Carbosiloxane and method for preparation thereof

The ring opening polymerization of 2,2,5,5-tetramethyl-2,5-disila-1-oxacyclopentane with a metal silanolate and alkenyl-functional halosilane produces carbosiloxanes with controlled polydispersity and improved compatibility, overcoming the drawbacks of existing polydimethylsiloxane polymerization methods.

WO2026235920A1PCT designated stage Publication Date: 2026-11-12DOW SILICONES CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/024779
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-05
Filing Date
2026-04-22
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for preparing polydimethylsiloxane monofunctional polymers face issues such as the formation of undesirable macrocyclic by-products, high cost, limited availability of starting materials, and poor compatibility with organics, particularly mineral oil.

Method used

A method involving the ring opening polymerization of 2,2,5,5-tetramethyl-2,5-disila-1-oxacyclopentane using a metal silanolate and a polar aprotic solvent, followed by termination with an alkenyl-functional halosilane, to produce a carbosiloxane with controlled polydispersity and improved compatibility.

Benefits of technology

The method produces alkenyl-terminated carbosiloxanes with low polydispersity and enhanced compatibility with organic materials, reducing the formation of macrocyclic by-products and addressing the limitations of existing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000001_0001
    Figure IMGF000001_0001
  • Figure IMGF000003_0001
    Figure IMGF000003_0001
  • Figure IMGF000003_0002
    Figure IMGF000003_0002
Patent Text Reader

Abstract

A carbosiloxane is a linear copolymer with a backbone made up of ethylene and dimethylsiloxy units. The carbosiloxane has different groups at each end. A method for preparing the carbosiloxane is provided.
Need to check novelty before this filing date? Find Prior Art

Description

CARBOSILOXANE AND METHOD FOR PREPARATION THEREOFCROSS REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of U.S. Provisional Patent Application Serial No.63 / 799,907 filed on 5 May 2025 under 35 U.S.C. §119 (e). U.S. Provisional Patent Application Serial No. 63 / 799,907 is hereby incorporated by reference.FIELD

[0002] This invention relates to a carbosiloxane and methods for preparation and use thereof. More particularly, the carbosiloxane is a linear copolymer with a backbone comprising ethylene and dimethylsiloxy units, and the carbosiloxane further comprises different terminal groups at each end.INTRODUCTION

[0003] Polydimethylsiloxane (PDMS) monofunctional polymers (which comprise linear siloxane backbones with different groups at each end) can be prepared by ring-opening polymerization (ROP) of D3. A lithium-based initiator (e.g., lithium siloxanolate, or butyl lithium) is typically used as an initiator of the ring opening reaction. The ROP of D3 is fast and can be done at room temperature (RT), but the reaction must be kept under kinetic control, and stopped with a terminating agent (e.g., a chlorosilane) before thermodynamic equilibration occurs, as stable macrocyclic by-products can be generated via depolymerization (back-biting). This method suffers from the drawbacks that the formation of the macrocyclic by-products (e.g., D4, D5, and D6) may be undesirable in some applications. In addition, the high price and limited availability of D3 can also be a barrier to some applications. Another drawback of the PDMS monofunctional polymers is the poor compatibility with some organics (e.g., mineral oil).SUMMARY

[0004] wherein subscript n is an integer with a value of 2 to 1,000, R is methyl or phenyl, and R4is an alkenyl- or alkoxy- functional organosilicon moiety. A method for preparing the carbosiloxane comprises ring opening polymerization of 2,2,5,5-tetramethyl-2,5-disila-l-oxacyclopentane and termination of the ring opening polymerization with a halosilane.DETAILED DESCRIPTION

[0005] The method for preparing the carbosiloxane introduced above comprises: 1) combining, under conditions to effect a ring opening polymerization reaction, starting materials comprising: A) 2,2,5,5-tetramethyl-2,5-disila-l-oxacyclopentane, B) a metal silanolate, and C) a polar aprotic solvent; thereby forming a ring opening polymerization reaction product; and 2) combining, under conditions to effect a reaction to terminate the ring opening polymerization reaction of step 1), starting materials comprising: the ring opening polymerization reaction product, and D) an alkenyl-functional halosilane of formula (R2)(R3)2SiX, wherein X is a halogen, each R3is an independently selected monovalent hydrocarbyl group free of aliphatic unsaturation, and R2is an alkenyl group; wherein a molar ratio of D) the alkenyl-functional halosilane to B) the metal silanolate is > 1, thereby preparing a reaction product comprising the carbosiloxane. The carbosiloxane in the reaction product produced in step 2) may be an a-TMS-, y-Vi- terminated carbosiloxane, e.g., an a-TMS-, y-Vi- terminated PEDS.

[0006] Step 1) of the method comprises combining, starting materials comprising: A) the 2,2,5,5-tetramethyl-2,5-disila-l-oxacyclopentane, B) the metal silanolate, and C) the polar aprotic solvent. Step 1) is performed under conditions to effect a ring opening polymerization reaction of starting materials A) and B), thereby forming a ring opening polymerization reaction product. Step 1) forms the backbone, which comprises ethylene and dimethylsiloxy blocks of the carbosiloxane (polymer) described herein, and a terminal group derived from the metal silanolate. Combining in step 1) may be performed by any convenient means in any convenient equipment, such as mixing in a reactor with mixing means such as baffles and / or an agitator. The reactor may have heating and / or cooling means, such as a jacket with heat transfer fluid, to control temperature of the reaction mixture inside the reactor. The starting materials may be combined in any order, however, B) the metal silanolate and A) the 2,2,5,5-tetramethyl-2,5-disila-1 -oxacyclopentane may be mixed in the reactor, and thereafter C) the polar aprotic solvent, such as THF, may be added to the reactor. Mixing the resulting reaction mixture may be performed at RT for a time sufficient for ring opening polymerization to occur. For example, mixing may be performed at RT for at least 5 min, alternatively at least 30 min, and alternatively at least 1 h, while at the same time, mixing may be performed for up to 24 h, alternatively up to 12 h, alternatively up to 8 h, and alternatively up to 2 h. Alternatively, step 1) may comprise mixing the reaction mixture at RT for 2 h to 24 h. Alternatively, A) the 2,2,5,5-tetramethyl-2,5-disila-1 -oxacyclopentane may be added, continuously or intermittently, into a reactor containing a mixture of B) the metal silanolate and C) the polar aprotic solvent, over a period of time. Without wishing to be bound by theory, it is thought that using this order of addition may result in the carbosiloxane having low polydispersity (e.g., 1 to 1.3).

[0007] Step 2) of the method comprises: combining, under conditions to effect a reaction to terminate the ring opening polymerization reaction of step 1), starting materials comprising: the ring opening polymerization reaction product prepared in step 1), and D) the alkenyl-functional halosilane. Step 2) may be referred to as quenching the ring opening polymerization reaction product formed in step 1). Step 2) may be performed after consumption (ring opening) of A) the 2,2,5,5-tetramethyl-2,5-disila-l-oxacyclopentane is complete, e.g., when the method is performed batchwise. Step 2) reacts a silyl moiety on to the end of the polymeric backbone. Step 2) forms a reaction product comprising the carbosiloxane, which is an alkenyl-terminated carbosiloxane. This reaction product may further comprise C) the polar aprotic solvent and optionally a side product, such as a salt including the sodium cation from starting material B), and / or an acid derived from D) the alkenyl-functional halosilane. The starting materials used in this method are described further below.

