Method for producing hard carbon material from lignin and uses thereof

A method for producing hard carbon from lignin through controlled thermal processes enhances its electrochemical properties, addressing capacity and efficiency issues in sodium-ion batteries.

WO2026235586A1PCT designated stage Publication Date: 2026-11-12RISE RES INST OF SWEDEN AB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/SE2026/010197
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Current hard carbon materials derived from biomass have lower sodium ion storage capacity and efficiency compared to graphite, and are affected by metal impurities, making the manufacturing process unreliable.

Method used

A method involving oxidatively thermostabilizing, grinding, initial carbonizing, milling, and final carbonizing lignin at specific temperatures to produce a hard carbon material with controlled porosity and particle size, suitable for sodium-ion batteries.

Benefits of technology

The method produces a hard carbon material with improved electrochemical performance, achieving a reversible specific capacity of up to 331 mAh/g and coulombic efficiency of up to 95% in sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SE2026010197_12112026_PF_FP_ABST
    Figure SE2026010197_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing a hard carbon material from lignin, comprising the following steps: - Providing lignin; - Oxidatively thermostabilising the lignin by heating at a first temperature of from 200 to 300 °C, such as from 230 to 270 °C, such as 250 °C; - Reducing the size of the oxidatively thermostabilised lignin by grinding or crushing; - Initial carbonising of the ground or crushed lignin by heating at a second temperature of from 500 to 700 °C, such as 550-650 °C, such as 580-620 °C, such as 600 °C; - Reducing the size of the initially carbonised lignin by milling; - Final carbonising of the initially carbonised, milled lignin by heating at a third temperature of from 1200 to 1400 °C, such as 1400 °C, thereby obtaining a hard carbon material. Further provided by the present invention are hard carbon materials and hard carbon electrodes for use in sodium-ion batteries, and a method for producing a hard carbon electrode.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR PRODUCING HARD CARBON MATERIAL FROM LIGNIN AND USES THEREOF

[0002] Field of the invention

[0003] The present invention relates to hard carbon material derived from renewable, non-fossil sources and uses thereof within the field of batteries. More particularly, the present invention is directed to a method for producing a hard carbon material from lignin, as well as the hard carbon material as such, a method for producing a hard carbon electrode, and a sodium-ion battery comprising a hard carbon electrode.

[0004] Background of the invention

[0005] Sodium-ion batteries (SIBs) are hitting the market as more sustainable and affordable alternatives to lithium-ion batteries (LIBs). They use sodium ions as charge carriers and have several advantages, including the abundance and low cost of sodium compared to lithium. Success in achieving large-scale deployment of SIBs hinges on securing the materials that are needed to make the cathodes and anodes of the batteries. The standard anode employed in state-of-the-art LIBs is graphite, which is obtained in the form of natural graphite or synthetic graphite. Both materials are derived from resources that are unsustainable and environmentally-polluting. In addition, the graphite anode with its highly crystalline structure is not suitable for sodium-ion storage and thus cannot be used in commercial SIBs.

[0006] Research has found that carbon materials that lack the structural order existing in graphite can store sodium ions to deliver capacities that are of interest to commercial batteries. Carbon with a disordered structure is commonly known as hard carbon. Compared to manufacturing of synthetic graphite, the production of hard carbon can be done more sustainably and affordably, and with a lower environmental impact, by carbonising biomass at lower temperatures than those required for the formation of graphite. Further, no chemical processing is needed, as opposed to graphite which requires purification using toxic chemicals such as hydrofluoric acid.

[0007] Different types of biomass have been used as starting material or precursor to produce hard carbon, for example lignin (see e.g., W02021250603 Al, or Fan et al, Energy Storage Materials 69 (2024) 103386). However, as described in Fan et al, there are challenges associated with the intrinsic properties of hard carbon material obtained from biomass. Thecapacity of currently known hard carbon materials to store sodium ions is lower than that of graphite’s capacity to store lithium ions in commercial LIBs. This is partly related to the physical and chemical characteristics, such as high surface area, porosity and oxygencontaining functionality groups coming from the biomass starting material and retained by the hard carbon at the end of the carbonisation process. Further, bio-based hard carbon materials have been reported to have an initial charge efficiency lower than 80 %. That is in stark contrast to commercial graphite electrodes in LIBs, which are > 93 % efficient during the first cycle and > 99.9 % throughout their lifetime. Additionally, the biomass used as starting material for the production of hard carbon often contains metal impurities that affect the atomic structure of hard carbon during the carbonisation process. Depending on the amount and type of metal impurities, the hard carbon can show different characteristics and performance in batteries, and this makes the whole manufacturing process unreliable.

[0008] Hence, there is a need to provide biomass-derived hard carbon materials that have improved electrochemical properties, and to provide methods for producing such hard carbons on an industrial scale.

[0009] Summary of the invention

[0010] The object of the invention is to provide an industrially applicable method for producing a hard carbon material with improved electrochemical performance, wherein the hard carbon material is derived from a renewable, non-fossil source of starting material.

[0011] More particularly, the present invention provides a method for producing a hard carbon material from lignin, comprising the following steps, to be performed in the order listed:

[0012] Providing lignin;

[0013] Oxidatively thermostabilising the lignin by heating at a first temperature of from 200 to 300 °C, such as from 230 to 270 °C, such as 250 °C;

[0014] Reducing the size of the oxidatively thermostabilised lignin by grinding or crushing;Initial carbonising of the ground or crushed lignin by heating at a second temperature of from 500 to 700 °C, such as 550-650 °C, such as 580-620 °C, such as 600 °C;

[0015] Reducing the size of the initially carbonised lignin by milling;Final carbonising of the initially carbonised, milled lignin by heating at a third temperature of from 1200 to 1400 °C, such as 1400 °C, thereby obtaining a hard carbon material.

[0016] The present invention further provides a hard carbon material produced by the herein disclosed method for producing a hard carbon material, characterised in that the hard carbon material has a specific surface area of from 3 to 7 m2 / g and a total pore volume of < 0.04 cm3 / g as evaluated based on nitrogen-gas adsorption data according to the Brunauer-Emmett-Teller (BET) method, a skeletal density of from 2.05 to 2.15 g / cm3as measured by helium pycnometry, and a median particle size by volume (D50) of from 4 to 7 pm as measured by laser diffraction technology based on Mie scattering theory.

[0017] Also provided is a hard carbon material for use in a hard carbon electrode for a sodium-ion battery, wherein the hard carbon is derived from lignin, such as kraft lignin, such as softwood kraft lignin or hardwood kraft lignin, characterised in that the hard carbon material has a specific surface area of from 3 to 7 m2 / g and a total pore volume of < 0.04 cm3 / g as evaluated based on nitrogen-gas adsorption data according to the Brunauer- Emmett-Teller (BET) method, a skeletal density of from 2.05 to 2.15 g / cm3as measured by helium pycnometry, and a median particle size by volume (D50) of from 4 to 7 pm as measured by laser diffraction technology based on Mie scattering theory.

[0018] The present invention further provides a method for producing a hard carbon electrode for use in a sodium-ion battery, comprising the following steps, to be performed in the order listed:

[0019] Providing a hard carbon material produced by the herein disclosed method for producing a hard carbon material, or a hard carbon material as disclosed herein;

[0020] Mixing the hard carbon material with a binding agent and water to obtain a slurry, optionally wherein the ratio of hard carbon material to binding agent is from 90:10 wt % to 95:5 wt %;

[0021] Coating a conductive substrate with the slurry, optionally wherein the conductive substrate is pre-coated with carbon;

[0022] Evaporating the water from the coating formed from the slurry, optionally by drying the slurry coating at room temperature;

[0023] Drying the coating formed from the slurry under vacuum at a temperature of from 120 °C to 150 °C for > 12 hours, thereby obtaining a hard carbon electrode.Additionally provided is a hard carbon electrode for use in a sodium-ion battery, wherein the hard carbon electrode has been produced by the herein disclosed method for producing a hard carbon electrode.

[0024] The present invention also provides a hard carbon electrode comprising the herein disclosed hard carbon material.

[0025] The herein disclosed hard carbon electrode may be characterised by a reversible specific capacity of > 311 mAh / g for the first discharge-charge cycle, a coulombic efficiency of > 87 % for the first discharge-charge cycle, a reversible specific capacity of > 306 mAh / g for the second discharge-charge cycle, and a coulombic efficiency of > 98.5 % for the second discharge-charge cycle, as determined by galvanostatic cycling in a half-cell configuration using an electrolyte solution comprising NaPF6 and diethylene glycol dimethyl ether solvent. The present invention further provides a sodium-ion battery comprising the herein disclosed hard carbon electrode, wherein the hard carbon electrode forms a positive electrode.

[0026] In the following, the invention will be described in more detail, by way of example only, with regard to non-limiting embodiments thereof, reference being made to the accompanying drawings.

[0027] Brief description of the drawings

[0028] Figure 1 is a schematic flowchart of the method for producing a hard carbon material according to the present invention.

[0029] Figure 2 is a schematic flowchart of the method for producing a hard carbon electrode for use in a sodium-ion battery according to the present invention.

[0030] Figure 3 is a graph presenting differential scanning calorimeter (DSC) thermograms of lignin samples.

[0031] Figure 4 is a graph showing the thermal decomposition profiles of lignin samples.

[0032] Figure 5 is a graph showing the quantitative31P NMR spectra and signal assignment of a lignin sample.

[0033] Figure 6 is a graph illustrating the particle size distribution by volume of lignin.

[0034] Figure 7 a-b are SEM images of lignin particles dispersed in water.Figure 8 a-e are graphs showing wide-angle X-ray scattering (WAXS) patterns of hard carbon samples from initial tests for screening carbonisation temperatures.

