Method of preparing sputtered thin-film insulators with substrate bias
Applying a negative bias voltage during the sputtering process inhibits negatively charged species and enhances etching, resulting in high-quality thin-film insulators with improved breakdown voltage and uniformity.
Patent Information
- Application Number
- PCT/US2026/025899
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-29
- Publication Date
- 2026-11-12
AI Technical Summary
Achieving high-quality thin-film insulators is challenging due to difficulties in preventing negatively charged species from embedding in the film, leading to low-voltage dielectric breakdown and non-uniform composition.
Applying a negative bias voltage to the substrate during the sputtering process to inhibit negatively charged species from reaching the substrate and enhance etching, allowing for higher reactive gas flow rates and improved film quality.
This method results in a substantial reduction of failure events associated with low-voltage dielectric breakdown, enabling higher breakdown voltages and more uniform thin-film insulators with enhanced electrical quality.
Smart Images

Figure US2026025899_12112026_PF_FP_ABST
Abstract
Description
[0001] METHOD OF PREPARING SPUTTERED THIN-FILM INSULATORS WITH SUBSTRATE BIAS
[0002] BACKGROUND
[0003] Technical Field
[0004] The present disclosure relates to formation of thin-film insulators.
[0005] Description of the Related Art
[0006] Thin-film insulators are central to the operation of organic light emitting diode (OLED) and liquid crystal display (LCD) in-plane transfer (IT) panels, and other applications. The quality of the thin-film insulators can affect the overall performance of such devices. However, it can be difficult to achieve high-quality thin-film insulators.
[0007] All of the subject matter discussed in the Background section is not necessarily prior art and should not be assumed to be prior art merely as a result of its discussion in the Background section. Along these lines, any recognition of problems in the prior art discussed in the Background section or associated with such subject matter should not be treated as prior art unless expressly stated to be prior art. Instead, the discussion of any subject matter in the Background section should be treated as part of the inventor’s approach to the particular problem, which, in and of itself, may also be inventive.
[0008] BRIEF SUMMARY
[0009] Embodiments of the present disclosure provide high quality thin-film insulators with improved uniformity of composition. Embodiments of the present disclosure perform a sputtering process to deposit a thin-film on a substrate. The sputtering process includes introducing a reactive gas into the environment of a metallic target prior to opening a shutter within the sputtering chamber. A negative bias is applied to a substrate. Upon opening the shutter, deposition of the thin-film insulatorbegins. The negative bias applied to the substrate helps to ensure that a high-quality thin-film insulator is deposited on the substrate. This results in a substantial reduction in failure events associated with low-voltage dielectric breakdown.
[0010] In some embodiments, applying the negative bias voltage has the effect of inhibiting negatively charged species of the reactive gas from reaching the substrate and becoming embedded in the thin film. Such trapped negatively charged species could reduce a breakdown voltage of the thin-film insulator. Beneficially, the number of such species that reach the substrate is reduced by the application of the negative bias voltage to the substrate. The negatively charged species can include negative ions of the reactive gas, negative ions of the sputtering gas, and secondary electrons from the target.
[0011] In some embodiment, applying the negative bias voltage has the effect of producing some sputtering based etching of the thin-film dielectric during the deposition process. The etching can result in ejecting from the thin-film insulator negatively charged species that were previously trapped. While the negative bias voltage reduces the number of negatively charged species that reach the substrate, negatively charged species with particularly high energy may still reach the substrate and become embedded in the thin-film insulator. Beneficially, the negative bias voltage can help eject such trapped species during sputtering-based etching that can occur during deposition. This can further reduce failure events associated with low-voltage dielectric breakdown.
[0012] In some embodiments, applying the negative bias voltage further enables relatively higher flow rates of the reactive gas during deposition. In the absence of the negative bias voltage, higher flow rates of the reactive gas can lead to larger concentrations of negatively charged species incorporated into the thin-film insulator. However, by applying the negative bias voltage to the substrate, higher flow rates of the reactive gas can be utilized without trapping large concentrations of negatively charged species in the thin-film insulator. Such higher flow rates of the reactive gas can lead to more effective poisoning of the target, resulting in higher quality thin-film insulators.In some embodiments, while the shutter is closed, the reactive gas flows into the portion of the deposition chamber in which the target is positioned. The reactive gas is a reactive gas, such as oxygen, selected to oxidize the target, also known as poisoning the target. Upon opening the shutter, the sputtering fluid source provides the sputtering fluid into the deposition chamber. Material is dislodged from the target and deposited on the substrate, in oxygen-rich phases.
[0013] In some embodiments, a method includes supporting a target within a sputtering chamber, supporting a substrate within the sputtering chamber, depositing a dielectric layer on the substrate by flowing a reactive gas and a sputtering gas into the sputtering chamber, and applying a bias voltage to the substrate while depositing the dielectric layer.
