Composition containing anhydride functionalized cyclic polyorganosiloxane
The composition of anhydride functionalized cyclic polyorganosiloxane with specific diradicals and anhydride groups addresses the need for optically clear, hard, and non-delaminating coatings on substrates, enhancing adhesion and durability.
Patent Information
- Application Number
- PCT/US2026/019266
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-03-16
- Publication Date
- 2026-11-12
AI Technical Summary
There is a need for alternative adhesion promoters that can form optically clear, hard, and non-delaminating coatings on various substrates such as paper, metal, and glass, as existing solutions do not adequately address these requirements.
A composition comprising anhydride functionalized cyclic polyorganosiloxane, divinyl-terminated polyphenylsiloxane, vinyl-terminated polyphenylsiloxane resin, hydrogenphenylsiloxane, and a hydrosilylation catalyst is used to create coatings that adhere to substrates, utilizing specific diradicals and anhydride groups for enhanced bonding.
The composition forms optically clear, hard, and non-delaminating coatings on substrates like paper, metal, and glass, providing effective adhesion and durability.
Smart Images

Figure IMGF000001_0001 
Figure IMGF000002_0001 
Figure IMGF000002_0002
Abstract
Description
Composition Containing Anhydride Functionalized Cyclic PolyorganosiloxaneCross Reference To Related Applications
[0001] This application claims the benefit of U.S. Provisional Patent Application Serial No. 63 / 802,109 filed on May 8, 2025, under 35 U.S.C. §119 (e). U.S. Provisional Patent Application Serial No. 63 / 802,109 is hereby incorporated by reference.Background of the Invention
[0002] The present invention relates to a compound which is an anhydride functionalized cyclic polyorganosiloxane. The composition of the present invention is capable of forming optically clear, hard, and non-delaminating coatings for a variety of substrates such as paper, metal, plastic, and glass.
[0003] The adhesion of silicone-based compositions to substrates such as glass, metal, and a variety of plastics is facilitated with an adhesion promoter, which includes functionalized organosiloxanes. For example. US 6,887,932 B2 (Azechi) discloses a vast number of adhesion promoters that are functionalized polyorganosiloxanes containing Si-H groups. CN 103467965 A (Shinetsu) discloses adhesion promoters that are cyclic organosiloxanes containing Si-H, anhydride, and fluoroalkyl groups. Similarly, EP 3850049 Bl (Felder) discloses adhesion promoters that are acid anhydride functionalized polyorganosiloxanes containing Si-H groups. WO 2021 / 262830 (Santos) discloses a telechelic anhydride terminated polyorganosiloxane of the following formula:where n is from 2 to 20.
[0004] There is still a need to develop alternative solutions for adhesion promoters.Summary of the Invention
[0005] The present invention addresses a need in the art by providing a composition comprising:a) a compound of Formula 1:RmDHx-RnFormula 1b) a divinyl-terminated polyphenylsiloxane;c) a vinyl -terminated poly phenyl siloxane resin;d) a hydrogenphenylsiloxane; ande) a hydrosilylation catalyst;where X is either a (bisphenylmethylsilyl)oxy diradical or a (bisdimethylsilyloxy)diphenylsilyl diradical; each R is a Cs-Cn-alkyl anhydride group; the sum of m and n is in the range of from 1 to 4; and -Dnx- is a mono- or diradical of the compound of Formula 2:\ / OU— oSi \. / HH ' \ ?'\0Ys<<vFormula 2where x is from 3 to 10, and y is x - 3.
[0006] Alternatively, in the composition above, a) may comprise an anhydride functionalized cyclic polyorganosiloxane compound of Formula la:independently has an average value of 2 to 18, each R4is an independently selected monovalenthydrocarbyl group, each R5is selected from the group consisting of H and a C3-Ci2-alkyl anhydride group, with the proviso that at least one R5per molecule is the C3-Ci2-alkyl anhydride group; each R6is an independently selected divalent hydrocarbyl group; and Lis a divalent R3R3I / RArorganosilicon linking moiety selected from the group consisting of O andAr^S‘\ / Si\O O , wherein each RA|is an independently selected monovalent aromatic group and each R3is an independently selected alkyl group.
[0007] The composition of the present invention is capable of forming optically clear, hard, and non-delaminating coatings for a variety of substrates such as paper, metal, plastic, and glass.Detailed Description of the Invention
[0008] The present invention relates to a composition comprising:a) a compound of Formula 1:Rm-D«DHX-RnFormula 1b) a divinyl-terminated polyphenyl siloxane;c) a vinyl-terminated polyphenylsiloxane resin;d) a hydrogenphenylsiloxane; ande) a hydrosilylation catalyst;where X is either a (bisphenylmethylsilyl)oxy diradical or a (bisdimethylsilyloxy)diphenylsilyl diradical; each R is a C -Ci2-alkyl anhydride group; the sum of m and n is in the range of from 1 to 4; and -DHX- is a mono- or diradical of the compound of Formula 2:Formula 2where x is from 3 to 10. and y is x - 3.
[0009] The terms (bisphenylmethylsilyl)oxy diradical and (bisdimethylsilyloxy)diphenylsilyl diradical refer to the following fragments:(Bisphenylmethylsilyl)oxy Diradical (Bisdimethylsilyloxy)diphenylsilyl Diradical where the squiggly lines represent the points of attachment to the compound of Formula 2.
[0010] Examples of suitable anhydride groups include succinic anhydride, maleic anhydride, oxalic anhydride, and phthalic anhydride groups. Where the anhydride group is a succinic anhydride group, R is represented by the following fragment:where z is from 1 to 10, and where the dotted line represents the point of attachment to the DHXdiyl group.
[0011] Preferably, y is 1, 2, or 3, (that is, x is 4, 5, or 6) or a mixture thereof. In one embodiment, X is a (bisphenylmethylsilyl)oxy diradical, m is 1, n is 1, and z is 1. Accordingly, a possible configuration of a compound of the present invention is represented by Formula 3:Formula 3
[0012] It is understood that the R groups can be attached to any of the Si atoms of the DHXgroups and that the DHXgroups may be a blend of DHXgroups. For example, the DHXgroup is preferably a mixture of DH4, DH5. and DH6 groups. It is further understood that the compound of Formula 1 may comprise a blend of mono-, di-, tri-, and tetrasubstituted alkyl anhydride groups. In one embodiment, the compound of Formula 1 comprises a blend of mono- and disubstituted alkyl anhydride groups; i.e., m + n is in the range of 1 to 2.
[0013] In another embodiment, X is a (bisdimethylsilyloxy)diphenylsilyl diradical, m is 1, n is 1, y is 1, 2, or 3 or a mixture thereof, and z is 1. Accordingly, another possible configuration of a compound of the present invention is represented by Formula 4:Formula 4
[0014] The compound of Formula 1 (where m is 1 and n is 1) can be prepared in 2 steps, as illustrated:Pt catFormula 1o[ t caL» Formula 1where Formula lois represented by the following structure:Formula l0and Anh is an anhydride group. Karstedt’s catalyst is an example of a suitable Pt catalyst. An inhibitor such as tetra- / ?- butyl thiuram disulfide is advantageously added to the compound of Formula loif it is desired to store this intermediate prior to carrying out the second step.