[0035] Figure 9 a-e are graphs showing WAXS patterns of hard carbon samples synthesised at 1200 °C.

[0036] Figure 10 a-e are graphs showing WAXS patterns of hard carbon samples synthesised at 1400 °C.

[0037] Figure 11 a-d are graphs illustrating the particle size distribution by volume of hard carbon samples.

[0038] Figure 12 a-b are SEM images showing the morphology and particle size distribution of hard carbon samples.

[0039] Figure 13 a-b are graphs showing galvanostatic discharge-charge curves for hard carbon electrodes based on presently disclosed hard carbon materials using an ether solvent.

[0040] Figure 14 a-b are graphs showing galvanostatic discharge-charge curves for hard carbon electrodes based on presently disclosed hard carbon materials using a carbonate solvent. Figure 15 a-b are graphs illustrating the reversible specific capacity and the coulombic efficiency, respectively, over 20 cycles for electrodes based on presently disclosed hard carbon materials prepared at 1400 °C.

[0041] Figure 16 a-b are graphs illustrating the reversible specific capacity and the coulombic efficiency, respectively, over 20 cycles for electrodes based on presently disclosed hard carbon materials prepared at 1200 °C.

[0042] Detailed description

[0043] As mentioned above, the present invention relates to an industrially applicable method for producing a lignin-derived hard carbon material with improved electrochemical performance. More particularly, as schematically illustrated in Fig. 1, according to a first aspect of the present invention, a method 100 for producing a hard carbon material from lignin is provided, which method comprises the following steps, to be performed in the order listed:

[0044] Providing 110 lignin;Oxidatively thermostabilising 120 the lignin by heating at a first temperature of from 200 to 300 °C, such as from 230 to 270 °C, such as 250 °C;

[0045] Reducing 130 the size of the oxidatively thermostabilised lignin by grinding or crushing;Initial carbonising 140 of the ground or crushed lignin by heating at a second temperature of from 500 to 700 °C, such as 550-650 °C, such as 580-620 °C, such as 600 °C;

[0046] Reducing 150 the size of the initially carbonised lignin by milling;

[0047] Final carbonising 160 of the initially carbonised, milled lignin by heating at a third temperature of from 1200 to 1400 °C, such as 1400 °C, thereby obtaining a hard carbon material.

[0048] An advantage of the presently disclosed method for producing hard carbon materials is that it can be performed with equipment currently used in the carbon industry. Further, as shown in the experimental section herein, by performing the method according to the first aspect of the invention, a hard carbon material is produced, which has intrinsic properties that are advantageous when using the hard carbon material in sodium-ion batteries. When such an improved hard carbon material is applied in a hard carbon electrode in a sodium-ion battery, it provides enhanced electrochemical performance to the battery, according to battery performance indicators such as a reversible sodium ion storage capacity of up to 331 mAh / g for the first cycle, and an initial coulombic efficiency of up to 95%, as shown herein.

[0049] Lignin is the starting material or precursor for producing hard carbon materials according to the present invention. Lignin is the second most abundant biomass polymer after cellulose, and it may be derived from softwood, hardwood or other plant-based sources. The paper industry is currently the main producer of lignin as a by-product of pulping processes.

[0050] Different pulping processes are used for producing pulp with differing properties, of which the kraft process is dominant. According to non-limiting embodiments, the lignin provided in step 110 of the presently disclosed method 100 may be softwood kraft lignin, hardwood kraft lignin, lignosulfonate, hydrolysis lignin or organosolv lignin. Softwood kraft lignin separated from black liquor of the kraft process is the currently preferred starting material.

[0051] According to a non- limiting embodiment, step 110 of providing lignin comprises providing lignin having an ash content of < 1%, such as 1%, 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2%, or 0.1%. Consequently, step 120 will comprise oxidatively thermostabilising lignin having an ash content of < 1%, such as 1%, 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%,0.3%, 0.2%, or 0.1%. The ash content means the inorganic content, which make up unwanted impurities and which includes for example trace amounts of metal. Battery-grade hard carbon requires high purity. The impurities, especially in the form of transition metals, reduce the electrochemical performance of the hard carbon produced. The lignin also includes impurities of organic origin, such as cellulose and hemicellulose, which have a less negative impact on the resulting hard carbon compared to the ash content. Starting with a purer material simplifies the following steps and reduces the need for additional purification steps. However, it is to be understood that lignin having a higher ash content than 1% could alternatively be provided in step 110, in which case one or more purification steps could be earned out in order to decrease the impurities present in the lignin, particularly the ash content, before proceeding to step 120 or later during method 100, preferably before step 160 of final carbonisation.

[0052] In a non- limiting embodiment, step 110 of providing lignin comprises providing lignin having a moisture content of < 5 wt%, such as 5%, 4%, 3%, 2% or 1%. Consequently, step 120 will comprise oxidatively thermostabilising lignin having a moisture content of < 5 wt%, such as 5%, 4%, 3%, 2% or 1%. An advantage of using lignin having a low moisture content is that less time and energy is required for heating of the lignin in the following steps of the method 100. A high moisture content could potentially also risk clogging the equipment used.

[0053] However, it is to be understood that step 110 could alternatively involve providing lignin having a higher moisture content than 5%, such as up to 20%, such as 15% or 10%, in which case the time required for step 120, i.e., oxidatively thermostabilising the lignin, by heating the lignin at a first temperature, may need to be prolonged compared to the time ranges specified below.

[0054] In a non- limiting embodiment, step 110 of providing lignin comprises providing lignin having an ash content of < 1%, and a moisture content of < 5 wt%. Consequently, step 120 will comprise oxidatively thermostabilising lignin having an ash content of < 1%, and a moisture content of < 5 wt%.

[0055] Step 120 of oxidatively thermostabilising the lignin normally comprises heating the lignin at a first temperature in the presence of air, such as under airflow. Oxygen from the air is incorporated to create carbon-oxygen cross-linking bonds in the lignin. Such cross-linking bonds prevent melting of the lignin. When cross-linking of the lignin occurs, oxidised (i.e.,oxidatively thermostabilised) lignin is obtained. The term “air” means a composition of gases comprising about 78% nitrogen, about 21% oxygen, and small amounts of other gases including argon and carbon dioxide. It is to be understood that step 120 may alternatively be carried out in the presence of a composition of gases wherein the gas fractions have been modified compared to air, however still retaining approximately the same level of oxidative capacity as air, preferably a level of oxidative capacity that is equal to or higher than the oxidative capacity of air.

[0056] Each step involving heating of the lignin, i.e. steps 120, 140 and 160, comprises a ramping time during which the temperature is increased, continuously or stepwise, from the starting ambient temperature to the target temperature, and a holding time, during which the target temperature is held. In step 120, the target temperature is the first temperature. In step 140, the target temperature is the second temperature. In step 160, the target temperature is the third temperature. The starting ambient temperature, or in other words the starting surrounding temperature, means the temperature surrounding the lignin sample at the start of a heating step, i.e., before the application of external heat has begun. In step 120, 140, and 160, respectively, the starting ambient temperature is normally about room temperature. In an embodiment, wherein the lignin is softwood kraft lignin, the first temperature may be from 230 to 270 °C, such as from 240 to 260 °C, such as 250 °C. According to this embodiment, step 120 of oxidatively thermostabilising the lignin may comprise heating the lignin during a ramping time to reach the first temperature and during a holding time at the first temperature, wherein the holding time is in a range of from 25 to 120 min, such as 25, 30, 40, 50, 60, 70, 80, 90, 100, 110 or 120 min. In a currently preferred embodiment, the first temperature is 250 °C, and the holding time is from 50 to 70 min, such as 60 min, for oxidative thermostabilisation of softwood kraft lignin.

[0057] In an alternative, non-limiting embodiment, wherein the lignin is hardwood kraft lignin, the first temperature may be from 200 to 260 °C, such as from 210 to 250 °C, such as 210, 220, 230, 240 or 250 °C. According to this embodiment, step 120 of oxidatively thermostabilising the lignin may comprise heating the lignin during a first ramping time to reach the first temperature and during a first holding time at the first temperature, wherein the first holding time is in a range of from 45 min to 180 min, such as from 60 min to 160 min, or 45, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 160, 170, or 180 min.According to a non- limiting embodiment, step 120 of oxidatively thermostabilising the lignin comprises applying a first heating rate during the first ramping time of from 0.1 °C / min to 2 °C / min from about room temperature to the first temperature, such as 0.1, 0.5, 1.0, 1.5, or 2.0 °C / min. Said heating rate interval is applicable to both softwood lignin and hardwood lignin. However, it may be preferable to select a heating rate at the lower end of the interval for hardwood lignin, such as from 0.1 °C / min to 1 °C / min, such as from 0.1 °C / min to 0.5 °C / min, the reason being that the glass transition temperature is usually lower for hardwood than for softwood. It is to be understood that the first heating rate may comprise a combination of different heating rates, each heating rate being applied during a part of the first ramping time.

[0058] Step 140 of initial carbonising comprises heating the oxidatively thermostabilised lignin during a second ramping time to reach the second temperature and during a second holding time at the second temperature, wherein the second holding time may be in a range of from 10 min to 90 min, such as from 20 min to 60 min, such as 30 min, or 10, 20, 30, 40, 50, 60, 70, 80, or 90 min.

[0059] According to a non- limiting embodiment, step 140 of initially carbonising the lignin comprises applying a second heating rate during the second ramping time of from 0.5 °C / min to 2 °C / min from the starting ambient temperature to the second temperature, such as 0.5, 1.0, 1.5, or 2.0 °C / min. Said heating rate interval is applicable to both softwood lignin and hardwood lignin. It is to be understood that the second heating rate may comprise a combination of different heating rates, each heating rate being applied during a part of the second ramping time.

