Anhydride functionalized cyclic polyorganosiloxane

Anhydride functionalized cyclic polyorganosiloxane addresses the challenge of low-temperature adhesion in silicone compositions by a two-step hydrosilylation process, enhancing adhesion to diverse substrates.

WO2026236333A1PCT designated stage Publication Date: 2026-11-12DOW SILICONES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/026862
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing adhesion promoters for silicone compositions face challenges in achieving fast and strong adhesion to substrates like PBT, PA, PC, Al, and Glass at low temperatures, necessitating the development of alternative solutions.

Method used

An anhydride functionalized cyclic polyorganosiloxane is synthesized through a two-step hydrosilylation reaction, combining alkenyl-functional siloxanes with cyclic polyorganohydrogensiloxanes and an unsaturated anhydride to introduce anhydride functionality, enhancing adhesion properties.

Benefits of technology

The anhydride functionalized cyclic polyorganosiloxane improves adhesion to various substrates at lower cure temperatures, providing faster cure times and stronger bond strength in silicone compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026026862_12112026_PF_FP_ABST
    Figure US2026026862_12112026_PF_FP_ABST
Patent Text Reader

Abstract

An anhydride functionalized cyclic polyorganosiloxane has formula, wherein each subscript n independently has an average value of 2 to 18, each R1 is an independently selected monovalent hydrocarbyl group; each R is independently selected from H or an anhydride-functional group; each D is an independently selected divalent hydrocarbyl group of 2 to 6 carbon atoms; and L is an organosilicon linker. The anhydride functionalized cyclic polyorganosiloxane is useful as an adhesion promoter in a curable silicone composition.
Need to check novelty before this filing date? Find Prior Art

Description

ANHYDRIDE FUNCTIONALIZED CYCLIC POLYORGANOS1LOXANECROSS REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefits of U.S. Provisional Patent Application No.63 / 802105 filed on 8 May 2025 under 35 U.S.C. § 119 (e). U.S. Provisional Patent Application No. 63 / 802105 is hereby incorporated by reference.FIELD

[0002] An anhydride functionalized cyclic polyorganosiloxane (organosiloxane) and methods for its preparation and use are disclosed. The organosiloxane comprises two cyclic organosiloxane moieties bonded to an aryl-functional organosilicon moiety. The organosiloxane is useful in curable silicone compositions as an adhesion promoter.INTRODUCTION

[0003] The adhesion of silicone-based compositions to substrates such as glass, metal, and a variety of plastics is facilitated with an adhesion promoter, which includes functionalized organosiloxanes. For example, US 6,887,932 B2 (Azechi) discloses a vast number of adhesion promoters that are functionalized polyorganosiloxanes containing Si-H groups. CN 103467965 A (Shinetsu) discloses adhesion promoters that are cyclic organosiloxanes containing Si-H, anhydride, and fluoroalkyl groups. Similarly, EP 3 850049 Bl (Felder) and WO 2021 / 262830 (Santos) disclose adhesion promoters that are acid anhydride functionalized polyorganosiloxanes containing Si-H groups.

[0004] Adhesion promoters are widely used to improve the adhesion of various silicone products (e.g., sealants, adhesives, and elastomers) to different inorganic and organic substrates. The choice of adhesion promoter is often specific to the composition and application, which requires the matching on properties such as chemical reactivity, solubility characteristics, compatibility, and thermal stability. Faster cure times at lower temperatures are desirable for curable silicone compositions such as liquid silicone rubber (LSR) compositions. However, a challenge frequently encountered at low temperature cure for LSR compositions is the lack of developing fast and strong adhesion for different substrates (e.g., PBT, PA, PC, Al, and / or Glass). There is still a need to develop alternative solutions for adhesion promoters.SUMMARY

[0005] An anhydride functionalized cyclic polyorganosiloxane (organosiloxane), and methods for preparation and use of the organosiloxane, are provided. This organosiloxane comprises formula:each subscript n independently has a value of 2 to 18;each R1is an independently selected monovalent hydrocarbyl group:each R2is independently selected from the group consisting of H and an anhydride-functional group; with the proviso that at least one instance of R2per molecule is the functional group; each D is independently a divalent hydrocarbyl group of 2 to 6 carbon atoms;L is a divalent linking moiety selected from the group consistingof R3RArR3| R3| RAr| R3and O O , wherein each RA|is an independently selected monovalent aromatic group and each R3is an independently selected alkyl group.