[0015] Alternatively, the composition may comprise:a) an anhydride functionalized cyclic polyorganosiloxane compound of Formula laFormula la, whereineach subscript v independently has an average value of 2 to 18, each R4is an independently selected monovalent hydrocarbyl group, each R5is selected from the group consisting of H and an anhydride group, with the proviso that at least one R5per molecule is the anhydride group; each R6is an independently selected divalent hydrocarbyl group; and Lis a divalentR3R3| R^ | R^ ^Si\ / 'Si\ organosilicon linking moiety selected from the group consisting of O andR3RArR3I R3| RAr| R3^Si\ / Si\O O , wherein each RAris an independently selected monovalent aromatic group and each R3is an independently selected alkyl group;b) a divinyl-terminated polyphenyl siloxane;c) a vinyl-terminated polyphenylsiloxane resin;d) a hydrogenphenylsiloxane; ande) a hydrosilylation catalyst.a) Anhydride functionalized Cyclic Polyorganosiloxane
[0016] Starting material a) in the composition is the anhydride functionalized cyclic polyorganosiloxane, which may have Formula la, above. In the linking moiety L in Formula la, suitable alkyl groups for R3may have 1 to 20 carbon atoms, alternatively 1 to 10 carbon atoms, alternatively 1 to 6 carbon atoms, and alternatively 1 to 4 carbon atoms. Suitable alkyl groups may be linear or branched and include methyl, ethyl, and propyl (including n-propyl and isopropyl), alternatively methyl.
[0017] In the linking moiety L in Formula la above, the aromatic group for RA|may have 6 to 20 carbon atoms, alternatively 6 to 12 carbon atoms. The aromatic groups may be monocyclic or polycyclic, alternatively monocyclic. Examples of suitable aromatic groups include phenyl, tolyl, xylyl, 1 -phenylethyl, 2-phenylethyl, 2-methyl-2-phenylethyl, 3-phenylpropyl, 4-phenylbutyl, benzyl, styryl, naphthyl and anthracenyl. Alternatively, the aromatic group may be selected from the group consisting of phenyl, tolyl and xylyl. Alternatively, the aromatic group may be selected from the group consisting of phenyl and tolyl. Alternatively, the aromatic group may be phenyl. Alternatively, L in Formula la may be selected from the group consisting of the (bisphenylmethylsilyl)oxy diradical and the (bisdimethylsilyloxy)diphenylsilyl diradical, each as described above for X in Formula I.
[0018] In Formula la), each R6is an independently selected divalent hydrocarbyl group of 2 to 6 carbon atoms, alternatively 2, 3, or 6 carbon atoms. The divalent hydrocarbyl group for R6may be linear, branched, or a combination thereof. Examples of divalent hydrocarbyl groups for R6include -CH2-CH2-, -CH(CH3)-, -CH2CH2-CH2-, -CH(CH3)-CH2-, -CH2-CH2-CH2-CH2-, -CH2-CH2-CH2-CH2-CH2-, - CH2-CH2-CH2-CH2-CH2-CH2-, and branched isomers of 4 to 6 carbon atoms. Alternatively, each R6may have 2 carbon atoms and may be a combination of -CH2-CH2- and -CH(CH3)-. Alternatively, each R6may be -CH2-CH2-.
[0019] In Formula la. each R4is an independently selected monovalent hydrocarbyl group, alternatively an alkyl group of 1 to 20 carbon atoms, which may be as described and exemplified above for R3. Alternatively, each R4may be methyl.
[0020] In Formula la, each R5is independently selected from the group consisting of H and an anhydride group, with the proviso that at least one R5per molecule is the anhydride group. Examples of suitable anhydride groups for R5in Formula la include those derived from the hydrosilylation reaction of the unsaturated anhydrides described below with a silicon bonded hydrogen atom. Alternatively, the anhydride group for R5may be an alkyl succinic anhydride, such as propyl succinic anhydride.
[0021] In Formula la, each subscript v independently has an average value of 2 to 18, alternatively 2 to 10, alternatively 2 to 6, alternatively 2 to 4.
[0022] The anhydride functionalized cyclic polyorganosiloxane compounds of Formula 1 and Formula la described above may be prepared by methods such as those described in the examples below or by the method in US Provisional Patent Application Serial Number 63 / 802105 filed on 8 May 2025, which is hereby incorporated by reference.
[0023] The method for preparing the anhydride functionalized cyclic polyorganosiloxane compounds of Formula 1 and Formula la described above comprises a first hydrosilylation reaction of an alkenyl-functional siloxane and a cyclic polyorganohydrogensiloxane in the presence of a platinum hydrosilylation reaction catalyst to prepare a first hydrosilylation reaction product comprising an organohydrogensiloxane, and a second hydrosilylation reaction of the organohydrogensiloxane and an unsaturated anhydride.
[0024] More particularly, the method comprises: 1) combining, under conditions to effect a first hydrosilylation reaction, starting materials comprising: A) a hydrosilylation reaction catalyst; B) an alkenyl-functional siloxane; and C) a cyclic polyorganohydrogensiloxane; thereby preparing a first hydrosilylation reaction product comprising an organohydrogensiloxane. The starting materials used the method may optionally further comprise an additional startingmaterial selected from the group consisting of D) a solvent, E) a hydrosilylation reaction inhibitor, F) a thiuram disulfide, and a combination thereof.
[0025] The first hydrosilylation reaction in step 1) may be carried out batchwise, semi-batch or continuous in any suitable equipment, such as a jacketed reactor with agitation means such as an impeller or baffles. Step 1) may be performed with mixing and heating, e.g., at a temperature of 50 °C to 100 °C. alternatively 60 °C to 90 °C. and alternatively 70 °C to 80 °C. The starting materials used in step 1) may be combined by any convenient means. For example, one or more of the starting materials, such as A) the hydrosilylation reaction catalyst may be dissolved in D) the solvent. The starting materials may be combined in any order. Alternatively, to minimize potential for generation of hydrogen, A) the hydrosilylation reaction catalyst may be kept separate from C) the cyclic polyorganohydrogensiloxane until reaction begins. For example, A) the hydrosilylation reaction catalyst, B) the alkenyl-functional siloxane, and optionally all or a portion of D) the solvent may be combined and the resulting mixture metered into a reactor containing C) the cyclic polyorganohydrogensiloxane or a mixture of C) the cyclic polyorganohydrogensiloxane and all or a portion of D) the solvent. Starting material E) the hydrosilylation reaction inhibitor may be added to one or both of the above mixtures to control hydrosilylation reaction rate.
[0026] The method for preparing the first hydrosilylation reaction product comprising the organohydrogensiloxane may optionally further comprise one or more additional steps. For example, the method may optionally further comprise, before step 1), treating (e.g., by stripping or distilling) one or more of the starting materials. For example, starting material B) and / or starting material C) may be treated to remove water (drying) or other impurities before step 1). Alternatively, the method may further comprise 2) purifying the organohydrogensiloxane produced during step 1). For example, after formation of first hydrosilylation reaction product comprising the organohydrogensiloxane, purifying may be performed by any convenient means, such as stripping and / or distillation with heating and optionally reduced pressure. The method may optionally further comprise step 3): adding F) the thiuram disulfide. All or a portion of the thiuram disulfide may be added during step 1). Alternatively, F) the thiuram disulfide may be added during step 1), for example, when the first hydrosilylation reaction will be carried out in the presence of the Pt-Thiuram complex at temperatures such as 80 °C to 90 °C. Alternatively, all or a portion of F) the thiuram disulfide may be added to the first hydrosilylation reactionproduct comprising the organohydrogensiloxane after step 1) and / or to the organohydrogensiloxane after step 1) or after step 2), when step 2) is present. Alternatively, the thiuram disulfide may be added to the first hydrosilylation reaction product after step 1) and before step 2) (e.g., to minimize potential for gelation of the organohydrogensiloxane during storage or purification in step 2), when step 2) is present. The thiuram disulfide may optionally be delivered in a solvent, such as starting material D). When step 1) uses a platinum catalyst for starting material A), then step 3) is present, and F) the thiuram disulfide is present in the first hydrosilylation reaction product. Without wishing to be bound by theory, it is thought that the selection and amount of F) the thiuram disulfide, and when it is added during the method depends on various factors including the selection and amounts of starting materials A) and B).