[0060] In a non- limiting embodiment, step 140 of initial carbonising the lignin is performed under an inert atmosphere, such as in the presence of N2, such as under flow of N2.

[0061] Step 160 of final carbonising comprises heating the initially carbonised lignin during a third ramping time to reach the third temperature and during a third holding time at the third temperature, wherein the third holding time may be in a range of from 10 min to 90 min, such as from 20 min to 60 min, such as 30 min, or 10, 20, 30, 40, 50, 60, 70, 80, or 90 min.

[0062] According to a non- limiting embodiment, step 160 of finally carbonising the lignin comprises applying a third heating rate during the third ramping time of from 1 °C / min to 5 °C / min from the starting ambient temperature to the third temperature, such as 1, 2, 3, 4, or 5 °C / min. Saidheating rate interval is applicable to both softwood lignin and hardwood lignin. It is to be understood that the third heating rate may comprise a combination of different heating rates, each heating rate being applied during a part of the third ramping time.

[0063] In a non- limiting embodiment, step 160 of finally carbonising the initially carbonised, milled lignin is performed under a reducing atmosphere, such as in the presence of a combination of Ar and H2, such as under flow of a mixture of Ar and H2.

[0064] According to an alternative, non- limiting embodiment, step 160 of finally carbonising the initially carbonised, milled lignin may be performed under an inert atmosphere, such as in the presence of N2, such as under flow of N2.

[0065] In a non-limiting embodiment, step 150 of reducing the size of the initially carbonised lignin by milling is followed by a step 155 of sieving the initially carbonised, milled lignin to remove lignin having a particle size of >50 pm. It is to be understood that if said optional step 155 is included in the method, it is carried out before performing step 160 of final carbonising of the initially carbonised, milled lignin. According to a non-limiting embodiment, the particle size of the initially carbonised, milled lignin may be from about 1 to 100 pm, currently preferred from about 5 to about 50 pm.

[0066] According to a second aspect, the present invention provides a hard carbon material produced by the herein described method 100 for producing a hard carbon material, characterised in that the hard carbon material has a specific surface area of from 3 to 7 m2 / g and a total pore volume of < 0.04 cm3 / g as evaluated based on nitrogen-gas adsorption data according to the Brunauer-Emmett-Teller (BET) method, a skeletal density of from 2.05 to 2.15 g / cm3as measured by helium pycnometry, and a median particle size by volume (D50) of from 4 to 7 pm as measured by laser diffraction technology based on Mie scattering theory.

[0067] It is to be understood that the second aspect, in more detail, encompasses a hard carbon material produced by the following steps, to be performed in the order listed below:

[0068] Providing 110 lignin;

[0069] Oxidatively thermostabilising 120 the lignin by heating at a first temperature of from 200 to 300 °C, such as from 230 to 270 °C, such as 250 °C;

[0070] Reducing 130 the size of the oxidatively themrostabilised lignin by grinding or crushing;Initial carbonising 140 of the ground or crushed lignin by heating at a second temperature of from 500 to 700 °C, such as 550-650 °C, such as 580-620 °C, such as 600 °C;Reducing 150 the size of the initially carbonised lignin by milling;

[0071] Final carbonising 160 of the initially carbonised, milled lignin by heating at a third temperature of from 1200 to 1400 °C, such as 1400 °C, thereby obtaining a hard carbon material;

[0072] the hard carbon material being characterised in that it has a specific surface area of from 3 to 7 m2 / g and a total pore volume of ≤ 0.04 cm3 / g as evaluated based on nitrogen-gas adsorption data according to the Brunauer-Emmett-Teller (BET) method, a skeletal density of from 2.05 to 2.15 g / cm3as measured by helium pycnometry, and a median particle size by volume (D50) of from 4 to 7 μm as measured by laser diffraction technology based on Mie scattering theory. A third aspect of the invention provides a hard carbon material for use in a hard carbon electrode for a sodium-ion battery, wherein the hard carbon is derived from lignin, such as kraft lignin, such as softwood kraft lignin or hardwood kraft lignin, characterised in that the hard carbon material has a specific surface area of from 3 to 7 m2 / g and a total pore volume of ≤ 0.04 cm3 / g as evaluated based on nitrogen-gas adsorption data according to the Brunauer-Emmett-Teller (BET) method, a skeletal density of from 2.05 to 2.15 g / cm3as measured by helium pycnometry, and a median particle size by volume (D50) of from 4 to 7 μm as measured by laser diffraction technology based on Mie scattering theory.

[0073] Specific surface area refers to the total surface area of a material per unit mass or volume. Total pore volume refers to the volume of open pores in a material. There may also be closed pores in a material. The density of a material is reflected by the open pores as well as the closed pores.

[0074] The Brunauer-Emmett-Teller (BET) method or analysis is a widely used technique for measuring the specific surface area and porosity of materials. It is based on the physical adsorption of gas molecules onto a solid surface, allowing characterisation of the surface properties of porous solids.

[0075] Skeletal density is estimated as the mass of a substance per unit volume, including any inaccessible or closed pores. In contrast, true density refers to the density of a material estimated as the ratio of the mass to the true volume, i.e., excluding all open and closed pores. In other words, the true density can be determined if there are no closed pores. Both true density and skeletal density are usually measured using gas pycnometry. Pycnometry uses helium gas to fill the voids in the powder bed to measure the volume taken up by the powder.Particle size, also referred to as "grain size" or "diameter," denotes the size of a single particle. However, most natural or industrial materials are not composed of uniform particles but consist of a mixture of particles of varying sizes. To quantify this variability, particle size distribution is employed. Particle size distribution refers to the range of sizes in a sample of particulate material. D50, the median particle size, is defined as the particle size value at which 50% of a sample's particles are smaller and 50% are larger.

[0076] As mentioned above, the hard carbon material may be characterised by having a specific surface area of from 3 to 7 m2 / g, such as 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, or 7 m2 / g, such as from 5 to 7 m2 / g, such as 5, 5.5, 6, 6.5, or 7 m2 / g; a total pore volume of ≤ 0.04 cm3 / g, such as 0.04, 0.035, 0.03, 0.025, 0.02, 0.015, or 0.01 cm3 / g; a true density of from 2.05 to 2.15 g / cm3, such as 2.05, 2.10, or 2.15 g / cm3, such as from 2.10 to 2.15 g / cm3; and a median particle size by volume (D50) of from 4 to 7 μm, such as 4, 5, 6, or 7 μm. In a non-limiting embodiment, the size of the largest hard carbon particles present in the hard carbon samples, produced by the herein disclosed method, may be about 10-20 μm.

[0077] According to a fourth aspect, as illustrated in Fig. 2, the invention provides a method for producing a hard carbon electrode for use in a sodium-ion battery, comprising the following steps, to be performed in the order listed:

[0078] Providing 210 a hard carbon material produced by the herein disclosed method 100 for producing a hard carbon material, or a hard carbon material according to the second or third aspect as disclosed herein;

[0079] Mixing 220 the hard carbon material with a binding agent and water to obtain a slurry, optionally wherein the ratio of hard carbon material to binding agent is from 90:10 wt % to 95:5 wt %;

[0080] Coating 230 a conductive substrate with the slurry, optionally wherein the conductive substrate is pre-coated with carbon;

[0081] Evaporating 240 the water from the coating formed from the slurry, optionally by drying (240a) the slurry coating at room temperature;

[0082] Drying 250 the coating formed from the slurry under vacuum at a temperature of from 120 °C to 150 °C for ≥ 12 hours, thereby obtaining a hard carbon electrode.Step 210 of the method 200 comprises providing a hard carbon material produced by method 100 in accordance with the first aspect of the present invention, or a hard carbon material according to the second aspect or the third aspect of the invention, as described further above. In non-limiting embodiments, the ratio of hard carbon material to binding agent is from 90:10 wt% to 95:5 wt%, such as 90:10 wt%, 91:9 wt%, 92:8 wt%, 93:7 wt%, 94:6 wt%, or 95:5 wt%. The binding agent is selected from water-soluble compounds. According to non-limiting embodiments, the binding agent may comprise carboxymethyl cellulose, styrene butadiene rubber, sodium alginate, polyacrylate, or carboxymethyl-chitosan, or a mixture of two or more of said compounds. In a currently preferred embodiment, the binding agent comprises a mixture of carboxymethyl cellulose and styrene butadiene rubber, more preferably 2.5% carboxymethyl cellulose and 2.5% styrene butadiene rubber.

[0083] In step 220 of mixing, the water used may be purified water, such as deionized water. The mixing 220 may be done by any suitable method of mixing or homogenisation. The aim is to obtain a homogeneous slurry. A non-limiting example of mixing is ball-milling.

[0084] In step 230 of coating, the conductive substrate may comprise aluminium, copper or nickel. The conductive substrate may be in the form of a foil. In a currently preferred embodiment, the conductive substrate is a foil of aluminium. More preferably, the foil of aluminium is precoated with a thin layer of carbon to enhance adhesion of the hard carbon coating.

[0085] In step 240 of evaporating the water, it is important to fully evaporate the water, to obtain a completely dry coating. Between step 240 and step 250, electrodes may optionally be shaped or formed from the conductive substrate coated with hard carbon, such as by punching or cutting out electrodes from the coated, conductive substrate.

[0086] Step 250 of drying may be performed at a temperature of from 120 °C to 150 °C, such as 120, 130, 140 or 150 °C. The drying 250 may be performed for ≥ 12 hours, such as but not limited to 12, 13, 14, 15, 16, 17, 18, 19, or 20 hours.