[0014] In some embodiments, a method includes flowing a reactive gas into a sputtering chamber while a shutter is closed between a target and a substrate during a startup phase of a sputtering process and applying a voltage to the target during the startup phase. The method includes initiating a deposition phase of the sputtering process by opening the shutter, depositing a dielectric film on the substrate during the deposition phase, applying a bias voltage to the target during the deposition phase.
[0015] In some embodiments, a system includes one or more computer memories storing software instructions and one or more processors configured to execute the software instructions to perform a sputtering process to deposit a dielectric layer. The sputtering process includes flowing a reactive gas into a sputtering chamber, flowing a reactive gas into the sputtering chamber, applying a voltage to a target in the sputtering chamber, and applying a bias voltage to a substrate in the sputtering chamber.
[0016] BRIEF DESCRIPTION OF THE SEVERAL VIEWS OF THE DRAWINGS
[0017] The detailed description is described with reference to the accompanying figures. The sizes and relative positions of elements in the figures are not necessarily drawn to scale. For example, the shapes of various elements and angles are not drawn to scale and some of these elements are enlarged and positioned to improve figurelegibility. As is understood by one of skill in the art, the shape of a particular element may be modified (e.g., rounded, thinned, elongated, etc.) to suit a particular application.
[0018] Figure 1 A is a simplified illustration of a sputtering system, in accordance with some embodiments.
[0019] Figure IB is a simplified illustration of the sputtering system of Figure 1 A in a startup phase of a sputtering process, in accordance with some embodiments.
[0020] Figure 1C is a simplified illustration of the sputtering system of Figure 1 A in a deposition phase of the sputtering process, in accordance with some embodiments.
[0021] Figure 2 is a timing diagram of a sputtering process, in accordance with some embodiments.
[0022] Figure 3 is a graph illustrating target voltage and a reactive gas flow rate, in accordance with some embodiments.
[0023] Figure 4 is a graph illustrating target voltage and a reactive gas flow rate, in accordance with some embodiments.
[0024] Figure 5 is a Weibull plot of breakdown fields and cumulative failure percentages for a sputtering process, in accordance with some embodiments.
[0025] Figures 6A and 6B are Weibull plots of breakdown fields and cumulative failure percentages for sputtering processes at different reactive gas flow rates, in accordance with some embodiments.
[0026] Figure 7 is a cross-sectional view of a thin-film transistor including a thin-film insulator, in accordance with some embodiments.
[0027] Figure 8 is a flow diagram of a method for performing a sputtering process, in accordance with some embodiments.
[0028] Figure 9 is a flow diagram of a method for performing a sputtering process, in accordance with some embodiments.
[0029] DETAILED DESCRIPTION
[0030] In the following description, certain specific details are set forth in order to provide a thorough understanding of various disclosed embodiments. However, oneskilled in the relevant art will recognize that embodiments may be practiced without one or more of these specific details, or with other methods, components, materials, etc. In other instances, well-known systems, components, and circuitry associated with integrated circuits have not been shown or described in detail, to avoid unnecessarily obscuring descriptions of the embodiments.
[0031] Unless the context requires otherwise, throughout the specification and claims which follow, the word “comprise” and variations thereof, such as, “comprises” and “comprising” are to be construed in an open, inclusive sense, that is as “including, but not limited to.” Further, the terms “first,” “second,” and similar indicators of sequence are to be construed as interchangeable unless the context clearly dictates otherwise.
[0032] Reference throughout this specification to “some embodiments” or “an embodiment” means that a particular feature, structure or characteristic described in connection with the embodiment is included in at least some embodiments. Thus, the appearances of the phrases “in some embodiments” or “in an embodiment” in various places throughout this specification are not necessarily all referring to the same embodiment. Furthermore, the particular features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.
[0033] As used in this specification and the appended claims, the singular forms “a,” “an,” and “the” include plural referents unless the content clearly dictates otherwise. It should also be noted that the term “or” is generally employed in its broadest sense, that is as meaning “and / or” unless the content clearly dictates otherwise.
[0034] Figure 1A is a simplified illustration of a reactive sputtering system 100, in accordance with some embodiments. As will be set forth in more detail below, the components of the sputtering system 100 cooperate to perform sputtering processes that result in the deposition of high quality thin-film insulators. In some embodiments, the sputtering system is a pulsed-DC sputtering system.
[0035] In some embodiments, the sputtering system 100 corresponds to a sputtering tool. For simplicity in illustrating principles of the present disclosure, Figure 1 A illustrates various components of the sputtering system 100 as simple blocks. Inpractice, the sputtering system 100 can have various compositions, arrangements, structures, and configurations without departing from the scope of the present disclosure.
[0036] In some embodiments, the sputtering system 100 includes a sputtering chamber 101. The sputtering chamber 101 may also be termed a deposition chamber. Deposition of thin-film insulators occurs within the sputtering chamber 101. Various other types of thin films may also be deposited with the sputtering chamber 101.
[0037] The sputtering chamber 101 includes a target support 102. The target mount 102 is configured to hold a target 104 during sputtering processes. The sputtering chamber includes a substrate support 106 configured to hold a substrate 108.
