% by weight to 0.5% by weight of the total composition.

[0036] It is preferred that the low surface energy non-absorbent substrates are made from a material selected from polyvinyl chloride, polyethylene and metalized foil paper.

[0037] In a preferred embodiment of the present invention, there is disclosed an aqueous primer for use in industrial inkjet printing on low surface energy non-absorbent substrates produced from the composition as abovementioned.

[0038] An exemplary embodiment of the present invention also discloses a method for producing an aqueous primer for use in industrial inkjet printing on low surface energy non-absorbent substrates, the method comprising the steps of dissolving calcium acetate in water to obtain an aqueous solution of calcium acetate, blending a mixture of additives comprising an aqueous wax dispersion, a humectant, a coalescing agent and a surfactant in the aqueous solution of calcium acetate to obtain a first mixture, blending an emulsion of styrene and acrylate copolymers, an aqueous dispersion of styrene-based and acrylate-based polymer resin particles, a first defoaming agent of a polyether siloxane copolymer emulsion and a second defoaming agent of an oigano -modified polysiloxane emulsion to obtain a second mixture and homogenizing the first mixture and the second mixture at a rotational speed of less than 60 rpm to obtain the aqueous primer.

[0039] Preferably the step of blending a mixture of additives comprising an aqueous wax dispersion, a humectant, a coalescing agent and a surfactant in the aqueous solution of calcium acetate to obtain a first mixture is performed at a rotational speed of less than 60 rpm for 10 minutes to 30 minutes.

[0040]

[0041] Preferably, the step of blending an emulsion of styrene and acrylate copolymers, an aqueous dispersion of styrene-based and acrylate -based polymer resin particles, a first defoaming agent of a polyether siloxane copolymer emulsion and a second defoaming agent of an organo-modified polysiloxane emulsion to obtain a second mixture is performed at a rotational speed ranging from 80 rpm to 120 rpm for 5 minutes to 15 minutes.

[0042] Preferably, the method further comprises a step of filtering the aqueous primer using a polypropylene filter having a pore size of 100 pm.

[0043] One skilled in the art will readily appreciate that the present invention is well adapted to carry out the objects and obtain the ends and advantages mentioned, as well as those inherent therein. The embodiment described herein is not intended as limitations on the scope of the invention.

[0044] BRIEF DESCRIPTION OF THE DRAWINGS

[0045] For the purpose of facilitating an understanding of the invention, there is illustrated in the accompanying drawing the preferred embodiments from an inspection of which when considered in connection with the following description, the invention, its construction and operation and many of its advantages would be readily understood and appreciated.

[0046] FIG. 1 shows microscopic images depicting surface roughness of an aqueous primer of the present invention and a conventional aqueous primer coated on the black side of a standard bar down paper.

[0047] FIG. 2 shows microscopic images depicting surface roughness of an aqueous primer of the present invention and a conventional aqueous primer coated on the white side of a

[0048]

[0049] standard bar down paper.

[0050] FIG. 3 shows microscopic images depicting surface roughness of an aqueous primer of the present invention and a conventional aqueous primer coated on a metalized foil paper.

[0051] FIG. 4 shows an SEM image of a polyvinyl chloride fdm coated with the aqueous primer of the present invention.

[0052] FIG. 5 shows an SEM image of a polyvinyl chloride film coated with the aqueous primer of the present invention and an additional black ink layer printed thereon.

[0053] DETAILED DESCRIPTION OF THE INVENTION

[0054] Hereinafter, the invention shall be described according to the preferred embodiments of the present invention and by referring to the accompanying description and drawings. However, it is to be understood that limiting the description to the preferred embodiments of the invention is merely to facilitate discussion of the present invention and it is envisioned that those skilled in the art may devise various modifications without departing from the scope of the appended claim.

[0055] The present invention relates to an aqueous primer composition for use in industrial inkjet printing particularly on non-absorbent substrates having relatively low surface energy. Generally, aqueous primers for inkjet printing are water-based coatings applied to substrates before printing to enhance ink adhesion, improve print quality and provide a better surface for subsequent processes such as lamination or varnishing. In various embodiments of the present invention, the aqueous primer composition enables inkjet ink to be printed on non-absorbent substrates. Generally, non-absorbent substrates are substrates that are not capable of drawing in or absorbing primer or ink into the

[0056]

[0057] substrates. Exemplary non-absorbent substrates may include, but not limited to, plastics, metals and glass. The non-absorbent substrates may have roughened surface whereby the inkjet ink settles into craters or pits formed on the surface but is still not able to be absorbed into the substrates.