[0008] Starting material A) used in the method is 2,2,5,5-tetramethyl-2,5-disila-l-oxacyclopentane of formula, which has CAS No. 7418-20-4 and is commercially available, e.g., from Gelest Inc. of Morrisville, Pennsylvania, USA.

[0009] Starting material B) used in the method for making the carbosiloxane is a metal CH3O'— Si — Rw+ ilsilanolate. The metal silanolate may have formula: 3;abbreviatedM+O Si(Me)2(R). The metal, M+, of the metal silanolate may be selected from the group consisting of lithium and sodium, alternatively sodium. In B) the metal silanolate, R may be a methyl group or a phenyl group, alternatively methyl. Alternatively, starting material B) may be a sodium silanolate. Metal silanolates are known in the art and are commercially available. Lithium trimethylsilanolate and sodium trimethylsilanolate (which has formula,anciCAS No. 18027-10-6) are commercially available from Sigma- Aldrich, Inc. of St. Louis, Missouri, USA. Alternatively, starting material B) may be a dimethylphenylsilanol sodium salt, 97%, with CAS No. 7646-75-5, which is commercially available from Thermo Scientific Chemicals. Amounts of starting materials A) and B) may beselected by one skilled in the art, however, a molar ratio of amounts of A) : B) may be sufficient to provide the alkenyl-functional carbosiloxane with the DP described herein, for example A):B) molar ratio may be 2:1 to 1,000:1, alternatively 2:1 to 250:1, alternatively 5:1 to 36:1, and alternatively 10:1 to 20:1.

[0010] Starting material C) used in the method is a solvent, which is capable of dissolving and / or dispersing starting materials A) and B) to facilitate combining them in step 1). The solvent may be a polar, aprotic solvent. The polar, aprotic solvent is exemplified by acetone with CAS No. 67-64-1, acetonitrile with CAS No. 75-05-8, dimethylformamide (DMF) with CAS No. 68-12-2, dimethyl sulfoxide (DMSO) with CAS No. 67-68-5, and tetrahydrofuran (THF) with CAS No. 109-99-9, all of which are commercially available from various sources including Sigma- Aldrich, Inc. The amount of solvent is sufficient to facilitate mixing of starting materials A) and B) and may be > 0 to 50 mol / L, alternatively > 0 to 13 mol / L, alternatively 6 to 50 mol / L, alternatively 6 to 12 mol / L, and alternatively 8 to 12 mol / L.

[0011] Starting material D) used in the method is an alkenyl-functional halosilane. Thealkenyl-functional halosilane may have formula, abbreviated (R2)(R3)2SiX, wherein X is a halogen, each R3is an independently selected monovalent hydrocarbyl group free of aliphatic unsaturation, and R2is an alkenyl group. Suitable monovalent hydrocarbyl groups for R3are exemplified by alkyl groups and aryl groups. Suitable alkyl groups may have 1 to 10 carbon atoms and are exemplified by methyl, ethyl, propyl (including n-propyl and isopropyl), butyl (including n-butyl, isobutyl, tert-butyl and sec-butyl); and pentyl, heptyl, octyl, nonyl, and decyl groups, as well as branched isomers with 5 to 10 carbon atoms. Suitable aryl groups include phenyl, tolyl, xylyl, 1 -phenylethyl, 2-phenylethyl, naphthyl, and anthracenyl; alternatively phenyl. Alternatively, each R3may be an alkyl group. Alternatively, each R3may be methyl. Suitable alkenyl groups for R2may have 2 to 8, alternatively 2 to 6 carbon atoms. The alkenyl group is capable of undergoing hydrosilylation reaction with an SiH moiety.Suitable alkenyl groups include vinyl, allyl, and hexenyl. X is a halogen, such as bromine (Br), chlorine (Cl), fluorine (F), or iodine (I); alternatively Br or Cl, and alternatively Cl. Alkenyl-functional halosilanes are commercially available and are exemplified by vinyldimethylchlorosilane with CAS No. 1719-58-0; allyldimethylchlorosilane with CAS No.4028-23-3; chloro, methyl, phenyl, vinyl silane with CAS No. 17306-05-7; and dimethyl(2-phenylethyl)chlorosilane with CAS No. 17146-08-6; are all available from Sigma-Aldrich, Inc.

[0012] Starting material B), the metal silanolate and starting material D) the alkenyl- functional halosilane, may be used in the method in amounts that provide a molar ratio of D) the alkenyl-functional halosilane to B) the metal silanolate (terminator / initiator ratio) > 1, alternatively > 1 to 2, and alternatively > 1 to 1.5. Without wishing to be bound by theory, it is thought that use of a molar excess of the halosilane minimizes or avoids formation of a silanol functional side product.

[0013] The method described above may further comprise an optional, additional step. For example, the method may optionally further comprise drying one or more of the starting materials before step 1), e.g., C) the polar aprotic solvent and / or A) the 2,2,5,5-tetramethyl-2,5- disila-1 -oxacyclopentane may be dried before use. Drying may be performed by any convenient means such as stripping, distillation, and / or contact with an adsorbent, such as alumina or molecular sieves. The method may optionally further comprise neutralizing the reaction product after step 2), e.g., by adding a neutralizing agent, such as calcium carbonate. Without wishing to be bound by theory, it is thought that polydispersity may be reduced by neutralizing the reaction product. The method may optionally further comprise step 3) recovering the alkenyl-terminated carbosiloxane after step 2) and / or neutralizing, when neutralizing is used. Recovering may be performed by any convenient means. For example, recovering may comprise diluting the reaction mixture prepared in step 2) with an incompatible solvent to precipitate out any salt side products. For example, the incompatible solvent may comprise an aliphatic hydrocarbon such as hexane to precipitate out the salt side product. The reaction mixture may then be centrifuged and decanted, or filtered, to remove the salt side product. Alternatively, or in addition, the reaction product may be distilled or stripped with heating and optionally with reduced pressure to recover the carbosiloxane, which is the alkenyl-terminated carbosiloxane.