[0087] According to a fifth aspect, the present invention provides a hard carbon electrode for use in a sodium-ion battery, wherein the hard carbon electrode has been produced by the herein disclosed method 200 for producing a hard carbon electrode.

[0088] It is to be understood that the fifth aspect, in more detail, encompasses a hard carbon electrode produced by the following steps, to be performed in the order listed below:Providing 210 a hard carbon material produced by the herein disclosed method 100 for producing a hard carbon material, or a hard carbon material according to the second or third aspect as disclosed herein;

[0089] Mixing 220 the hard carbon material with a binding agent and water to obtain a slurry, optionally wherein the ratio of hard carbon material to binding agent is from 90:10 wt % to 95:5 wt %;

[0090] Coating 230 a conductive substrate with the slurry, optionally wherein the conductive substrate is pre-coated with carbon;

[0091] Evaporating 240 the water from the coating formed from the slurry, optionally by drying (240a) the slurry coating at room temperature;

[0092] Drying 250 the coating formed from the slurry under vacuum at a temperature of from 120 °C to 150 °C for ≥ 12 hours, thereby obtaining a hard carbon electrode.

[0093] Additionally, a sixth aspect of the present invention provides a hard carbon electrode comprising the herein disclosed hard carbon material.

[0094] The herein disclosed hard carbon electrode may be characterised by:

[0095] a reversible specific capacity of ≥ 311 mAh / g, such as but not limited to 311, 315, 320, 325, 330, or 331 mAh / g, for the first discharge-charge cycle;

[0096] a coulombic efficiency of ≥ 87 %, such as but not limited to 87, 88, 89, 90, 91, 92, 93, 94, or 95 %, for the first discharge-charge cycle;

[0097] a reversible specific capacity of ≥ 306 mAh / g, such as but not limited to 306, 310, 315, 320, 325, or 326 mAh / g, for the second discharge-charge cycle; and

[0098] a coulombic efficiency of ≥ 98.5%, such as but not limited to 98.5, 99.0, 99.1, 99.2, 99.3, 99.4, 99.5, 99.6, 99.7, 99.8, 99.9, or 100 %, for the second discharge-charge cycle;

[0099] as determined by galvanostatic cycling in a half-cell configuration using an electrolyte solution comprising NaPF6 and diethylene glycol dimethyl ether solvent.

[0100] The term “reversible capacity” refers to the amount of charge a battery can store and release during discharge-charge cycles, excluding any irreversible losses. It is a measure of the usable capacity of the battery after accounting for any capacity lost due to side reactions or other irreversible processes. In the context of the present invention, the reversible capacity more particularly means the sodium-ion storing reversible capacity.The term “reversible specific capacity” is the reversible capacity of a battery normalized to the mass of the active material, typically expressed in milliampere-hours per gram (mAh / g). It provides a measure of how much charge can be stored per unit mass of the active material, which is useful for comparing the performance of different materials or batteries.

[0101] The term “coulombic efficiency” describes the charge efficiency by which electrons are transferred in batteries. It is the ratio of the charge capacity to discharge capacity.

[0102] The reversible specific capacity for the first and second discharge-charge cycle may alternatively be called the initial reversible specific capacity and second reversible specific capacity, respectively.

[0103] The coulombic efficiency for the first and second discharge-charge cycle may alternatively be called the initial coulombic efficiency and second coulombic efficiency, respectively.

[0104] The term “galvanostatic” refers to an experimental technique whereby an electrode is maintained at a constant current in an electrolyte. This technique may be used for example to measure electrochemical reactions.

[0105] Sodium hexafluorophosphate, NaPF6, is commonly used as a component in the electrolytes of rechargeable sodium-ion batteries. It helps in the conduction of sodium ions within the battery, facilitating the charge and discharge processes. It is contemplated that instead of NaPF6, another salt may be included in the electrolyte solution, for example sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI), sodium bis(oxalato)borate (NaBOB), or sodium triflate (NaTOf).

[0106] The function of a half-cell is to measure the electrode potential of a single electrode. A halfcell may be used for testing and verification of the electrochemical properties of the herein disclosed hard carbon materials and hard carbon electrode in a battery application.

[0107] In the context of the present invention, the above-mentioned method of determining reversible specific capacity and coulombic efficiency, comprising galvanostatic cycling in a half-cell configuration using an electrolyte solution comprising NaPF6 and diethylene glycol dimethyl ether solvent, is to be seen as the standard test method for the electrochemical characterisation of a hard carbon electrode according to the present invention. However, instead of using said ether solvent, an ethylene carbonate and diethyl carbonate solvent may be used. It is to be understood that if said carbonate solvent is used instead of the ether solvent, the values ofreversible specific capacity and coulombic efficiency obtained in the test method may differ from those obtained when using the ether solvent.

[0108] A half-cell, to be used in a test method as described herein, may for example be produced by a method comprising the following steps, to be performed in the order specified:

[0109] Providing a hard carbon electrode produced as disclosed elsewhere herein;

[0110] Mounting the hard carbon electrode and a sodium metal electrode, spaced apart by at least one separator, to obtain an electrode-separator assembly;

[0111] Wetting the electrode-separator assembly with an electrolyte solution comprising a sodium salt, such as NaPF6, and a solvent selected from a carbonate solvent and an ether solvent;

[0112] Enclosing the wetted electrode-separator assembly by a packaging material to obtain a half-cell;

[0113] Sealing the half-cell under vacuum.

[0114] In a non-limiting embodiment, the sodium metal electrode may be in the form of a disk. The at least one separator may for example comprise glass fibre or a polymeric microporous membrane (e.g. Celgard). In an embodiment, two separators are mounted between the hard carbon electrode and the sodium metal electrode, for example one glass fibre separator and one polymeric microporous membrane separator.

[0115] In a non-limiting embodiment, the packaging material is made of plastic-laminated aluminium foil.

[0116] According to a seventh aspect, the present invention further provides a sodium-ion battery comprising the herein disclosed hard carbon electrode, wherein the hard carbon electrode forms a positive electrode, i.e., an anode.

[0117] The sodium-ion battery further comprises an electrolyte solution, which is in contact with the hard carbon electrode. Said electrolyte solution comprises a sodium salt, such as NaPF6, and a solvent. According to a non-limiting embodiment, the solvent is an ether solvent. A currently preferred ether solvent is a diethylene glycol dimethyl ether solvent (alternatively called a diglyme solvent).

[0118] According to an alternative embodiment, the solvent is a carbonate solvent, such as but not limited to a solvent comprising a combination of:(i) ethylene carbonate (EC) and diethyl carbonate (DEC);

[0119] (ii) ethylene carbonate (EC) and ethyl methyl carbonate (EMC);

[0120] (iii) vinylene carbonate (VC) and diethyl carbonate (DEC); or

[0121] (iv) vinylene carbonate (VC) and ethyl methyl carbonate (EMC).

[0122] In a currently preferred embodiment, the carbonate solvent comprises a combination of ethylene carbonate (EC) and diethyl carbonate (DEC), more preferably EC to DEC in a ratio of 1:1, according to an industrial standard for different types of batteries.

[0123] It is to be understood that the sodium-ion battery provided according to the seventh aspect additionally comprises a negative electrode (i.e. a cathode) and a second electrolyte, which is in contact with the negative electrode. Methods for constructing a sodium-ion battery are known in the art.

[0124] The embodiments described above are to be understood as illustrative examples of the methods, materials and products according to the present invention. It will be understood by those skilled in the art that various modifications, combinations and changes may be made to the embodiments. All embodiments may be combined with each other and are applicable to all aspects unless otherwise stated.

[0125] As shown in the experimental section following below, the present invention provides improved hard carbon materials, which when applied in a hard carbon electrode for use in a sodium-ion battery, provides enhanced electrochemical performance, more particularly a reversible specific sodium ion storage capacity of up to about 330 mAh / g for the first cycle, and a coulombic efficiency for the first cycle of up to about 95%.

[0126] EXPERIMENTAL SECTION

[0127] Example: Synthesis and Characterisation of Hard Carbon Samples

[0128] Materials and Methods

[0129] Precursor and Characterisation thereof

[0130] PrecursorA LignoBoost softwood kraft lignin (Tomani, Cellul. Chem. Technol., 44 (2010), pp. 53-58), produced at RISE LignoDemo (Bäckhammar, Sweden) from pine / spruce black liquor, was used as the precursor, or starting material, for synthesizing of hard carbon samples. The lignin was fully characterised for its composition, thermal, and chemical properties.

[0131] Ash Content and Compositional Analysis

[0132] The ash content of the lignin sample was deteimined using standard methods, in accordance with ASTM E1755 Standard Test Method for Ash in Biomass, ASTM International: West Conshohocken, Pennsylvania, 2020; TAPPI Standard T 222 Om-11. Acid-Insoluble Lignin in Wood and Pulp, TAPPI Press, Atlanta, USA (2011); TAPPI Useful Methods UM 250. Acid-Soluble Lignin in Wood and Pulp, TAPPI Press, Atlanta, USA (2011); and SCAN Standard CM 71:09. Pulps - Carbohydrate Content, Scandinavian Pulp, Paper and Board Testing Committee, Stockholm, Sweden (2009). The standard methods employed involved combustion at 575 °C. A two-step acid hydrolysis method was employed for compositional analysis to quantify lignin and carbohydrate content. Acid-soluble and acid-insoluble lignins were measured gravimetrically and by UV spectroscopy, while carbohydrate content was assessed using high-performance liquid chromatography (HPLC). The metal and inorganic content were analyzed using a PerkinElmer Optima 8300 Inductively Coupled Plasma Optical Emission Spectroscopy (ICP-OES) following digestion in hydrogen peroxide and nitric acid through microwave-assisted digestion.