[0058] In embodiments where the non-absorbent substrates are made from plastic materials, the plastic substrates may be sheets of polyvinyl chloride or polyethylene. In embodiments where the non-absorbent substrates are metallic, the metallic substrates may be metal-containing substrates such as metallized foil paper or metallized board. In the context of the present invention, the aforementioned non-absorbent substrates of plastic sheets made from polyvinyl chloride or polyethylene generally have low surface energy and repel liquid, thereby making them very difficult to bond with inkjet ink. On the other hand, metalized paper, whilst having a metallic appearance, can still exhibit low surface energy, making it challenging to bond with inkjet ink, similar to other low surface energy substrates like plastic.

[0059] In the context of non-absorbent substrates, the term “low surface energy” refers to the substrate material’s resistance to wetting and adhesion due to weak molecular attraction forces at its surface. Due to the inherently low surface energy of non-absorbent substrates, poor adhesion of inkjet ink on the surface of the non-absorbent substrates is inevitable which results in a host of problems such as poor tape resistance, poor scratch resistance, chalky finishing and opacity issues. Tape resistance refers to how well the printed substrates withstands the application and removal of adhesive tapes without the ink lifting off the surface. In the instance whereby the inkjet ink does not bond well with non-absorbent substrate, the inkjet ink will peel or detach when tape is applied and removed. This results in peeling or flaking of the printed substrates, leading to poor product quality and reduced durability. Furthermore, in industrial applications or products that are handled frequently, poor scratch resistance leads to scuffed or damaged prints, making them look unprofessional and reducing their longevity. A

[0060]

[0061] chalky finish occurs when the surface of the print feels dry and powdery. This usually indicates poor cohesion between the non-absorbent substrate and inkjet ink, or between the ink layers themselves. The aqueous primer composition of the present invention is provided to solve the aforementioned problems.

[0062] The aqueous primer composition of the present invention typically comprises a blend of polymeric resins, an alkaline earth metal salt having dual functionality of promoting adhesion and modifying surface rheology of the non-absorbent substrates, a diluent and a mixture of additives. In a preferred embodiment of the present invention, the aqueous primer composition comprises a styrene -acrylic resin, an aqueous dispersion of styrene-based and acrylate-based polymer resin particles, calcium acetate, water and a mixture of additives. In the preferred embodiment, water is provided as the main solvent in the aqueous primer composition and is responsible for adjusting viscosity and facilitating even distribution of other components in the composition.

[0063] In the preferred embodiment, the styrene -acrylic resin in the present invention is provided in the form of an emulsion or aqueous solution that comprises styrene-acrylate copolymers where the styrene and acrylate monomers have undergone polymerization and exists as small polymer particles suspended in water. In the present invention, the styrene-acrylate copolymer emulsion serves as the film-forming component and forms a continuous polymer network after drying that is responsible for adhesion, flexibility and mechanical strength of the dried primer film. By way of example, the styrene-acrylate copolymer matrix forms the structural backbone of the aqueous primer composition of the present invention, holding all other components in place. Essentially, the styrene-acrylate copolymer emulsion works in tandem with the calcium acetate to enhance adhesion of the non-absorbent substrate. As such, the styrene-acrylate copolymer emulsion is provided as a bulk constituent in the aqueous primer composition and is present in an amount ranging from 5% by weight to 90% by weight of the total composition. In a preferred embodiment of the present invention, the

[0064]

[0065] emulsion of styrene-acrylate copolymers has a total solid content ranging from 35% to 55%. The substantially high solid content ensures that the aqueous primer of the present invention forms a continuous, uniform layer on the low surface energy non-absorbent substrate. Due to the low molecular attraction forces of low surface eneigy nonabsorbent substrate, a high solid content ensures sufficient polymer deposition thereby enhancing surface modification and adhesion. Preferably, the particle size of the solids in the emulsion of styrene-acrylate copolymers is less than 40 microns to create a more uniform primer film, thereby ensuring better interaction with inkjet ink droplets. Since low surface energy non-absorbent substrates require primers that can spread well, finer particles improve surface coverage to increase contact points for adhesion.

[0066] In the preferred embodiment, the aqueous dispersion of styrene-based and acrylate-based polymer resin particles is provided in the form of a mixture where individual styrene-based polymer resin particles and acrylate-based polymer resin particles are dispersed in water. In the present invention, the aqueous dispersion of styrene-based polymer resin particles and acrylate-based polymer resin particles is provided as a secondary reactive component to finetune the properties of the primer film, contributing to flexibility without compromising hardness. By enhancing flexibility, the aqueous dispersion of styrene-based and acrylate-based polymer resin particles complements the film-forming binder of the styrene-acrylate copolymer emulsion to create a resilient primer film layer that resists cracking. In the present invention, the aqueous dispersion of styrene-based and acrylate -based polymer resin particles plays a secondary role to modify and finetune primer properties without acting as the main binder. As such, the aqueous dispersion of styrene-based and acrylate -based polymer resin particles in the present invention is present in an amount ranging from 2% by weight to 45% by weight of the total composition. In a preferred embodiment of the present invention, the aqueous dispersion of styrene-based and acrylate -based polymer resin particles has a total solid content ranging from 35% to 50%. Preferably, the particle size of the solids in the aqueous dispersion of styrene-based and acrylate-based polymer resin particles

[0067]

[0068] is less than 40 microns. As aforementioned, the substantially high solid content ensures the aqueous primer of the present invention forms a continuous, uniform layer on low surface energy non-absorbent substrates, enhancing polymer deposition and adhesion. The fine particle size of less than 40 microns creates a smooth primer film, improving ink interaction and surface coverage, which increases contact points for adhesion.