[0014] The alkenyl-terminated carbosiloxane has formula:, wherein R is methyl or phenyl, R2is the alkenyl group, each R3is the independently selected monovalent hydrocarbyl group free of aliphatic unsaturation, each as described and exemplified above, and subscript n represents degree of polymerization of the alkenyl-terminated carbosiloxane. Subscript n has an average value of 2 to 1,000. Alternatively, subscript n may be at least 2, alternatively at least 3, alternatively at least 4, alternatively at least 5, alternatively at least 6, alternatively at least 7,alternatively at least 8, and alternatively at least 10; while at the same time, subscript n may be up to 1,000, alternatively up to 500, alternatively up to 250, alternatively up to 150, alternatively up to 100, alternatively up to 50, alternatively up to 45, alternatively up to 40, alternatively up to 36, alternatively up to 35, and alternatively up to 30. The alkenyl-terminated carbosiloxane may have a poly dispersity (PD), which is defined as weight average molecular weight divided by number average molecular weight (Mw / Mn), wherein PD < 1.5, alternatively PD < 1.4, and alternatively PD < 1.3. Without wishing to be bound by theory, it is thought that the alkenyl-terminated carbosiloxane may have a low polydispersity, for example when appropriate method conditions are selected, e.g., PD may be 1 to 1.3, alternatively 1 to < 1.3, alternatively 1 to 1.2, and alternatively 1 to 1.1; and use of a sodium silanolate may facilitate formation of an alkenyl-terminated carbosiloxane with PD values in the lower part of the range. Without wishing to be bound by theory, it is also thought that DP and PD may be more readily controlled when the method of this invention is used with a sodium silanolate initiator.

[0015] The alkenyl-terminated carbosiloxane may be used as an intermediate for further reaction, to prepare the alkoxy -terminated carbosiloxane. A method for preparing the alkoxyterminated carbosiloxane comprises practicing the method comprising steps 1) and 2) and optionally 3), and optionally one or more of the additional steps, as described above, to make the alkenyl-terminated carbosiloxane. The method for making the alkoxy -terminated carbosiloxane further comprises: 4) combining, under conditions to effect hydrosilylation reaction, starting materials comprising: E) the alkenyl-terminated carbosiloxane prepared as described above; F) an SiH functional siloxane oligomer; and G) a hydrosilylation reaction catalyst. An optional, additional starting material may be used, e.g., H) a solvent may be used to facilitate mixing and delivery of one or more starting materials used in step 4), such as G) the hydrosilylation reaction catalyst. Suitable solvents for starting material H) include aliphatic hydrocarbons such as heptane and octane; aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; and monohydric alcohols such as isopropanol. , all of which are known in the art and are commercially available. Starting material I), a hydrosilylation reaction inhibitor, may optionally be used in the method for preparing the alkoxy -terminated carbosiloxane as well.

[0016] Combining in step 4) may be performed by any convenient means in any convenient equipment, such as mixing in a reactor with mixing means such as baffles and / or an agitator. The reactor may have heating and / or cooling means to control temperature of the reaction mixture inside the reactor. The same reactor used in the method for step 1) and / or step 2) may be used for step 4). Alternatively, a different reactor may be used. The starting materials may be combined in any order, such as by mixing starting materials comprising E) the alkenyl-terminated carbosiloxane prepared as described above and F) the SiH functional oligomer andthereafter adding G) the hydrosilylation reaction catalyst, which may optionally be delivered in H) the solvent. Alternatively, to control the exotherm generated by the hydrosilylation reaction, one of E) the alkenyl-terminated carbosiloxane and F) the SiH functional oligomer (reactants) may be placed in the reactor, and the other reactant may be metered into the reactor continuously or intermittently to control reaction rate and exotherm. The hydrosilylation reaction catalyst may be metered into the reactor separately or may be combined with E) the alkenyl-terminated carbosiloxane. However, to minimize potential for side reactions, G) the hydrosilylation reaction catalyst and F) the SiH functional oligomer may be kept separate until just prior to starting the hydrosilylation reaction. One skilled in the art would recognize that in step 4), either the reaction product prepared in step 2) of the method described above, or E) the alkenyl-terminated carbosiloxane recovered in step 3) (when step 3) is present), may be used to deliver the alkenyl-terminated carbosiloxane. For example, when step 3) is absent the reaction product prepared in step 2), which comprises E) the alkenyl-terminated carbosiloxane and other components, described above, may be used as the starting material in step 4).

[0017] Starting material F) is an SiH functional siloxane oligomer. The SiH moiety of starting material F) may react with the alkenyl group in the alkenyl-terminated carbosiloxane prepared as described above via hydrosilylation reaction catalyzed with G) the hydrosilylation reaction catalyst. The SiH functional siloxane oligomer may have formula:, wherein each R is an independently selected alkyl group of 1 to 10 carbon atoms, and D1is an alkylene group of 2 to 8 carbon atoms. Suitable alkyl groups for R1may have 1 to 10 carbon atoms and are exemplified by methyl, ethyl, propyl (including n-propyl and isopropyl), butyl (including n-butyl, isobutyl, tert-butyl and sec-butyl); and pentyl, heptyl, octyl, nonyl, and decyl groups, as well as branched isomers with 5 to 10 carbon atoms. Alternatively, each R1may be independently selected from the group consisting of methyl, ethyl, propyl, and butyl; alternatively methyl and ethyl, and alternatively each R1may be methyl. D1is an alkylene group that may have 2 to 8, alternatively 2 to 6 carbon atoms. D1may have empirical formula (CXH2X), wherein subscript x is 2 to 6. Alternatively, D1may have an empirical formula selected from the group consisting of (C2H4), (C3H6), and (C6H12); alternatively (C2H4). D1may be linear or branched, alternatively a combination of linear and branched isomers. The SiH functional siloxane oligomer may be a mixture of isomers wherein some have D1being linear and some have D1being branched. For example, when D1has two1 carbon atoms in the formula shown above D1comprisesin a molar ratio of linear (n) to branched (i) isomers of 65:35 to 95:5 (the (n):(i) ratio).Alternatively, the (n):(i) ratio may be 90:10 to 95:5. The SiH functional oligomer of the formula shown above may be prepared, for example, as described in US Patents 10968317, 11098163, and 11492448; and the references cited therein.

[0018] Amounts of starting materials E) and F) may be selected by one skilled in the art, and for example, starting materials E) and F) may be used in amounts sufficient to provide a 1:1 molar ratio of E):F). Alternatively, starting materials E) and F) may be used in a molar ratio ranging from 1:0.1 to 1:100 E):F).

[0019] Starting material G) is a hydrosilylation reaction catalyst. Suitable hydrosilylation reaction catalysts are known in the art and are commercially available. Said catalyst comprises a platinum group metal. The platinum group metal may be selected from the group consisting of platinum, rhodium, ruthenium, palladium, osmium, and iridium. Alternatively, the platinum group metal may be platinum. The hydrosilylation reaction catalyst may be the platinum group metal or a compound or complex of the platinum group metal. For example, the hydrosilylation reaction catalyst may be a compound such as chloridotris(triphenylphosphane)rhodium(I) (Wilkinson’s Catalyst), a rhodium diphosphine chelate such as [1,2-bis(diphenylphosphino)ethane]dichlorodirhodium or [1,2-bis(diethylphospino)ethane]dichlorodirhodium, chloroplatinic acid (Speier’s Catalyst), chloroplatinic acid hexahydrate, platinum dichloride, or a complex of such a compound with an organopolysiloxane such as l,3-diethenyl-l,l,3,3-tetramethyldisiloxane complexes with platinum (Karstedt’s Catalyst) or Pt(0) complex intetramethyltetravinylcyclotetrasiloxane (Ashby’s Catalyst). Alternatively, the compound or complex may be microencapsulated in a matrix or coreshell type structure. Hydrosilylation reaction catalysts are known in the art, for example, as described in US Patent 12195593 and the references cited therein. Hydrosilylation reaction catalysts are commercially available, for example, SYL-OFF™ 4000 Catalyst and SYL-OFF™ 2700 are available from Dow Silicones Coiporation of Midland, Michigan, USA. The amount of hydrosilylation reaction catalyst may be selected by one skilled in the art and may be, for example, 1 ppm to 1000 ppm, based on combined weights of starting materials E) and F), alternatively 5 ppm to 100 ppm.