[0133] Particle Size and Morphology

[0134] The particle size distribution of the lignin sample, dispersed in DI water, was determined by laser light diffraction on a Malvern Mastersizer 3000 (Malvern Panalytical Ltd., Malvern, UK) using Mie scattering theory. Particle size distribution graphs were plotted based on the median particle size by volume, D50, with three measurements collected for each sample. The data derived from the plots were summarized in the related tables. Morphological analysis of the lignin particles was performed using a Quanta 250 FEG ESEM (FEI Instruments) scanning electron microscope (SEM) in both dry and wet states (dispersed in water) in SEM and STEM (scanning transmission electron microscope) modes.

[0135] Elemental CompositionThe organic elemental composition of the lignin was determined using a PerkinElmer 2400II CHNS / O combustion elemental analyzer based on the Pregl-Dumas method (Patterson, Anal. Chem., 45 (1973), pp. 605-609). The absolute contents of carbon (C), hydrogen (H), nitrogen (N), and sulfur (S) were quantified, while the oxygen content was calculated as 100% minus the sum of C, H, N, S, and ash.

[0136] Molar Mass Distribution

[0137] Size exclusion chromatography (SEC) was used to determine the molar mass distribution of the lignin samples. The analysis was performed using a Waters SEC system equipped with a Knauer K-2501 UV detector. Two PSS MCX columns (1000 and 100000 A) were connected in series, with a pH 12 buffer solution as the mobile phase (flow rate: 0.5 mL / min). Lignin samples were dissolved in NaOH solution (pH 12) and diluted to an appropriate concentration. The injection volume was 100 μL. Calibration was performed using sulfonated polystyrene standards with molecular weights ranging from 250 to 200,000 g / mol.

[0138] Thermal Analysis

[0139] Thermogravimetric analysis (TGA) was conducted using a TA Instruments Q5000 analyzer. Approximately 7 mg of lignin was placed in a TGA pan and heated from room temperature to 100 °C, held for 10 minutes to remove residual moisture, then further heated to 1000 °C at a rate of 10 °C / min under a nitrogen atmosphere (25 mL / min).

[0140] The glass transition temperature (Tg) of the lignin was determined using a TA Instruments Q2000 differential scanning calorimeter (DSC). Approximately 3 mg of lignin was tested in triplicate. Samples were heated from 25°C to 150°C at 20°C / min under nitrogen (50 mL / min), held at 150°C for 5 minutes to remove moisture and erase thermal history, cooled to 25°C, and reheated to 220°C at the same rate. Tgand the corresponding heat capacity change (ACp) were determined from the second heating trace.

[0141] Hydroxyl Group Quantification

[0142] Quantitative31P NMR spectroscopy was employed to measure hydroxyl groups. Lignin samples (30 mg) were dissolved in a dimethylformamide / pyridine (1:1 v / v) mixture and combined with 100 μL of a solution containing N-hydroxy-5-norbornene-2,3-dicarboxylic acid imide (20 mg / mL) and chromium (III) acetylacetonate (5 mg / mL) as the internal standard andrelaxation agent, respectively. The lignin samples were derivatized using 100 μL of 2-chloro-4,4,5,5-tetramethyl-1,3,2-dioxaphospholane (TMDP) and analyzed using an Avance III 400 MHz NMR spectrometer equipped with a broadband PFG 5 mm probe.

[0143] Synthesis of Hard Carbons

[0144] Screening Carbonisation Temperatures (“Screening method”)

[0145] Initially, a set of samples was synthesized to determine the optimal carbonisation temperature for lignin-derived hard carbon. The thermal conversion process for each sample was conducted in two steps: initial carbonisation at 600°C, followed by final carbonisation at a final temperature of 800, 1000, 1200, 1400, or 1600 °C, respectively.

[0146] In the first step, lignin was initially carbonised at 600 °C in an MTI tube furnace (OTF-1200X) under a nitrogen atmosphere (0.3 L / min flow rate). The heating rate was 1 °C / min from room temperature to 600 °C, followed by a 30-minute isothermal hold. The initially carbonised sample was then ground using a Retsch laboratory jaw crusher and finally carbonised at the respective, final temperature in an Entech tube furnace (EFT 70 / 18-III). The heating rate for this step was 3 °C / min, with a 30-minute hold at the target temperature under a nitrogen flow of 0.3 L / min.

[0147] The electrochemical performance of these samples as Na-ion battery anode materials was evaluated to identify the optimal carbonisation temperature for producing high-performance lignin-based hard carbon.

[0148] Synthesis of Hard Carbon with Controlled Particle Morphology

[0149] Hard carbon samples with controlled morphology were synthesized using two approaches: including oxidative thermostabilisation (method of invention) and excluding oxidative thermostabilisation (comparative testing), respectively.

[0150] Method Including Oxidative Thermostabilisation (“Method 1”):

[0151] For the approach including oxidative thermostabilisation, lignin powder was oxidatively thermostabilised at 250 °C in an MTI Box Furnace (KSL-1200X). The heating rate was 0.5 °C / min from room temperature to 250 °C, followed by a 60-minute isothermal hold at 250 °Cunder an airflow of 10 L / min. The total time of the oxidative thermostabilisation step was 465 min.

[0152] The thermostabilised lignin was then ground using a Retsch laboratory jaw crusher and initially carbonised at 600 °C in an MTI tube furnace (OTF-1200X) under a nitrogen atmosphere (0.3 L / min flow rate). The heating rate was 1 °C / min, followed by a 30-minute hold at 600 °C. The total time of the initial carbonisation step was 605 min.

[0153] The initially carbonised sample was ball-milled for 8 hours using a Fritsch Planetary Mill (Pulverisette 6). Particles larger than 50 pm were removed using a Retsch laboratory sieve. The milled and sieved samples were finally carbonised at 1200 °C or 1400 °C, respectively, under either nitrogen or a reducing argon+hydrogen (95:5) gas mixture in an Entech tube furnace (EFT 70 / 18-111). The heating rate was 3 °C / min, followed by a 30-minute hold at the final temperature under a 0.3 L / min gas flow. The total time of the final carbonisation step at 1400 °C was 488 min.

[0154] Using this method, four different hard carbon samples were produced, varying in carbonisation temperature and atmosphere.

[0155] Method Excluding Oxidative Thermostabilisation (“Method 2”):

[0156] For the approach excluding oxidative thermostabilisation, (herein alternatively called the direct carbonisation approach), lignin was initially carbonised at 600 °C in an MTI tube furnace (OTF-1200X) under a nitrogen atmosphere (0.3 L / min flow rate). The heating rate was 1 °C / min, followed by a 30-minute hold at 600 °C.

[0157] The initially carbonised sample was ground using a Retsch laboratory jaw crasher and subsequently ball-milled for 8 hours in a Fritsch Planetary Mill (Pulverisette 6). Particles larger than 50 pm were removed using a Retsch laboratory sieve. The milled and sieved samples were then finally carbonised at 1200 °C or 1400 °C, respectively, under either nitrogen or a reducing argon+hydrogen (95:5) gas mixture in an Entech tube furnace (EFT 70 / 18-III). The heating rate was 3 °C / min, with a 30-minute hold at the final temperature under a 0.3 L / min gas flow. Using this method, four hard carbon samples were synthesized, varying in carbonisation temperature and environment.Table 1 shows a comparison of Method 1 and Method 2, pointing out the similarities and differences. Table 2 lists all hard carbon samples prepared, using either the screening method, Method 1 or Method 2.

[0158] Table 1. Comparison of the two production methods: key differences and similarities.

[0159]

[0160] Table 2. List of different synthesized hard carbon samples.

[0161] Sample I Synthesis Method

[0162]

[0163] SKL-800 Screening method: initially carbonised at 600 °C,

[0164] finally carbonised at 800 °C under N2

[0165] SKL-1000 Screening method: initially carbonised at 600 °C,

[0166] finally carbonised at 1000 °C under N2

[0167] SKL-1200 Screening method: initially carbonised at 600 °C,

[0168] finally carbonised at 1200 °C under N2

[0169]

[0170] SKL: softwood Kraft lignin; BM: ball-milled; BM-S: oxidatively thermostabilised sample, ball-milled and carbonised under nitrogen (inert) atmosphere; BM-S-R: oxidatively thermostabilised sample, ball-milled and carbonised under reducing (argon + hydrogen) atmosphere; BM-R: ball-milled and carbonised under reducing (argon + hydrogen) atmosphere

[0171] Physical characterisation of Hard Carbons

[0172] Analysis of Morphology and Particle Size Distribution

[0173] The particle size distribution of the hard carbon samples was determined using a Malvern Mastersizer 3000 (Malvern Panalytical Ltd., UK) equipped with laser diffraction technology, based on Mie scattering theory. The carbon samples were dispersed in a binaiy ethanol-water solvent system (50:50 v / v). The analysis was conducted with three independent measurements per sample, and the particle size distribution graphs were plotted based on the median particle size by volume (D50). The results were presented graphically, and key data were summarized in the corresponding tables.

[0174] The morphology of the hard carbons was evaluated using a SU3500 Hitachi scanning electron microscope (SEM).

[0175] Analysis of Carbon Structure by X-ray Scattering Techniques

[0176] Wide-angle X-ray scattering (WAXS) and small-angle X-ray scattering (SAXS) measurements of the carbon samples were performed using an Anton Paar SAXSpoint 2.0 WAXS / SAXS instrament equipped with a Dectris Inside 2D EIGER R HPC detector. The X-ray source was a microfocus Cu tube with a point focus ( ~ 1.54 A), operating at 50 kV and 1 mA.