[0069] As abovementioned, non-absorbent substrates have relatively low surface energy which hinders adhesion of inkjet ink droplets thereonto. To further enhance adhesion, when the aqueous primer composition comprises a blend of polymeric resins, it also incorporates the use of an alkaline earth metal salt having dual functionality of promoting adhesion and modifying surface rheology of the non-absorbent substrates. In a preferred embodiment of the present invention, the alkaline earth metal salt is calcium acetate that serves as a multifunctional component enhancing adhesion by providing ionic cross-linking between the primer and the non-absorbent substrate. In the preferred embodiment, the calcium acetate is present in an amount ranging from 0.1% by weight to 10% by weight of the total composition. In the aqueous primer composition, the alkaline earth metal salt of calcium acetate dissociates into calcium ions (Ca2+) and acetate ions (CH? COO ) which the Ca2+ions acts as cross-linking agents between the inkjet ink components and the non-absorbent substrate. By way of example, inkjet ink typically contains binders such as acrylics, polyurethanes and other polymers that may have negatively charged functional groups such as carboxyl (-COOH) or phosphate (-PO43') groups. When the inkjet ink is applied onto the surface of the non-absorbent substrate treated with the aqueous primer composition of the present invention, the Ca2+ions to form ionic bonds between the negatively charged functional groups of the inkjet ink. This ionic bonding is provided to strengthen adhesion between the inkjet ink and the non-absorbent substrate by creating a three-dimensional cross-linked network. This reaction is represented in Equation (1) below:

[0070]

[0071] 2R - COOH + Ca(CH3CO(R)2R — C00~)2+ Ca2++ 2H++ 2CH3COO~ -> Ca(R - C00)2+ 2CH3COOH

[0072] (1)

[0073] Herein, R-COOH represents the carboxyl group in the inkjet ink whereby Ca2+ions forms a bridge between two such carboxyl groups, thereby strengthening the ionic bond with the non-absorbent substrate. The larger alkyl groups (R-) tend to have higher electron-donating abilities compared to smaller functional groups such as CH3- in the acetate ions, leading to stronger binding with the Ca2+ions. As a result, the cross-linking reaction leads to a more rigid and durable bond between the inkjet ink and the nonabsorbent substrate, improving the inkjet ink’s resistance to peeling, scratching and tape removal.

[0074] In addition to establishing cross-links between the inkjet ink and the non-absorbent substrate, the presence of calcium acetate in the aqueous primer composition of the present invention also contributes to surface modification of the non-absorbent substrate; in other words, calcium acetate functions to modify the surface rheology of the non-absorbent substrate when the aqueous primer composition of the present invention is applied thereon. In the context of the present invention, non-absorbent substrates made from materials such as polyvinyl chloride, polyethylene and metalized foil paper are low surface energy material generally having surface energy of about 35 dynes / cm and a contact angle of about 89°. These properties make it difficult for inkjet ink to adhere well on the surface of non-absorbent substrates due to poor wetting. Materials with low surface energy tend to repel liquids, making them hard to wet. Wetting is critical for inkjet ink adhesion because poor wetting results in beads of inkjet ink forming on the surface of the non-absorbent substrates rather than spreading evenly. In the present invention, Ca2+ions from the calcium acetate interact with the surface of the non-absorbent substrate to increase its surface energy. Without being bound by theory, Ca2+ions form a thin layer of ionic bonds leading to surface rearrangement at

[0075]

[0076] the molecular level, thereby making the surface more hydrophilic. Essentially, the increased surface energy improves wetting of the non-absorbent substrate by reducing the contact angle whereby a lower contact angle indicates better wetting, leading to stronger bond between the inkjet ink and the non-absorbent substrate.

[0077] Furthermore, electrostatic forces play a crucial role in adhesion, especially when dealing with polar materials or charged surfaces. In the context of the present invention, inkjet ink or non-absorbent substrate may sometimes carry negative charges, leading to electrostatic repulsion that hinders adhesion. For example, polyvinyl chloride can become negatively charged due to its non-polar nature or due to the presence of anions in the environment. Ca2+ions of the calcium acetate in the aqueous primer composition of the present invention are positively charged and can neutralize any negative charges on the surface of the non-absorbent substrate. By neutralizing these charges, the Ca2+ions reduce electrostatic repulsion between the inkjet ink and the non-absorbent substrate. Consequently, this neutralization promotes better contact between the inkjet ink and the non-absorbent substrate thereby facilitating improved adhesion.

