Catalysts and ethylene-based polymers produced therefrom
A catalyst system with group III or lanthanide series metal centers and quinoline-containing ligands addresses the inconsistency of solution phase catalysts in gas and slurry phase reactors, producing ethylene-based polymers with high molecular weight and broad molecular weight distributions, enhancing processability and meeting regulatory requirements.
Patent Information
- Application Number
- PCT/US2026/024537
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-05
- Filing Date
- 2026-04-21
- Publication Date
- 2026-11-12
AI Technical Summary
Existing catalysts optimized for solution phase polymerization reactions are ineffective in gas phase and slurry phase reactors due to heterogeneity, leading to inconsistent reaction conditions and poor processability of high molecular weight polymers.
A catalyst system comprising a group III or lanthanide series metal center and quinoline-containing ligands, supported on an inert medium, is used to produce ethylene-based polymers in gas and slurry phase reactors, achieving ultra-high molecular weight polymers with broad molecular weight distributions.
The catalyst system provides polymers with improved processability and performance, reducing catalyst design complexity and meeting regulatory demands for non-chrome alternatives.
Smart Images

Figure IMGF000006_0001 
Figure IMGF000007_0001 
Figure IMGF000007_0002
Abstract
Description
[0001] CATALYSTS AND ETHYLENE-BASED POLYMERS PRODUCED THEREFROM
[0002] BACKGROUND
[0003] Field of the disclosure
[0004] The present disclosure relates to catalysts, and more specifically to catalysts, pre-catalysts and ethylene polymers produced therefrom.
[0005] Introduction
[0006] High molecular weight polymers are known for their ability to significantly improve the mechanical properties of resins and resin blends. These polymers can enhance the strength, durability, and overall performance of the materials. However, a common challenge with high molecular weight polymers is poor processability during product fabrication. A good balance between polymer performance and processability is needed for polymers to be useful for practical applications.
[0007] Catalysts comprising scandium metal centers and quinoline-containing ligands have been studied in polymerization reactions. For example, Stereoselective Polymerization of Styrene with Cationic Scandium Precursors Bearing Quinolyl Aniline Ligands, Organometallics 2010, 29, 1916-1923, discloses the use of scandium metal centers and quinoline-containing ligands in the room temperature solution phase polymerization of styrene. Similarly, the article Development of Improved Amidoquinoline Polyolefin Catalysts with Ultrahigh Molecular Weight Capacity, Organometallics, 2015, 34, 1354-1363, discloses the use of group four metals in conjunction with amidoquinoline ligands to polymerize ethylene and octene in a solution phase reactor. See also United States patent number 8,153,544 for methods of preparing non-metallocene polymerization catalysts. The successful use of catalysts in solution phase reactors does not mean that the same catalyst will perform equally well in a gas phase or slurry phase reactor. For example, solution phase reactors allow catalysts to operate in a homogeneous environment, allowing for precise control over reaction conditions and molecular interactions. Conversely, gas phase and slurry phase polymerization reactions occur in heterogeneous environments where catalysts must interact with gaseous or slurry media. This heterogeneity introduces variability in reaction conditions, making it difficult to achieve the same level of control and consistency as in solution phase reactions. Additionally, the physical and chemical properties of catalysts optimized for solutionphase reactions may not be suitable for the dynamic and often unpredictable conditions of gas phase and slurry phase polymerization assets. As a result, the effectiveness of solution phase catalysts in these environments remains uncertain, posing a significant challenge for industrial applications.
[0008] In view of the foregoing, it would be surprising to identify a catalyst comprising a group III or lanthanide series metal center and quinoline-containing ligands that forms an ethylenebased polymer in gas phase and slurry phase reactors.
[0009] SUMMARY OF THE DISCLOSURE
[0010] The inventors of the present disclosure have discovered a catalyst comprising a group III or lanthanide series metal center and quinoline-containing ligands capable of producing an ethylene-based polymer in gas phase and slurry phase reactors. Further, the inventors of the present disclosure have surprisingly discovered that a single catalyst system, as disclosed here, provides polymer features that traditionally either require a two catalyst bimodal system or a chrome-based catalyst. Such a single catalyst system with the capability in producing polymers with features similar to those dual catalyst systems is advantageous in reducing catalyst design complexity. Such a feature is also advantageous as regulatory pressures increase on chrome-based catalysts and nonchrome alternatives that provide similar polymeric properties are in demand.
[0011] The invention is the result of discovering that non-metallocene group III or lanthanide series catalysts are capable of producing ultra-high molecular weight (“HMW”) polymers with broad molecular weight distributions (“MWD”). The combination of HMW polymers with broad MWD feature is desirable to improve polymer performance with a good balance of processability.
[0012] According to a first feature of the disclosure, a method of making an ethylene-based polymer comprises the steps of (a) contacting ethylene and an alpha olefin comonomer with a catalyst in the presence of molecular hydrogen gas inside of a gas phase polymerization reactor or a slurry phase polymerization reactor, wherein the catalyst is formed by activation of a precatalyst of Structure (I) and (b) forming an ethylene-based polymer.
[0013] According to another feature of the disclosure, the precatalyst is supported using an inert medium.
[0014] According to another feature of the disclosure, the precatalyst is supported on a fumed silica substrate.According to another feature of the disclosure, the precatalyst is activated into the catalyst by aluminoxane or methylaluminoxane.
[0015] According to another feature of the disclosure, the precatalyst has Structure (II) wherein R8to R11are each independently selected from hydrogen, methyl, ethyl, propyl, isopropyl; R12is methyl, aryl, hetetroaryl; and X is selected from methyl; trimethyl silylmethyl; phenyl; benzyl; or halides.
[0016] According to another feature of the disclosure, the precatalyst has one of structures (III) to (VII).
[0017] According to another feature of the disclosure, the step of forming the ethylene-based polymer is performed at a temperature of 80°C to 110 °C.
[0018] According to another feature of the disclosure, the ethylene-based polymer exhibits one or more of the following properties: (i) a density of 0.93 g / cc to 0.97 g / cc as measured according to ASTM D792; (ii) a melt index (I2) of 3 g / 10 min or less as measured according to ASTM D1238; (iii) a melt index (I5) of 5.0 g / 10 min or less as measured according to ASTM D1238; (iv) a melt index (I21) of 30.0 g / 10 min or less as measured according to ASTM D1238; (v) a short chain branching per 1000 TC (total carbons) of 0 to 20 as measured according to Gel Permeation Chromatography; and (vi) a C6 comonomer content of 0 wt% to 10 wt% as measured according to Gel Permeation Chromatography.
[0019] According to another feature of the disclosure, the ethylene-based polymer exhibits one or more of the following properties: (i) a molecular weight distribution of 5 or greater; (ii) a molecular weight distribution of 10 or greater; (iii) a molecular weight distribution of 20 or greater; and (iv) a molecular weight distribution of 30 or greater.
[0020] According to another feature of the disclosure, the ethylene-based polymer exhibits one or more of the following properties: (i) a weight average molecular weight of 10, 000 to 2,000,000 g / mol as measured according to Gel Permeation Chromatography; (ii) a weight average molecular weight of 30,000 to 300,000 g / mol as measured according to Gel Permeation Chromatography; and (iii) a weight average molecular weight of 200,000 to 900,000 g / mol as measured according to Gel Permeation Chromatography.
[0021] According to another feature of the disclosure, the ethylene-based polymer exhibits one or more of the following properties: (i) a Mz / Mw ratio of 5 or greater; (ii) a Mz / Mw ratio of 10 or greater; and (iii) a Mz / Mw ratio of 20 or greater.According to another feature of the disclosure, the ethylene-based polymer exhibits one or more of the following properties: (i) a Tm value of 120 °C to 140 °C as measured according to ASTM D 3418-08; and (ii) a Tm value of 120 °C to 130°C as measured according to ASTM D 3418-08.