[0038] The target 104 includes a target material. The target material is the material that will be utilized to form a thin film on the exposed surface of the substrate 108 during a sputtering process, as will be set forth in more detail below. In some embodiments, the target 108 includes a metal. The sputtering process deposits a thin-film insulator (or dielectric layer) corresponding to an oxide of the metal of the target 108. In one example, the target 104 includes aluminum and the sputtering process deposits aluminum oxide as the thin-film insulator on the substrate 108. Other target materials and other types of thin-films can be utilized without departing from the scope of the present disclosure. In some embodiments, the target includes titanium, hafnium, tantalum, silicon, yttrium, or other suitable materials.
[0039] In the example of Figure 1 A, the target 104 is held above the substrate 108 such that the bottom surface of the target 104 faces the top surface of the substrate 108. However, in other examples, the positions of the target support 102 and the substrate support 106 may be reversed such that the upward facing surface of the target 104 faces the downward facing surface of the substrate 108. Various other configurations and orientations of targets and substrates can be utilized without departing from the scope of the present disclosure.
[0040] A substrate support 106 is positioned within the thin-film deposition chamber 102. The substrate support 106 supports the substrate 108 during thin-film deposition processes. At the beginning of a thin-film deposition process, a substrate108 may be transferred into the thin-film deposition chamber 102 and positioned on the substrate support 106. After a thin-film deposition process is performed on the substrate 108, the substrate 108 can be transferred out of the thin-film deposition chamber 102. The substrate 108 can include an insulator substrate, a wafer, or another type of substrate.
[0041] In some embodiments, the target support 102 and the substrate support 106 correspond to, or may include electrodes. Voltages may be applied between the target support 102 and the substrate support 106 during the sputtering process. These voltages can include DC voltages, AC voltages, or combinations of DC offsets and AC voltages.
[0042] In some embodiments, the substrate support 106 includes a heater. The heater can heat the substrate 108 during thin-film deposition processes. Heating of the substrate 108 during thin-film deposition processes can help promote redistribution or settling of deposition materials on the surface of the substrate 108 to help ensure even thicknesses of the deposition material on the substrate 108.
[0043] In some embodiments, the sputtering system 100 includes a power source 110. The power source 110 is coupled to the target support 102 and the substrate support 106. The power source 110 is configured to apply a voltage between the target support 102 and the substrate support 106. In some embodiments, this corresponds to applying a voltage to the target 104. As will be set forth in more detail below, the power source applies a bias voltage to the substrate 108 (by applying the bias voltage to the substrate support 106) during a deposition process in order to deposit a high quality thin-film insulator on the substrate.
[0044] In some embodiments, the sputtering chamber 101 includes a shutter 109. The shutter 109 is illustrated by a dashed line in Figure 1 A. The shutter 109 can be opened or closed. When the shutter 109 is closed, the shutter 109 corresponds to a physical barrier between the target 104 and the substrate 108. When the shutter 109 is closed, the shutter 109 prevents sputtering of material from the target 104 onto the substrate 108. When the shutter 109 is open, material can be sputtered from the target 104 onto the substrate 108. As will be set forth in more detail below, the shutter 109 isclosed during a startup phase of a sputtering process and is open during a deposition phase of the sputtering process. In some embodiments, the shutter 109 is grounded when the shutter 109 is closed. In some embodiments the bias voltage is applied to the substrate 106 while the shutter 109 is closed.
[0045] In some embodiments, the sputtering system 100 includes a reactive gas source 116. The reactive gas source 116 is configured to supply a reactive gas (or other type of conditioning gas) into the sputtering chamber 101. The reactive gas is selected to react with the target 104 in order to condition the target 104 so that sputtering the target will result in deposition of a high-quality thin film. In some embodiments, the reactive gas includes oxygen. In some embodiments, the reactive gas includes nitrogen.
[0046] In some embodiments, a valve 118 is coupled between the reactive gas source 116 and a fluid inlet 120. The valve 118 controls supply of the reactive gas 116 into the sputtering chamber 101. The valve 118 can stop flow of the reactive gas, enable flow of the reactive gas, and adjust the flow rate of the reactive gas.
[0047] The fluid inlet 120 is positioned such that when the shutter 109 is closed, the reactive gas can be provided onto the target 104. In the example configuration of Figure 1 A, the shutter 109 separates an upper portion of the sputtering chamber 101 from a lower portion of the sputtering chamber 101. The target 104 is supported in the upper portion of the sputtering chamber 101. The substrate 108 is positioned in the lower portion of the sputtering chamber 101. The fluid inlet 120 opens into the upper portion of the sputtering chamber 101. Other configurations can be utilized without departing from the scope of the present disclosure.