[0078] In a preferred embodiment of the present invention, the aqueous primer composition also further comprises a mixture of additives to enhance properties thereof. Ensuring optimal effectiveness, performance and print quality. In the preferred embodiment, the mixture of additives may be selected from an aqueous wax dispersion, a humectant, a coalescing agent, a surfactant, a first defoaming agent and a second defoaming agent.

[0079] In a preferred embodiment of the present invention, the aqueous wax dispersion used in the mixture of additives is a high-density polyethylene wax that is provided to improve slip properties, scratch resistance and barrier protection of the aqueous primer composition. Without being bound by theory, high-density polyethylene wax particles tend to migrate to the surface of the dried primer film to form a thin, low-energy barrier layer that reduces surface friction, thereby allowing for smoother interaction between

[0080]

[0081] the printed inkjet ink and external objects which reduces the chances of mechanical damage due to handling, stacking or transport. High-density polyethylene wax also forms a microstructured surface layer that disperses mechanical stress thereby preventing localized wear. Furthermore, high-density polyethylene wax increase hydrophobicity of the aqueous primer composition thereby reducing moisture and chemical penetration that prevents dirt, oil and other foreign material from embedding into the surface thereof. Preferably, the high-density polyethylene wax is present in an amount ranging from 0.5% by weight to 25% by weight of the total composition.

[0082] In a preferred embodiment of the present invention, the humectant used in the mixture of additives is monopropylene glycol. Without being bound by theory, monopropylene glycol is hygroscopic that absorbs and retains moisture from the environment. During application and drying of the aqueous primer composition of the present invention, monopropylene glycol delays water evaporation and prevents rapid drying and cracking of the primer fdm. This ensures that the primer remains flexible so as to reduce brittleness and improve adhesion to the low surface energy non-absorbent substrates. Preferably, the monopropylene glycol is present in an amount ranging from 1% by weight to 10% by weight of the total composition. Alternatively, glycerine may be used.

[0083] In a preferred embodiment of the present invention, the coalescing agent used in the mixture of additives is dipropylene glycol methyl ester. In the context of the present invention, polymer particles from the styrene -acrylate emulsion and dispersion are suspended in water and require controlled drying for proper primer fdm formation. Dipropylene glycol methyl ester used herein temporarily softens the polymer particles so as to allow them to move, align and merge into a uniform, defect-free primer film before the water evaporates. Essentially, this ensures complete coalescence to reduce the risk of void and pinhole formation or poor adhesion. Furthermore, dipropylene glycol methyl ester slows down the evaporation rate of the aqueous primer composition of the present invention to ensure a gradual, uniform drying process. Preferably, the

[0084]

[0085] dipropylene glycol methyl ester is present in an amount ranging from 0.5% by weight to 10% by weight of the total composition.

[0086] In a preferred embodiment of the present invention, the surfactant used in the mixture of additives is a polydimethylsiloxane dispersion. Without being bound by theory, polydimethylsiloxane molecules tend to migrate to the surface of the primer film during the drying process. The silicone-rich surface forms a low-friction, hydrophobic layer to reduce intermolecular adhesion and therefore improves slip properties. This effect is crucial for reducing friction between primer coated surfaces which makes handling, stacking and packaging easier without damage. Furthermore, aqueous primers typically have higher surface tension which can lead to uneven spreading, cratering and pinholes. The polydimethylsiloxane is provided herein to reduce surface tension of the aqueous primer composition of the present invention so as to allow uniform flow thereof across the low surface energy non-absorbent substrate. Advantageously, this prevents defects such as craters and pinholes. Preferably, the polydimethylsiloxane dispersion is present in an amount ranging from 0.01% by weight to 0.5% by weight of the total composition.

[0087] Generally, in water-based or aqueous primer formulations, foam formation occurs due to high-speed mixing during the production process. To prevent and eliminate formation of foam, defoaming agents are incorporated. In the present invention, two defoaming agents are used synergistically. In a preferred embodiment of the present invention, the first defoaming agent used in the mixture of additives is a polyether siloxane copolymer emulsion whereas the second defoaming agent is an organo-modified polysiloxane emulsion. In the context of the present invention, the first defoaming agent of poly ether siloxane copolymer emulsion functions primarily during the mixing phase which prevents microfoam formation that suppresses foam stabilization by breaking down surface-active components such as surfactants. Unlike the first defoaming agent, the second defoaming agent of organo-modified polysiloxane emulsion focuses on eliminating macrobubbles formed during application and film

[0088]

[0089] formation of the aqueous primer composition of the present invention by removing trapped air and surface bubbles. Preferably, the first defoaming agent of polyether siloxane copolymer emulsion is present in an amount ranging from 0.1% by weight to 1% by weight of the total composition whereas the second defoaming agent of organo-modified polysiloxane emulsion is present in an amount ranging from 0.05% by weight to 0.5% by weight of the total composition.