[0027] Hydrosilylation reaction catalysts suitable for starting material A) in the method for preparing the first hydrosilylation reaction product comprising the organohydrogensiloxane are known in the art and are commercially available. Hydrosilylation reaction catalysts include platinum metal. Alternatively, the hydrosilylation catalyst may be a compound of platinum, for example, chloroplatinic acid (Speier’s Catalyst), hexachloroplatinic acid hexahydrate, platinum dichloride, and complexes of said compounds with organopolysiloxanes or platinum compounds microencapsulated in a matrix or coreshell type structure. Complexes of platinum with alkenyl-functional organopolysiloxanes include l,3-diethenyl-l,l,3,3-tetramethyldisiloxane complexes with platinum (Karstedt’s Catalyst) and methylvinylcyclosiloxane complexes with platinum (Ashby’s Catalyst). These complexes may be microencapsulated in a resin matrix. Exemplary hydrosilylation reaction catalysts are described in US Patent 12195593 and the references cited therein. Alternatively, in step 1) of the method, the platinum group metal may be platinum. The amount used may be sufficient to provide 1 ppm to 1,000 ppm of platinum group metal based on combined weights of starting materials A), B), and C). Alternatively, in step 1), the amount of platinum may be up to 5 ppm, alternatively < 5 ppm, alternatively up to 2 ppm, and alternatively < 2ppm; while at the same time, the amount of platinum is > 0 ppm, alternatively at least 1 ppm, each based on combined weights of starting materials A), B), and C). Without wishing to be bound by theory, it is thought that using > 0 ppm to 5 ppm, alternatively 1 ppm to 5 ppm, of platinum may minimize side reactions such as crosslinking and / or gelation.
[0028] Starting material B) used in the method described above is an alkenyl-functional siloxane. The alkenyl-functional siloxane is selected from the group consisting of B-l)R3R3R3RArR3| _RAr| _RAr| R3| _RAr| R3RV1O RV1and B-2) RV1O O RV1, wherein each RA|is an independently selected monovalent aromatic group, each R3is an independently selected alkyl group, both as described and exemplified above, and each RV1is an independently selected alkenyl group of 2 to 6 carbon atoms, alternatively 2, 3, or 6 carbon atoms. Alternatively, each RV1may be vinyl or hexenyl, and alternatively vinyl. Examples of alkenyl-functional siloxanes of formula B-2) include l,5-divinyl-l,l,5,5-tetramethyl-3,3-diphenyltrisiloxane with CAS #18586-22-6, which is available from various sources, such as TCI America and Cymit Qulmica S.L. of Barcelona, Spain. Examples of alkenyl-functional siloxanes of formula B-l) include 1,3-divinyl-l,3-dimethyl-l,3-diphenyldisiloxane with CAS #2627-97-6 and which is available from various sources such as Alpha Chemistry of Holbrook, New York, USA.
[0029] Starting material C) for the method described herein is a cyclic polyorganohydrogensiloxane of formula C-l): (R4HSiO2 / 2)k, where subscript k has an average value of 4 to 20, and each R4is as described above. Alternatively, subscript k may have an average value of at least 4, alternatively at least 5, and alternatively at least 6; while at the same time subscript k may have a value up to 20, alternatively up to 15, alternatively up to 12, alternatively up to 10, alternatively up to 8, and alternatively up to 6. Alternatively, subscript k may have an average value of 4 to 10, and alternatively 4 to 8. Alternatively, subscript k may have an average value of 4 to 6, alternatively 4 to 5, alternatively > 4 to 5. and alternatively 4.5 to 5.
[0030] Examples of suitable cyclic polyorganohydrogensiloxanes for starting material C) include tetramethylcyclotetrasiloxane (with CAS No. 2370-88-9), pentamethylcyclopentasiloxane (with CAS No. 6166-86-5), hexamethylcyclohexasiloxane (with CAS No. 6166-87-6), and combinations of two or more thereof. Suitable cyclic polyorganohydrogensiloxanes are known in the art and are commercially available, e.g., DOWSIL™ MH- 1109 Fluid from Dow Silicones Corporation of Midland, Michigan, USA and SIP6718.0 and SIT7530.0 both from Gelest.
[0031] The amounts of B) the alkenyl-functional siloxane and C) the cyclic polyorganohydrogensiloxane may be in the method used in amounts such that the molar ratio of cyclic polyorganohydrogensiloxane : alkenyl-functional siloxane, C:B, is > 2:1, alternatively >3:1, alternatively > 4:1, and alternatively > 6:1. Alternatively, starting materials B) and C) may be used in amounts such that the content of silicon bonded hydrogen atoms in starting material C) to content of silicon bonded alkenyl in starting material B) (SiH : Vi mole ratio) is 10:1 to 40:1, alternatively 10:1 to 20:1, and alternatively 10:1 to 15:1. Alternatively, SiH : Vi ratio may be at least 4:1, alternatively at least 6:1, alternatively at least 8:1, alternatively at least 9:1, alternatively at least 12:1, alternatively at least 13:1, alternatively at least 14:1, alternatively at least 15:1, and alternatively at least 45: 1; while at the same time, SiH : Vi ratio may be up to 180 : 1, alternatively up to 90: 1; alternatively up to 50:1. Alternatively, the SiH : Vi ratio may be 4:1 to 8:1, and alternatively 4:1 to 6:1.
[0032] A solvent may be used in the method described herein. The solvent may facilitate introduction of certain starting materials, such as A) the hydrosilylation reaction catalyst and / or F) the thiuram disulfide. Solvents used herein are those that help fluidize the starting materials. Solvent may be selected based on solubility the starting materials and volatility of the solvent. The solubility refers to the solvent being sufficient to dissolve and / or disperse the starting materials. Volatility refers to vapor pressure of the solvent.
[0033] Suitable solvents may be hydrocarbons. Suitable hydrocarbons include aromatic hydrocarbons such as benzene, toluene, or xylene; and / or aliphatic hydrocarbons such as heptane, hexane, or octane. Alternatively, the solvent may be a halogenated hydrocarbon such as dichloromethane, 1,1,1 -trichloroethane or methylene chloride.
[0034] The amount of solvent can depend on various factors including the type of solvent selected and the amount and type of other starting materials selected. However, the amount of solvent may range from 0.1% to 99%, alternatively 2% to 50%, based on combined weights of A) the hydrosilylation reaction catalyst, B) the alkenyl-functional siloxane, and C) the cyclic polyorganohydrogensiloxane.