[0048] A sputtering gas source 122 supplies a sputtering gas (or other fluid) into the thin-film deposition chamber 102. In some embodiments, the sputtering gas includes an inert gas, such as argon, or another inert gas. During operation, the power source 110 applies a voltage to the target support 102 and a bias voltage to the substrate support 106. The applied voltage causes ionization of the atoms of the fluid. When the atoms of the sputtering gas source become ionized, the atoms are drawn toward the target 104 via electrostatic force. For example, the target support 102 may receive a negative voltage that causes positively charged ions to be drawn toward the target 104and that causes negatively charged species to be pushed away from the target 104. When the positively charged ions impact the target 104, the positively charged ions cause some of the material of the target 104 to be ejected from the target 104 and to travel toward the substrate 108. The ejected target material accumulates on the substrate, thereby forming a thin film of the target material on the substrate 108.
[0049] In some embodiments, the bias voltage applied to the substrate 108 is a negative bias voltage. In some embodiments, the bias voltage is an RF bias voltage. Inn some embodiments, the negative bias voltage is between -10 V and -100 V. In some embodiments, the negative bias voltage is between -40 V and -60 V. In some embodiments, the negative bias voltage is -50 V. As will be set forth in more detail below, these voltages can help ensure that high quality thin-film insulators are deposited on the substrate 108.
[0050] In some embodiments, a valve 124 is coupled between the sputtering gas source 122 and a fluid inlet 122. The valve 124 controls supply of the sputtering gas into the sputtering chamber 101. The valve 124 can stop flow of the sputtering gas, enable flow of the sputtering gas, and adjust the flow rate of the sputtering gas. In some embodiments, the fluid inlet 122 supplies the sputtering gas into the lower portion of the sputtering chamber 101, though other configurations can be utilized without departing from the scope of the present disclosure.
[0051] The sputtering system 101 includes an exhaust outlet 126. The exhaust outlet 126 carries exhaust fluids, byproducts, and access reactive gas and sputtering gas from that the sputtering chamber 101. Though not shown, the sputtering system 101 can include one or more pumps and other control valves to control flow of exhaust fluids and byproducts from the sputtering chamber 101.
[0052] The sputtering system 100 includes a control system 128. The control system 128 controls the function of the various components of the sputtering system 100. For example, the control system 128 executes the sputtering process including controlling the power source 110 to apply selected voltages, controlling the valves 118 and 124 to control flow of the conditioning and sputtering gasses, and controlling any other functions.In some embodiments, the control system 128 includes one or more processors and one or more memories. The one or more memories store instructions which, when executed by the one or more processors, cause the sputtering system 100 to execute a sputtering process. Further details regarding the sputtering process are set forth below.
[0053] Figure IB is an illustration of the sputtering system 100 of Figure 1A during a startup phase of a sputtering process, in accordance with some embodiments. During the startup phase, the shutter 109 is closed. The closing of the shutter 109 is indicated by the solid line that had previously been dashed in Figure 1 A. A voltage is applied to the target 104 via the power source 110. In some embodiments, the bias voltage as described above is applied to the substrate support 108 during the startup phase. In some embodiments, ground voltage (0 V) is applied to the shutter 109.
[0054] After a selected duration of time, the reactive gas source 116 begins to supply the reactive gas 134 into the sputtering chamber 101 with a selected flow rate. In some embodiments, the flow rate is a relatively high flow rate, enabled partly by use of the bias voltage, as will be set forth in more detail below. One effect of the high flow rate of the reactive gas is that a larger portion (or an entirety) of the target 104 reacts with the reactive gas, thereby changing the composition of the target 104 prior to opening of the shutter 109.
[0055] As set forth previously, in one example, the target 104 is aluminum and the reactive gas 134 is oxygen. The high flow rate of oxygen ensures that the target 104 reaches an oxidized state prior to shutter 109 opening.
[0056] Though not shown, in some embodiments the process includes a precleaning phase prior to changing a composition (poisoning) the target 104.
[0057] Figure 1C illustrates the sputtering system 100 of Figure 1A during a deposition phase of the sputtering process, in accordance with some embodiments. In Figure 1C, the shutter 109 has been opened. The valve 124 is opened and the sputtering gas source 122 provides the sputtering gas 136 into the sputtering chamber 101. As was described previously, the sputtering gas 136 becomes ionized and is driven toward the target 108. The impact of the ionized sputtering gas 136 with the target 104 causesmaterial 138 from the target 104 to become dislodged or to otherwise break away from the target 104. The material 138 is driven onto the substrate 108. The accumulation of the material 138 from the target 104 on the substrate 108 results in deposition of a thin-film insulator.
[0058] Returning to the example in which the target is aluminum and the reactive gas 134 is oxygen, a high-quality film of aluminum oxide (AI2O3) is deposited on the substrate 108. When the shutter opens the voltage of the target (target voltage), gradually decreases towards the desired value for the process (process voltage).
[0059] In some circumstances, such a decrease in the voltage after opening the shutter 109 could lead to deposition of a low-quality film. However, applying the bias voltage to the substrate support 108 during the deposition phase can help ensure that a high-quality film is deposited.
[0060] As set forth previously, in some embodiments, the bias voltage applied to the substrate support 108 is a negative bias voltage. During the sputtering process, various charged species are generated within the sputtering chamber 101. The charged species can include negatively charged reactive gas species (e.g., negatively charged oxygen), positively charged reactive gas species (e.g., positively charged oxygen), negatively charged sputtering gas species, positively charged sputtering gas species, free electrons including secondary electrons from the target 104, negatively charged compounds from the target 104, and positively charged compounds from the target 104.