[0090] An exemplary embodiment of the present invention also describes a method for producing the aforementioned aqueous primer for use in inkjet printing on low surface energy non-absorbent substrates. The method is commenced with a step of dissolving calcium acetate in water to obtain an aqueous solution of calcium acetate. Generally, calcium acetate is highly soluble in water which ensures complete dissociation into Ca2+ions and ensures uniform distribution of ionic species throughout the aqueous primer. The water also serves as a medium for the subsequent incorporation of other components of the aqueous primer. For example, the temperature of the water may range from 25 °C to 40°C to aid dissolution.

[0091] The method of the present invention is then followed by a step of blending a mixture of additives comprising an aqueous wax dispersion, a humectant, a coalescing agent and a surfactant, as abovementioned, in the aqueous solution of calcium acetate to obtain a first mixture. The mixture of additives may be blended with the aqueous solution of calcium acetate using any types of mixers known in the art, such as high-shear mixer, rotor-stator homogenizer, bead mills and high-pressure homogenizer. Nevertheless, it is preferred that the first mixture is blended at a relatively low speed to prevent excessive shear that could destabilize the aqueous wax dispersion. In a preferred embodiment of the present invention, the step of blending the mixture of additives in the aqueous solution of calcium acetate is conducted at a mixing speed of less than 60 rpm for 10 minutes to 30 minutes so as to ensure uniform blending without introducing excess air bubbles.

[0092]

[0093] Next, a second homogenous mixture is then prepared by incorporating polymer emulsions and defoaming agents separately. In a preferred embodiment of the present invention, the method comprises a step of blending an emulsion of styrene and acrylate copolymers, an aqueous dispersion of styrene-based and acrylate-based polymer resin particles, a first defoaming agent of a polyether siloxane copolymer emulsion and a second defoaming agent of an organo-modified polysiloxane emulsion, as abovementioned, to obtain a second mixture. Similarly, the polymer emulsions and defoaming agents may be blended with the aqueous solution of calcium acetate using any types of mixers known in the art, such as high-shear mixer, rotor-stator homogenizer, bead mills and high-pressure homogenizer. Nevertheless, it is preferred that the second mixture is blended at a speed that is relatively higher than stated in the prior step, preferably at a mixing speed ranging from 80 rpm to 120 rpm for 5 minutes to 15 minutes. The mixing speed in this step is substantially higher because it involves dispersing styrene-acrylate copolymer emulsion, polymer particles, and defoaming agents, which require greater shear force for effective dispersion and uniform distribution. For example, styrene-acrylate polymer dispersion contains fine solid particles that may form weak agglomerates. As such, higher shear ensures proper deagglomeration which leads to even dispersion throughout the aqueous primer of the present invention.

[0094] Thereafter, the first mixture and the second mixture as obtained from the prior steps in the method of the present invention are then combined and homogenized to obtain the final product of aqueous primer. Similarly, the first and second mixtures may be homogenized using any types of mixers known in the art, such as high-shear mixer, rotor-stator homogenizer, bead mills and high-pressure homogenizer. Nevertheless, it is preferred that the first and second mixtures are homogenized at a relatively low speed to prevent destabilization of polymer emulsions and minimize air incorporation. In a preferred embodiment of the present invention, the step of homogenizing the first

[0095]

[0096] mixture and the second mixture is conducted at a rotational speed of less than 60 rpm.

[0097] In a preferred embodiment of the present invention, the method also comprises a final step of filtering the aqueous primer using a propylene filter to remove any undissolved particles, contaminants or aggregates that could affect performance of the aqueous primer. Preferably, the propylene filter has a pore size of 100 pm.

[0098] EXAMPLE

[0099] The following non-limiting example has been carried out to illustrate the preferred embodiments of the invention.

[0100] Example 1 : Rub Resistance Test

[0101] Rub resistance test evaluates the durability of a printed surface or primer film under conditions of friction or abrasion. This test determines how well the primer film resists being rubbed off or damaged when subjected to mechanical stress. In this test, a metalized foil paper is used as the non-absorbent substrate as its slick surface presents challenges for ink adhesion and durability, making it a good test substrate. Firstly, a layer of the aqueous primer of the present invention is applied onto the metalized foil paper. The primer-coated metalized foil paper is then placed in an oven set to 90°C for 5 minutes to accelerate the drying process. After drying in the oven, the primer-coated metalized foil paper is left to sit overnight at room temperature to ensure that the primer coating has fully dried and reached a stable state before the rub resistance test is performed.

[0102] The rub resistance test is conducted using a rubbing machine that applies consistent mechanical stress on the surface of the primer-coated metalized foil paper. A first set of the rub resistance test is conducted by subjecting the primer-coated metalized foil paper

[0103]

[0104] to 500 strokes using a 500-gram weight, which simulates moderate abrasion or friction that a product coated with the aqueous primer of the present invention may face during handling, transport or regular use. A second set of the rub resistance test is also conducted by subjecting a separate primer-coated metalized foil paper to 500 strokes using a 1000-gram weight, which simulates harsher conditions or prolonged use. The aforementioned steps of the rub resistance test are repeated using a conventional aqueous primer without calcium acetate.