[0035] Starting material E) is a hydrosilylation reaction inhibitor that may be used in the method for making the first hydrosilylation reaction product comprising the organohydrogensiloxane. The hydrosilylation reaction inhibitor may be for example, an acetylenic alcohol such as methyl butynol or ethynyl cyclohexanol, a silylated acetylenic alcohol, an unsaturated hydrocarbon diester; a conjugated ene-yne, an olefinic siloxane, a maleate, a fumarate, or a combination thereof. The amount of inhibitor may be an amount effective to control hydrosilylation reaction rate because hydrosilylation reaction is exothermic. The amountof inhibitor selected depends on various factors including the type and amount of hydrosilylation reaction catalyst and inhibitor selected, however, if used, the amount may be sufficient to provide 1 ppm to 1.000 ppm of the platinum group metal based on combined weights of reactants (e.g., B) the alkenyl-functional siloxane and C) the cyclic polyorganohydrogensiloxane). Suitable hydrosilylation reaction inhibitors are known in the art and are described, for example, described as ingredient i) in US Patent 9593209 at col. 15, line 35 to col. 16, line 17. Alternatively, the first hydrosilylation reaction may be performed in a semi-batch or continuous process, such that a hydrosilylation reaction inhibitor described herein as starting material E) is not required, for example the exothermic hydrosilylation reaction can be controlled by the order of addition of the starting materials, e.g., by metering starting materials B) and / or C).
[0036] Starting material F) is a thiuram disulfide. Without wishing to be bound by theory, it is thought that the thiuram disulfide will complex with the platinum from A) the hydrosilylation reaction catalyst (when a platinum catalyst is used) to form an inhibited platinum at temperatures of 120 °C and lower, alternatively 100 °C and lower, alternatively 80 °C and lower, such that the inhibited platinum does not catalyze a hydrosilylation reaction, and such that side reactions such as gelation of the organohydrogensiloxane are minimized or avoided during purification, storage, or both, as described herein. The thiuram disulfide may have formula F-l):S RJ„ 0 IRNS F-l), wherein RH, RN, RJ, and RKare each an independently selected monovalent hydrocarbyl group having 1 to 20 carbon atoms, which may be saturated or unsaturated; a heteroatom-containing monovalent hydrocarbyl group having 1 to 20 carbon atoms, which may be saturated or unsaturated; or combinations thereof. Suitable heteroatoms may include, for example, an oxygen atom. RHand RNgroups may combine to form one or more carbocyclic groups having 4 to 20 carbon atoms. RJand RKgroups may combine to form one or more carbocyclic groups having 4 to 20 carbon atoms.
[0037] In formula F-l), RH, RN, RJ, and RKcan be the same or different, and alternatively, these groups may be the same. Alternatively RH, RN, RJ, and RKmay be each independently selected from an alkyl group having 1 to 20 carbon atoms, alternatively 1 to 12, alternatively 1 to 6, alternatively 1 to 4, or alternatively 1 to 2 carbon atoms; an aromatic group having 6 to 20carbon atoms, such as phenyl or benzyl; or combinations thereof. Alternatively, RH, RN, RJ, and RKare each independently selected alkyl groups. Alternatively, RH, RN, RJ, and RKare each independently selected from methyl, iso-butyl, n-butyl. or combinations thereof.
[0038] Specific examples of suitable thiuram disulfides include tetrabenzylthiuram disulfide (with CAS No. 10591-85-2), tetramethylthiuram disulfide (with CAS No. 137-26-8), tetraethylthiuram disulfide (with CAS No. 97-77-8), tetra(iso-propyl)thiuram disulfide, tetra(iso-butyl)thiuram disulfide (with CAS No. 3064-73-1), and tetra(n-butyl)thiuram disulfide (with CAS No. 1634-02-2), all of which are commercially available from various sources such as Sigma- Aldrich, Inc., TCI America, Fischer Scientific, or Cymit Qufmica S.L. Alternatively, the thiuram disulfide may be selected from tetramethylthiuram disulfide, tetra(n-butyl)thiuram disulfide, or mixtures thereof.
[0039] The thiuram disulfide may be optionally diluted in a solvent before use in the method. The solvent may be any material that can dissolve the thiuram disulfide, as described and exemplified above for starting material D). Alternatively, the solvent for the thiuram disulfide may be selected from aromatic hydrocarbons such as benzene, halogenated hydrocarbons, ethers, or mixtures thereof. Without wishing to be bound by theory, it is thought that it may be desirable to use as little solvent as possible to facilitate dissolving the thiuram disulfide and, if desired, to later remove the solvent, e.g., by evaporation, distillation, and / or stripping. Examples of suitable solvents may include halogenated hydrocarbons such as dichloromethane, chloroform (CHCh), and / or tetrachloromethane. The solvent may be used in an amount of 0.1% to 5% by weight based on the weight of the thiuram disulfide.
[0040] The thiuram disulfide may be added in an amount such that the molar ratio of the thiuram disulfide to platinum in the hydrosilylation reaction catalyst (F / Pt ratio) may range from 0.9 to 100. Alternatively, this molar ratio may be 1 or higher, alternatively greater than 1, alternatively 1.1 or higher, and alternatively 1.2 or higher, alternatively 2 or higher, alternatively 3 or higher, alternatively 4 or higher, alternatively 5 or higher, alternatively 6 or higher, alternatively 7 or higher, alternatively 8 or higher, alternatively 9 or higher; while at the same time this ratio may be 100 or lower, alternatively 75 or lower, alternatively 50 or lower, alternatively 40 or lower, alternatively 30 or lower, alternatively 20 or lower, alternatively 10 or lower, alternatively 5 or lower, alternatively 3 or lower, alternatively 2 or lower, and alternatively 1.2 or lower. Alternatively, this F / Pt ratio may be 1 to 10, alternatively 1 to 5, alternatively 2 to5, alternatively 2 to 3.5, alternatively 1 to 2, and alternatively, 1 to 1.2.
[0041] Alternatively, at low platinum concentration (e.g., > 0 ppm to 5 ppm based on combined weights of starting materials A), B), and C) described above), the F / Pt ratio may be 3 to 3.5, and this may allow for higher purification (e.g., stripping) temperatures. Without wishing to be bound by theory, it is thought that the Pt- thiuram complex is stable at temperatures below 120 °C, alternatively 115 °C or below, and alternatively 110 °C or below. Therefore, stripping under conditions of 95 °C at 0 - 3 mbar wherein the Pt-Thiuram complex is stable can be performed while gelation is avoided or minimized.
[0042] The first hydrosilylation reaction product of the method described above comprises a) the organohydrogensiloxane. This reaction product may further comprise unreacted starting materials (e.g., unreacted B) alkenyl-functional siloxane or unreacted C) cyclic polyorganohydrogensiloxane, when one or the other is used in molar excess), residual A) hydrosilylation reaction catalyst, and when used D) the solvent, E) the hydrosilylation reaction inhibitor, and / or F) the thiuram disulfide, at least a portion of which may be complexed with the platinum from A) the hydrosilylation reaction catalyst. The organohydrogensiloxane a’)Hcomprises formula a’-l): subscript v and R4, R6, and L are as described above for formula la.
[0043] Alternatively, the organohydrogensiloxane may have formula a’ -2):R3, R^, and subscript v are as described above. Alternatively, the organohydrogensiloxane maysubscript v independently has an average value of 2 to 4, and Ph means phenyl.
[0044] Alternatively, the organohydrogensiloxane may have formula a’ -4):and subscript v are as described above. Alternatively, the organohydrogensiloxane may compriseformula a’ -5): each subscript v independently has an average value of 2 to 4, and Ph means phenyl.