[0022] DETAILED DESCRIPTION
[0023] As used herein, the term “and / or,” when used in a list of two or more items, means that any one of the listed items can be employed by itself, or any combination of two or more of the listed items can be employed. For example, if a composition is described as containing components A, B, and / or C, the composition can contain A alone; B alone; C alone; A and B in combination; A and C in combination; B and C in combination; or A, B, and C in combination.
[0024] All ranges include endpoints unless otherwise stated.
[0025] Test methods refer to the most recent test method as of the priority date of this document unless a date is indicated with the test method number as a hyphenated two-digit number. References to test methods contain both a reference to the testing society and the test method number. Test method organizations are referenced by one of the following abbreviations: ASTM refers to ASTM International (formerly known as American Society for Testing and Materials); IEC refers to International Electrotechnical Commission; EN refers to European Norm; DIN refers to Deutsches Institut fur Normung; and ISO refers to International Organization for Standards.
[0026] As used herein, the term weight percent (“wt%”) designates the percentage by weight a component is of a total weight of the polymeric composition unless otherwise specified.
[0027] Melt index (E) values herein refer to values determined according to ASTM method D1238 at 190 degrees Celsius (°C) with 2.16 Kilogram (kg) mass and are provided in units of grams eluted per ten minutes (“g / 10 min”).
[0028] Density values herein refer to values determined according to ASTM D792 at 23°C and are provided in units of grams per cubic centimeter (“g / cc”).
[0029] As used herein, Chemical Abstract Services registration numbers (“CAS#”) refer to the unique numeric identifier as most recently assigned as of the priority date of this document to a chemical compound by the Chemical Abstracts Service.Method
[0030] The present disclosure is generally directed to a method of making an ethylene-based polymer. The method may comprise the steps of (a) contacting ethylene and an alpha olefin comonomer with a catalyst in the presence of molecular hydrogen gas inside of a gas phase polymerization reactor or a slurry phase polymerization reactor, wherein the catalyst is formed by activation of a precatalyst, and (b) forming an ethylene-based polymer. It will be understood that the activation of the precatalyst may also, to some degree, take place upon the introduction of methylaluminoxane to supported examples of the precatalyst.
[0031] As highlighted in Step (a), the method may use a gas-phase polymerization reactor. Exemplary gas phase polymerization reactors include stirred-bed gas phase polymerization reactors (SB-GPP reactor) or a fluidized-bed gas-phase polymerization reactors (FB-GPP reactor). Such gas phase polymerization reactors and methods are generally well known in the art. For example, the FB-GPP reactor / method may be as described in US 3,709,853; US 4,003,712; US 4,011,382; US 4,302,566; US 4,543,399; US 4,882,400; US 5,352,749; US 5,541,270; EP-A-0802 202; and Belgian Patent No. 839,380. These SB-GPP and FB-GPP polymerization reactors and processes either mechanically agitate or fluidize by continuous flow of gaseous monomer and diluent the polymerization medium inside the reactor, respectively. The alpha-olefin comonomer used in Step (a) may be one or more C3-C20 alpha olefin comonomers such as propylene, 1 -butene, 1 pentene, 4-methyl-l -pentene, 1 -hexene, and 1 -octene.
[0032] Additionally or alternatively, the method may use a slurry reactor. Examples of slurryphase polymerization reactors and slurry-phase polymerization conditions can be found in, but not limited to, those described in U.S. Pat. No. 10,344,101 B2. The precatalyst of the present disclosure may be slurried prior to entering the slurry reactor, where such slurries are known in the art, or introduced into the slurry reactor as a dry solid. For example, the precatalyst may be mixed in mineral oil, or mineral oil and a non-reactive hydrocarbon (e.g.. toluene) or mixture of hydrocarbons. The slurry may be fed to the slurry phase reactor for the polymerization process and / or the slurry may be dried, e.g., spray dried, prior to being fed to the reactor for the polymerization process.
[0033] Step (b) of the method includes forming an ethylene-based polymer. The ethylene-based polymer is formed in the reactor by creating specific polymerization conditions which cause polymerization thereby forming the ethylene-based polymer. In gas phase polymerization reactorexamples, the polymerization conditions may comprise the following conditions: (a) the gas phase polymerization reactor having a fluidized resin bed at a bed temperature from 80 to 110 degrees Celsius (° C.), alternatively from 100 to 108° C., alternatively from 104 to 106° C.; (b) an alpha olefin-to-ethylene (Cx / C2) molar ratio from 0.001 to 0.8, alternatively from 0.005 to 0.10; (c) a hydrogen-to-ethylene (H2 / C2) molar ratio from 0.0001 to 2.0, alternatively from 0.001 to 0.050. with respect to polymerization condition (a), in other words, the step of forming the ethylene-based polymer may be performed at a temperature of 80°C to 110 °C. The average residence time of the polyethylene blend in the reactor may be from 2 to 5 hours, alternatively from 2.5 to 4.5 hours.
[0034] Precatalyst
[0035] The ethylene-based polymer is formed by a catalyst formed by activation of the precatalyst of Structure (I).
[0036] R4R5
[0037] R2T^N^^R7
[0038]
[0039] In Structure (I), M is scandium (Sc), yttrium (Y), or a lanthanide metal having an oxidation state of +3. As used herein, the term “lanthanide metal” includes elements 57 through 71 (lanthanum (La) to lutetium (Lu)). R1is a C1-C30 hydrocarbyl, a C1-C30 heterohydrocarbyl, a -Si(Rc)s, a C6-C30 aryl, or a C5-C30 heteroaryls. It will be understood that although expressed as a range for convenience and brevity, Applicant hereby expressly discloses each individual subunit of any range provided with respect to the precatalyst structures provided herein. R2to R7are each independently selected from hydrogen, a C1-C30 hydrocarbyl, a C1-C30 heterohydrocarbyl. a -Si(Rc)3, a C6-C30 aryl, a C5-C30 heteroaryl. Rcis a C1-C20 a hydrocarbyl or a C6-C20 aryl or a C5-C20 heteroaryl. In Structure (I) X is an anionic leaving group. Each X is independently selected from methyl, ethyl, 1-propyl, 2-propyl, 1-butyl, 2,2, dimethylpropyl; trimethyl silylmethyl; phenyl; benzyl; or halides. The term “halide” means anionic form of the halogen atom: fluoride (F-), chloride (Cl-), bromide (Br-), or iodide (I-). The term “halogen atom” or “halogen” means the radical of a fluorine atom (F), chlorine atom (Cl), bromine atom (Br), or iodine atom (I). InStructure (I) Lis a coordinating Lewis base. In Structure (I) wherein L is independently selected from coordinating groups EtiO, tetrahydrofuran, 2-methyl-tetrahydrofuran, MeOtBu, EtsN, PhNMe2, MePh2N, pyridine and dimethylsulfide.
[0040] Under certain exemplary combinations of the variables of Structure (I), the precatalyst may be represented by Structure (II).
[0041] R11
[0042]
[0043] Structure (II)
[0044] In Structure (II), R8to R11are each independently selected from hydrogen, methyl, ethyl, propyl, and isopropyl, R12is methyl, aryl, or heteroaryl; and X is selected from methyl; trimethylsilylmethyl; phenyl; benzyl; or halides.
[0045] Under certain exemplary combinations of the variables of Structure (II), the precatalyst may be represented by any one of precatalyst Structures (III) to (VII):
[0046]
[0047] As explained above, the precatalyst is activated into a catalyst through the use of an activator. The activator can include any metal containing compound, material or combination of compounds and / or substances, whether unsupported or supported on a support material, that can activate a precatalyst to give a catalyst and an activator species. The activating may comprise, for example, abstracting at least one leaving group (e.g., the X variables of Structure (I)) from a metal of a precatalyst to give the catalyst. The catalyst may be generically named by replacing the leaving group portion of the name of the precatalyst with "complex". The activator may be a Lewis acid, a non-coordinating ionic activator, or an ionizing activator, or a Lewis base, an alkylaluminum, or an alkylaluminoxane. The alkylaluminum may be a trialkylaluminum, alkylaluminum halide, or alkylaluminum alkoxide (diethylaluminum ethoxide). The trialkylaluminum may be trimethylaluminum, triethylaluminum ("TEAI"), tripropylaluminum, triisobutylaluminum, and the like. The alkylaluminum halide may be diethylaluminum chloride, ethylaluminum dichloride. The alkylaluminoxane may be a methyl aluminoxane (MAO), ethyl aluminoxane, or isobutylaluminoxane. The activator may be a MAO that is a modified methylaluminoxane (MMAO).