[0006] The method for preparing the organosiloxane comprises:combining, under conditions to effect a first hydrosilylation reaction, starting materials comprising:A) a hydrosilylation reaction catalyst;B) an alkenyl-functional siloxane selected from the group consisting ofR3R3R3RArR3| . RAr| _RAr| R3| RAr| R3 / Si\ / S'C ^Si\RVlO RV1and RV1O O RV1, wherein R3and RAlare as described above, and each RV1is an independently selected alkenyl group; andC) a cyclic polyorganohydrogensiloxane of unit formula (R1HSiO2 / 2)v, wherein subscript v has an average value of 4 to 20 (v = n-2), and each R1is as described above; thereby preparing a first hydrosilylation reaction product comprising a) an organohydrogensiloxane and the hydrosilylation reaction catalyst; andcombining, under conditions to effect a second hydrosilylation reaction, starting materials comprisingthe first hydrosilylation reaction product or a) the organohydrogensiloxane, and c) a reactive species having an average, per molecule at least one aliphatically unsaturated group capable of undergoing an addition reaction with a silicon bonded hydrogen atom of a) the organohydrogensiloxane and further comprising a moiety comprising an anhydride-functional group;thereby preparing a second hydrosilylation reaction product comprising the organosiloxane.DETAILED DESCRIPTION

[0007] As introduced above, the anhydride functionalized cyclic polyorganosiloxane (organosiloxane) comprises formula:each subscript n independently has a value of 2 to 18;each R1is an independently selected monovalent hydrocarbyl group;each R2is independently selected from the group consisting of H and an anhydride -functional group; with the proviso that at least one instance of R2per molecule is the functional group; each D is independently a divalent hydrocarbyl group of 2 to 6 carbon atoms;R3R3| RAr| RArL is a divalent linking moiety selected from the group consistingof O R3RArR3| R3| RAr| R3and O O , wherein each RA|is an independently selected monovalent aromatic group and each R3is an independently selected alkyl group.

[0008] The method for preparing the organosiloxane comprises:1) combining, under conditions to effect a first hydrosilylation reaction, starting materials comprising:A) a hydrosilylation reaction catalyst;B) an alkenyl-functional siloxane selected from the group consisting ofR3R3R3RArR3| R^ | R^ | R3| RAr| R3RVlO / siC RV1and RVl / Si\ 0 ^si\ O / ^si\ RV1, wherein R3and RA|are as described above, and each RV1is an independently selected alkenyl group;C) a cyclic polyorganohydrogensiloxane of unit formula (R1HSiO2 / 2)v, wherein subscript v has an average value of 4 to 20 (v = n-2), and each R1is as described above;optionally E) a hydrosilylation reaction inhibitor;optionally D) a solvent; andoptionally all or a portion of F) a thiuram disulfide; thereby preparing a first hydrosilylation reaction product comprising a) an organohydrogensiloxane and the hydrosilylation reaction catalyst, and, when present the hydrosilylation reaction inhibitor, and / or the solvent; and optionally 2) combining the hydrosilylation reaction product or a) the organohydrogensiloxane and all or a portion of F) the thiuram disulfide; andoptionally 3) purifying the organohydrogensiloxane.4) combining, under conditions to effect a second hydrosilylation reaction, starting materials comprisingthe first hydrosilylation reaction product or a) the organohydrogensiloxane, optionally b) a second hydrosilylation reaction catalyst, andc) a reactive species having an average, per molecule at least one aliphatically unsaturated group capable of undergoing an addition reaction with a silicon bonded hydrogen atom of a) the organohydrogensiloxane and further comprising a moiety comprising a functional group;thereby preparing a second hydrosilylation reaction product comprising the organosiloxane;optionally 5) adding a thiuram disulfide to the second hydrosilylation reaction product; and optionally 6) recovering the organosiloxane.