[0061] In some cases, some amount of free electrons or other negatively charged species can become embedded within the thin-film insulator during deposition. An accumulation of such trapped charges can result in relatively low breakdown voltages of the thin-film insulator. This can be highly problematic.
[0062] However, beneficially, by applying the negative bias voltage to the substrate 106, fewer negatively charged particles become embedded in the thin-film insulator. Instead, they are repelled by electrostatic force away from the substrate 106. This results in fewer negatively charged species being embedded in the thin-film insulator. This can greatly increase the overall electrical quality of the thin-filminsulator, leading to much higher breakdown voltages and better functioning electronic devices.
[0063] In some cases, even with the negative bias voltage applied to the substrate 106, some negatively charged species will become embedded in the thin-film insulator. In some embodiments, applying the negative bias voltage to the substrate 106 can cause some etching of the thin-film insulator during the deposition process. This etching can beneficially release trapped negatively charged species, which are then ejected from the thin-film insulator by electrostatic force due to the negative bias voltage applied to the substrate 106. In this way, the negative bias voltage can further enhance the robustness of the thin-film insulator.
[0064] Figure 2 is a graph 200 illustrating parameters of a sputtering process, in accordance with some embodiments. The sputtering process of Figure 2 is one example of the sputtering process described in relation to Figures 1 A-1C. In Figure 2, the target 104 includes aluminum and the reactive gas 134 includes molecular oxygen (O2).
[0065] However, other materials can be utilized without departing from the scope of the present disclosure. Figure 2 illustrates the target voltage, reactive gas pressure, and chamber pressure versus time during a deposition process.
[0066] Though not shown in the graph of Figure 2, in some embodiments the bias voltage is applied to the substrate 106 both while the shutter is closed and after the shutter is open. In some embodiments, the bias voltage is applied to the substrate substantially simultaneously with the voltage applied to the target 104.
[0067] Figure 2 illustrates a startup phase of a deposition process, in accordance with some embodiments. The startup phase includes the portion of the deposition cycle during which the shutter is closed. In one example, at time 0 s, the pressure within the sputtering chamber is increased to about 50 mTorr. After about 40 seconds, the voltage of the target begins to increase from 0 V to about 370 V, beyond a process voltage of 350 V corresponding to a voltage at which deposition will primarily take place. In some embodiments, the bias voltage is also applied to the substrate at this time. Shortly after the initial application of voltage to the target, the pressure drops to about 2 mTorr.Other values of voltage and pressure can be utilized without departing from the scope of the present disclosure.
[0068] At about 250 seconds, the flow of the reactive gas O2 is initiated while the shutter is closed. In some embodiments, the flow rate of the reactive gas is about 400 seem. In some embodiments, the flow rate of the reactive gas is held steady during the remainder of the startup phase and during the deposition phase. Alternatively, in some embodiments, the flow rate of the reactive gas can be adjusted at various moments within the sputtering process. Other flow rates can be utilized without departing from the scope of the present disclosure.
[0069] When the O2 begins to flow into the sputtering chamber, the aluminum target 104 begins to react with the O2. This reaction causes the target 104 to oxidize, becoming AI2O3.
[0070] At about 575 seconds, the shutter 109 opens. This corresponds to the end of the startup phase and the beginning of the deposition phase of the sputtering process. In some embodiments, the opening of the shutter results in a decrease of the target voltage to the deposition voltage. As set forth previously, in some embodiments, the deposition voltage is about 350 V, though other voltages can be utilized without departing from the scope of the present disclosure. In some cases, this period of decreasing voltage could lead to an initial poor quality of the thin-film insulator.
[0071] However, due to the application of the negative bias voltage to the substrate 106, such problems are avoided and a robust thin-film insulator is deposited.
[0072] In some embodiments, the sputtering system 100 operates in a constant power mode during the deposition process. Power is a product of voltage and current. Changes in the reactive gas flow rate result in changes in current. Because the system is operating in a constant power mode, changes in current result in changes in the voltage. Accordingly, changing the flow rate of the reactive gas results in changes in the voltage of the target 104. These relationships are described in further detail below.
[0073] Figures 3 and 4 and their descriptions are utilized to assist in an understanding of principles of the present disclosure. Figure 3 is a graph illustrating target voltage vs oxygen flow rate during O2 addition and O2 extraction with an openshutter, in accordance with some embodiments. The flow rate has a range between 0 seem and 10 seem. O2 addition corresponds to a state in which the reactive gas is flowing into the deposition chamber. O2 extraction corresponds to a state in which the reactive gas is flowing out of the deposition chamber. As can be seen, there is some hysteresis in the target voltage based on in-flow and out-flow of O2. Most notably within a range between about 2 seem and 6 seem, the process voltage is higher for a given flow rate in the extraction state than for the addition state. The hysteresis is a result of the target having a metastable oxidization state.