[0020] Starting material I) is the hydrosilylation reaction inhibitor introduced above. The hydrosilylation reaction inhibitor may be for example, an acetylenic alcohol such as methylbutynol or ethynyl cyclohexanol, a silylated acetylenic alcohol, an unsaturated hydrocarbon diester; a conjugated ene-yne, an olefinic siloxane, a maleate, a fumarate, or a combination thereof. The amount of inhibitor may be an amount effective to control hydrosilylation reaction rate because hydrosilylation reaction is exothermic. The amount of inhibitor selected depends on various factors including the type and amount of hydrosilylation reaction catalyst and inhibitor selected. Suitable hydrosilylation reaction inhibitors are known in the art and are described, for example, described as ingredient i) in US Patent 9593209 at col. 15, line 35 to col.16, line 17.

[0021] Alternatively, starting material I) the hydrosilylation reaction inhibitor may be a thiuram disulfide compound (thiuram disulfide). Without wishing to be bound by theory, it is thought that the thiuram disulfide will complex with the platinum from G) the hydrosilylation reaction catalyst (when a platinum catalyst is used) to form an inhibited platinum at temperatures of 120 °C and lower, alternatively 100 °C and lower, alternatively 80 °C and lower, such that the inhibited platinum does not catalyze a hydrosilylation reaction, and such that side reactions such as gelation of F) the SiH functional oligomer and / or the hydrosilylation reaction product are minimized or avoided during recovery (e.g., in step 5), storage, or both. The thiuram disulfidemay have formulaI- 1 ), wherein RH, RN, RJ, and RKare each an independently selected monovalent hydrocarbyl group having 1 to 20 carbon atoms, which may be saturated or unsaturated; a heteroatom-containing monovalent hydrocarbyl group having 1 to 20 carbon atoms, which may be saturated or unsaturated; or combinations thereof. Suitable heteroatoms may include, for example, an oxygen atom. RHand RNgroups may combine to form one or more carbocyclic groups having 4 to 20 carbon atoms. RJand RKgroups may combine to form one or more carbocyclic groups having 4 to 20 carbon atoms.

[0022] In formula 1-1), RH, RN, RJ, and RKcan be the same or different, and alternatively, these groups may be the same. Alternatively, RH, RN, RJ, and RKmay be each independently selected from an alkyl group having 1 to 20 carbon atoms, alternatively 1 to 12, alternatively 1 to 6, alternatively 1 to 4, or alternatively 1 to 2 carbon atoms; an aromatic group having 6 to 20 carbon atoms, such as phenyl or benzyl; or combinations thereof. Alternatively, RH, RN, RJ, and RKare each independently selected alkyl groups. Alternatively, RH, RN, RJ, and RKare each independently selected from methyl, iso-butyl, n-butyl, or combinations thereof.

[0023] Specific examples of suitable thiuram disulfides include tetrabenzylthiuram disulfide (with CAS No. 10591-85-2), tetramethylthiuram disulfide (with CAS No. 137-26-8),tetraethylthiuram disulfide (with CAS No. 97-77-8), tetra(iso-propyl)thiuram disulfide, tetra(iso-butyl)thiuram disulfide (with CAS No. 3064-73-1), and tetra(n-butyl)thiuram disulfide (with CAS No. 1634-02-2), all of which are commercially available from various sources such as Sigma- Aldrich, Inc., TCI America, Fischer Scientific, or Cymit Quimica S.L. Alternatively, the thiuram disulfide may be selected from tetramethylthiuram disulfide, tetra(n-butyl)thiuram disulfide, or mixtures thereof.

[0024] The thiuram disulfide may be optionally diluted in a solvent before use in the method. The solvent may be any material that can dissolve the thiuram disulfide, as described and exemplified above for starting material H). Alternatively, the solvent for the thiuram disulfide may be selected from aromatic hydrocarbons such as benzene, halogenated hydrocarbons, ethers, or mixtures thereof. Without wishing to be bound by theory, it is thought that it may be desirable to use as little solvent as possible to facilitate dissolving the thiuram disulfide and, if desired, to later remove the solvent, e.g., by evaporation, distillation, and / or stripping. Examples of suitable solvents may include halogenated hydrocarbons such as dichloromethane, chloroform (CHCh), and / or tetrachloromethane. The solvent may be used in an amount of 0.1% to 5% by weight based on the weight of the thiuram disulfide.

[0025] The thiuram disulfide compound may be added in an amount such that the molar ratio of the thiuram disulfide to platinum in G) the hydrosilylation reaction catalyst ( I / Pt ratio) may range from 0.9 to 100. Alternatively, this molar ratio may be 1 or higher, alternatively greater than 1, alternatively 1.1 or higher, and alternatively 1.2 or higher, alternatively 2 or higher, alternatively 3 or higher, alternatively 4 or higher, alternatively 5 or higher, alternatively 6 or higher, alternatively 7 or higher, alternatively 8 or higher, alternatively 9 or higher; while at the same time this ratio may be 100 or lower, alternatively 75 or lower, alternatively 50 or lower, alternatively 40 or lower, alternatively 30 or lower, alternatively 20 or lower, alternatively 10 or lower, alternatively 5 or lower, alternatively 3 or lower, alternatively 2 or lower, and alternatively 1.2 or lower. Alternatively, this I / Pt ratio may be 1 to 10, alternatively 1 to 5, alternatively 2 to 5, alternatively 2 to 3.5, alternatively 1 to 2, and alternatively, 1 to 1.2.Alternatively, at low platinum concentration (e.g., > 0 ppm to 5 ppm based on combined weights of starting materials E), F), and G) described above), the I / Pt ratio may be 3 to 3.5, and this may allow for higher recovery (e.g., stripping) temperatures. Without wishing to be bound by theory, it is thought that the Pt-thiuram complex is stable at temperatures below 120 °C, alternatively 115 °C or below, and alternatively 110 °C or below. Therefore, stripping under conditions of 95 °C at 0 - 3 mbar wherein the Pt-Thiuram complex is stable can be performed while gelation is avoided or minimized.