[0105] Any visible signs of scratching, scuffing or peeling of the primers from the metalized foil paper are examined and summarized in Table 1 below. The coated-to-coated rub resistance test measures how well two primer-coated metalized foil papers withstand rubbing against each other whereas the coated-to-uncoated mb resistance test measures how a primer-coated metalized foil paper resists abrasion when rubbed against an uncoated metalized foil paper.

[0106] Table 1

[0107] Conventional Aqueous Primer

[0108] Aqueous Primer Test of the Present

[0109] without Calcium Invention

[0110] Acetate Off-line rub Coated-to-Coated Slightly Poor Slightly Poor resistance (500g, Coated-to- Poor Poor 500 strokes) Uncoated

[0111] Off-line rub Coated-to-Coated Slightly Poor Slightly Poor resistance (1000g, Coated-to- Poor Poor 500 strokes) Uncoated

[0112]

[0113] Example 2: Blocking Resistance Test

[0114]

[0115] Blocking resistance test evaluates a primer coating’s ability to resist sticking or bonding to other surfaces when subjected to pressure or elevated temperatures. In the first part of coated-to-coated blocking resistance test, two metalized foil papers coated with the aqueous primer of the present invention are placed face-to-face to simulate real-world conditions where coated surfaces may come into contact during stacking or packaging. The first part of this test is conducted at 40°C with relative humidity controlled at 80%, which mimics real-world warm storage areas and where moisture in the air could increase likelihood of blocking, respectively. In the second part of coated-to-uncoated blocking resistance test, a metalized foil paper coated with the aqueous primer of the present invention is placed face-to-face with an uncoated metalized foil paper and subjected to elevated temperatures and humidity condition as aforementioned. The aforementioned steps of the blocking resistance test are repeated using a conventional aqueous primer without calcium acetate.

[0116] Results of blocking resistance test are often rated on a scale of 1 to 5, where: “5” indicates no sticking whereby the surfaces separate cleanly with no signs of adhesion or residue transfer; “4” indicates slight sticking showing some resistance when separating, but no damage or residue is left behind; “3” indicates moderate sticking showing noticeable resistance, minor coating damage, or residue on one surface; “2” indicates severe sticking showing strong adhesion, with visible damage to the coating or transfer of the coating onto the other surface; and “1” indicates complete sticking whereby the surfaces cannot be separated, and the coating has completely bonded to the other surface, resulting in unusable materials. Results of the blocking resistance test conducted herein are shown in FIGS. 3 and 4 and summarized in Table 2 below.

[0117] Table 2

[0118] Blocking Resistance Test at Contact

[0119] Coatings 40°C, Relative Humidity of Surface

[0120] 80%

[0121]

[0122]

[0123] Coated-to- 5

[0124] Aqueous Primer of the Coated

[0125] Present Invention Coated-to- 5

[0126] Uncoated

[0127] Coated-to- 5 Conventional Aqueous Primer Coated

[0128] without Calcium Acetate Coated-to- 5

[0129] Uncoated

[0130]

[0131] Example 3: Taping Test

[0132] Taping test assesses the adhesion quality of a primer and ink to a non-absorbent substrate by simulating the effects of mechanical stress and adhesive forces. This test provides a straightforward way to evaluate whether the primer coating and ink adhere properly or are prone to lifting or peeling when subjected to tape pulling. Firstly, a layer of the aqueous primer of the present invention is applied onto the metalized foil paper. The primer-coated metalized foil paper is then placed in an oven set to 90°C for 5 minutes to accelerate the drying process. After drying in the oven, the primer-coated metalized foil paper is left to sit overnight at room temperature to ensure that the primer coating has fully dried and reached a stable state before the taping test is performed.

[0133] After the primer coating is dried and cooled, the primer-coated metalized foil paper is subjected to a printing process whereby a standard ink is printed onto the primer-coated metalized foil paper. After printing, the metalized foil paper is dried again at 60°C for 5 minutes to ensure that the ink adheres properly to the primer-coated metalized foil paper before performing the taping test. Following the drying process, the metalized foil paper is left to rest overnight at room temperature to ensure that the ink and primer have enough time to fully cure and adhere to the metalized foil paper, simulating rea-world drying conditions. A piece of adhesive tape is then applied to the surface of the

[0134]

[0135] metalized foil paper by pressing down and rubbing moderately to ensure good contact with the surface. After applying the tape, it is then pulled off quickly and intensely to test how well the primer and ink adhere to the metalized foil paper. The aforementioned steps of the taping test are repeated using a conventional aqueous primer without calcium acetate. Results of the taping test conducted herein are shown in Table 3 below.