[0048] Any of Structures (I) to (VII), and optionally the activator, may be unsupported or supported (i.e., positioned on a support material). The support material for the support-containing embodiments of the precatalyst may be an inorganic oxide material. The terms “support” and “support material” are the same as used herein and refer to a porous inorganic substance or organic substance. In some examples, desirable support materials may be inorganic oxides that include Group 2, 3, 4, 5, 13 or 14 oxides, alternatively Group 13 or 14 atoms. Examples of inorganic oxidetype support materials are silica, alumina, titania, zirconia, thoria, and mixtures of any two or more of such inorganic oxides. Examples of such mixtures are silica-chromium, silica-alumina, and silica-titania. The support material may be uncalcined or calcined prior to being contacted with the catalysts. The support material may be a hydrophobic fumed silica (e.g., a fumed silica treated with dimethyldichlorosilane). The unsupported or supported catalyst system may be in the form of a powdery, free-flowing particulate solid. The precatalyst may be spray dried or not.
[0049]
[0050] lymer
[0051] One feature of the present disclosure is the ethylene-based polymer. As used herein, “ethylene-based” polymers are polymers in which greater than 50 wt% of the monomers areethylene though other co-monomers may also be employed. Ethylene-based polymers include ethylene and one or more C3-C20 a-olefin comonomers such as propylene, 1 -butene, 1 pentene, 4-methyl-1 -pentene, 1 -hexene, and 1 -octene. The ethylene-based polymer may be produced in a gas phase polymerization reactor or in a slurry phase reactor.
[0052] The ethylene-based polymer may comprise 50 wt% or greater, 60 wt% or greater, 70 wt% or greater, 80 wt% or greater, 85 wt% or greater, 90 wt% or greater, or 91 wt% or greater, or 92 wt% or greater, or 93 wt% or greater, or 94 wt% or greater, or 95 wt% or greater, or 96 wt% or greater, or 97 wt% or greater, or 97.5 wt% or greater, or 98 wt% or greater, or 99 wt% or greater, or 99.5 wt% or greater, or 99.8 wt% or greater, while at the same time, 99.9 wt% or less, or 99.5 wt% or less, or 99 wt% or less, or 98 wt% or less, or 97 wt% or less, or 96 wt% or less, or 95 wt% or less, or 94 wt% or less, or 93 wt% or less, or 92 wt% or less, or 91 wt% or less, or 90 wt% or less, or 85 wt% or less, or 80 wt% or less, or 70 wt% or less, or 60 wt% or less of ethylene monomers as measured using Nuclear Magnetic Resonance (NMR), Fourier-Transform Infrared (FTIR) Spectroscopy or Gel Permeation Chromatography. The comonomer content of the ethylene-based polymer may also be determined by Gel Permeation Chromatography as explained in greater detail below. In a specific example, the ethylene-based polymer may have a C>, comonomer content of 0 wt% or greater, or 1 wt% or greater, or 2 wt% or greater, or 3 wt% or greater, or 4 wt% or greater, or 5 wt% or greater, or 6 wt% or greater, or 7 wt% or greater, or 8 wt% or greater, or 9 wt% or greater, while at the same time, 10 wt% or less, or 9 wt% or less, or 8 wt% or less, or 7 wt% or less, or 6 wt% or less, or 5 wt% or less, or 4 wt% or less, or 3 wt% or less or 2 wt% or less as measured according to Gel Permeation Chromatography.
[0053] The density of the ethylene-based polymer may be from 0.930 g / cc to 0.970 g / cc as measured according to ASTM D792. For example, the density of the ethylene-based polymer may be 0.930 g / cc or greater, or 0.932 g / cc or greater, or 0.934 g / cc or greater, or 0.936 g / cc or greater, or 0.938 g / cc or greater, or 0.940 g / cc or greater, or 0.942 g / cc or greater, or 0.944 g / cc or greater, or 0.946 g / cc or greater, or 0.948 g / cc or greater, or 0.950 g / cc or greater, or 0.952 g / cc or greater, or 0.954 g / cc or greater, or 0.956 g / cc or greater, or 0.958 g / cc or greater, or 0.960 g / cc or greater, or 0.962 g / cc or greater, or 0.964 g / cc or greater, or 0.966 g / cc or greater, or 0.968 g / cc or greater, while at the same time, 0.970 g / cc or less, or 0.968 g / cc or less, or 0.966 g / cc or less, or 0.964 g / cc or less, or 0.952 g / cc or less, 0.960 g / cc or less, or 0.958 g / cc or less, or 0.956 g / cc or less, or 0.954 g / cc or less, or 0.952 g / cc or less, or 0.950 g / cc or less, or 0.948 g / cc or less, or 0.946 g / cc or less,or 0.944 g / cc or less, or 0.942 g / cc or less, or 0.940 g / cc or less, 0.940 g / cc or less, or 0.938 g / cc or less, or 0.936 g / cc or less, or 0.934 g / cc or less, or 0.932 g / cc or less as measured according to ASTM D792. In specific examples, the ethylene-based polymer may exhibit any one of the following density ranges: a density of 0.930 g / cc to 0.940 g / cc as measured according to ASTM D792; a density of 0.940 g / cc to 0.960 g / cc as measured according to ASTM D792; and a density of 0.930 g / cc to 0.960 g / cc as measured according to ASTM D792.
[0054] The ethylene-based polymer may have a melt index (I2) of 0.01 g / 10 min to 3 g / 10 min. as measured according to ASTM D1238 (190 °C, 2.16 kg). For example, the ethylene-based polymer may have a melt index (I2) of 0.01 g / 10 min or greater, or 0.1 g / 10 min or greater, or 0.2 g / 10 min or greater, or 0.4 g / 10 min or greater, or 0.6 g / 10 min or greater, or 0.8 g / 10 min or greater, or 1.0 g / 10 min or greater, or 1.2 g / 10 min or greater, or 1.4 g / 10 min or greater, or 1.6 g / 10 min or greater, or 1.8 g / 10 min or greater, or 2.0 g / 10 min or greater, or 2.2 g / 10 min or greater, or 2.4 g / 10 min or greater, or 2.6 g / 10 min or greater, or 2.8 g / 10 min or greater, while at the same time, 3 g / 10 min or less, or 2.8 g / 10 min or less, or 2.6 g / 10 min or less, or 2.4 g / 10 min or less, or 2.2 g / 10 min or less, or 2.0 g / 10 min or less, or 1.8 g / 10 min or less, or 1.6 g / 10 min or less, or 1.4 g / 10 min or less, or 1.2 g / 10 min or less, or 1.0 g / 10 min or less, or 0.8 g / 10 min or less, or 0.6 g / 10 min or less, or 0.4 g / 10 min or less, or 0.2 g / 10 min or less, or 0.1 g / 10 min or less as measured according to ASTM D1238.
[0055] The ethylene-based polymer may have a melt index (I5) of 0.1 g / 10 min to 5 g / 10 min. as measured according to ASTM D1238 (190 °C, 5 kg). For example, the ethylene-based polymer may have a melt index (I5) of 0.1 g / 10 min or greater, or 1.0 g / 10 min or greater, or 1.5 g / 10 min or greater, or 2.0 g / 10 min or greater, or 2.5 g / 10 min or greater, or 3.0 g / 10 min or greater, or 3.5 g / 10 min or greater, or 4.0 g / 10 min or greater, or 4.5 g / 10 min or greater, while at the same time, 5 g / 10 min or less, or 4.5 g / 10 min or less, or 4.0 g / 10 min or less, or 3.5 g / 10 min or less, or 3.0 g / 10 min or less, or 2.5 g / 10 min or less, or 2.0 g / 10 min or less, or 1.5 g / 10 min or less, or 1.0 g / 10 min or less, or 0.5 g / 10 min or less as measured according to ASTM D1238.