[0009] In the method above, the first hydrosilylation reaction product comprising the organohydrogensiloxane may be prepared as follows. Step 1) comprises combining, under conditions to effect a first hydrosilylation reaction, starting materials comprising: A) a hydrosilylation reaction catalyst; B) an alkenyl-functional siloxane; and C) a cyclic polyorganohydrogensiloxane; thereby preparing the first hydrosilylation reaction product comprising the organohydrogensiloxane. The starting materials used the method may optionally further comprise an additional starting material selected from the group consisting of D) a solvent, E) a hydrosilylation reaction inhibitor, F) a thiuram disulfide compound, and a combination thereof.

[0010] The first hydrosilylation reaction in step 1) may be carried out batchwise, semi-batch or continuous in any suitable equipment, such as a jacketed reactor with agitation means such as an impeller or baffles. Step 1) may be performed with mixing and heating, e.g., at a temperature of 50 °C to 100 °C, alternatively 60 °C to 90 °C, and alternatively 70 °C to 80 °C. The starting materials used in step 1) may be combined by any convenient means. For example, one or more of the starting materials, such as A) the hydrosilylation reaction catalyst may be dissolved in D) the solvent. The starting materials may be combined in any order. Alternatively, starting materials comprising the solvent and hydrosilylation reaction catalyst may be placed in a reactor, and a mixture comprising the cyclic polyorganohydrogensiloxane and the alkenyl-functional siloxane may be metered into the reactor. Alternatively, to minimize potential for generation of hydrogen, A) the hydrosilylation reaction catalyst may be kept separate from C) the cyclic polyorganohydrogensiloxane until reaction begins. For example, A) the hydrosilylation reaction catalyst, B) the alkenyl-functional siloxane, and optionally all or a portion of D) the solvent may be combined and the resulting mixture metered into a reactor containing C) the cyclic polyorganohydrogensiloxane or a mixture of C) the cyclic polyorganohydrogensiloxane and all or a portion of D) the solvent. Starting material E) the hydrosilylation reaction inhibitor may be added to one or both of the above mixtures to control hydrosilylation reaction rate.

[0011] The method for preparing the first hydrosilylation reaction product comprising the organohydrogensiloxane may optionally further comprise one or more additional steps. For example, the method may optionally further comprise, before step 1), treating (e.g., by stripping or distilling) one or more of the starting materials. For example, starting material B) and / or starting material C) may be treated to remove water (drying) or other impurities before step 1). Alternatively, the method may further comprise 2) purifying the organohydrogensiloxane produced during step 1). For example, after formation of first hydrosilylation reaction product comprising the organohydrogensiloxane, purifying may be performed by any convenient means, such as stripping and / or distillation with heating and optionally reduced pressure. The method may optionally further comprise step 3): adding F) the thiuram disulfide compound. All or a portion of the thiuram disulfide compound may be added during step 1). Alternatively, F) the thiuram disulfide compound may be added during step 1), for example, when the first hydrosilylation reaction will be carried out in the presence of the Pt-Thiuram complex at temperatures such as 80 °C to 90 °C. Alternatively, all or a portion of F) the thiuram disulfide compound may be added to the first hydrosilylation reaction product comprising the organohydrogensiloxane after step 1) or after step 3), when step 2) is performed after step 3). Alternatively, the thiuram disulfide compound may be added to the first hydrosilylation reaction product after step 1) and before step 3) (e.g., to minimize potential for gelation of theorganohydrogensiloxane during storage or purification in step 3), when step 3) is present. The thiuram disulfide compound may optionally be delivered in a solvent, such as starting material D). When step 1) uses a platinum catalyst for starting material A), then step 2) is present, and F) the thiuram disulfide compound may be present in the first hydrosilylation reaction product. Without wishing to be bound by theory, it is thought that the selection and amount of F) the thiuram disulfide compound, and when it is added during the method depends on various factors including the selection and amounts of starting materials A) and B).