[0136] Table 3

[0137] Conventional Aqueous Aqueous Primer of the

[0138] Test Primer without Calcium Present Invention

[0139] Acetate Good ink adhesion on 2ndSlightly poor ink adhesion Taping Test

[0140] day on 2ndday

[0141]

[0142] Example 4: Cracking Test

[0143] Cracking test evaluates the flexibility, durability and adhesion properties of the primer and ink when subjected to mechanical stress such as folding and tape application which may lead to cracking or peeling. Firstly, a layer of the aqueous primer of the present invention is applied onto the metalized foil paper. The primer-coated metalized foil paper is then placed in an oven set to 90°C for 5 minutes to accelerate the drying process. After drying in the oven, the primer-coated metalized foil paper is left to sit overnight at room temperature to ensure that the primer coating has fully dried and reached a stable state before the cracking test is performed.

[0144] After the primer coating is dried and cooled, the primer-coated metalized foil paper is subjected to a printing process whereby a standard ink is printed onto the primer-coated metalized foil paper. After printing, the primer-coated metalized foil paper is further applied with a layer of topcoat and dried again at 60°C for 5 minutes to ensure both the ink and topcoat are adequately cured. The prepared metalized foil paper is left to rest

[0145]

[0146] overnight at room temperature allowing all layers of primer, ink and topcoat to fully stabilize and cured before performing the cracking test.

[0147] The prepared metalized foil paper is folded along a line to create a point of stress which simulates how printed materials may bend or fold during handling, transportation or use. Adhesive tape is then applied along the fold line which is critical for testing the primer’s ability to withstand mechanical stress, particularly at the point where cracking or delamination is most likely to occur. The adhesive tape is rubbed down onto the folded metalized foil paper to ensure it has strong contact with the surface. Once the tape is firmly applied, it is pulled off to observe how well the ink, primer and topcoat layers resist the stress. Any signs of cracking, peeling or delamination at the fold lines are observed. The aforementioned steps of the cracking test are repeated using a conventional aqueous primer without calcium acetate. Results of the cracking test conducted herein are shown in Table 4 below.

[0148] Table 4

[0149] Conventional Aqueous Aqueous Primer of the

[0150] Test Primer without Calcium Present Invention

[0151] Acetate Little cracking or little Little cracking or little amount of ink chipped amount of ink chipped Cracking Test

[0152] away from the metalized away from the metalized foil paper foil paper

[0153]

[0154] Example 5: Heat Seal Strength Test

[0155] Heat seal strength test evaluates the bonding strength between coated surfaces, specifically focusing on how well the primer, when cured, can adhere to non-absorbent substrate under heat and pressure. In this test, polyvinyl chloride film is used as the

[0156]

[0157] non-absorbent film. Firstly, a standard bar down paper is applied with a thin layer of the aqueous primer of the present invention and then cured at a temperature of 90°C for 5 minutes. The primer-coated paper is subjected to heat sealing at temperatures ranging from 120°C to 200°C using 3 bar pressure for 3 seconds of contact time under a condition, namely coated-to-PVC whereby one primer-coated paper is heat-sealed to a polyvinyl chloride film. After heat sealing, the samples are cut into strips and clamped into a tensile strength testing machine. The machine applies force to the samples, pulling the unsealed part to apply stress on the sealed part. The aforementioned steps of the heat seal strength test are repeated using a conventional aqueous primer without calcium acetate. Results of the heat seal strength test conducted for the aqueous primer of the present invention and conventional aqueous primer are shown in Table 5 below.

[0158] Table 5

[0159] Heat Seal Strength (N / 15mm)

[0160] Coated-to-PVC

[0161] Aqueous Primer of Samples Conventional

[0162] the Present Aqueous Primer

[0163] Invention 120 1.038 1.546

[0164] 140 1.300 1.807 Temperature

[0165] 160 1.364 2.142

[0166] (°C)

[0167] 180 2.100 2.252

[0168] 200 2.355 2.124

[0169]

[0170] Example 6: Microscopic Image Test

[0171] Microscopic image test is performed to visually observe the surface morphology, film uniformity and adhesion characteristics of the primer applied to non-absorbent substrate under a microscope. Firstly, a standard bar down paper and a metalized foil paper are

[0172]

[0173] applied with a layer of the aqueous primer of the present invention and then cured at a temperature of 90°C for 5 minutes . Both samples are then cut into strips with the coated-side up for viewing under a microscope. The aforementioned steps of the microscopic image test are repeated using a conventional aqueous primer without calcium acetate. Various aspects such as surface morphology, fdm uniformity, adhesion and defects including pinholes, air bubbles or cracking are observed, as shown in FIGS. 1, 2 and 3.