[0056] The ethylene-based polymer may have a melt index (I21) of 0.1 g / 10 min to 30 g / 10 min. as measured according to ASTM D1238 (190 °C, 21.6 kg). For example, the ethylene-based polymer may have a melt index (I21) of 0.1 g / 10 min or greater, or 1.0 g / 10 min or greater, or 5 g / 10 min or greater, or 10 g / 10 min or greater, or 15 g / 10 min or greater, or 20 g / 10 min or greater, or 25 g / 10 min or greater, while at the same time, 30 g / 10 min or less, or 25 g / 10 min or less, or20 g / 10 min or less, or 15 g / 10 min or less, or 10 g / 10 min or less, or 5 g / 10 min or less, or 1 g / 10 min or less, or 0.5 g / 10 min or less as measured according to ASTM D1238.
[0057] The ethylene-based polymer may exhibit a short chain branching per 1000 TC (total carbons) of 0 to 20 as measured according to Gel Permeation Chromatography. For example, the ethylene-based polymer may exhibit a short chain branching per 1000 TC of 0 or greater, or 1 or greater, or 2 or greater, or 3 or greater, or 4 or greater, or 5 or greater, or 6 or greater, or 7 or greater, or 8 or greater, or 9 or greater, or 10 or greater, or 11 or greater, or 12 or greater, or 13 or greater, or 14 or greater, or 15 or greater, or 16 or greater, or 17 or greater, or 18 or greater, or 19 or greater, while at the same time, 20 or less, or 19 or less, or 18 or less, or 17 or less, or 16 or less, or 15 or less, or 14 or less, or 13 or less, or 12 or less, or 11 or less, or 10 or less, or 9 or less, or 8 or less, or 7 or less, or 6 or less, or 5 or less, or 4 or less, or 3 or less, or 2 or less as measured according to Gel Permeation Chromatography
[0058] The ethylene-based polymer may exhibit a melt flow ratio (I21 / I2) of 0 to 80. For example, the ethylene-based polymer may have exhibit a melt flow ratio (I21 / I2) of 0 or greater, or 1 or greater, or 5 or greater, or 10 or greater, or 20 or greater, or 30 or greater, or 40 or greater, or 50 or greater, or 60 or greater, or 70 or greater, while at the same time, 80 or less, or 70 or less, or 60 or less, or 50 or less, or 40 or less, or 30 or less, or 20 or less, or 10 or less, or 5 or less, or 1 or less.
[0059] The ethylene-based polymer may exhibit a weight average molecular weight (“Mw”) of 10,000 g / mol to 2,000,000 g / mol as measured according to Gel Permeation Chromatography. For example, the ethylene-based polymer may exhibit a weight average molecular weight of 10,000 g / mol or greater, or 50.000 g / mol or greater, or 100,000 g / mol or greater, or 200,000 g / mol or greater, or 400,000 g / mol or greater, or 600,000 g / mol or greater, or 800,000 g / mol or greater, or 1,000,000 g / mol or greater, or 1,200,000 g / mol or greater, or 1,400,000 g / mol or greater, or 1,600,000 g / mol or greater, or 1,800,000 g / mol or greater, while at the same time. 2,000,000 g / mol or less, or 1,800,000 g / mol or less, or 1,600,000 g / mol or less, or 1,400,000 g / mol or less, or 1,200,000 g / mol or less, or 1,000,000 g / mol or less, or 800,000 g / mol or less, or 600,000 g / mol or less, or 400,000 g / mol or less, or 200,000 g / mol or less, or 100,000 g / mol or less, or 50,000 g / mol or less as measured according to Gel Permeation Chromatography.
[0060] The ethylene-based polymer may exhibit a number average molecular weight (“Mn”) of 10,000 g / mol to 50,000 g / mol as measured according to Gel Permeation Chromatography. Forexample, the ethylene-based polymer may exhibit a number average molecular weight of 10,000 g / mol or greater, or 15,000 g / mol or greater, or 20,000 g / mol or greater, or 25,000 g / mol or greater, or 30.000 g / mol or greater, or 35,000 g / mol or greater, or 40,000 g / mol or greater, or 45,000 g / mol or greater, while at the same time, 50,000 g / mol or less, or 45,000 g / mol or less, or 40,000 g / mol or less, or 35,000 g / mol or less, or 30,000 g / mol or less, or 25,000 g / mol or less, or 20,000 g / mol or less, or 15,000 g / mol or less as measured according to Gel Permeation Chromatography.
[0061] The ethylene-based polymer may exhibit a Z average molecular weight (“Mz”) of 5,000,000 g / mol to 9,000,000 g / mol as measured according to Gel Permeation Chromatography. For example, the ethylene-based polymer may exhibit a Z average molecular weight of 5,000,000 g / mol or greater, or 5,500,000 g / mol or greater, or 6,000,000 g / mol or greater, or 6,500,000 g / mol or greater, or 7,000.000 g / mol or greater, or 7.500,000 g / mol or greater, or 8,000,000 g / mol or greater, or 8,500,000 g / mol or greater, while at the same time, 9,000,000 g / mol or less, or 8,500,000 g / mol or less, or 8,000,000 g / mol or less, or 7,500,000 g / mol or less, or 7,000,000 g / mol or less, or 6,500,000 g / mol or less, or 6.000,000 g / mol or less, or 5,500,000 g / mol or less as measured according to Gel Permeation Chromatography.
[0062] The ethylene-based polymer may exhibit a unimodal molecular weight distribution as defined by having a single peak maxima. The ethylene-based polymer may exhibit a molecular weight distribution (Mw / Mn) from 1 to 50. For example, the ethylene-based polymer may exhibit a Mw / Mn of 1 or greater, or 5 or greater, or 10 or greater, or 15 or greater, or 20 or greater, or 25 or greater, or 30 or greater, or 35 or greater, or 40 or greater, or 45 or greater, while at the same time, 50 or less, or 45 or less, or 40 or less, or 35 or less, or 30 or less, or 25 or less, or 20 or less, or 15 or less, or 10 or less, or 5 or less.
[0063] The ethylene-based polymer may exhibit a Mz / Mwratio from 1 to 40. For example, the ethylene-based polymer may exhibit a Mz / Mqof 1 or greater, or 5 or greater, or 10 or greater, or 15 or greater, or 20 or greater, or 25 or greater, or 30 or greater, or 35 or greater, while at the same time, 40 or less, or 35 or less, or 30 or less, or 25 or less, or 20 or less, or 15 or less, or 10 or less, or 5 or less.
[0064] The ethylene-based polymer may exhibit a melting temperature (“Tm”) of 120 °C to 140 °C as measured according to ASTM D 3418-08. For example, the ethylene-based polymer may exhibit a melting temperature of 120 °C or greater, or 125 °C or greater, or 130 °C or greater, or135 °C or greater, while at the same time, 140 °C or less, or 135 °C or less, or 130 °C or less, or 125 °C or less as measured according to ASTM D 3418-08.
[0065] Test Methods
[0066] Melt Index: Melt index (I2) was determined according to ASTM D1238 (190 °C. 2.16 kg), melt index (I5) was determined according to ASTM D1238 (190 °C, 5 kg), melt index (I21) was determined according to ASTM D1238 (190 °C, 21.6 kg).
[0067] Melt Temperature (Tm): Melt temperatures were determined using Differential Scanning Calorimetry according to ASTM D 3418-08, with a scan rate of 10 °C / min on a sample of 10 mg and the second heating cycle was used to determine Tm.