[0012] Hydrosilylation reaction catalysts suitable for starting material A) in the method for preparing the first hydrosilylation reaction product comprising the organohydrogensiloxane are known in the art and are commercially available. Hydrosilylation reaction catalysts include platinum group metal catalyst, e.g., the hydrosilylation catalyst can be a metal selected from platinum, rhodium, ruthenium, palladium, osmium, and iridium. Alternatively, the hydrosilylation catalyst may be a compound of such a metal, for example, chloroplatinic acid (Speier’s Catalyst), hexachloroplatinic acid hexahydrate, platinum dichloride, and complexes of said compounds with organopolysiloxanes or platinum compounds microencapsulated in a matrix or coreshell type structure. Complexes of platinum with alkenyl-functional organopolysiloxanes include l,3-diethenyl-l,l,3,3-tetramethyldisiloxane complexes with platinum (Karstedt’s Catalyst) and methylvinylcyclosiloxane complexes with platinum (Ashby’s Catalyst). These complexes may be microencapsulated in a resin matrix. Exemplary hydrosilylation reaction catalysts are described in US Patent 12195593 and the references cited therein. Alternatively, in step 1) of the method, the platinum group metal may be platinum. The amount used may be sufficient to provide 1 ppm to 1,000 ppm of platinum group metal based on combined weights of starting materials A), B), and C). Alternatively, in step 1), the amount of platinum may be up to 5 ppm, alternatively < 5 ppm, alternatively up to 2 ppm, and alternatively < 2ppm; while at the same time, the amount of platinum is > 0 ppm, alternatively at least 1 ppm, each based on combined weights of starting materials A), B), and C). Without wishing to be bound by theory, it is thought that using > 0 ppm to 5 ppm, alternatively 1 ppm to 5 ppm, of platinum may minimize side reactions such as crosslinking and / or gelation, particularly because the alkenyl-functional siloxane has a short chain.

[0013] Starting material B) used in the method described above is an alkenyl-functional siloxane. The alkenyl-functional siloxane, may be selected from the group consisting of B-l) R3R3R3RA1R3| RAr| RAr| R3| . RAr| R3RV1O RV1and B-2) RV1O O RV1, wherein each RA|is anindependently selected monovalent aromatic group, each R3is an independently selected alkyl group, and each RV1is an independently selected alkenyl group. Suitable alkenyl groups for RV1may have 2 to 6 carbon atoms and are exemplified by vinyl, allyl, and hexenyl. Alternatively, each RV1may be vinyl. Suitable alkyl groups for R3may have 1 to 20 carbon atoms. Suitable alkyl groups may be linear or branched and include methyl, ethyl, and propyl (including n-propyl and isopropyl). Alternatively, each R3may be methyl. The monovalent aromatic group for RA|may have 6 to 20 carbon atoms. The aromatic groups may be monocyclic or polycyclic, alternatively monocyclic. Examples of suitable aromatic groups for RArinclude phenyl, tolyl, xylyl, 1 -phenylethyl, 2-phenylethyl, 2-methyl-2-phenylethyl, 3 -phenylpropyl, 4-phenylbutyl, benzyl, styryl, naphthyl and anthracenyl. Alternatively, RArmay be selected from the group consisting of phenyl, tolyl and xylyl. Alternatively, RA|may be selected from the group consisting of phenyl and tolyl. Alternatively, each RA1may be phenyl. Examples of alkenyl-functional siloxanes for starting material B) include l,5-divinyl-l,l,5,5-tetramethyl-3,3-diphenyltrisiloxane with CAS #18586-22-6, which is available from various sources, such as TCI America and Cymit Quimica S.L. of Barcelona, Spain; and l,3-divinyl-l,3-dimethyl-l,3-diphenyldisiloxane with CAS #2627-97-6 and which is available from various sources such as Alpha Chemistry of Holbrook, New York, USA.

[0014] Starting material C) for the method described herein is a cyclic polyorganohydrogensiloxane of formula C-l): (R1HSiO2 / 2)v, where subscript v has an average value of 4 to 20, and each R1is an independently selected monovalent hydrocarbyl group, alternatively an alkyl group, which may be as described and exemplified above for R3.Alternatively, subscript v may have an average value of at least 4, alternatively at least 5, and alternatively at least 6; while at the same time subscript v may have a value up to 20, alternatively up to 15, alternatively up to 12, alternatively up to 10, alternatively up to 8, and alternatively up to 6. Alternatively, subscript v may have an average value of 4 to 10, and alternatively 4 to 8. Alternatively, subscript v may have an average value of 4 to 6, alternatively 4 to 5, alternatively > 4 to 5, and alternatively 4.5 to 5. In formula C-l), R1may be an alkyl group of 1 to 6 carbon atoms. Alternatively, each R1may be independently selected from methyl, ethyl, or propyl. Alternatively, each R1may be methyl.