[0177] For WAXS data analysis, the interp lanar spacing of the graphene layer planes (^ / -spacing) in both the (002) and (100) crystal lattice structures were determined using Bragg's Law:

[0178] , nA

[0179] a = - 2sm0

[0180] where X is the X-ray wavelength (1.54 A), n is the order of reflection (set to 1), and 0 is the Bragg angle corresponding to the (002) or (100) reflections.The crystallite sizes, both out-of-plane (£, ) and in-plane (Lf, were calculated using the Debye-Scherrer equation from the characteristics of the (002) and (100) peaks, respectively:

[0181] Kk

[0182] L = - fcos0

[0183] where is the wavelength, 0 is the Bragg angle of the (002) or (100) reflections, f is the full width at half maximum intensity (FWHM) of the respective peaks, and K is a constant, taken as 0.89 for the (002) diffraction peak and 1.84 for the (100) diffraction peak (Shao et al, Carbon 129, 357-366 (2018)).

[0184] Scanning Electron Microscopy (SEM) imaging

[0185] Scanning electron microscopy (Zeiss Merlin) was used to investigate the morphology and microstructures of the hard carbon samples. Powder samples were mounted on a carbon tape (Agar scientific) fixed on aluminium tabs. Loose particles were removed by blowing a pressurized nitrogen gas flow over the samples. Images were collected at a working distance of 8 mm using a 5keV electron beam, a probe current of 100 pA, using secondary electrons with HE-SE2 detectors.

[0186] Analysis of BET specific surface area and pore volume

[0187] The Brunauer-Emmet-Teller (BET) specific surface area and total pore volume of the hard carbon powder were evaluated based on the N2-gas physisorption at 77 K. Measurements were conducted using the ASAP2020 analyzer from Micromeritics®. In a typical measurement, a known amount of the hard carbon powder (about 200-400 mg) was introduced into a sample tube with calibrated volume and degassed at 100 °C under 20 pmHg for about 4 h and at 250 °C under 20 mmHg for 6 h prior to gas adsorption / desorption analysis. The mass of the sample was weighed again after degassing. The sample tube was then mounted on the analysis port, and the N2 adsorption / desorption experiment was conducted in the pressure range of 8 to 746 mmHg. The specific surface area was determined using the BET equation from adsorption data obtained in the relative pressure range of 0.05 to 0.3, while the total pore volume (single point adsorption pore volume) was obtained from the adsorption data at a relative pressure of 0.99.

[0188] Analysis of skeletal densityThe skeletal density of the hard carbon sample was determined using a helium pycnometer (AccuPycII 1340 from Micromeritics). About 300 mg of hard carbon powder was loaded into the sample container and then subjected to helium gas flow inside the analysis chamber. The volume measured from helium gas displacement and the measured sample mass were used to calculate the skeletal density.

[0189] Electrode fabrication

[0190] A hard carbon electrode was fabricated by coating a slurry on carbon-coated aluminium foil (Hohsen, Japan) using a bar coater (RK Control Coater) setting the thickness to 300 pm using a doctor blade (ZFR 2040, Zehntner testing instruments). To prepare the slurry, 95% by weight of hard carbon powder, 5 % binding agent (2.5% carboxymethyl cellulose + 2.5% styrene butadiene rubber), and deionized water were loaded into a jar with ceramic balls and homogenized using a Retch 400 shaker (operated at 30 Hz for 1 h). The coating was dried at ambient conditions and electrodes of 13-16 mm in diameter were punched out using a perforator (Hohsen electrode puncher). The electrodes were further dried at 120-150 °C under vacuum for at least 12 hours before applying them in sodium half-cells or sodium-ion batteries.

[0191] Half-cell assembling

[0192] A sodium half-cell was prepared in a glovebox maintained at a maximum of 0.2 ppm oxygen and water levels. To prepare the sodium half-cell, a 13-16 mm hard carbon electrode (prepared as described above) was combined with a 16-18 mm sodium metal disk and spaced apart by two separators (one Whatman glass fibre separator from Cytiva, USA, and one Celgard separator from Asahi Kasei, Japan). The separators and electrodes were wetted with a 100- 150 pL of an electrolyte (1 M NaPF6 in EC: DEC at a ratio of 1:1, or 1 M NaPF6 in diglyme, respectively). The whole electrode-separator assembly was then put in a pouch made of plastic-laminated aluminium foil and sealed under vacuum.

[0193] Electrochemical Performance

[0194] Analysis of reversible specific capacity

[0195] The reversible specific capacity was obtained from galvanostatic (constant-current) measurements, in which a 20 mA / g current (I) was applied on the half-cell between a voltagerange of 0 to 2.5 V. At the beginning, the half-cell was discharged to 0 V leading insertion of sodium ions into the hard carbon electrode. The reversible specific capacity (Cch) was calculated from the reverse process, meaning charge, which involved extracting sodium ions from the hard carbon. Given the specific current (I) and the time taken to charge the cell (t), the reversible specific capacity is calculated as follows:

[0196] CCh= I x t

[0197] Analysis of coulombic efficiency

[0198] The coulombic efficiency (CE), usually given in percentage, is the ratio of charge capacity (Cch) to discharge capacity (Cdch), determined by galvanostatic cycling as described above.

[0199] CE = (Cch / Cdch) x 100%

[0200] Results

[0201] Properties of Lignin

[0202] Composition of Lignin Sample

[0203] Table 3 summarizes the data related to the composition of the lignin sample. The inorganic composition analysis results are summarized in Table 4. The lignin sample has low impurities due to additional washing in the LignoBoost process. Additionally, the content of the transition metals, especially iron, is relatively low. Sulfur is the main contaminant in the lignin, which comes from the kraft process.

[0204] Table 3. Composition of the lignin sample.

[0205] Content

[0206] Component

[0207] (%)

[0208] ~C 653)

[0209] H 5.78

[0210] N 0.18

[0211] O127.2

[0212] S 1.81

[0213] Ash20.38Carbohydrates 0.61

[0214] Purity 99.1

[0215] 1Subtracted from C, H, N, and ash.2Ash was determined using the ASTM standard method.

[0216] Table 4. The inorganic elemental content.

[0217] Content

[0218] Element

[0219] (PPm)

[0220] Al 45

[0221] Ba 5.1

[0222] Ca 14

[0223] Cu 1.9

[0224] Fe 35

[0225] K 256

[0226] Mg 7.5

[0227] Mn 8.2

[0228] Na 817

[0229] P 2.7

[0230] S 16845

[0231] Si 78

[0232] Zn 2.5

[0233] Molecular weight of lignin

[0234] Table 5 presents the molecular weight characteristics of the lignin sample.

[0235] Table 5. Molar mass and poly dispersity of the lignin sample by SEC.

[0236] Parameter Value

[0237] Mw(g / mol) 4680

[0238] A / ,, (g / mol) 1270

[0239] PD 3.7

[0240] Mn'. Number average molecular weight; MwWeight average molecular weight; PD:

[0241] Polydispersity index ( r / A-C)Thermal properties of lignin

[0242] Figure 3 presents the DSC thermograms of the lignin sample (three replicates), with the glass transition temperature (Tg) data summarized in Table 6.

[0243] Table 6. Summary of the DSC results for the lignin sample.

[0244] Parameter Value

[0245] Tg(°C) 162

[0246] Delta Cp (J / g°C) 0.52

[0247] Transition width (°C) 21

[0248] Tg. glass transition temperature

[0249] The thermal decomposition profiles of the lignin are presented in Figure 4 and summarized in Table 7. The onset of thermal decomposition, important for the thermal pre-treatment of lignin, is at 260 °C. The char yield at 1000 °C, corresponding to fixed carbon (ash subtracted), is about 38%.

[0250] Table 7. Summary of key data related to the thermal decomposition of the lignin sample. Parameter Value

[0251] C) 260

[0252] Trnax (°C) 387

[0253] A Mass at Zinax (%) 72.4

[0254] Residue at 1000 °C (%) 38.6

[0255] Z5wt%: starting thermal decomposition temperature (the temperature at 5% weight loss); Tmaxtemperature of maximum decomposition rate (taken from the derivative thermogravimetric analysis (DTG))

[0256] Quantifying hydroxyl group distribution in lignin

[0257] Figure 5 presents the31P NMR spectra, while Table 8 summarizes the number and distribution of hydroxyl groups (OH) in the lignin sample.

[0258] Table 8. Results of quantitative analysis of hydroxyl groups of lignin using31P NMR spectroscopy (mmol / g).Carboxylic Phenolic OH Total

[0259] Aliphatic Acid OH p- Condensed Phenolic

[0260] Guaiacyl OH

[0261] (COOH) Hydroxyphenyl Phenolic OH

[0262] 0.35 0.17 1.34 1.91 3.42 1.35

[0263] Morphology and particle size distribution

[0264] Figure 6 illustrates the lignin particle size distribution by volume, with the extracted data summarized in Table 9. Most of the lignin particles are below 100 pm, and the mean diameter is 29.1 pm. The lignin particles have a random shape and morphology, as shown in Figure ata, which are SEM images of lignin particles dispersed in water.

[0265] Table 9. Particle size distribution of the samples (Dx indicates that x% volume of the particles is smaller than the value stated).