[0045] The method described above further comprises functionalizing the above-described a’) organohydrogensiloxane to form a) the anhydride functionalized cyclic polyorganosiloxane used in the composition described herein. The method for functionalizing a’) the organohydrogensiloxane comprises: i) practicing the method comprising step 1), and optionally one or more of the additional steps, described above to prepare the first hydrosilylation reaction product comprising a) the organohydrogensiloxane described above, and ii) combining, under conditions to effect a second hydrosilylation reaction, starting materials comprising the firsthydrosilylation reaction product, or a’) the organohydrogensil oxane, as described above; optionally b’) a hydrosilylation reaction catalyst; and c’) an unsaturated anhydride; thereby preparing a second hydrosilylation reaction product comprising a) the anhydride functionalized cyclic polyorganosiloxane. The second hydrosilylation reaction may be carried out batchwise or continuous in any suitable equipment, such as a jacketed reactor with agitation means such as an impeller or baffles.
[0046] In the method to form a) the anhydride functionalized cyclic polyorganosiloxane described herein, the hydrosilylation reaction may be performed by optionally dissolving or dispersing b’) the hydrosilylation reaction catalyst (as described above for starting material A)) in d’) a solvent (such as that described above as starting material D)) to facilitate mixing.Starting materials comprising a’) the organohydrogensiloxane or c’) the unsaturated anhydride may be placed in the reactor with b’) the hydrosilylation reaction catalyst, and the other of c’) the unsaturated anhydride and a’) the organohydrogensiloxane may be fed into the reactor continuously or intermittently to control any exotherm. The reactor may be heated or cooled, such that the reaction mixture may be maintained a temperature of 50 °C to 150 °C, alternatively 60 °C to 100 °C, alternatively 70 °C to 90 °C. The same reactor used to prepare the first hydrosilylation reaction product may be used herein to prepare the second hydrosilylation reaction product comprising a) the anhydride functionalized cyclic polyorganosiloxane.Alternatively, a different reactor may be used.
[0047] Alternatively, the method for functionalizing a’) the organohydrogensiloxane to form a) the anhydride functionalized cyclic polyorganosiloxane compound may optionally further comprise an additional step. For example, this method may further comprise iii) adding e’) a hydrosilylation reaction inhibitor to the hydrosilylation reaction product; and / or iv) recovering the anhydride functionalized cyclic polyorganosiloxane from the second hydrosilylation reaction product. Recovering may be performed by any convenient means, such as stripping and / or distillation with heating, and optionally under vacuum.
[0048] Hydrosilylation reaction catalysts suitable for starting material b’) in the method for functionalizing the organohydrogensiloxane as described and exemplified above for starting material A) in the method for preparing the first hydrosilylation reaction product comprising the organohydrogensiloxane. Starting material b’) is optional, for example, additional hydrosilylation reaction catalyst may not be needed if starting material A) is present in the firsthydrosilylation reaction product or if said catalyst is not inhibited, deactivated, or removed from the organohydrogensiloxane of formula a’-l). Alternatively, starting material b’) may be added when A) the hydrosilylation reaction catalyst used to make the organohydrogensiloxane is a platinum hydrosilylation reaction catalyst that is complexed with F) the thiuram disulfide in the method as described above. Alternatively, starting material b) may not be needed even if A) the platinum hydrosilylation reaction catalyst is complexed with F) the thiuram disulfide in the first hydrosilylation reaction product if the conditions (e.g., temperature) selected for the method for functionalizing the organohydrogensiloxane are sufficient to decomplex starting materials A) and F). Starting material b’) may be the same or a different species as that selected for use above to make the first hydrosilylation reaction product comprising organohydrogensiloxane. For example, starting material b’) may be a hydrosilylation reaction catalyst comprising a platinum group metal other than platinum, e.g., a rhodium catalyst. Without wishing to be bound by theory, it is thought that when the thiuram disulfide is tetra(methyl)thiuram disulfide, then starting material b’) is present and comprises the metal other than platinum; however, when the starting material F) is a thiuram disulfide other than tetra(methyl)thiuram disulfide, then starting material b’) is optional. However, the amount of the hydrosilylation reaction catalyst used in this method to functionalize the organohydrogensiloxane may be sufficient to provide 1 ppm to 1,000 ppm of platinum group metal based on combined weights of starting materials a’), b’), and c’). Alternatively, when starting material b’) is used, it may be added at a concentration of 1 ppm or more, alternatively 10 ppm or more, alternatively 20 ppm or more, alternatively 30 ppm or more, alternatively 40 ppm or more, alternatively 50 ppm or more, alternatively 60 ppm or more, alternatively 70 ppm or more, alternatively 80 ppm or more, alternatively 90 ppm or more, alternatively 100 ppm or more, alternatively 120 ppm or more, alternatively 140 ppm or more, alternatively 160 ppm or more, alternatively 180 ppm or more; while at the same time starting material b’) may be added at a concentration of 200 ppm or less, alternatively 180 ppm or less, alternatively 160 ppm or less, alternatively 140 ppm or less, alternatively 120 ppm or less, alternatively 110 ppm or less, alternatively 100 ppm or less, alternatively 80 ppm or less, on the same basis above.
[0049] Starting material c’) the unsaturated anhydride is any suitable compound that can produce the anhydride group described above via hydrosilylation reaction with a silicon bonded hydrogen atom. By the term “anhydride functionality” it is meant that the anhydride group forR5comprises the following structure: -C(=O)O-C(=O)-. Unsaturated anhydrides include maleic anhydride, alkenyl succinic anhydrides, polyisobutylenylsuccinic anhydride, citraconic anhydride, bromomaleic anhydride, crotonic anhydride, diphenic anhydride, isatoic anhydride, itaconic anhydride, phenylmaleic anhydride, nadic anhydride, 3- (but-3-enyl)-l, 2,3,6-tetrahydrophthalic anhydride, and cis- 1,2, 3, 6- tetrahydrophthalic anhydride and phenylsuccinic anhydride. The anhydride functionality may also be formed from unsaturated anhydrides featuring bridged heterocyclic structures, such as bicyclooctenedicarboxylic anhydrides such as CAS 6708-37-8, carbic anhydrides (CAS 129-64- 6), bicyclooctenetetracarboxylic dianhydrides such as bicyclo[2,2,2]oct-7-ene-2,3,5,6- tetracarboxylic dianhydride (CAS 1719-83-1), ethenocyclobutabenzofuran-triones such as CAS 55054-47-2, and ethenocycloheptafuran-diones such as CAS 5650-01-1 and their isomeric variants. For example, the anhydride functionality in the anhydride group for R5can be, and alternatively is, a cyclic anhydride i.e., in a fivemembered or six membered ring. Alternatively, the unsaturated anhydride may comprise one or more of allyl succinic anhydride (CAS # 7539-12-0); 3-(2-methallyl)succinic anhydride); dihydro-3-(l,l,2-trimethyl-2-propen-l-yl)-2,5-furandione; 3-(l,2-dimethyl-2-propen-l-yl)dihydro-2,5-Furandione; and 3-(2-neopentylallyl)tetrahydrofuran-2, 5-dione.
[0050] Starting material e’) the hydrosilylation reaction inhibitor may be as described and exemplified above for starting material E) in the method for preparing the first hydrosilylation reaction product comprising a) the organohydrogensiloxane. The amount of e’) inhibitor selected for use in this method for preparing the second hydrosilylation reaction product comprising a) the anhydride functionalized cyclic polyorganosiloxane depends on various factors including the type and amount of catalyst and inhibitor selected, however, the amount may be 0.00001 to 3 parts by weight, per 100 parts by weight of c’) the unsaturated anhydride.
[0051] The starting materials used in the method for functionalizing the organohydrogensiloxane may optionally further comprise one or more additional starting materials. The additional starting materials may be those additional ingredients disclosed in US Patent 9593209 at col. 10. line 48 to col. 16, line 17. The additional starting materials selected from the group consisting of filler, with or without treating agent, non-reactive resin, chain extender, endcapper, and hydrosilylation reaction catalyst inhibitor as described above.