[0015] Examples of suitable cyclic polyorganohydrogensiloxanes for starting material C) include tetramethylcyclotetrasiloxane (with CAS No. 2370-88-9), pentamethylcyclopentasiloxane (with CAS No. 6166-86-5), hexamethylcyclohexasiloxane (with CAS No. 6166-87-6), and combinations of two or more thereof. Suitable cyclic polyorganohydrogensiloxanes are known in the art and are commercially available, e.g., DOWSIL™ MH- 1109 Fluid from Dow Silicones Corporation of Midland, Michigan, USA andSIP6718.0 and SIT7530.0 both from Gelest.

[0016] The amounts of B) the alkenyl -functional siloxane and C) the cyclic polyorganohydrogensiloxane may be in the method used in amounts such that the molar ratio of cyclic polyorganohydrogensiloxane : alkenyl-functional siloxane, C:B, is > 2:1, alternatively > 3:1, alternatively > 4:1, and alternatively > 6:1. Alternatively, starting materials B) and C) may be used in amounts such that the content of silicon bonded hydrogen atoms in starting material C) to content of silicon bonded alkenyl in starting material B) (SiH : Vi mole ratio) is 10:1 to 40:1, alternatively 10:1 to 20:1, and alternatively 10:1 to 15:1. Alternatively, SiH : Vi ratio may be at least 4: 1, alternatively at least 6:1, alternatively at least 8:1, alternatively at least 9:1, alternatively at least 12:1, alternatively at least 13:1, alternatively at least 14:1, alternatively at least 15:1, and alternatively at least 45:1; while at the same time, SiH : Vi ratio may be up to 180 : 1, alternatively up to 90: 1; alternatively up to 50:1. Alternatively, the SiH : Vi ratio may be 4:1 to 8:1, and alternatively 4:1 to 6:1.

[0017] Starting material D is the solvent, which optionally may be used in the method described herein. The solvent may facilitate introduction of certain starting materials, such as A) the hydrosilylation reaction catalyst and / or F) the thiuram disulfide. Solvents used herein are those that help fluidize the starting materials. Solvent may be selected based on solubility the starting materials and volatility of the solvent. The solubility refers to the solvent being sufficient to dissolve and / or disperse the starting materials. Volatility refers to vapor pressure of the solvent.

[0018] Suitable solvents may be hydrocarbons. Suitable hydrocarbons include aromatic hydrocarbons such as benzene, toluene, or xylene: and / or aliphatic hydrocarbons such as heptane, hexane, or octane. Alternatively, the solvent may be a halogenated hydrocarbon such as dichloromethane, 1,1,1 -tri chloroethane or methylene chloride. Alternatively, the solvent may comprise an alcohol, exemplified by a monohydric alcohol, such as isopropanol, which may be used, for example to deliver the hydrosilylation reaction catalyst. For example, certain catalysts, such as chloroplatinic acid hexahydrate, may be delivered in an alcohol.

[0019] The amount of solvent can depend on various factors including the type of solvent selected and the amount and type of other starting materials selected. However, the amount of solvent may range from 0.1% to 99%, alternatively 2% to 50%, based on combined weights of A) the hydrosilylation reaction catalyst, B) the alkenyl-functional siloxane, and C) the cyclic polyorganohydrogensiloxane.

[0020] Starting material E) is a hydrosilylation reaction inhibitor that may be used in the method for making the first hydrosilylation reaction product comprising the organohydrogensiloxane. The hydrosilylation reaction inhibitor may be for example, anacetylenic alcohol such as methyl butynol or ethynyl cyclohexanol, a silylated acetylenic alcohol, an unsaturated hydrocarbon diester; a conjugated ene-yne, an olefinic siloxane, a maleate, a fumarate, or a combination thereof. The amount of inhibitor may be an amount effective to control hydrosilylation reaction rate because hydrosilylation reaction is exothermic. The amount of inhibitor selected depends on various factors including the type and amount of hydrosilylation reaction catalyst and inhibitor selected, however, if used, the amount may be sufficient to provide 1 ppm to 1,000 ppm of the platinum group metal based on combined weights of reactants (e.g., B) the alkenyl-functional siloxane and C) the cyclic polyorganohydrogensiloxane). Suitable hydrosilylation reaction inhibitors are known in the art and are described, for example, described as ingredient i) in US Patent 9593209 at col. 15, line 35 to col. 16, line 17. Alternatively, the first hydrosilylation reaction may be performed in a semi-batch or continuous process, such that a hydrosilylation reaction inhibitor described herein as starting material E) is not required, for example the exothermic hydrosilylation reaction can be controlled by the order of addition of the starting materials, e.g., by metering starting materials B) and / or C).