[0266] Dio D50 (pm) D90 Volume mean

[0267] (pm) (pm) diameter (pm)

[0268] 1.55 12.4 77.6 29.1

[0269] Physical characteristics of Hard Carbons

[0270] Structure of hard carbons — X-ray scattering analysis

[0271] The wide-angle X-ray scattering (WAXS) patterns of various hard carbon samples, along with their corresponding crystallographic data, are presented in Figures 8, 9, and 10 and summarized in Tables 10, 11, and 12, respectively. Based on the results, the main differences in the crystallography results of the samples are increasing crystallite size and reducing the d-spacing values by increasing carbonisation temperature in the screening method (Figure 8a-e, Table 10), indicating the formation of ordered domains in the disordered carbon structure. In the ball-milled samples, the stack height was slightly reduced in some samples as a result of milling (Table 11 and Table 12). However, its impact was limited, and most samples have similar crystallography characteristics, especially in the case of interlayer spacing. Figure 9a-e are graphs showing WAXS patterns of hard carbon samples synthesised at 1200 °C. Figure lOa-e are graphs showing WAXS patterns of hard carbon samples synthesised at 1400 °C.

[0272] Table 10. Crystallography data of the hard carbons obtained by the initial screening method.

[0273] d()02 (A) dooi (A) Lc La (nm)

[0274] Samples

[0275] (nm)

[0276] SKL-800 3.91 2.07 1.16 3.42

[0277] SKL-1000 3.83 2.07 1.19 4.28

[0278] SKL-1200 3.81 2.07 1.20 4.58

[0279] SKL-1400 3.75 2.07 1.25 4.91

[0280] SKL-1600 3.66 2.07 1.31 5.27

[0281] doo2: Interplanar spacing (002); Lc: out-of-plane crystallite size (stack height); doo: Interplanar spacing (001); La: in-plane crystallite size (stack size)

[0282] Table 11. Crystallography data of the hard carbons synthesized at 1200 °C.

[0283] doo2 dooi (A) Lc La (nm)

[0284] Samples

[0285] (A) (nm)

[0286] SKL-1200 3.81 2.07 1.20 4.58

[0287] SKL-BM-S-1200 3.82 2.07 1.36 4.48

[0288] SKL-BM-S-R-1200 3.81 2.07 1.09 4.52

[0289] SKL-BM-1200 3.81 2.07 1.20 4.46

[0290] SKL-BM-R-1200 3.78 2.07 1.15 4.63

[0291] doo2: Interplanar spacing (002); Lc: out-of-plane crystallite size (stack height); doo: Interplanar spacing (001); La: in-plane crystallite size (stack size)

[0292] Table 12. Crystallography data of the hard carbons synthesized at 1400 °C.

[0293] doo2 dooi (A) Lc La (nm)

[0294] Samples

[0295] (A) (nm)

[0296] SKL-1400 3.75 2.07 1.25 4.91

[0297] SKL-BM-S-1400 3.78 2.07 1.08 4.53

[0298] SKL-BM-S-R-1400 3.74 2.07 1.24 4.78

[0299] SKL-BM-1400 3.75 2.07 1.06 4.69SKL-BM-R-1400 3.73 2.07 1.32 4.98

[0300] doo2: Interplanar spacing (002); Lc: out-of-plane crystallite size (stack height); dooi: Interplanar spacing (001); La: in-plane crystallite size (stack size)

[0301] Morphology and particle size distribution

[0302] Figure lla-d illustrate the hard carbon samples' particle size distribution by volume, with the extracted data summarized in Table 13. The hard carbon samples have a D50 particle size in the range of 4-7 pm. The addition of an oxidative thermostabilisation step resulted in reducing particle size and it was consistent in all samples prepared at 1200 °C and 1400 °C. Additionally, the particle size distribution of the samples was relatively narrow in all samples which is desirable for electrochemical applications.

[0303] Table 13. Particle size distribution of the samples (Dx indicates that x% volume of the particles is smaller than the value stated).

[0304] Samples Dio D50 (pm) D90 Volume mean

[0305] (pm) (μm) diameter (pm)

[0306] SKL-BM-S-1200 1.84 4.15 8.38 4.72

[0307] SKL-BM-S-R-1200 1.85 4.17 8.41 4.75

[0308] SKL-BM-S-1400 1.93 4.30 8.53 4.86

[0309] SKL-BM-S-R-1400 1.90 4.18 8.36 4.74

[0310] SKL-BM-1200 2.53 6.77 14.3 7.75

[0311] SKL-BM-R-1200 2.21 6.07 13.2 7.04

[0312] SKL-BM-1400 2.57 6.86 14.5 7.83

[0313] SKL-BM-R-1400 2.50 6.79 14.3 7.72

[0314] Figure 12a-b are SEM images showing the morphology and particle size distribution of SKL-BM-S-R-1200 and SKL-BM-S-R-1400 hard carbon powder, respectively.

[0315] Conclusions

[0316] As shown in Figure 12a-b, the two samples prepared from the stabilised and ball-milled precursors and finally carbonised at 1200 C or 1400 C, respectively, exhibit similar particle morphology and size distributions.Skeletal density, BET specific surface area and pore volume

[0317] Table 14 gives a summary of the skeletal density, BET specific surface area, pore volume and D50 particle size of hard carbon samples prepared from oxidatively thermostabilised (S) or non-thermostabilised softwood Kraft lignin (SKL), respectively, which had then been initially carbonised at 600 °C, ball-milled (BM), and finally carbonised at 1200 or 1400 °C, respectively, under inert atmosphere or reducing atmosphere (R), respectively.

[0318] Table 14. Physical characteristics of hard carbon samples.

[0319]

[0320] Conclusions

[0321] As shown in Table 14, the hard carbon samples from oxidatively thermostabilised lignin show higher skeletal density and smaller D50 particle sizes compared to those without oxidative thermostabilisation. Further, all hard carbon samples have very low pore volume. The generally low surface area of all hard carbon samples is beneficial for the initial coulombic efficiency. The carbonisation atmosphere has only marginally affected the physical characteristics of the hard carbon samples.

[0322] Electrochemical performance

[0323] Screening method: Electrochemical performance relative to carbonisation temperatureTable 15 and Table 16 summarize the skeletal density and electrochemical performance data for hard carbon materials synthesized according to the so-called screening method as described further above, i.e. the method including initial carbonisation at 600 °C and final carbonisation at temperatures ranging from 800 to 1600 °C, without oxidative thermostabilisation and without ball-milling of starting materials and intermediate products (the latter meaning no ball-milling after initial carbonisation). The electrodes were tested using the two electrolytes mentioned above.

[0324] Table 15 shows the skeletal density and electrochemical performance data for hard carbon materials, where electrochemical testing of the electrodes was performed using the electrolyte containing 1 M NaPF₆ in diglyme.

[0325] Table 15. Skeletal density of hard carbons and electrochemical data using 1 M NaPF₆ in diglyme electrolyte.

[0326]

[0327] Table 16 shows the skeletal density and electrochemical performance data for hard carbon materials, where electrochemical testing of the electrodes was performed using the electrolyte containing 1 M NaPF₆ in EC / DEC (1:1 volume ratio).

[0328] Table 16. Skeletal density of hard carbons and electrochemical data using 1 M NaPF₆ in EC / DEC electrolyte.

[0329]

[0330]

[0331] Conclusions

[0332] The skeletal density decreases with increasing temperature, which could be due to the formation of closed pores within the bulk of the hard carbon particles. The reversible specific capacity and coulombic efficiency increase as the temperature increases. Final carbonisation at 1200 and 1400 °C, respectively, yielded hard carbon materials with the highest reversible specific capacity values. Consequently, 1200 and 1400 °C were chosen as the final carbonisation temperatures for the subsequent production of hard carbon materials using Method 1 or Method 2, as described in detail further above.

[0333] Method 1 and Method 2: First and second cycle

[0334] Table 17 shows electrochemical testing data for hard carbon electrodes, wherein each hard carbon electrode comprised one of the hard carbon materials, respectively, produced with oxidative thermostabilisation (S) or without oxidative thermostabilisation, as described further above. The electrochemical testing was performed by applying galvanostatic cycling in a halfcell, prepared as described further above, and using an electrolyte containing 1 M NaPF₆ in diglyme.

[0335] Figure 13a-b show the galvanostatic discharge-charge curves of the first and second cycles for two different hard carbon electrodes based on hard carbon samples tested in a sodium halfcell using the electrolyte containing 1 M NaPF₆ in diglyme. Figure 13a relates to the SKL-BM-S-1400 sample. Figure 13b relates to the SKL-BM-S-R-1400 sample.

[0336] Table 17. Sodium-ion storing reversible capacity and coulombic efficiency of hard carbon electrodes with electrolyte 1 M NaPF₆ in diglyme.

[0337]

[0338] Table 18 shows electrochemical testing data for hard carbon electrodes, wherein each hard carbon electrode comprises one of the hard carbon materials, respectively, produced with oxidative thermostabilisation (S) or without oxidative thermostabilisation, as described further above. The electrochemical testing was performed by applying galvanostatic cycling in a halfcell, prepared as described further above, and using an electrolyte containing 1 M NaPF₆ in EC / DEC (1:1 volume ratio).

[0339] Figure 14a-b show the galvanostatic discharge-charge curves of the first and second cycles for two different hard carbon electrodes based on hard carbon samples tested in a sodium half-cell using the electrolyte containing 1 M NaPF₆ in EC / DEC. Figure 14a relates to the SKL-BM-S-1400 sample. Figure 14b relates to the SKL-BM-S-R-1400 sample.

[0340] Table 18. Sodium-ion storing reversible capacity and coulombic efficiency of hard carbon electrodes with electrolyte 1 M NaPF₆ in EC / DEC.