[0052] The method described above produces the second hydrosilylation reaction product comprising a) the anhydride functionalized cyclic polyorganosiloxane compound. The anhydridefunctionalized cyclic polyorganosiloxane compound comprises formula a-1):, where subscript v, R4. R6, and L are as described above, and each R3is independently selected from the group consisting of H and an anhydride group (which is derived from c;), the unsaturated anhydride, via hydrosilylation reaction, as described above), with the proviso that at least one R5per molecule is the anhydride group (i.e., at least one instance of R5per molecule is not hydrogen). Alternatively, 1 to 4 instances of R5per molecule are anhydride groups. Alternatively 1 to 3, alternatively 1 to 2, and alternatively an average of two instances of R5per molecule are the anhydride groups.Alternatively, one instance of R5on each cyclic siloxane ring may be the anhydride group and the other instances of R5may be H. Alternatively, two instances of R5on each cyclic siloxane ring may be the anhydride group and the other instances of R5may be H. Alternatively, three instances of R5on each cyclic siloxane ring may be the anhydride group and the other instances of R5may be H. The anhydride group for R5is derived from starting material c’) the unsaturated anhydride described above. The anhydride group for R5may be propyl succinic anhydride. Alternatively, in formula a-1) each subscript v may independently have an average value of 2 to 4, alternatively > 2 to 4, alternatively 2 to 3. alternatively > 2 to 3. alternatively 2, and alternatively 3.
[0053] Alternatively, the anhydride functionalized cyclic polyorganosiloxane may haveformula a-2): where R4, R5, subscript v, R6, R3, and RArare as described and exemplified above. Alternatively,the anhydride functionalized cyclic polyorganosiloxane may comprise formula a-3):where each subscript v has an average value of 2 to 4, Ph means phenyl, and each R5is H or an alkyl succinic anhydride group, such as propyl succinic anhydride, with the proviso that at least one instance of R5per molecule is the alkyl succinic anhydride group.
[0054] Alternatively, the anhydride functionalized cyclic polyorganosiloxane may haveformula a-4): where R4, R5, subscript v. R6, R3, and RArare as described and exemplified above. Alternatively, the anhydride functionalized cyclic polyorganosiloxane may comprise formula a-5):has an average value of 2 to 4, Ph means phenyl, and each R3is H or an alkyl succinic anhydride group, such as propyl succinic anhydride, with the proviso that at least one instance of R5per molecule is the alkyl succinic anhydride group.
[0055] The anhydride functionalized cyclic polyorganosiloxane compound of Formula la and / or the compound of Formula 1 described above, are useful in curable compositions, e.g., asadhesion promoters. The compound of Formula 1 has been found to be useful as an adhesion promoter in a composition used to improve the adhesion of an organopolysiloxane to a substrate such as paper, metal, plastic, or glass.
[0056] The term “divinyl-terminated polyphenylsiloxane” is preferably a compound of Formula 5:Me / ph \ Me- Si - O— (— Si - O - Si - AM1e V \R' / nMeFormula 5where Ph is phenyl; each R' is independently Ci-Ce-alkyl or phenyl; and n is from 1 or from 5 or from 10 to 500 or to 200 or to 100. Preferred Ci-Ce-alkyl groups are methyl groups. Preferably, each R' is methyl. Preferably, the concentration of the divinyl-terminated polyphenylsiloxane, is in the range of from 1 or from 2 or from 4 weight percent, to 30 or to 10 or to 8 weight percent, based on the weight of the composition.
[0057] The vinyl-terminated polyphenylsiloxane resin is conveniently prepared by reacting together a tri-Ci-Ce-alkoxyphenylsilane and a compound of Formula 6:Formula 6where n' is from 1 to 20, preferably to 10, and more preferably to 5; most preferably, n' is 1 and each R' is methyl. This most preferred vinyl-terminated polyphenylsiloxane resin, MMeP11V1aTPhb, where a and b are mole fractions, wherein a + b = 1, can be conveniently prepared by contacting trimethoxyphenylsilane with l,3-dimethyl-l,3-diphenyl-l,3-divinyldisiloxane in the presence of an acid catalyst. Mole fraction a is preferably in the range of from 0.10 to 0.40 and mole fraction b is preferably in the range of from 0.60 to 0.90. MMePhV1is represented by the following fragment:PhSi - OMeand TPhis represented by the following fragment:Ph0 - Si - 0O.where the dotted lines represent bonds to other silicon atoms in the vinyl-terminated polyphenylsiloxane resin. Preferably, the concentration of the vinyl-terminated polyphenylsiloxane resin is in the range of from 50 to 80 weight percent, based on the weight of the composition.
[0058] The term “hydrogenphenylsiloxane” refers to a compound of Formula 7:(MHR"2)e(DHR")d(DR"2)e(TR")fwhere each R'' is independently phenyl or Ci-Ce-alkyl, with the proviso that at least one of the R'' groups is a phenyl group; c, d, e, and f are mole fractions wherein c + d + e + f= 1; wherein c is from 0.01 to 0.75; d is from 0 to 0.4; e is from 0 to 0.96; and f is from 0 to 0.6; wherein MHR"2, DHR", DR 2and, TR" are defined as follows:R" R" R" O I l l i H - Si - O — W — o - Si - O— — O - Si - O — W. — O - Si — o —R I" Hl Rl" Ri" MHR"2DHR" DR"2TR” An example of a hydrogenphenylsiloxane is a compound of Formula 7a:Me / Ph \ Me1II I1M ie T \Ri" / TmM ieFormula 7awhere m is from 1 to 50 or to 20 or to 10. Preferably m is 1. Preferred Ci-Ce-alkyl groups aremethyl groups. Preferably, each R" is phenyl. Preferably, the concentration of the hydrogenphenylsiloxane is in the range of from 10 to 30 weight percent.