[0026] Step 4) prepares a hydrosilylation reaction product comprising the alkoxy -terminated carbosiloxane. The hydrosilylation reaction product further comprises residual hydrosilylation reaction catalyst and optionally an additional component, such as an unreacted reactant (when E)or F) is used in molar excess and H) a solvent, when used). The method may optionally further comprise one or more additional steps, such as 5) recovering the alkoxy-terminated carbosiloxane. Recovering may be performed by any convenient means such as stripping or distillation with heating and optionally reduced pressure.

[0027] The alkoxy-terminated carbosiloxane has formula:wherein R, R3, D1, R1and subscript n are as described and exemplified above. D2is an alkylene group formed via hydrosilylation reaction of SiH moiety of F) the siloxane oligomer and R2, the alkenyl group in E) the alkenyl-terminated carbosiloxane. D2may have 2 to 8, alternatively 2 to 6 carbon atoms. D2may have an empirical formula selected from the group consisting of (C2H4), (C3H6), and (C6H12); alternatively (C2H4). D2may be linear or branched, alternatively linear.EXAMPLES

[0028] The following examples are provided to illustrate the invention to one skilled in the art and are not to be construed so as to limit the scope of the invention set forth in the claims. The starting materials used in these examples are summarized below in Table 1.Table 1 - Starting Materials

[0029] In this Synthesis Example 1, a.-Si-TMS / oj-Vi polyethylenedimethylsiloxane (TMS-PEDS-Vi) samples were synthesized as follows: The reaction was performed in a glovebox under inert atmosphere. To a 100 mL round-bottom flask equipped with a magnetic stir bar, was added sodium trimethylsilanolate (various quantities, see Table 2), followed by 2, 2,5,5-tetramethyl-2,5-disila-l -oxacyclopentane (25 g, 155.9 mmol, 1.0 equiv.). THF (10 mL) was added in one portion to start the reaction. The reaction mixture was stirred at 600 RPM (ensuring that the stirring was vigorous and homogeneous) at room temperature for 2 h. Upon complete consumption of 2,2,5,5-tetramethyl-2,5-disila-l-oxacyclopentane, the reaction mixture was quenched with the dimethylvinylchlorosilane (various quantities, see Table 2) and stirred at room temperature overnight. The reaction mixture was then diluted in hexanes to precipitate out the salt and centrifuged. The resulting liquid phase was collected. This step was repeated until the solution was clear. In case of subscript n <10, a significant amount of salt was generated. Alternatively, the solution was washed with water twice, dried over N 2SCU and concentrated in vacuo (200 mbars) at 40 °C to afford a clear colorless oil with 100% conversion (as determinedby1H NMR) and > 99% purity. A 1 :1 molar ratio of initiator / terminator led to up to 30% of a silanol containing impurity. An excess of terminator allowed this reaction to reach 100% pure a-trimethylsiloxy-, y-vinyl- terminated poly(ethylenedimethylsiloxane) (TMS-PEDS-Vi) withvalues for subscript n shown below in Table 2 were prepared.Table 2: Molar ratio and quantities of initiator / terminator

[0030] In this Synthesis Example 2, additional samples of (TMS-PEDS- Vi) were prepared as described in Synthesis Example 1. Changes to the procedure of Synthesis Example 1 are noted in Table 3, below. The samples were prepared in THF eluent at a concentration of 0.5 mg / mL polymer. The solution was shaken on a flat-bed shaker at ambient temperature for approximately 2 hours. The solution was filter through a 0.45 pm PTFE syringe filter prior to injection. SEC was performed on a Waters 2695 LC pump and autosampler. The flow rate was set at 1 mL / min, and the injection volume was set at 100 pL of solution. SEC separation was carried out on 2 Agilent Plgel Mixed-C columns held at 35 °C. The detector was a Shodex RI-501 differential refractive index detector held at 35 °C.

[0031] Data analysis was performed using an in-house package written in the R programming language and accessed with a Shiny application deployed using RStudio Connect. The application is hosted on Posit Connect, and the code can be accessed at the dedicated Azure DevOps repository.

[0032] A total of 16 PS linear narrow molecular weight standards from Agilent having Mp values from 3.750 to 0.58 kg / mol were used for molecular weight calibration. A 3rd order polynomial was used for calibration curve fitting. Thus, all molecular weight averages, distributions and references to molecular weight provided in this report are PS equivalent values.

[0033] Samples 2-1, 2-2 and 2-3 differ by their n value or processing time. While the composition and process of samples 2-2 and 2-3 were the same, samples 2-1 and 2-2 were quenched after 1 h while sample 2-3 was quenched after 24 h. No significant variation in molecular weights and polydispersities were observed, confirming the robustness of the method for making alkenyl-terminated carbosiloxanes of this invention. Additionally, using lithium trimethylsilanolate (to prepare sample 2-4 instead of sodium trimethylsilanolate led to higher MW, but the sample still had low polydispersity, which indicated formation of the (mono) alkenyl-terminated carbosiloxane. Without wishing to be bound by theory, it is thought that, sodium trimethylsilanolate was more soluble and led to improved molecular weights and polydispersities in samples 2-1, 2-2, and 2-3. The sample made with potassium trimethylsilanolate (2-5) instead of sodium trimethylsilanolate had both higher dispersity and higher MW, which suggested a side reaction occurred. Finally, trimethylsilanol + 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) as abase was investigated (sample 2-6) as initiator, and this led to a sample with high poly dispersity (> 1.3) and a side reaction. The results are shown below in Table 3Table 3 - Molecular Weight and Polydispersity of Samples prepared in Synthesis Example 2

[0034] In this Synthesis Example 3, additional samples of (TMS-PEDS-Vi) were prepared as described in Synthesis Example 1 using sodium trimethylsilanolate as initiator. These are summarized below in Table 4, and their properties were measured as follows:Brookfield Viscosity Measurement:

[0035] Viscosity measurements were performed using a Brookfield Helipath with a T-C spindle, at 150 rpm and RT. Viscosity measurements were recorded at consistent time intervals of 4 seconds, with each testing run lasting a total of 54 seconds, resulting in 14 data points per trial. An average viscosity was calculated from these multiple measurements, ensuring reliability in the data.Refractive Index Measurement:

[0036] The refractive index (RI) samples was determined using a Bausch & Lomb refractometer (Model No. 33-45-58, Serial No. 3) to assess optical properties and confirm consistency across different formulations. Isopropyl alcohol (IP A) was used as a reference standard to validate the instrument’s accuracy, with its measured RI closely matching the literature value of 1.3772 at 20 °C.

[0037] Each sample’s refractive index was measured once. For each measurement, two drops of the sample were placed onto the refractometer’s measuring prism, ensuring even coverage of the surface to minimize inconsistencies. The instrument’s adjustment knobs were used to align the boundary line precisely within the field of view, allowing for an accurate determination of the refractive index. To prevent cross-contamination, the prism surface was thoroughly cleaned between each sample measurement and before initial use. All measurements were conducted under controlled conditions at a temperature of 24.7 °C.Tg: Differential Scanning Calorimetry (DSC):

[0038] The glass transition temperature (Tg) of samples was assessed using a TA Instruments DSC Q2000, following a standard thermal analysis protocol. Testing employed a helium purge and a low pan mass to minimize thermal lag. All samples were thoroughly dried prior to analysis to remove any residual solvent that could impact the Tg measurement. The temperature ramp was set from -170 °C to 100 °C at a rate of 20 °C / min.Table 4: property / performance table.