[0068] Gel Permeation Chromatography Testing: A chromatographic system consisted of a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with an internal IR5 infra-red detector (IR5). The autosampler oven compartment was set at 160 °C and the column compartment was set at 150 °C. The columns used were 4 Agilent “Mixed A” 30cm 20-micron linear mixed-bed columns. The chromatographic solvent used was 1,2,4 trichlorobenzene and contained 200 ppm of butylated hydroxytoluene (BHT). The solvent source was nitrogen sparged. The injection volume used was 200 microliters and the flow rate was 1.0 milliliters / minute.
[0069] Calibration of the GPC column set was performed with 21 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 to 8,400,000 g / mol and were arranged in 6 cocktail mixtures with at least a decade of separation between individual molecular weights. The standards were purchased from Agilent Technologies. The polystyrene standards were prepared at 0.025 grams in 50 milliliters of solvent for molecular weights equal to or greater than 1,000,000, and 0.05 grams in 50 milliliters of solvent for molecular weights less than 1,000,000. The polystyrene standards were pre-dissolved at 80 °C with gentle agitation for 30 minutes then cooled and the room temperature solution is transferred cooled into the autosampler dissolution oven at 160 °C for 30 minutes. The polystyrene standard peak molecular weights were converted to polyethylene molecular weights using Equation 1 (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)).:
[0070]
[0071] ‘^polyethylene A X (^polystyrene) (EQI)
[0072] where M is the molecular weight, A has a value of 0.4061 and B is equal to 1.0. A fifth order polynomial was used to fit the respective polyethylene-equivalent calibration points.
[0073] The total plate count of the GPC column set was performed with decane which was introduced into blank sample via a micropump controlled with the PolymerChar GPC-IR system. The plate count for the chromatographic system should be greater than 18,000 for the 4 Agilent “Mixed A” 30 cm 20-micron linear mixed-bed columns.
[0074] Samples were prepared in a semi-automatic manner with the PolymerChar Instrument Control Software, wherein the samples were weight-targeted at 2 mg / ml, and the solvent (contained 200ppm BHT) was added to a pre nitrogen-sparged septa-capped vial, via the PolymerChar high temperature autosampler. The samples were dissolved for 2 hours at 160 °C under low speed shaking.
[0075] The calculations of MU(GPC), MW(GPC), and MZ(GPC) were based on GPC results using the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph according to Equations 2-4, using PolymerChar GPCONE software, the baseline-subtracted IR chromatogram at each equally-spaced data collection point (i), and the polyethylene equivalent molecular weight obtained from the narrow standard calibration curve for the point (i) from Equation 1.
[0076] MniGPC) =
[0077] (EQ 2)
[0078] polyethylene i MW(GPC) =
[0079] (EQ 3)
[0080]
[0081] 2 polyethylene j MZ(GPC) = — r (EQ 4)
[0082]
[0083] polyethylene i
[0084] To monitor the deviations over time, a flowrate marker (decane) was introduced into each sample via a micropump controlled with the PolymerChar GPC-IR system. This flowrate marker (FM) was used to linearly correct the pump flowrate (Flowrate(nominal)) for each sample by RV alignment of the respective decane peak within the sample (RV(FM sample)) to that of the decane peak within the narrow standards calibration (RV<FM calibrated)). Any changes in the time of the decane marker peak are then assumed to be related to a linear- shift in flowrate (Flowrate(effective)) for the entire run. After calibrating the system based on a flow marker peak, the effective flowrate (with respect to the narrow standards calibration) is calculated as Equation 5. Processing of the flow marker peak was done via the PolymerChar GPCONE Software. Acceptable flowrate correction is such that the effective flowrate should be within + / -0.5% of the nominal flowrate.
[0085] Flowrate(effective) = Flowrate(nominal) * (RV(FM Calibrated) / RV(FM Sample)) (EQ5) IR5 GPC Octene Composition Calibration is discussed as follows.
[0086] A calibration for the IR5 detector rationing was performed using at least ten ethylene-based polymer standards (Octene as comonomer) made by single-site metallocene catalyst from a single reactor in solution process (polyethylene homopolymer and ethylene / octene copolymers) of a narrow SCB distribution and known comonomer content (as measured by13C NMR Method, Qiu et al.. Anal. Chem.2009, 81, 8585-8589), ranging from homopolymer (0 SCB / 1000 total C) to approximately 40 SCB / 1000 total C, where total C = carbons in backbone + carbons in branches. Each standard had a weight-average molecular weight from 36,000 g / mole to 126,000 g / mole measured by GPC. Each standard had a molecular weight distribution (Mw / Mn) from 2.0 to 2.5. Polymer properties for the SCB standards are shown in Table A.
[0087] Table A: Copolymer Standards
[0088] Wt % Comonomer IR5 Area ratio SCB / 1000 Total C Mw Mw / Mn 23.1 0.2411 28.9 37,300 2.22
[0089] 14.0 0.2152 17.5 36,000 2.19
[0090] 0.0 0.1809 0.0 38,400 2.20
[0091]
[0092] 35.9 0.2708 44.9 42,200 2.18 5.4 0.1959 6.8 37,400 2.16
[0093] 8.6 0.2043 10.8 36,800 2.20
[0094] 39.2 0.2770 49.0 125,600 2.22
[0095] 1.1 0.1810 1.4 107,000 2.09
[0096] 14.3 0.2161 17.9 103,600 2.20
[0097] 9.4 0.2031 11.8 103,200 2.26
[0098]
[0099] The IR5 Area. Ratio (or IR5 Methyl Channel Area / IR5 Measurement Channel Area ’)” of “the baseline-subtracted area response of the IR5 methyl channel sensor” to “the baseline-subtracted area response of IR5 measurement channel sensor” (standard filters and filter wheel as supplied by PolymerChar: Part Number IR5 FWM01 included as part of the GPC-IR instrument) was calculated for each of the “Copolymer” standards. A linear fit of the Wt% Comonomer frequency versus the “IR5 Area Ratio” was constructed in the form of the following Equation 6:
[0100] Wt% Comonomer = Ao + [Ai x (IR5 Methyl Channel Area / IR5 Measurement Channel Area)] (EQ 6)
[0101] where Ao is the “Wt% Comonomer” intercept at an “IR5 Area Ratio” of zero, and Ai is the slope of the “Wt% Comonomer” versus “IR5 Area Ratio” and represents the increase in the Wt% Comonomer as a function of “IR5 Area Ratio.” The IR5 area ratio is equal to the IR5 height ratio for narrow PDI and narrow SCBD standard materials.
[0102] The comonomer distribution in an ethylene / a- olefin copolymer can be characterized as either normal (also referred to as having a Zeigler-Natta distribution), reverse, or flat. Several reported methods are utilized to quantify a Broad Orthogonal Composition Distribution (BOCD). Herein, a simple line fit is utilized such that the normal or reverse nature of the comonomer distribution can be quantified by the molecular weight composition distribution index (MWCDI), which is the slope of the linear regression of the comonomer distribution in weight precent comonomer taken from a compositional GPC measurement, wherein the x-axis is Log(MW) and the y-axis is weight percent of comonomer. The molar MWCDI, or MWCDIn, is similarly the slope of the linear regression of the in mole precent comonomer taken from a compositional GPC measurement, wherein the x-axis is Log(MW) and the y-axis is weight percent of comonomer. A reverse comonomer distribution is defined when the MWCDI > 0 and a normal comonomerdistribution is defined when the MWCDI < 0. When the MWCDI = 0 the comonomer distribution is said to be flat. Additionally, the MWCDI quantifies the magnitude of the comonomer distribution. Comparing two polymers that have MWCDI > 0. the polymer with the greater MWCDI value is defined to have a greater, i.e., increased, BOCD; in other words, the polymer with the greater MWCDI value has a greater reverse comonomer distribution. Similar is true for MWCDIn. Polymers with a relatively greater MWCDI, i.e., BOCD, can provide one or more improved physical properties, as compared to polymers having a relatively lesser MWCDI. Data used for the MWCDI calculation excluded data according to SCBf x MW signal < 0.5, where SCBf is the short chain branching frequency and MW signal is the detect response of the MW signal in the GPC measurement. Additionally, a cut-off criteria of MW signal < 0.009 was used for the GPC parameters reported including Mn, Mw, Mz, and Mp.