[0059] The hydrosilylation catalyst is a catalyst that promotes hydrosilylation. Examples of suitable hydrosilylation catalysts are as described above, and alternatively include platinum(II) acetoacetonate, platinum(O) 1, 3-divinyl-l,l, 3, 3-tetramethyldisiloxane complex and trimethyl(methylcyclopentadienyl)platinum (IV). The composition may further contain an inhibitor for the platinum catalyst such as those described above, alternatively phenylbutynol or methyl (tris(l,l-dimethyl-2-propynyl) oxy) silane, and a pigment such as STAN-TONE 40SP03 Blue pigment.ExamplesExample 1 - Preparation of Compound of Formula 4A. Preparation of Intermediate AFormula 2 Divinylsiloxane Int. A Intermediate A
[0060] A 3L 4-neck round bottom flask equipped with a dropping funnel, a multiport with 2 inlets for dry N2 and dry air, a temperature controller, a reflux condenser, and a magnetic stir bar, was placed on a hot plate. Toluene (400 g) and chloroplatinic acid hexahydrate (1 wt.% in isopropanol, 0.18 g) were added to the flask, and a mixture of the compound of Formula 2 (y = 1, 2, and 3; 938 g) and Divinyl Intermediate A (500 g) was loaded into the dropping funnel. The mixture in the flask was heated to 75 °C with stirring and dry air flow, followed by dropwise addition of the mixture from the dropping funnel. After addition was completed, the reaction mixture was stirred for 1 h at 75 °C. An aliquot of the reaction mixture was removed forNMR spectroscopic analysis to verify that the vinyl groups were fully consumed. The reaction mixture was cooled to 60 °C, at which temperature tetra- / ?-butyl thiuram disulfide (1 wt.% in toluene solution, 0.64 g) was added. The reaction mixture was stirred for an additional 3 h, cooled to room temperature, then transferred to another flask. The volatile materials were removed in vacuo at 95 °C and 0.1 mbar for 2 h, and the residue liquid (1014g) was transferred into a Nalgene bottle and kept under N2. The product was characterized by1H,13C, and29SiNMR spectroscopies.B. Preparation of Compound of Formula 4Intermediate Aallyl succinic anhydride Formula 4
[0061] A 4-neck round bottom flask was charged with Intermediate A (94.1 g). The flask was equipped with a glass stir rod with a Teflon stir paddle, a cooled condenser equipped with an outlet leading to a bubbler, a thermocouple fitted with a nitrogen inlet, and an addition funnel, which was charged with allyl succinic anhydride (ASA, 26.5 g). Intermediate A was heated to 50-75 °C and stirred. A portion of ASA (1.3 g) was then added to the flask from the addition funnel, followed by addition of Karstedt’s catalyst (1 wt% solution in toluene, 0.024 g) with a micropipette. The remainder of the ASA was added slowly to ensure that the reaction temperature remained below 90 °C. After ASA addition was completed, additional Karstedt’s catalyst (1 wt% solution in toluene, 0.024 g) was added, and the reaction mixture was stirred at 80 °C for another 30 min. The reaction mixture was cooled to ambient temperature, then charged with 1-ethynyl-l -cyclohexanol (ETCH, 0.204 g), before being transferred to a Nalgene bottle. The product was characterized by 'H,13C and29Si NMR spectroscopy, as well as by FTIR spectroscopy.Example 2 - Preparation of Compound of Formula 3A. Preparation of Intermediate BFormula 2 Divinyl Siloxane Tnt. BIntermediate B
[0062] A 3L 4-neck round bottom flask equipped with a dropping funnel, a multiport with 2 inlets for dry N2 and dry air, a temperature controller, a reflux condenser, and a magnetic stir bar, was placed on a hot plate. Toluene (217 g) and chloroplatinic acid hexahydrate (1 wt.% in isopropanol, 0.10 g) were added to the flask, and a mixture of the compound of Formula 2(y = 1 , 2, and 3; 577 g) and Divinyl Siloxane Intermediate B (248 g) was loaded into the dropping funnel. The mixture in the flask was heated to 75 °C with stirring and dry air flow, followed by dropwise addition of the mixture from the dropping funnel. After addition was completed, the reaction mixture was stirred for 1 h at 75 °C. An aliquot of the reaction mixture was removed for]H NMR spectroscopic analysis to verify that the vinyl groups were fully consumed. The reaction mixture was cooled to 60 °C, at which temperature n-butyl thiuram (1 wt% in toluene solution, 0.36 g) was added. The reaction mixture was stirred for an additional 3 h, cooled to room temperature, then transferred to another flask. The volatile materials were removed in vacuo at 95 °C and 0.1 mbar for 2 h, and the residue liquid (585g) was transferred into a Nalgene bottle and kept under N2. The product was characterized by1H,13C, and29Si NMR spectroscopies.B. Preparation of the Compound of Formula 3
[0063] A 4-neck round bottom flask was charged with Intermediate B (173.3 g). The flask was equipped with a Teflon coated magnetic stir bar, a cooled condenser equipped with an outlet leading to a bubbler, a thermocouple fitted with a nitrogen inlet, and an addition funnel which was charged with allyl succinic anhydride (ASA, 57.4 g). Intermediate B was heated to 80 °C, followed by the addition of ca. 2.9 g ASA upon stirring. Karstedt’s catalyst (1 wt% solution in toluene, 0.030 g) was added via micropipette. Exotherm was observed immediately. ASA was added gradually at a rate to keep the reaction temperature below 100°C. After the addition of ASA was complete, additional Karstedt’s catalyst (1 wt% solution in toluene, 0.060 g) was added in two aliquots and the reaction mixture was stirred at 80 °C for another 30 minutes. The SiH consumption was monitored by a Perkin Elmer FTIR fitted with an ATR plate. After cooled to ambient temperature, the reaction mixture was charged and mixed with ETCH (0.358 g), before transferred to a Nalgene bottle. The product was characterized by!H,13C and29Si NMR as well as FTIR and GPC.Example 3 - Preparation of UV-Heat Curable Organosiloxane Composition with Formula 3Adhesion Promoter
[0064] A curable organopolysiloxane composition was prepared by blending MV1DPh2sMV1(6.5 parts by weight, pbw), MPhV1o.23TPho.77 (68.1 pbw), MHDPh2MH(20.4 pbw); methyl(tris(l,l-dimethyl-2-propynyl) oxy) silane (0.001 pbw); and the compound of Formula 3 (1.0 pbw). The mixture was blended for 2 min at 1,500 rpm, after which time Reolsil DM-30S fumed silica (3 pbw) was added. The composition was further blended for 2 min at 2,000 rpm, then for another 2 min at 2000 rpm. 1%-Trimethyl(methylcyclopentadienyl)platinum (IV) in methyltrimethoxysilane (1 pbw) was then added to the mixture, and blending was reinitiated for 2 min at 1,500 rpm. The sample was packaged in 30-mL syringes and vacuum sealed. The syringes were stored in an aluminum bag -5 °C. The sample was cured first by exposing it to LED UV (Firejet FJ800) at 365 nm and a UVA dosage of 5,000 mJ / cm2; the cure was completed by storing the sample in an oven at 70 °C for 30 min.Example 4 - Preparation of Pt -Catalyzed Heat Curable Organosiloxane Composition with the Compound of Formula 3
[0065] A curable organopolysiloxane composition was prepared by blending MV1DPh2sMV1(6.5 pbw), MPhVlo.23TPho.77 (68.8 pbw), MHDPh2MH(20.6 pbw); methyl(tris(l,l-dimethyl-2-propynyl) oxy) silane (0.001 pbw); and the compound of Formula 3 (1.0 pbw). The mixture was blended for 2 min at 1,500 rpm, after which time Reolsil DM-30S fumed silica (3 pbw) was added. The composition was further blended for 2 min at 2,000 rpm, then for another 2 min at 2000 rpm. 0.5%- Platinum, l,3-diethenyl-l,l,3,3-tetramethyldisiloxane complexes in Methyltrimethoxysilane (0.04 pbw) was then added to the mixture, and blending was reinitiated for 2 min at 1,500 rpm. The sample was packaged in 30-mE syringes and vacuum sealed. The syringes were stored in an aluminum bag -5 °C. The sample was heat cured at 150 °C for 1 h. Example 5 - Preparation of UV-Heat Curable Organosiloxane Composition with the Compound of Formula 4
[0066] The composition was prepared and cured substantially as described in Example 3, except that the compound of Formula 4 (1.0 pbw) was used instead of the compound of Formula 3.Example 6 - Preparation of Pt -Catalyzed Heat Curable Organosiloxane Composition with the Compound of Formula 4
[0067] The composition was prepared substantially and cured as described in Example 4,except that the compound of Formula 4 (1.0 pbw) was used instead of the compound of Formula 3.Comparative Example 1 - Preparation of UV-Heat Curable Organosiloxane Composition with no Adhesion Promoter
[0068] The composition was prepared substantially as described in Example 3 without the inclusion of the compound of Formula 3. MPhVlo.23TPho.77 was increased to 68.8 pbw and MHDPh2MHwas increased to 20.7 pbw.Comparative Example 2 - Preparation of Pt -Catalyzed Heat Curable Organosiloxane Composition with no Adhesion Promoter
[0069] The composition was prepared substantially as described in Example 4 without the inclusion of the compound of Formula 4. MPhV1o.23TPho.77 was increased to 69.6 pbw and MHDPh2MHwas increased to 20.9 pbw.Crosshatch Procedure
[0070] ASTM D3359 was used to measure the area removed on a coated glass slide. The coated surface was etched in a crosshatched fashion and tested. The crosshatch test classifications are illustrated in Table ETable 1 - Crosshatch Test ClassificationsClassification % Area Removed0B > 65%IB 35-65%2B 15-35%3B 5-15%4B < 5%5B 0%Adhesion Lap Shear Testing
[0071] Lap shear testing was carried out using an Instron 3366 mechanical testing system. The cured samples (10-mm thick) were sandwiched between two 0.5-mm thick glass or aluminum (Al) substrates; each substrate was pulled and pushed parallel to the sample until breakage occurred due to adhesive failure (AF), cohesive failure (CF), or substrate failure (SF). The results of the adhesion lap shear, crosshatch testing, and failure modes of the samples are illustrated in Table 2.