[0039] In Table 4, the performance target for RI was > 1.41; higher RI is preferred.

[0040] In Table 4, PDMS 100 cst was XIAMETER™ PMX-200 fluid 100 cSt, a bis-trimethylsiloxy -terminated polydimethylsiloxane, evaluated for comparison with the TMS PEDS-Vi carbosiloxanes of the present invention. The samples of the present invention had higher RI, higher Tg, and higher viscosities than TMS-PDMS-TMS comparative sample with comparable DP.Compatibility

[0041] To test the compatibility with mineral oil, 1 mL of either TMS-PEDS-Vi or TMS-PDMS-TMS was added to a vial. 1 mL of mineral oil was added. The resulting mixture was stirred at RT with a stir bar at 1,000 RPM for 1 min. A visual assessment at t=0 and after 24 h was performed to determine whether the samples were compatible or not. Compatible (C) materials lead to a single clear phase, while incompatible (I) materials lead to a biphasic system. Table 5 - Compatibility assessment of TMS-PEDS-Vi vs. PDMS with mineral oil in 1:1 ratio(C = compatible; I = incompatible)

[0042] The data in Table 5 show that the alkenyl-terminated carbosiloxane of this invention had better compatibility with an organic (mineral oil) than the trimethylsiloxy-terminated poly dimethylsiloxanes .

[0043] In this Synthesis Example 5, polydispersity was studied by varying reaction conditions. The methods used are summarized below in Table 6. TMSONa refers to sodium trimethylsilanolate, TDOP refers to the monomer shown above in Table 1, CDMVS refers to Dimethylvinylchlorosilane, and IPA refers to isopropanol.Table 6. Development of polymerization methods to achieve narrow poly dispersity (PD) in a-tri methylsi ly 1-co-vi ny 1 PEDS.

[0044] In Table 6, “Equiv.” means Equivalent, and the methods have the following descriptions.Method A. Polymerization Targeting DP 15Method B. Initiation Solvation PolymerizationMethod C. Acid-Base Equilibrium Investigation using CaCO3Method D. Control (Method A Protocol)Method E. Kinetic Control of Dispersity via Dropwise TDOP AdditionMethod F. Dispersity Evolution During Extended Reaction Time

[0045] Bolded steps indicate deviations from the synthesis examples above. Reaction duration (h) in the sixth column is defined as the time elapsed from the point when TMSONa, TDOP, and THF were combined to the subsequent addition of CDMVS.

[0046] Method B Initiation Solvation Polymerization in Table 6 was performed as follows: To minimize residual water content, TDOP was dried over activated molecular sieves added directly to the monomer bottle three days prior to reaction and permanently retained within the monomer storage container. TDOP (10 g, 62.4 mmol, 40 equiv.) was polymerized using TMSONa (0.175 g, 1.56 mmol, 1.0 equiv.) in 25 mL of anhydrous THF. TMSONa was stirred in THF for ~8 minutes until fully suspended, followed by instantaneous TDOP addition and a 5 mL THF rinse of the flask to ensure complete transfer. The reaction mixture was stirred for 4 hours before termination by addition of CDMVS (0.282 g, 2.03 mmol, 1.5 equiv.). This yielded a DP ~ 35 with a narrower molecular weight distribution (PD = 1.5) compared to earlier trials at similar DP (n = 30 to 36), which exhibited broader polydispersities (PD = 1.8).TMS-PEDS-Vinyl

[0047] Method C Acid-Base Equilibration using CaCCE shown in Table 6 was performed as follows: TDOP (2 g, 12.5mmol, 15 equiv) was polymerized using TMSONa (0.0933 g, 0.831 mmol, 1.0 equiv) as the initiator in anhydrous THF (5.00 mL). Upon confirming complete monomer consumption by 'H NMR after 4 hours, CDMVS (0.1003 g, 0.831 mmol, 1.0 equiv) was added to quench the reaction. At the same DP, the copolymer prepared by this Method C exhibited a lower dispersity (PD = 1.4) than the copolymer prepared by Method A (with PD = 1.6). Quenching traces of dimethylvinylchlorosilane with CaCCE showed an improved (lowered) polydispersity relative to a control (quenched with IPA instead of CaCOa), as described in methods A and D in Table 6.

[0048] Methods E and F, Kinetic Control of Dispersity via Dropwise TDOP Addition wereperformed as follows: Previous synthesis examples primarily utilized either instantaneous monomer addition, without examining the effects of continuous dropwise addition. To evaluate the effect of monomer dropwise addition, reactions were conducted with periodic monitoring of dispersity (PD) by size exclusion chromatography (SEC). TDOP (4 g, 24.9 mmol, 15 equiv,) was polymerized using a suspension of TMSONa (0.186 g, 1.66 mmol, 1.0 equiv) as the initiator in anhydrous THF (10.00 mL). The initiator suspension was stirred for 10 minutes prior to TDOP addition. TDOP was added dropwise to the initiator mixture under stirring at RT.Aliquots were withdrawn at 1, 2, and 3 hours to monitor dispersity (PD) evolution by SEC. Upon confirming complete monomer consumption by1H NMR after 3 hours, the polymerization was terminated by addition of CDMVS (0.20 g, 1.66 mmol, 1.0 equiv.), followed by neutralization with CaCCh.

[0049] A steady decrease in polydispersity with time was observed, from PD = 1.35 at 1 hour to PD = 1.2 after 3 hours of reaction. Without wishing to be bound by theory, it is thought that narrowing of molecular weight distribution suggested that copolymer chain growth became more uniform as the reaction proceeded, likely due to improved monomer consumption kinetics and minimized localized heating under the dropwise addition conditions.

[0050] In this Synthesis Example A, a-Si-TMS / co-Vi polyethylenedimethylsiloxane was synthesized as follows: The reaction was performed in a glovebox under inert atmosphere. To a 100 mL round-bottom flask equipped with a magnetic stir bar, was added sodium trimethylsilanolate (0.47g, 4.16 mmol, 1.0 eq), followed by 2,2,5,5-tetramethyl-2,5-disila-l-oxacyclopentane (10g, 62.4 mmol, 15 eq). THF (10 mL) was added in one portion to start the reaction. The reaction mixture was stirred at 600 RPM (ensuring that the stirring was vigorous and homogeneous) at RT for 2 h. Upon complete consumption of 2,2,5,5-tetramethyl-2,5-disila-1 -oxacyclopentane, the reaction mixture was quenched with the dimethylvinylchlorosilane (1.18g, 9.75 mmol, 1.5 eq) and stirred at RT overnight. The resulting product was then diluted in toluene to precipitate out the salts and centrifuged. The clear liquid phase was collected. This step was repeated until the resulting solution was clear. The solution was concentrated in vacuo (10 mbars) at 50 °C to afford a clear colorless oil with 100% conversion (as determined by1H NMR) and > 99% purity. The reaction scheme is shown below.sodium trimethylsilanolateCH, CH,rH2,2,5 ,5 -tetramethyl-2.5 -disila- 1 -oxacyclopentane chlorodimethyl(vinyl)silanewherein subscript n was 13.