[0103] Sample Preparation
[0104] Provided below is the experimental procedures to prepare the inventive examples (“IE”) and the comparative examples (“CE”).
[0105] Synthesis of Structure (III): The synthesis of Structure (III) was performed according to Synthesis 1. In a nitrogen filled glovebox, ScCh (0.077, 0.51 mmol) was suspended in tetrahydrofuran (“THF”) (10 mL) in a 40 mL vial and the suspension was stirred vigorously at 23 °C overnight. MeLi (0.78 mL, 1.57 M, 1.23 mmol) in diethyl ether was added to the suspension slowly and stirred for 20 minutes. Upon addition of MeLi, the reaction suspension turned into a light yellow solution. Then, a solution of LI (0.1g, 0.36 mmol) in THF (5 mL) was added to the reaction slowly and stirred overnight at 23 °C. The reaction solution changed from light yellow to bright orange when adding the ligand to the reaction. The following day, solvent was removed in vacuo, solid was re-dissolved in toluene (10 mL) and filtered through a syringe filter. After removing solvent under vacuum, product was obtained as an orange powder (0.132 g, 87%). 1H NMR (400 MHz, CDC13): 5 6.95 (m, 3H), 6.83 (t, 1H, J - 6.81 Hz), 6.68 (d, 1H, J - 8.10 Hz), 6.33 (s, 1H), 5.97 (d, 1H. J= 7.70 Hz), 3.34 (broad, 4H. THF), 2.93(s. 3H), 2.14(s, 6H). 1.99(s, 3H), 0.82(broad, 4H, THF), 0.00(s, 6H).
[0106]
[0107] Synthesis 1
[0108] Synthesis of Structure (IV): The synthesis of Structure (IV) was performed according to Synthesis 2. In a nitrogen filled glovebox, ScC13 (0.064 g, 0.42 mmol) was suspended in THF (10 mb) in a 40 mL vial and the suspension was stirred vigorously at room temperature overnight. MeLi (0.65 mL, 1.57 M, 1.02 mmol) in diethyl ether was added to the suspension slowly and stirred for 20 min. Upon addition of MeLi, reaction suspension turned light yellow solution. Then, a solution of L2 (0.1 g, 0.30 mmol) in THF (5 mL) was added to the reaction slowly and stirred overnight at room temperature. Reaction solution changed from light yellow to bright orange when adding the ligand to the reaction. The following day, solvent was removed in vacuo, solid was redissolved in toluene (10 mL) and filtered through a syringe filter. After removing solvent under vacuum, product was obtained as an orange powder (0.128 g, 89%). 1H NMR (400 MHz, CDC13): 57.13 (m, 3H), 7.02 (d, 1H, J = 7.92 Hz), 6.72(d, 1H, I = 8.75 Hz), 6.35 (s, 1H), 6.05(d, 2H, J = 7.84 Hz), 3.74(broad, 6H), 2.96(s, 3H), 2.00(s, 3H), 1.15(d, 6H, I = 6.77 Hz), 1.01(d, 6H, I = 7.03 Hz), 0.00(s, 6H).
[0109] Me P Synthesis 2
[0110]
[0111] Synthesis of Structure (V): Synthesis of Structure (V) was performed according to Synthesis 3. In a dinitrogen fdled glovebox, a solution of L3 (0.2 g, 0.72 mmol) ligand in THF (3 mb) was added slowly to a solution of Sc(CH2SiMe3)3(THF)2 (0.36 g, 0.80 mmol) in THF (5 mb). Upon addition of ligand, reaction changed from yellow to orange immediately. After stirring at 23 °C for 4 hours, volatiles were removed in vacuo to provide product as an orange powder (0.40 g, 98%). 1H NMR (400 MHz, C6D6): 5 7.44 (d, 1H, J = 8.4 Hz), 6.96 (t, 1H, J = 7.9 Hz), 6.73(s, 2H), 6.56(t, 2H, J = 8.1 Hz), 5.93 (d, 1H, J = 7.8 Hz), 3.53 (broad, 4H), 2.92(s, 3H), 2.09 (s, 3H), 2.08(s,6H), 0.87 (broad, 4H), 0.12 (d, 2H, J = 12.0 Hz), 0.00( s, 18H), -0.17(d, 2H, J = 12.0 Hz).
[0112] ’'SiMe3
[0113] 0"" " i'
[0114] StMes
[0115]
[0116] Synthesis 3
[0117] Synthesis of Structure (VI): Synthesis of Structure (VI) was performed according to Synthesis 4. In a dinitrogen fdled glovebox, a solution of L2 (0.2 g, 0.60 mmol) ligand in THF (3 mb) was added slowly to a solution of Sc(CH2SiMe3)3(THF)2 (0.3 g, 0.66 mmol) in THF (5 mb). Upon addition of ligand, reaction solution changed from yellow to orange immediately. After stirring at 23 °C for 3 hours, volatiles were removed in vacuo to give product as a bright orange powder (0.35 g, 94%). 1HNMR (400 MHz, C6D6): 67.08(m, 3H), 6.91 (t, 1H, J = 8.0 Hz), 6.66(d, 2H, J = 8.30 Hz), 6.44(s, 1H), 5.92 (d, 1H, 8.27 Hz), 3.53 (broad, 4H), 3.39(hept, 2H, J = 6.8 Hz), 2.95(s, 3H), 2.00 (s, 3H), 1.12(d, 6H, J = 6.9 Hz), 1 ,02(broad, 4H), 0.96(d, 6H, J = 6.7 Hz), 0.08(d, 2H, J = 11.9 Hz), 0.00(s, 18H), -0.16(d, 2H, J = 11.9 Hz).
[0118]
[0119] Synthesis 4
[0120] Synthesis of Structure (VII): Synthesis of Structure (VII) was performed according to Synthesis 5. In a dinitrogen filled glovebox, a solution of L4 (0.2 g, 0.55 mmol) ligand in THF (3 mb) was added slowly to a solution of Sc(CH2SiMe3)3(THF)2 (0.28 g, 0.61 mmol) in THF (5 mb). Upon addition of ligand, reaction solution changed from yellow to red immediately. After stirring at 23 °C for 16 hours, volatiles were removed in vacuo, hexane (10 mb) was added to the solid residue and placed in the freezer overnight. The following day, red solid settled at the bottom of the vial was separated from the solvent via decantation and dried in vacuo to afford clean product as red powder (0.27 g, 75%). 1HNMR (400 MHz, C6D6): 87.57(d, 1H, J= 8.3 Hz), 7.09-7.04 (m, 3H), 6.97 - 6.91 (m, 1H), 6.85 - 6.78 (m, 2H), 6.73(t, 2H, J = 7.6 Hz), 6.66 (d, 1H, J = 7.8 Hz), 6.08 (d, 1H, J = 7.9Hz), 3.56(broad, 4H), 2.25(s, 6H), 1.06 (broad, 4H), -0.10-0.14 (broad, 24H).
[0121] 19F NMR ((376 MHz, C6D6): 8 -106.71 (s, 2F).
[0122]
[0123] Preparation of catalyst 1 : The spray-dried catalyst sample was prepared and sprayed in a nitrogen-purged glove box. In an oven-dried glass bottle, 1.38 g of fumed silica (Cabosil TS-610) was slurried in 35 g of toluene until well dispersed, then 11.1 of a 10 % solution by weight of methylaluminoxane (obtained from Grace) in toluene and Structure (III) (0.02 g) were added. Theslurried mixture was allowed to stir for 30 to 60 minutes. The mixture was spray-dried using a Buchi Mini Spray Dryer B-290 with the following parameters to yield the dried sample: Set Temperature - 140°C. Outlet Temperature - 75 °C (min.), Aspirator - 60%, and Pump Speed -130 rpm.