[0341]

[0342]

[0343] Conclusions

[0344] In general, hard carbon materials produced without an oxidative thermostabilisation step are slightly less dense. Hard carbon materials produced from oxidatively thermostabilised lignin (BM-S and BM-S-R) have higher reversible specific capacity than non-thermostabilised lignin (BM and BM-R). Carbonisation in reducing atmosphere boosts initial coulombic efficiency, though the reversible specific capacity decreases slightly. It should also be noted that the higher initial coulombic efficiencies are observed for tests conducted using the diglyme-based electrolyte, which in turn indicates that the materials have better compatibility with electrolytes containing ether solvents. In the diglyme-based electrolyte, the bestperforming materials SKL-BM-S(-R)-1400 have a reversible capacity ranging from 318-330 mAh / g for the first cycle, with initial coulombic efficiency of 92-95% (see Table 17).

[0345] Method 1 and Method 2: 20 cycles

[0346] Figures 15 and 16 show electrochemical testing data for four different hard carbon electrodes, each based on a different hard carbon material, respectively, produced as described further above. Galvanostatic cycling for 20 cycles was tested in a sodium half-cell using 1 M NaPF₆ in diglyme electrolyte.

[0347] Figure 15a shows the reversible specific capacity over 20 cycles, and Figure 15b shows the coulombic efficiency, for four electrodes based on different hard carbon materials prepared at 1200 °C.Figure 16a shows the reversible specific capacity, and Figure 16b shows the coulombic efficiency, over 20 cycles for four electrodes based on different hard carbon materials prepared at 1400 °C.

[0348] Conclusions

[0349] All hard carbon electrodes, whether based on hard carbon produced with or without oxidative thermostabilisation, showed a high and stable reversible specific capacity and coulombic efficiency over 20 cycles.References

[0350] W02021250603 Al

[0351] Fan et al, Research progress on hard carbon materials in advanced sodium-ion batteries. Energy Storage Materials 69 (2024) 103386

[0352] Tomani, The Ligno Boost Process. Cellul. Chem. Technol., 44, 53-58 (2010)

[0353] ASTM E1755 Standard Test Method for Ash in Biomass, ASTM International: West Conshohocken, Pennsylvania (2020)

[0354] TAPPI Standard T 222 Om-11. Acid- Insoluble Lignin in Wood and Pulp, TAPPI Press, Atlanta, USA (2011)

[0355] TAPPI Useful Methods UM 250. Acid-Soluble Lignin in Wood and Pulp, TAPPI Press, Atlanta, USA (2011)

[0356] SCAN Standard CM 71:09. Pulps - Carbohydrate Content, Scandinavian Pulp, Paper and Board Testing Committee, Stockholm, Sweden (2009)

[0357] Patterson, Automated Pregl-Dumas technique for determining total carbon, hydrogen, and nitrogen in atmospheric aerosols. Anal. Chem., 45, 605-609 (1973)

[0358] Shao et al, Biocarbons from microfibrillated cellulose / lignosulfonate precursors: A study of electrical conductivity development during slow pyrolysis. Carbon 129, 357-366 (2018)

Claims

Claims1. A method (100) for producing a hard carbon material from lignin, comprising the following steps, to be performed in the order listed:Providing (110) lignin;Oxidatively thermostabilising (120) the lignin by heating at a first temperature of from 200 to 300 °C, such as from 230 to 270 °C, such as 250 °C;Reducing (130) the size of the oxidatively thermostabilised lignin by grinding or crushing;Initial carbonising (140) of the ground or crashed lignin by heating at a second temperature of from 500 to 700 °C, such as 550-650 °C, such as 580-620 °C, such as 600 °C;Reducing (150) the size of the initially carbonised lignin by milling;Final carbonising (160) of the initially carbonised, milled lignin by heating at a third temperature of from 1200 to 1400 °C, such as 1400 °C, thereby obtaining a hard carbon material.

2. The method (100) according to claim 1, wherein the lignin is softwood kraft lignin, the first temperature is from 230 to 270 °C, and the step of oxidatively thermostabilising (120) the lignin comprises heating the lignin during a ramping time to reach the first temperature and during a holding time at the first temperature, wherein the holding time is in a range of from 25 min to 120 min, such as from 30 min to 90 min, such as 60 min.

3. The method (100) according to claim 1, wherein the lignin is hardwood kraft lignin, the first temperature is from 200 to 260 °C, and the step of oxidatively thermostabilising (120) the lignin comprises heating the lignin during a first ramping time to reach the first temperature and during a first holding time at the first temperature, wherein the first holding time is in a range of from 45 min to 180 min, such as from 60 min to 160 min.

4. The method (100) according to any one of claims 1-3, wherein the step of oxidatively thermostabilising (120) the lignin comprises applying a first heating rate during the first ramping time of from 0.1 °C / min to 2 °C / min from about room temperature to the first temperature.

5. The method (100) according to any one of the preceding claims, wherein the step of initial carbonising (140) comprises heating the oxidatively thermostabilised lignin during a second ramping time to reach the second temperature and during a second holding time at the second temperature, wherein the second holding time is in a range of from 10 min to 90 min, such as from 20 min to 60 min, such as 30 min.

6. The method (100) according to any one of the preceding claims, wherein the step of final carbonising (160) comprises heating the initially carbonised lignin during a third ramping time to reach the third temperature and during a third holding time at the third temperature, wherein the third holding time is in a range of from 10 min to 90 min, such as from 20 min to 60 min, such as 30 min.

7. The method (100) according to any one of the preceding claims, wherein the step of final carbonising (160) is performed under a reducing atmosphere, such as in the presence of a combination of Ar and H2.

8. The method (100) according to any one of claims 1-6, wherein the step of final carbonising (160) is performed under an inert atmosphere, such as in the presence of N2.

9. The method (100) according to any one of the preceding claims, wherein the step of providing (110) lignin comprises providing lignin having an ash content of < 1%, and / or a moisture content of < 5 wt%.

10. The method (100) according to claim 9, wherein the step of providing (110) lignin comprises providing lignin having an ash content of < 1%, and a moisture content of < 5 wt%.

11. The method (100) according to claim 10, wherein the step of oxidatively thermostabilising (120) lignin comprises oxidatively thermostabilising the lignin having an ash content of < 1% and a moisture content of < 5 wt%.

12. The method (100) according to any one of the preceding claims, wherein the step of reducing (150) the size of the initially carbonised lignin by milling is followed by a step of sieving (155) the initially carbonised, milled lignin to remove lignin having a particlesize of > 50 μm, before performing the step of final carbonising (160) of the initially carbonised, milled lignin.

13. A hard carbon material produced by the method (100) according to any one of claims 1-12, characterised in that the hard carbon material has a specific surface area of from 3 to 7 m2 / g and a total pore volume of < 0.04 cm3 / g as evaluated based on nitrogen-gas adsorption data according to the Brunauer-Emmett-Teller (BET) method, a skeletal density of from 2.05 to 2.15 g / cm3as measured by helium pycnometry, and a median particle size by volume (D50) of from 4 to 7 μm as measured by laser diffraction technology based on Mie scattering theory.

14. A hard carbon material for use in a hard carbon electrode for a sodium-ion battery, wherein the hard carbon is derived from lignin, such as kraft lignin, such as softwood kraft lignin or hardwood kraft lignin, characterised in that the hard carbon material has a specific surface area of from 3 to 7 m2 / g and a total pore volume of < 0.04 cm3 / g as evaluated based on nitrogen-gas adsorption data according to the Brunauer-Emmett-Teller (BET) method, a skeletal density of from 2.05 to 2.15 g / cm3as measured by helium pycnometry, and a median particle size by volume (D50) of from 4 to 7 μm as measured by laser diffraction technology based on Mie scattering theory.

15. A method (200) for producing a hard carbon electrode for use in a sodium-ion battery, comprising the following steps, to be performed in the order listed:Providing (210) a hard carbon material produced by the method (100) according to any one of claims 1-12, or a hard carbon material according to any one of claims 13- 14;Mixing (220) the hard carbon material with a binding agent and water to obtain a slurry, optionally wherein the ratio of hard carbon material to binding agent is from 90:10 wt % to 95:5 wt %;Coating (230) a conductive substrate with the slurry, optionally wherein the conductive substrate is pre-coated with carbon;Evaporating (240) the water from the coating formed from the slurry, optionally by drying (240a) the slurry coating at room temperature;Drying (250) the coating formed from the slurry under vacuum at a temperature of from 120 °C to 150 °C for > 12 hours, thereby obtaining a hard carbon electrode.

16. A hard carbon electrode for use in a sodium-ion battery, wherein the hard carbon electrode has been produced by the method (200) according to claim 15.

17. A hard carbon electrode comprising the hard carbon material according to any one of claims 13-14.

18. The hard carbon electrode according to claim 16 or 17, characterised by a reversible specific capacity of > 311 mAh / g for the first discharge-charge cycle, a coulombic efficiency of > 87 % for the first discharge-charge cycle, a reversible specific capacity of > 306 mAh / g for the second discharge-charge cycle, and a coulombic efficiency of > 98.5 % for the second discharge-charge cycle, as determined by galvanostatic cycling in a half-cell configuration using an electrolyte solution comprising NaPF6 and diethylene glycol dimethyl ether solvent.

19. A sodium-ion battery comprising a hard carbon electrode according to any one of claims 16-18, wherein the hard carbon electrode forms a positive electrode.

20. The sodium-ion battery according to claim 19, further comprising an electrolyte solution comprising (a) a sodium salt, such as NaPF6, and (b) an ether solvent, such as a diethylene glycol dimethyl ether solvent, or a carbonate solvent, such as a solvent comprising ethylene carbonate and diethyl carbonate.