[0051] In this Synthesis Example B, a-Si-TMS / oj-OMes polyethylenedimethylsiloxane was synthesized as follows: To a 40 ml dram vial was added L-ETM (0.50 g, 1.77 mmol, 1.0 eq) and a-Si-TMS / w-Vi poly(ethylenedimethylsiloxane) (4.45 g, 1.80mol, 1.0 eq) prepared as described above in Synthesis Example A. The components were stirred at 250 RPM using a magnetic stir bar then heated to 70 °C. A N2 purge was supplied to the sample using a septum sealed cap. Once at temperature, a solution of platinum hydrosilylation reaction catalyst (Pt) in toluene (1.72 pL or 5 ppm) was added, and the sample was allowed to exotherm. The reaction ran for 3 hours then was stopped and sealed. The following day, an additional 1.5 ppm of Pt was added and allowed to react for 3 hours for a total of 6 hours.NMR was used to confirm formation of the alkoxy -terminated carbosiloxane, which had the formula shown in the scheme below, wherein subscript n was an integer with a value of 13; and D1was the group as described above in Table 1 for the L-ETM starting material.wherein n was 13. and each D1was independently selected from the group consisting ofmolar ratio of 90:10 to 95:5.Industrial Applicability

[0052] The examples above show that the alkenyl-terminated carbosiloxane may be prepared with a low polydispersity, i.e., polydispersity < 1.3 using the method described herein. The alkenyl-terminated carbosiloxane of this invention may be useful as an intermediate for further reaction to prepare the alkoxy-terminated carbosiloxane of this invention according to the method described herein. The alkoxy-terminated carbosiloxane may be used as a surface treating agent for, e.g., anti-fingerprint coatings.Definitions and Usage of Terms

[0053] All amounts, ratios, and percentages are by weight unless otherwise indicated. The amounts of all starting materials in a composition total 100% by weight. The SUMMARY and ABSTRACT are hereby incorporated by reference. The articles ‘a’, ‘an’, and ‘the’ each refer to one or more, unless otherwise indicated by the context of specification. The singular includes the plural unless otherwise indicated. The disclosure of ranges includes the range itself and also anything subsumed therein, as well as endpoints. Similarly, the disclosure of Markush groups includes the entire group and also any individual members and subgroups subsumed therein.

[0054] The halogen atoms described herein may be selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br), iodine (I), and a combination of two or more thereof. Alternatively, the halogen atom may be selected from Br, Cl, or F. Alternatively, the halogen atom may be selected from Cl or Br. Alternatively, the halogen atom may be Cl.

[0055] Hydrocarbyl groups may independently be linear, branched, cyclic, or combinations thereof. Cyclic hydrocarbyl groups encompass aryl groups as well as saturated or nonconjugated cyclic groups. Cyclic hydrocarbyl groups may be monocyclic or polycyclic. Linear and branched hydrocarbyl groups may independently be saturated or unsaturated. One example of a combination of a linear and cyclic hydrocarbyl group is an alkyl substituted aryl group. By “substituted,” it is meant that one or more hydrogen atoms may be replaced with atoms other than hydrogen (e.g., a halogen atom, such as Cl, Br, F, or I) or groups other than hydrogen. Suitable alkyl groups are exemplified by, but not limited to, methyl, ethyl, propyl e.g., isopropyl and / or n-propyl), butyl e.g., isobutyl, n-butyl, tert-butyl, and / or sec-butyl), pentyl (e.g., isopentyl, neopentyl, and / or tert-pentyl), hexyl, as well as branched saturated hydrocarbon groups of 6 carbon atoms. Suitable aryl groups are exemplified by, but not limited to, phenyl, tolyl, xylyl, naphthyl, benzyl, 1 -phenylethyl, 2-phenylethyl, and dimethylphenyl. Suitable alkenyl groups include vinyl, allyl, propenyl, isopropenyl, butenyl, isobutenyl, pentenyl, heptenyl, hexenyl, and cyclohexenyl groups. Suitable monovalent halogenated hydrocarbon groups include, but are not limited to, a halogenated aryl group of 6 to 10 carbon atoms. Suitable halogenated aryl groups are exemplified by, but not limited to, the aryl groups described above where one or more hydrogen atoms is replaced with a halogen atom, such as F or Cl. For example, chloroaryl and fluoroaryl are suitable halogenated aryl groups.

[0056] Abbreviations used in the specification have the definitions in Table A, below.Table A - AbbreviationsEmbodiments of the Invention

[0057] In a first embodiment, a carbosiloxane has formula, wherein subscript n is an integer with a value of 2 to 1,000, R is methyl or phenyl, and R4is selected from the group consisting of, wherein each R3is an independently selected monovalent hydrocarbyl group free of aliphatic unsaturation, R2is an alkenyl group, D2is an alkylene group with 2 to 8 carbon atoms, D1is an alkylene group with 2 to 8 carbon atoms, and each R1is an independently selected alkyl group of 1 to 10 carbon atoms.

[0058] In a second embodiment, in the carbosiloxane of the first embodiment each R3is methyl, R2is vinyl, R4is an alkenyl-functional organosilicon moiety of formula, and the carbosiloxane is an alkenyl-terminated carbosiloxane of formulainteger with a value of 5 to 36.

[0059] In a third embodiment, a method for making the alkenyl-terminated carbosiloxane of the second embodiment comprises:1) combining, under conditions to effect ring opening polymerization reaction, starting materials comprising:A) 2,2,5,5-tetramethyl-2,5-disila-l -oxacyclopentane;B) a metal silanolate selected from the group consisting of sodium trimethylsilanolate and lithium trimethylsilanolate; andC) a polar aprotic solvent; thereby forming a ring opening polymerizationreaction product; and2) combining, under conditions to effect a reaction to terminate the ring opening polymerization reaction of step 1), starting materials comprising:the ring opening polymerization reaction product, andD) vinyldimethylchlorosilane; and3) recovering the alkenyl-terminated carbosiloxane from the reaction product of step 2).

[0060] In a fourth embodiment, in the method of the third embodiment, B) the metal silanolate is sodium trimethylsilanolate, and the alkenyl-terminated carbosiloxane has a polydispersity of I to 1.3.

[0061] In a fifth embodiment, in the carbosiloxane of the first embodiment, each R3is methyl, R is methyl, and R4is an alkoxy-functional organosilicon moiety of formulathe carbosiloxane is an alkoxyterminated carbosiloxane of formula:wherein subscript n is an integer with a value of 5 to 36, and D1has empirical formula (C2H4).