[0124] Preparation of catalyst 2: The spray-dried catalyst sample was prepared and sprayed in a nitrogen-purged glove box. In an oven-dried glass bottle. 1.34 g of fumed silica (Cabosil TS-610) was slurried in 34 g of toluene until well dispersed, then 10.7 g of a 10 % solution by weight of methylaluminoxane (obtained from Grace) in toluene and Structure (IV) (0.022 g) were added. Then slurried mixture was allowed to stir for 30-60 minutes. The mixture was spray-dried using a Buchi Mini Spray Dryer B-290 with the following parameters to yield the dried sample: Set Temperature - 140°C. Outlet Temperature - 75 °C (min.), Aspirator - 60%, and Pump Speed -130 rpm.
[0125] Preparation of catalyst 3: The spray-dried catalyst sample was prepared and sprayed in a nitrogen-purged glove box. In an oven-dried glass bottle. 1.28 g of fumed silica (Cabosil TS-610) was slurried in 34 g of toluene until well dispersed, then 10.6 g of a 10 % solution by weight of methylaluminoxane (obtained from Grace) in toluene and Structure (IV) (0.054 g) were added. The slurried mixture was allowed to stir for 30-60 minutes. The mixture was spray-dried using a Buchi Mini Spray Dryer B-290 with the following parameters to yield the dried sample: Set Temperature - 140°C. Outlet Temperature - 75 °C (min.), Aspirator - 60%, and Pump Speed -130 rpm.
[0126] Preparation of catalyst 4: The spray-dried catalyst sample was prepared and sprayed in a nitrogen-purged glove box. In an oven-dried glass bottle. 1.38 g of fumed silica (Cabosil TS-610) was slurried in 36 g of toluene until well dispersed, then 11.2 g of a 10 % solution by weight of MAO (obtained from Grace) in toluene and Structure (V) (0.027 g) were added. The slurried mixture was allowed to stir for 30-60 minutes. The mixture was spray-dried using a Buchi Mini Spray Dryer B-290 with the following parameters to yield the dried sample: Set Temperature -140°C, Outlet Temperature - 75 °C (min.), Aspirator - 60%, and Pump Speed - 130 rpm.
[0127] Preparation of catalyst 5: The spray-dried catalyst sample was prepared and sprayed in a nitrogen-purged glove box. In an oven-dried glass bottle, 1.40 g of fumed silica (Cabosil TS-610) was slurried in 36 g of toluene until well dispersed, then 11.2 g of a 10 % solution by weight of MAO (obtained from Grace) in toluene and Structure (VI) (0.03 g) were added. The slurriedmixture was allowed to stir for 30-60 minutes. The mixture was spray-dried using a Buchi Mini Spray Dryer B-290 with the following parameters to yield the dried sample: Set Temperature -140°C, Outlet Temperature - 75 °C (min.), Aspirator - 60%. and Pump Speed - 130 rpm.
[0128] Preparation of catalyst 6: The spray-dried catalyst sample was prepared and sprayed in a nitrogen-purged glove box. In an oven-dried glass bottle, 1.34 g of fumed silica (Cabosil TS-610) was slurried in 35 g of toluene until well dispersed, then 10. 8 g of a 10 % solution by weight of MAO (obtained from Grace) in toluene and Structure (VII) (0.03 g) were added. The slurried mixture was allowed to stir for 30-60 minutes. The mixture was spray-dried using a Buchi Mini Spray Dryer B-290 with the following parameters to yield the dried sample: Set Temperature -140°C, Outlet Temperature - 75 °C (min.), Aspirator - 60%, and Pump Speed - 130 rpm.
[0129] Preparation of chrome catalyst used for CE1 and CE2: Chrome catalyst used for comparative examples CE1 and CE2 was from a batch prepared on a large scale as follows. About 1116 kg (2460 pounds) of porous silica support (Grade Sylopol 955 chromium on silica, produced by Davison Catalyst division of W. R. Grace and Co.), having a particle size of about 40 microns and a surface area of about 300 square meters per gram was charged to a fluidized bed heating vessel. There it was heated slowly at a rate of about 100°C per hour under dry nitrogen up to 325°C and the nitrogen stream was then replaced with a stream of dry air. The silica support was heated slowly at a rate of about 100°C per hour to 600°C where it was activated for about 1.5 hours. The calcined support was then cooled with dry air (at ambient temperature) to about 300°C and further cooled from 300°C to room temperature with dry nitrogen (at ambient temperature). The resulting cooled powder was stored under nitrogen atmosphere until treated with a chromium compound and then a reducing agent as described below. In supporting the silyl chromate compound on the silica, the support was placed in a vertical catalyst blender with a helical ribbon agitator under an inert atmosphere. About 5.8 liters of isopentane solvent were charged per kilogram (0.70 gallons per pound) of silica. The resulting mixture was stirred and heated to about 45°C. Then 3.15 kilograms of bis (triphenylsilyl) chromate was charged for every 100 kilograms of silica. This was stirred at about 45°C for 10 hours. A 25 wt % solution of DEALE in isopentane was then added to the surface of the catalyst slurry at a selected rate over a selected time period to obtain a selected molar ratio of diethylalumminum ethoxide (DEALE) / Cr. The mixture was agitated at a selected agitation rate at a temperature of approximately 45 °C during the selected addition time. The mixture was further agitated at a selected rate for about 2 hours. Then the solvent was substantiallyremoved by drying at a jacket temperature of approximately 75°C and slightly above atmospheric pressure for about 24 hours. The resulting dry, free flowing powder was then stored under nitrogen until used.
[0130] Dual catalyst preparation used for CE3 and CE4: Toluene (17.8 kg), 10 wt% solution of methylaluminoxane (11.3 kg), Evonik Aerosil R-972 (1.71 kg), bis(2- (pentamethylphenylamido)ethyl)amine zirconium dibenzyl (69.9 grams), (tetramethyclopentadiene)(propylcyclopentadiene) zirconium dimethyl (13.6 grams) were mixed for 1 hour. The resulting mixture was introduced into an atomizing device, producing droplets that were then contacted with a hot nitrogen gas stream to evaporate the liquid and form a powder. The powder was separated from the gas mixture in a cyclone separator and discharged into a container. Spray-dried in a dryer inlet temperature at 144° C. and outlet temperature 70° to 84° C. Collected the spray-dried catalyst as a powder.
[0131]
[0132] The spray dried catalysts were contacted with ethylene and an alpha olefin comonomer in the presence of molecular hydrogen gas inside of a gas phase polymerization reactor to form the ethylene-based polymer. The reactor was a 2 liter semi-batch autoclave polymerization reactor equipped with a mechanical agitator. For the experimental runs, the reactor was first dried for 1 hour, charged with 200 g of NaCl and dried by heating at 100 °C under nitrogen for 30 minutes. After baking out the reactor, 5 g of SMAO (supported methylaluminoxane) was introduced as a scavenger under nitrogen pressure. After adding SMAO, the reactor was sealed, and components were stirred. The reactor was then charged with hydrogen and 1-hexene pressurized with ethylene. Once the system reached a steady state, the catalyst was charged into the reactor at 80 °C to start polymerization. The reactor temperature was brought to the desired reaction temperature and maintained at this temperature, and at the ethylene, 1-hexene, and hydrogen feed ratios throughout the 1 hour run. At the end of the run, the reactor was cooled down, vented and opened. The resulting product mixture was washed with water and methanol, then dried. Polymerization efficiency (grams polymer / gram Scandium) was determined as the ratio of polymer produced to the amount of catalyst metal added to the reactor. The reactor was operated in condition A (80 °C, 0.016 Ce / C2, 0.0005 H2 / C2, C2= 1.516 MPa), condition B (80 °C, 0.004 C6 / C2, 0.0005 H2 / C2, C2= 1.516 MPa) or C (100 °C, 0.004 C6 / C2, 0.004 H2 / C2, C2= 1.516 MPa).Results
[0133] Tables 1 and 2 provide the properties of the ethylene-based polymers embodied by IE1- IE11 and CE1-CE4. The ethylene-based polymers were produced using the identified examples and run conditions (“Cond.”).