[0021] Starting material F) is a thiuram disulfide compound (thiuram disulfide). Without wishing to be bound by theory, it is thought that the thiuram disulfide will complex with the platinum from A) the hydrosilylation reaction catalyst (when a platinum catalyst is used) to form an inhibited platinum at temperatures of 120 °C and lower, alternatively 100 °C and lower, alternatively 80 °C and lower, such that the inhibited platinum does not catalyze a hydrosilylation reaction, and such that side reactions such as gelation of the organohydrogensiloxane are minimized or avoided during purification, storage, or both, as described herein. The thiuram disulfide may have formula F- 1):S RJrNS F- 1 ), wherein RH, RN, RJ, and RKare each an independently selected monovalent hydrocarbyl group having 1 to 20 carbon atoms, which may be saturated or unsaturated; a heteroatom-containing monovalent hydrocarbyl group having 1 to 20 carbon atoms, which may be saturated or unsaturated; or combinations thereof. Suitable heteroatoms may include, for example, an oxygen atom. RHand RNgroups may combine to form one or more carbocyclic groups having 4 to 20 carbon atoms. RJand RKgroups may combine to form one or more carbocyclic groups having 4 to 20 carbon atoms.

[0022] In formula F-l), RH, RN, RJ, and RKcan be the same or different, and alternatively, these groups may be the same. Alternatively RH, RN, RJ, and RKmay be each independentlyselected from an alkyl group having 1 to 20 carbon atoms, alternatively 1 to 12, alternatively 1 to 6, alternatively 1 to 4, or alternatively 1 to 2 carbon atoms; an aromatic group having 6 to 20 carbon atoms, such as phenyl or benzyl; or combinations thereof. Alternatively, RH, RN, RJ, and RKare each independently selected alkyl groups. Alternatively, RH, RN, RJ, and RKare each independently selected from methyl, iso-butyl, n-butyl, or combinations thereof.

[0023] Specific examples of suitable thiuram disulfides include tetrabenzylthiuram disulfide (with CAS No. 10591-85-2), tetramethylthiuram disulfide (with CAS No. 137-26-8), tetraethylthiuram disulfide (with CAS No. 97-77-8), tetra(iso-propyl)thiuram disulfide, tetra(iso-butyl)thiuram disulfide (with CAS No. 3064-73-1), and tetra(n-butyl)thiuram disulfide (with CAS No. 1634-02-2), all of which are commercially available from various sources such as Sigma-Aldrich, Inc., TCI America, Fischer Scientific, or Cymit Quimica S.L. Alternatively, the thiuram disulfide may be selected from tetramethylthiuram disulfide, tetra(n-butyl)thiuram disulfide, or mixtures thereof.

[0024] The thiuram disulfide may be optionally diluted in a solvent before use in the method. The solvent may be any material that can dissolve the thiuram disulfide, as described and exemplified above for starting material D). Alternatively, the solvent for the thiuram disulfide may be selected from aromatic hydrocarbons such as benzene, halogenated hydrocarbons, ethers, or mixtures thereof. Without wishing to be bound by theory, it is thought that it may be desirable to use as little solvent as possible to facilitate dissolving the thiuram disulfide and, if desired, to later remove the solvent, e.g., by evaporation, distillation, and / or stripping. Examples of suitable solvents may include halogenated hydrocarbons such as dichloromethane, chloroform (CHCb), and / or tetrachloromethane. The solvent may be used in an amount of 0.1% to 5% by weight based on the weight of the thiuram disulfide.