[0074] In Figure 3, there is an initial curve between about 0 seem and 2 seem in which there is little hysteresis. There is also a portion between 6 seem and 10 seem where there is relatively little hysteresis. Thin-films deposited in the initial curve region tend to have higher concentration of metal, resulting in higher conductivity and lower breakdown voltages. Films deposited in the higher flow rate regime have higher oxygen content, resulting in lower conductivity and higher breakdown voltages. A single film deposited with portions in both of these conditions would have non-uniform composition.
[0075] As set forth previously, in some embodiments the sputtering system 100 is operated in a constant power mode. Power is a product of voltage and current. Accordingly, a drop in voltage, as seen in Figure 3, will result from a corresponding increase in current. The increase in current is based on secondary electron emission yield during the sputtering process. However, due to the application of the negative bias voltage, in accordance with some embodiments, fewer of such secondary electrons become embedded in the thin-film insulator and some of those secondary electrons that initially become embedded can later be ejected, as described previously.
[0076] Figure 4 is a graph illustrating target voltage vs oxygen flow rate during O2 addition and O2 extraction with a closed shutter, in accordance with some embodiments. As can be seen, the voltage is higher in Figure 4 beyond the 3 seem flow rate than for the same flow rate in Figure 3 with the shutter open. The steady high voltage below about 6 seem is an indication that there is a lack of oxidization of thetarget in that range. This would correspond to deposition of a thin film with higher concentration of metal and lower breakdown voltages.
[0077] Beneficially, the process described in relation to Figures 1 A-2 ensures both a high degree of oxidization before the shutter opens by utilizing the high flow rate during the startup phase and the deposition phase. The result is a high quality thin-film insulator with low conductivity, high uniformity of composition, high breakdown voltages, and low leakage currents.
[0078] Figure 5 illustrates a failure rates vs breakdown field of thin-film insulators for a process in which the negative bias voltage is not applied and for a process in which the negative bias voltage is applied.
[0079] The data shown at left compares the two processes in terms of dielectric breakdown. The left axis is a special function of the cumulative failure (CF) referred to as a Weibull plot. The right y-axis is the cumulative failure percentage.
[0080] The use of a Weibull plot accentuates two main components of the distribution: the head and tail. The head of the distribution is the most vertical part at higher breakdown field. This part is associated with the intrinsic field strength (e.g., breakdown field of AI2O3). The tail of the distribution is associated with defective regions and is called extrinsic.
[0081] As can be seen, the process of Figure 2 including the bias voltage of -50 V has no tail. The result is that the breakdown field is increased from < 0.1 V / nm to > 0.4 V / nm. This 4X increase in breakdown field means that the improved thin-film insulator can withstand a 4X larger applied voltage before reducing yield. This is a substantial improvement.
[0082] Thin-films formed without the bias voltage have been shown to be linked to a significant reduction in the yield of MIM and MIS capacitors, due to a reduction in breakdown voltage. The reduction in breakdown voltage is related to the deposition of oxygen-deficient suboxides during the early stages of reactive sputtering of aluminum oxide, a phenomenon which is generally applicable to other gate insulators which would also be deposited via reactive sputtering (e.g., silicon dioxide, hafnium dioxide, zirconium dioxide, etc.).As set forth in relation to Figures 1 A-2 and 5, the process utilizing the bias voltage during deposition avoids electrically-poor AlOx suboxides. The result is a 4X increase in the maximum voltage which could be safely applied across any capacitor encompassing the reactively-sputtered gate insulator. A higher applied voltage leads to a lower resistance of all switching thin-film transistors in their ON states, and a corresponding increase in refresh rate obtainable in an LCD or OLED IT panels.
[0083] Figure 6A illustrates a graph 600 plotting the characteristics shown in Figure 5, but for processes using a plurality of different reactive gas flow rates (1.5, seem, 2.5 seem, 3.5 seem, and 4.5 seem) all without the application of the bias voltage to the substrate.
[0084] Figure 6B illustrates a graph 602 plotting the characteristics shown in Figure 5, but for processes using a plurality of different reactive gas flow rates (3.0, seem, 4.0 seem, 4.5 seem, 4.6 seem, 4.7 seem, and 4.8 seem) all with the application of the bias voltage to the substrate.
[0085] As can be seen in the graph 600, higher oxygen flow rates result in reduced dielectric strength. A flow rate of 1.5 seem provides the best results. As can be seen in the graph 602 of Figure 6B, higher oxygen flow rates result in increased dielectric strength when the negative bias voltage is applied to the substrate 106. This enables utilization of higher oxygen flow rates.
[0086] Figure 7 is a cross-sectional view of a thin-film transistor 140, in accordance with some embodiments. The thin-film transistor includes a thin-film insulator 146 formed in accordance with the process described in relation to Figures 1A-2 and 5.