[0174] Example 7: Scanning Electron Microscopy (SEMI Image Test

[0175] Seaming electron microscopy (SEM) showcases the thickness and adhesion properties of a non-absorbent substrate with a primer coating and ink. As can be seen in FIG. 4 depicting an SEM image of a polyvinyl chloride fdm coated with the aqueous primer of the present invention, firm adhesion is observed where there is no gap or pocket seen between the primer and the polyvinyl chloride film. This suggests that the aqueous primer bonds well to the polyvinyl chloride film, indicating good material compatibility or application technique. FIG. 5 shows an SEM image of a polyvinyl chloride film coated with the aqueous primer of the present invention and an additional black ink layer printed thereon. It is observed that the black ink layer is anchored into the primer coating firmly without gap or pocket, indicating that the ink adheres to the primer coating beneath it, maintaining structural integrity across all layers.

[0176] The present disclosure includes as contained in the appended claims, as well as that of the foregoing description. Although this invention has been described in its preferred form with a degree of particularly, it is understood that the present disclosure of the preferred form has been made only by way of example and that numerous changes in the details of construction and the combination and arrangements of parts may be resorted to without departing from the scope of the invention.

Claims

CLAIMS1. An aqueous primer composition for use in industrial inkjet printing on low surface energy non-absorbent substrates, the composition comprising:an emulsion of styrene-acrylate copolymers;an aqueous dispersion of styrene-based and acrylate-based polymer resin particles;calcium acetate present in an amount ranging from 0.1% by weight to 10% by weight of the total composition;an aqueous wax dispersion of a high-density polyethylene wax present in an amount ranging from 0.5% by weight to 25% by weight of the total composition; andwater.

2. The composition according to Claim 1, wherein the emulsion of styreneacrylate copolymers is present in an amount ranging from 5% by weight to 90% by weight of the total composition.

3. The composition according to Claim 2, wherein the emulsion of styreneacrylate copolymers has a total solid content ranging from 35% to 55%.

4. The composition according to Claim 3, wherein the particle size of the solids in the emulsion of styrene-acrylate copolymers is less than 40 microns.

5. The composition according to Claim 1, wherein the aqueous dispersion of styrene-based and acrylate-based polymer resin particles is present in an amount ranging from 2% by weight to 45% by weight of the total composition.

6. The composition according to Claim 5, wherein the aqueous dispersion ofstyrene-based and acrylate -based polymer resin particles has a total solid content ranging from 35% to 50%.

7. The composition according to Claim 6, wherein the particle size of the solids in the aqueous dispersion of styrene-based and acrylate-based polymer resin particles is less than 40 microns.

8. The composition according to Claim 1 further comprising a mixture of additives selected from a humectant, a coalescing agent, a first defoaming agent and a second defoaming agent.

9. The composition according to Claim 8, wherein the humectant used in the mixture of additives is monopropylene glycol present in an amount ranging from 1% by weight to 10% by weight of the total composition.

10. The composition according to Claim 8, wherein the coalescing agent used in the mixture of additives is dipropylene glycol methyl ether present in an amount ranging from 0.5% by weight to 10% by weight of the total composition.

11. The composition according to Claim 8, wherein the first defoaming agent used in the mixture of additives is a polyether siloxane copolymer emulsion present in an amount ranging from 0.1% by weight to 1% by weight of the total composition.

12. The composition according to Claim 8, wherein the second defoaming agent used in the mixture of additives is an organo-modified polysiloxane emulsion present in an amount ranging from 0.05% by weight to 0.5% by weight of the total composition.

13. The composition according to Claim 1, wherein the low surface energy nonabsorbent substrates are made from a material selected from polyvinyl chloride, polyethylene and metalized foil paper.

14. An aqueous primer for use in industrial inkjet printing on low surface energy non-absorbent substrates produced from the composition according to any one of the preceding claims.

15. A method for producing an aqueous primer for use in industrial inkjet printing on low surface energy non-absorbent substrates, the method comprising the steps of:a) dissolving calcium acetate in water to obtain an aqueous solution of calcium acetate;b) blending a mixture of additives comprising an aqueous wax dispersion, a humectant, a coalescing agent and a surfactant in the aqueous solution of calcium acetate to obtain a first mixture;c) blending an emulsion of styrene and acrylate copolymers, an aqueous dispersion of styrene-based and acrylate-based polymer resin particles, a first defoaming agent of a polyether siloxane copolymer emulsion and a second defoaming agent of an organo-modified polysiloxane emulsion to obtain a second mixture; andd) homogenizing the first mixture and the second mixture at a rotational speed of less than 60 rpm to obtain the aqueous primer.

16. The method according to Claim 15, wherein step (b) is performed at a rotational speed of less than 60 rpm for 10 minutes to 30 minutes.

17. The method according to Claim 15, wherein step (c) is performed at a rotational speed ranging from 80 rpm to 120 rpm for 5 minutes to 15 minutes.

18. The method according to Claim 15 further comprising a step of filtering the aqueous primer using a polypropylene filter having a pore size of 100 pm.5