[0062] In a sixth embodiment, the alkoxy -terminated carbosiloxane of the fifth embodiment is1 a mixture of isomers, wherein D comprisesmolar ratio of 90:10 to 95:5.

[0063] In a seventh embodiment, a method for making the alkoxy-terminated carbosiloxane of the fifth embodiment or the sixth embodiment comprises:1) combining, under conditions to effect ring opening polymerization reaction, starting materials comprising:A) 2,2,5,5-tetramethyl-2,5-disila-l -oxacyclopentane;B) a metal silanolate selected from the group consisting of sodiumtrimethylsilanolate and lithium trimethylsilanolate; andC) a polar aprotic solvent; thereby forming a ring opening polymerization reaction product; and2) combining, under conditions to effect a reaction to terminate the ring opening polymerization reaction of step 1), starting materials comprising:the ring opening polymerization reaction product, andD) vinyldimethylchlorosilane; thereby preparing a reaction product comprising an alkenyl-terminated carbosiloxane; and3) recovering the alkenyl-terminated carbosiloxane from the reaction product of step 2); 4) combining, under conditions to effect hydrosilylation reaction, starting materials comprising:E) the alkenyl-terminated carbosiloxane;F) an SiH functional oligomer of formula, wherein R1and D1are as described above; andG) a hydrosilylation reaction catalyst.

[0064] In an eighth embodiment, in the method of the seventh embodiment, B) the metal silanolate is sodium trimethyl silanolate.

[0065] In a ninth embodiment, in the method of the seventh embodiment or the eighth embodiment, the starting materials in step 4) further comprise a hydrosilylation reaction inhibitor.

[0066] In a tenth embodiment, in the method of the ninth embodiment, the hydrosilylation reaction catalyst comprises platinum, and the hydrosilylation reaction inhibitor comprises a thiuram disulfide.

[0067] In an eleventh embodiment, a composition comprises:the alkoxy-terminated carbosiloxane of the fifth embodiment or the sixth embodiment, and a thiuram disulfide.

Claims

CLAIMS:

1. An alkenyl-terminated carbosiloxane of formula:subscript n is an integer with a value of 2 to 1,000;R is methyl or phenyl;R2is an alkenyl group; andeach R3is an independently selected monovalent hydrocarbyl group free of aliphatic unsaturation.

2. The alkenyl-terminated carbosiloxane of claim 1, wherein R is methyl, R2is an alkenyl group of 2 to 6 carbon atoms, and each R3is an alkyl group of 1 to 10 carbon atoms.

3. The alkenyl-terminated carbosiloxane of claim 1 or claim 2, wherein R is methyl, R2is vinyl, and each R3is methyl.

4. A method for making the alkenyl-terminated carbosiloxane of any one of claims 1 to 3, wherein the method comprises:1) combining, under conditions to effect ring opening polymerization reaction, starting materials comprising:A) 2, 2, 5, 5-tetramethyl-2,5-disila-l -oxacyclopentane;B) a metal silanolate of formula:, wherein the metal, M+, of the metal silanolate is selected from the group consisting of lithium and sodium, and R is methyl or phenyl; andC) a polar aprotic solvent; thereby forming a ring opening polymerization reaction product; and2) combining, under conditions to effect a reaction to terminate the ring opening polymerization reaction of step 1), starting materials comprising:the ring opening polymerization reaction product, andD) an alkenyl-functional halosilane of formula (R2)(R3)2SiX, wherein X is a halogen, each R3is the independently selected monovalent hydrocarbyl group free of aliphatic unsaturation, and R2is the alkenyl group; wherein a molar ratio of D) the alkenyl-functional halosilane to B) the metal silanolate is > 1, thereby preparing a reaction product; andoptionally 3) recovering the alkenyl-terminated carbosiloxane from the reaction product of step 2).

5. The method of claim 4, wherein B) the metal silanolate is sodium trimethyl silanolate.

6. The method of claim 4 or claim 5, wherein R is methyl, R2is vinyl, and each R3is methyl.

7. The method of claim 6, wherein D) the alkenyl-functional halosilane is vinyldimethylchlorosilane.

8. An alkoxy-terminated carbosiloxane comprising formula:whereinsubscript n is an integer with a value of 2 to 1,000;R is methyl or phenyl;each R3is an independently selected monovalent hydrocarbyl group free of aliphatic unsaturation;D2is an alkylene group of 2 to 8 carbon atoms;D1is an alkylene group of 2 to 8 carbon atoms; andeach R1is an independently selected alkyl group of 1 to 10 carbon atoms.

9. The alkoxy-terminated carbosiloxane of claim 8, whereinR is methyl,D1has empirical formula (C2H4),D2has empirical formula (C2H4),each R1is methyl, andeach R3is methyl.

10. The alkoxy -terminated carbosiloxane of claim 9, wherein the alkoxy-terminated1 carbosiloxane comprises a mixture of isomers, and D1comprisesmolar ratio of 65:35 to 95:5.

11. A method for preparing the alkoxy -terminated carbosiloxane of any one of claims 8 to 10, wherein the method comprises:1) combining, under conditions to effect ring opening polymerization, starting materials comprising:A) 2, 2, 5, 5-tetramethyl-2,5-disila-l -oxacyclopentane;B) a metal silanolate of formula:, wherein the metal, M+, of the metal silanolate is selected from the group consisting of lithium and sodium, and R is methyl or phenyl; andC) a polar aprotic solvent, thereby forming a ring opening polymerization reaction product; and2) combining, under conditions to effect a reaction to terminate the ring opening polymerization of step 1), starting materials comprising:the ring opening polymerization reaction product, andD) an alkenyl-functional halosilane of formula (R2)(R3)2SiX, wherein X is a halogen, each R3is an independently selected monovalent hydrocarbyl group free of aliphatic unsaturation, and R2is an alkenyl group, wherein a molar ratio of D) the alkenyl-terminated halosilane to B) the metal silanolate is > 1, thereby preparing a reaction product comprising an alkenyl-terminated carbosiloxane; andoptionally 3) recovering the alkenyl-terminated carbosiloxane from the reaction productof step 2); and4) combining, under conditions to effect hydrosilylation reaction, starting materials comprising:E) the alkenyl-terminated carbosiloxane;F) an SiH functional oligomer of formulawherein R1and D1are as described above; andG) a hydrosilylation reaction catalyst.

12. The method of claim 11, wherein B) the metal silanolate is sodium trimethyl silanolate.

13. The method of claim 11 or claim 12, whereinR is methyl,R2is an alkenyl group of 2 to 6 carbon atoms,each R3is an alkyl group of 1 to 10 carbon atoms,14. The method of any one of claims 11 to 13, whereinR is methyl,R2is vinyl,each R3is methyl,X is Cl,each R1is methyl, andeach D1has empirical formula (C2H4).

15. The method of claim 14, wherein the alkoxy-terminated carbosiloxane comprises amixture of isomers wherein D1comprisesmolar ratio of 65:35 to 95:5.