[0087] The thin-film transistor 140 includes a gate electrode 144 positioned on a substrate 102. In some embodiments, the substrate 102 includes a substantially nonconductive material. The substrate can be glass, a polymer, plastic, or other materials. In some embodiments, the substrate is glass, a polymer, plastic, or other material. In other embodiments, the substrate is a rubber. As used herein, “rubber” includes polymers of isoprene as well as forms of polyisoprene. In some such embodiments, the substrate is a plastic. Any suitable plastic may be used. In someembodiments, the plastic is a polyimide, an arylamide, acrylamide, polybenzimidazole (PBI), polyetherimide, polyetherketoneketone (PEKK), polyether ether ketone (PEEK), polyamide, polyimide, polyamide-imides, polystyrene (PS), polyphenylene oxide (PPO), polyphthalamide (PPA), polyvinyl alcohol (PVA), acrylonitrile butadiene styrene (ABS), polycarbonate (PC), thermoset, PBI-PEEK, urea, epoxies, polyurethanes, or any combination thereof. In some embodiments, the plastic is a polyethylene. In particular embodiments, the plastic is a high-density polyethylene.
[0088] In some embodiments, the gate electrode 144 includes a conductive material such as titanium aluminum. In some embodiments, the gate electrode includes TiAh. The thickness of the TiAh is between 80 nm and 100 nm, though other thicknesses can be used without departing from the scope of the present disclosure. The TiAh can have an amorphous structure.
[0089] In some embodiments, the thin-film transistor includes a gate insulator 146 corresponding to a thin-film insulator formed by the process described in relation to forgoing Figures. In some embodiments, the gate insulator 146 includes hafnium oxide. The gate insulator 146 can include AI2O3, though other materials can be utilized without departing from the scope of the present disclosure. The gate insulator 146 can have a thickness between 10 nm and 20 nm, though other thicknesses can be utilized without departing from the scope of the present disclosure.
[0090] The thin-film transistor 140 includes a source electrode 146 and drain electrode 148 on the thin-film insulator 146. The source electrode 146 and the drain electrode 148 can include a metal such as copper, aluminum, titanium, tungsten, or other suitable metals.
[0091] In some embodiments, the thin-film transistor 140 includes a semiconductor layer 150. The semiconductor layer 150 can include one or more of IGZO (compositions of In, Ga, Zn, and O), low temperature poly crystalline silicon (LTPS), amorphous silicon, or other suitable semiconducting materials. In an example in which the gate insulator 146 includes AI2O3 between 10 nm and 20 nm in thickness, the semiconductor material 150 can include IGZO between 30 nm and 50 nm in thickness, formed with a PVD process. In an example in which the gate insulator 146includes AI2O3 between 5 nm and 15 nm in thickness and the gate electrode 144 includes molybdenum, the semiconductor material 150 can include LTPS between 40 nm and 60 nm in thickness, formed with a PECVD process followed by an ELA process. In an example in which the gate insulator 146 includes AI2O3 between 3 nm and 8 nm in thickness, the semiconductor material 150 can include amorphous silicon between 40 nm and 60 nm in thickness, formed with a PECVD process. In an example in which the gate insulator 146 includes AI2O3 between 5 nm and 15 nm in thickness and the gate electrode 144 includes titanium, the semiconductor material 150 can include IGZO between 15 nm and 25 nm in thickness, formed with a PVD process followed by an ELA process.
[0092] In some embodiments, the thin-film transistor 140 includes a passivation layer 152 on the semiconductor layer 150. The passivation layer 152 can include a dielectric material with a thickness between 50 nm and 500 nm. The passivation layer 152 can include one or more of silicon dioxide, silicon nitride, or other dielectric materials.
[0093] Figure 8 is a flow diagram of a method 800 for forming a thin-film insulator, in accordance with some embodiments. The method 800 can utilize processes, systems, and components described in relation to foregoing figures. At 802, the method 800 includes supporting a target within a sputtering chamber. At 804, the method 800 includes supporting a substrate within the sputtering chamber. At 806, the method 800 includes depositing a dielectric layer on the substrate by flowing a reactive gas and a sputtering gas into the sputtering chamber. At 808, the method 800 includes applying a bias voltage to the substrate coincident with and throughout an entirety of the deposition process such that, a Weibull plot of a cumulative breakdown voltage (V) of the dielectric layer is linear, and breakdown voltage data expressed in Weibull form is described by a two-parameter fit of the following form, with parameters ft and r / defined as ln(— ln(l — F)) = p ln(V) — pin (p), wherein a difference in parameters extracted from Weibull plots for top-injection versus bottom -injection relative to the dielectric layer are statistically insignificant.Figure 9 is a flow diagram of a method 900 for forming a thin-film insulator, in accordance with some embodiments. The method 900 can utilize processes, systems, and components described in relation to foregoing figures. At 902, the method 900 includes flowing a reactive gas into a sputtering chamber while a shutter is closed between a target and a substrate during a startup phase of a sputtering process. At 904, the method 900 includes applying a voltage to the target during the startup phase. At 906, the method 900 includes initiating a deposition phase of the sputtering process by opening the shutter. At 908, the method 900 includes depositing a dielectric film on the substrate during the deposition phase. At 910, the method 900 includes applying a bias voltage to the target during the deposition phase.