[0072] Table 2 illustrates adhesion lap shear and crosshatch classification for aluminum and glass substrates, and failure mode for glass substrates. Lap shear is measured in MPa. CF refersto cohesive failure, and AF refers to adhesion failure. For glass substrates, the minimum requirement for adhesion lap shear was > 4 MPa; for aluminum substrates, the minimum requirement for adhesion lap shear was > 3 MPa. CF and a crosshatch classification of 4B or 5B were also required.Table 2 - Failure Mode and Crosshatch EvaluationEx. 3 Ex. 4 Ex. 5 Ex. 6 CEx. 1 CEx 2 Adhesion lap shear - Glass > 5.50 > 5.50 > 5.50 > 5.50 3.86 > 5.50 Failure mode - Glass CF CF CF CF AF CF Adhesion lap shear - Al 3.80 10.69 4.30 10.16 2.49 1.70Crosshatch Classification 5B 5B 5B 5B 0B 5B
[0073] The data show that heat cured samples containing the compounds of Formulas 3 and 4 (Examples 4 and 6) gave superior adhesion strength for aluminum substrates as compared with Comparative Example 2, which contained no adhesion promoter. The data further show that the properties of the UV-heat cured samples containing the compounds of Formulas 3 and 4 (Examples 3 and 5) are superior in all respects to Comparative Example 1, which contained no adhesion promoter.
Claims
Claims:
1. A composition comprising:a) a compound of Formula 1:Formula 1b) a divinyl-terminated polyphenylsiloxane;c) a vinyl-terminated polyphenylsiloxane resin;d) a hydrogenphenylsiloxane; ande) a hydrosilylation catalyst;where X is either a (bisphenylmethylsilyl)oxy diradical or a (bisdimethylsilyloxy)diphenylsilyl diradical; each R is a Cj-Ci2-alkyl anhydride group; the sum of m and n is in the range of from 1 to 4; and -DHX- is a mono- or diradical of the compound of Formula 2:Formula 2where x is from 3 to 10, and y is x - 3.
2. The composition of Claim 1 where x is from 4 to 6; and R is a Cs-Ci2-alkyl succinic anhydride, C3-Ci2-alkyl maleic anhydride, C3-Ci2-alkyl oxalic anhydride, or a C3-Ci2-alkyl phthalic anhydride group; and wherein the divinyl-terminated polyphenylsiloxane is a compound of Formula 5:Me / Ph \ Me- Si - O— (— Si - O - Si -M1e \ \Rl' / nMeFormula 5where Ph is phenyl; each R' is independently methyl or phenyl; and n is from 1 to 500.
3. The composition of Claim 2 where the R is a fragment of the following formula:where z is from 1 to 10; and the dotted line represents the point of attachment to the DHXdiyl group; the vinyl terminated polyphenylsiloxane has the formula MMePhV1aTPhb, where a is a mole fraction in the range of from 0.10 to 0.40, and b is a mole fraction in the range of from 0.60 to 0.90, where a + b = 1; and the hydrogenphenylsiloxane is a compound of Formula 7:Me / Ph \ Me1J-1I1i T i T iMe \Me / mMewhere m is from 1 to 50.
4. The composition of Claim 3 where z is 1; and y is 1, 2, or 3, or a mixture thereof.
5. The composition of any of Claims 1 to 4 wherein the compound of Formula 1 is represented by the compound of Formula 3:Formula 3where y is 1, 2, or 3. or a mixture thereof.
6. The composition of any of Claims 1 to 4 wherein the compound of Formula 1 is represented by Formula 4:Formula 4where y is 1, 2, or 3, or a mixture thereof.
7. A composition comprising:a) an anhydride functionalized cyclic polyorganosiloxane compound of Formula la:independently has an average value of 2 to 18, each R4is an independently selected monovalent hydrocarbyl group, each R5is selected from the group consisting of H and a C3-Ci2-alkyl anhydride group, with the proviso that at least one R5per molecule is the Cs-Cn-alkyl anhydride group; each R6is an independently selected divalent hydrocarbyl group; and Lis a divalent R3R3| ,RAr| R^organosilicon linking moiety selected from the group consisting of O andR3RArR3| R3| RAr| R3^S’ \ x^Si\ / Si\O O , wherein each RAris an independently selected monovalent aromatic group and each R3is an independently selected alkyl group;b) a divinyl-terminated polyphenylsiloxane;c) a vinyl -terminated poly phenyl siloxane resin;d) a hydrogenphenylsiloxane; ande) a hydrosilylation catalyst.
8. The composition of claim 7, where a) the anhydride functionalized cyclic polyorganosiloxane compound comprises formula a-2):subscript v, R6, R3, and RArare as described above.
9. The composition of claim 8, where a), the anhydride functionalized cyclic polyorganosiloxane may comprise formula a-3):subscript v has an average value of 2 to 4, Ph means phenyl, and each R5is H or an alkyl succinic anhydride group, with the proviso that at least one instance of R5per molecule is the alkyl succinic anhydride group.
10. The composition of claim 7, where a) the anhydride functionalized cyclic polyorganosiloxane comprises formula a-4):v, R6, R3, and RArare as described above.
11. The composition of claim 10, where the anhydride functionalized cyclic polyorganosiloxane comprises formula a-5):H3C\ / CH3R5- Si - O CH3 PhPh H3C O - Si - R5 / \ / | / CH3| CH3\ / \°v VS1\ / siQ VSiv y°[ S li\ - O | T \HJ -40\ H2 / - / O - / SIiA\D5 CH3 / . \H3C p5 / ' 'vwhere each subscript v has an average value of 2 to 4, Ph means phenyl, and each R3is H or an alkyl succinic anhydride functional group, with the proviso that at least one instance of R5per molecule is the alkyl succinic anhydride group.
12. The composition of any one of claims 7 to 11 further comprising a thiuram disulfide.
13. A method for preparing the composition of any one of claims 7 to 12, wherein the method comprises mixing starting materials comprising a) the anhydride functionalized cyclic polyorganosiloxane compound; b) the divinyl-terminated polyphenylsiloxane; c) the vinyl-terminated polyphenylsiloxane resin; d) the hydrogenphenylsiloxane; and e) the hydrosilylation catalyst.
14. A method for preparing a coated article, where the method comprisesapplying the composition of any one of claims 7 to 12 to a surface of a substrate, and curing the composition.