[0134] Table 1
[0135] Yield Efficiency
[0136] Ex Catalyst Cond. 12 15 I21
[0137] (g / 10min) (g / 10min) (g / lOmin) (g) (g / g)
[0138] IE1 Catalyst 1 B 0.436 2.156 26.425 14.80 330,294
[0139] IE2 Catalyst 2 A N / A N / A N / A 12.78 283,585
[0140] IE3 Catalyst 2 B No Flow No Flow No Flow 7.59 140,125
[0141] IE4 Catalyst 3 A N / A N / A N / A 8.38 154,582
[0142] IE5 Catalyst 3 B N / A N / A N / A 6.92 51,157
[0143] IE6 Catalyst 4 A N / A N / A N / A 6.79 50,267
[0144] IE7 Catalyst 4 B N / A N / A N / A 4.99 55,605
[0145] IE8 Catalyst 5 A N / A N / A N / A 5.80 64,502
[0146] IE9 Catalyst 5 B No Flow 0.235 7.284 8.19 91,192
[0147] IE10 Catalyst 6 A N / A N / A N / A 11.20 124,555
[0148] IE11 Catalyst 6 B N / A N / A N / A 4.40 48,932
[0149]
[0150] Table 2
[0151] Mn MWD
[0152] Condition Mw SCB / 1000 Example Catalyst (g / mol) (g / mol) Mz (g / mol) (Mw / Mn) TC (>, (wt%) IE1 Catalyst 1 B 17,194 236,935 7,408,156 13.8 1.93 * IE2 Catalyst 2 A 36,008 846,745 7,220,626 23.5 8.5 5.12 IE3 Catalyst 2 B 29,347 814,094 7,369,418 27.7 1.6 0.98 IE4 Catalyst 3 A 39,225 878,230 6,277,782 22.4 10.30 6.17 IE5 Catalyst 3 B 34,932 1,235,939 7,503,900 35.4 1.80 1.10 CE1 Chrome A 6,856 277,999 2,134,909 40.55 4.44 2.67 catalyst
[0153] CE2 Chrome B 8,238 317,356 2,245,647 38.52 1.59 0.96 catalyst
[0154] Bimodal
[0155] CE3 A 52,039 594,061 2,285,533 11.42 5.33 3.20 catalyst
[0156] CE4 Bimodal
[0157] C 22,595 328,009 1,176,128 14.52 1.75 1.05
[0158]
[0159] catalyst
[0160] *Below detection limitReferring now to Tables 1 and 2, IE1-IE11 surprisingly demonstrate catalysts / precatalysts comprising a group III metal center and quinoline-containing ligands that form an ethylene-based polymer in gas phase reactors. As can be seen from the Mw, Mz data, the inventive catalysts demonstrate either similar or exceedingly higher molecular weight capability compared to CE1-CE2 chrome based catalyst and to the dual catalyst system of CE3-CE4. Moreover, the inventive catalysts produced polymers with broad MWD as demonstrated in Table 2, a feature that is often obtained with chrome or catalysts systems comprising of two active catalysts. The inventive catalysts disclosed here are single catalyst systems that are capable of producing polymers with high molecular weight and broad MWD, which are desirable features to improve polymer performance while having good polymer processability needed for target product fabrication. Data from Catalysts 4-6 as IE6-IE11 are not provided as the ethylene-based polymers produced therefrom exhibited an ultra-high molecular weight that that is outside of the detection limit for gel permeation chromatography. This further illustrates the advantages of the inventive catalysts.
Claims
CLAIMSWhat is claimed is1. A method of making an ethylene-based polymer, the method comprising the steps of:(a) contacting ethylene and an alpha olefin comonomer with a catalyst in the presence of molecular hydrogen gas inside of a gas phase polymerization reactor or a slurry phase polymerization reactor, wherein the catalyst is formed by activation of a precatalyst of Structure (I):R4R5R2Utx R6R2"N-N - M1 i 'Structure (I)wherein M is scandium (Sc), yttrium (Y), or a lanthanide metal having an oxidation state of +3;R1is a C1-C30 hydrocarbyl, a C1-C30 heterohydrocarbyl, a -Si(Rc)3. a C6-C30 aryl, or a C5-C30 heteroaryls;R2to R7are each independently selected from hydrogen, a C1-C30 hydrocarbyl, a C1-C30 heterohydrocarbyl, a -Si(Rc)3, a C6-C30 aryl, a C5-C30 heteroaryl. ;Rcis a C1-C20 a hydrocarbyl or a C6-C20 aryl or a C5-C20 heteroaryl.X is selected from methyl, ethyl, 1-propyl, 2-propyl, 1-butyl, 2,2, dimethylpropyl; trimethylsilylmethyl; phenyl; benzyl; or halides, andL is independently selected from coordinating groups Et2O, tetrahydrofuran, 2- methyl-tetrahydrofuran, MeOtBu, EtsN, PhNMe2, MePh2N, pyridine and dimethylsulfide; and(b) forming an ethylene-based polymer.
2. The method of claim 1, wherein the precatalyst is supported using an inert medium.
3. The method of any one of claims 1 and 2, wherein the precatalyst is supported on a fumed silica substrate.
4. The method of any one of claims 1 to 3, wherein the precatalyst is activated into the catalyst by aluminoxane or methylaluminoxane.
5. The method of any one of claims 1 to 4, wherein the precatalyst has Structure (II):RStructure (II)wherein R8to R11are each independently selected from hydrogen, methyl, ethyl, propyl, isopropyl;R12is methyl, aryl, heteroaryl; andX is selected from methyl; trimethylsilylmethyl; phenyl; benzyl; or halides.
6. The method of any one of claims 1-5, wherein the precatalyst has one of structures (III) to (VII):Structure (III)7. The method of any one of claims 1-6, wherein the step of forming the ethylene-based polymer is performed at a temperature of 80 °C to 110 °C.
8. The method of any one of claims 1-7, wherein the ethylene-based polymer exhibits one or more of the following properties:(i) a density of 0.93 g / cc to 0.97 g / cc as measured according to ASTM D792;(ii) a melt index (I2) of 3 g / 10 min or less as measured according to ASTM D1238;(iii) a melt index (I5) of 5.0 g / 10 min or less as measured according to ASTM D1238; (iv) a melt index (T21) of 30.0 g / 10 min or less as measured according to ASTM DI 238; (v) a short chain branching per 1000 TC (total carbons) of 0 to 20 as measured according to Gel Permeation Chromatography; and(vi) a G, comonomer content of 0 wt% to 10 wt% as measured according to Gel Permeation Chromatography.
9. The method of any one of claims 1-8, wherein the ethylene-based polymer exhibits one or more of the following properties:(i) a molecular weight distribution of 5 or greater;(ii) a molecular weight distribution of 10 or greater;(iii) a molecular weight distribution of 20 or greater; and(iv) a molecular weight distribution of 30 or greater.
10. The method of any one of claims 1-9, wherein the ethylene-based polymer exhibits one or more of the following properties:(i) a weight average molecular weight of 10, 000 to 2,000,000 g / mol as measured according to Gel Permeation Chromatography;(ii) a weight average molecular weight of 30,000 to 300,000 g / mol as measured according to Gel Permeation Chromatography; and(iii) a weight average molecular weight of 200,000 to 900,000 g / mol as measured according to Gel Permeation Chromatography.
11. The method of any one of claims 1-10, wherein the ethylene-based polymer exhibits one or more of the following properties:(i) a Mz / Mw ratio of 5 or greater;(ii) a Mz / Mw ratio of 10 or greater; and(iii) a Mz / Mw ratio of 20 or greater.
12. The method of any one of claims 1-11, wherein the ethylene-based polymer exhibits one or more of the following properties:(i) a Tm value of 120 °C to 140 °C as measured according to ASTM D 3418-08; and (ii) a Tm value of 120 °C to 130°C as measured according to ASTM D 3418-08.