[0094] These and other changes can be made to the embodiments in light of the above-detailed description. In general, in the following claims, the terms used should not be construed to limit the claims to the specific embodiments disclosed in the specification and the claims, but should be construed to include all possible embodiments along with the full scope of equivalents to which such claims are entitled. Accordingly, the claims are not limited by the disclosure.
Claims
CLAIMS1. A method, comprising:supporting a target within a sputtering chamber;supporting a substrate within the sputtering chamber;depositing a dielectric layer on the substrate by flowing a reactive gas and a sputtering gas into the sputtering chamber;applying a bias voltage to the substrate while depositing the dielectric layer.
2. The method of claim 1, wherein the bias voltage is an RF bias voltage.
3. The method of claim 1, wherein the bias voltage is a negative bias voltage.
4. The method of claim 3, wherein the negative bias voltage is between -10 V and -100 V.
5. The method of claim 4, wherein the negative bias voltage is between -40 V and -60 V.
6. The method of claim 1, wherein the reactive sputtering chamber is a pulsed DC sputtering chamber.
7. The method of claim 1, wherein the reactive gas includes oxygen.
8. The method of claim 1, wherein the target includes aluminum.
9. The method of claim 1, further comprising forming a thin-film transistor on the substrate, wherein the dielectric layer is part of the thin-film transistor.
10. The method of claim 1, further comprising forming a tunneling device on the substrate, wherein the dielectric layer is part of the tunneling device.
11. The method of claim 1, further comprising:poisoning the target during a startup phase of a sputtering process for depositing the dielectric layer by flowing the reactive gas into the chamber while a shutter is closed between the target and a substrate;initiating a deposition phase of the sputtering process by opening the shutter;flowing the sputtering gas into the deposition chamber during the deposition phase, wherein applying the bias voltage to the substrate includes applying the bias voltage to the substrate during the deposition phase.
12. The method of claim 10, wherein applying the bias voltage to the substrate includes applying the bias voltage to the substrate during the startup phase.
13. A method, compri sing :flowing a reactive gas into a sputtering chamber while a shutter is closed between a target and a substrate during a startup phase of a sputtering process;applying a voltage to the target during the startup phase;initiating a deposition phase of the sputtering process by opening the shutter;depositing a dielectric film on the substrate during the deposition phase; andapplying a bias voltage to the target during the deposition phase.
14. The method of claim 13, further comprising applying the bias voltage to the target during the startup phase.
15. The method of claim 13, wherein applying the bias voltage to the substrate includes applying the bias voltage to a substrate mount coupled to the substrate.
16. The method of claim 13, wherein the reactive gas includes oxygen or nitrogen.
17. The method of claim 16, wherein the target includes one or more of aluminum, titanium, hafnium, tantalum, silicon, or yttrium.
18. The method of claim 13, further comprising applying the bias voltage to the substrate coincident with and throughout an entirety of the sputtering process such that, a Weibull plot of a cumulative breakdown voltage (V) of the dielectric layer is linear, and breakdown voltage data expressed in Weibull form is described by a two-parameter fit of the following form, with parameters ft and r / defined as ln(— ln(l — F)) = p ln(V) — pin (p), wherein a difference in parameters extracted from Weibull plots for top-injection versus bottom -injection relative to the dielectric layer are statistically insignificant.
19. The method of claim 13, wherein the bias voltage is a negative bias voltage.
20. The method of claim 13, further comprising forming a thin-film transistor on the substrate, wherein the dielectric layer is part of the thin-film transistor.
21. The method of claim 13, further comprising forming a tunneling device on the substrate, wherein the dielectric layer is part of the tunneling device.
122. The method of claim 13, further comprising increasing the voltage of the target beyond a deposition voltage during the startup phase and reducing the voltage of the target to the deposition voltage during the deposition phase.
23. The method of claim 13, wherein the voltage is between is between 300 V and 400 V.
24. The method of claim 13, wherein the negative bias voltage is an RF voltage.
25. The method of claim 13, wherein a flow rate of the reactive gas is constant before opening shutter and after opening the shutter.
26. The method of claim 13, further comprising grounding the shutter during the startup phase.
27. A system, comprising:one or more computer memories storing software instructions;one or more processors configured to execute the software instructions to perform a sputtering process to depositing a dielectric layer, the sputtering process including:flowing a reactive gas into a sputtering chamber;flowing a reactive gas into the sputtering chamber;applying a voltage to a target in the sputtering chamber; and applying a bias voltage to a substrate in the sputtering chamber.
28. The system of claim 27, wherein the negative bias voltage is an RF bias voltage.
29. The system of claim 27, wherein the bias voltage is a negative bias voltage.
30. The system of claim 29, wherein the negative bias voltage is between -10 V and -100 V.
31. The system of claim 30, wherein the negative bias voltage is between -40 V and -60 V.
32. The system of claim 27, wherein the reactive sputtering chamber is a pulsed DC sputtering chamber.