[0025] The thiuram disulfide compound may be added in an amount such that the molar ratio of the thiuram disulfide to platinum in the hydrosilylation reaction catalyst (F / Pt ratio) may range from 0.9 to 100. Alternatively, this molar ratio may be 1 or higher, alternatively greater than 1, alternatively 1.1 or higher, and alternatively 1.2 or higher, alternatively 2 or higher, alternatively 3 or higher, alternatively 4 or higher, alternatively 5 or higher, alternatively 6 or higher, alternatively 7 or higher, alternatively 8 or higher, a alternatively 9 or higher; while at the same time this ratio may be 100 or lower, alternatively 75 or lower, alternatively 50 or lower, alternatively 40 or lower, alternatively 30 or lower, alternatively 20 or lower, alternatively 10 or lower, alternatively 5 or lower, alternatively 3 or lower, alternatively 2 or lower, and alternatively 1.2 or lower. Alternatively, this F / Pt ratio may be 1 to 10, alternatively 1 to 5, alternatively 2 to 5, alternatively 2 to 3.5, alternatively 1 to 2, and alternatively, 1 to 1.2.Alternatively, at low platinum concentration (e.g., > 0 ppm to 5 ppm based on combined weightsof starting materials A), B), and C) described above), the F / Pt ratio may be 3 to 3.5, and this may allow for higher purification (e.g., stripping) temperatures. Without wishing to be bound by theory, it is thought that the Pt-thiuram complex is stable at temperatures below 120 °C, alternatively 115 °C or below, and alternatively 110 °C or below. Therefore, stripping under conditions of 95 °C at 0 - 3 mbar wherein the Pt-Thiuram complex is stable can be performed while gelation is avoided or minimized.

[0026] The first hydrosilylation reaction product of the method described above comprises a) the organohydrogensiloxane. This reaction product may further comprise unreacted starting materials (e.g., unreacted B) alkenyl-functional siloxane or unreacted C) cyclic polyorganohydrogensiloxane, when one or the other is used in molar excess), residual A) hydrosilylation reaction catalyst, and when used D) the solvent, E) the hydrosilylation reaction inhibitor, and / or F) the thiuram disulfide compound, at least a portion of which may be complexed with the platinum from A) the hydrosilylation reaction catalyst. The organohydrogensiloxane a) comprises formula a-1):independently has an average value of 2 to 18 (i.e., n = (v - 2), where subscript v has an average value of 4 to 20 as defined above), and R1, D, and L are as described above. Alternatively, each subscript n independently may have an average value from 2 to 4, alternatively > 2 to 4, alternatively > 2 to 3, and alternatively 2.5 to 3, and alternatively 3.

[0027] Alternatively, the organohydrogensiloxane may comprise formula a-2):R3, RAr, and subscript n are as described above. Alternatively, the organohydrogensiloxane may comprise formula a-3):where each subscript n independently has an average value of 2 to 4, and Ph means phenyl.

[0028] Alternatively, the organohydrogensiloxane may comprise formula a-4):and subscript n are as described above. Alternatively, the organohydrogensiloxane maywhere each subscript n independently has an average value of 2 to 4, and Ph means phenyl. One skilled in the art would recognize that the formulas shown above are not limiting. In addition to the compounds with the formulas shown above, one skilled in the art would recognize that the first hydrosilylation reaction product may further comprise additional species that may have more than two cyclic groups per molecule and more than one linear group L bonded to a cyclic group via the divalent hydrocarbyl group D. For example, a silicon bonded hydrogen atom in a cyclic group may optionally be replaced with a group of formula, where D, R1and subscript n are as described above.and subscript n are as described above, may be present e.g., as an impurity in the cyclic siloxane starting material or when water is present during the first hydrosilylation reaction.

[0029] The organohydrogensiloxane (e.g., either in the first hydrosilylation reaction product or purified in step 3) described above) may be used as an intermediate for further reaction, as follows. The method described above further comprises functionalizing the above-described a) organohydrogensiloxane to form a’) the anhydride functionalized cyclic polyorganosiloxane (organosiloxane). The method for functionalizing a) the organohydrogensiloxane comprises step 4): combining, under conditions to effect a second hydrosilylation reaction, starting materials comprising the first hydrosilylation reaction product, or a) the organohydrogensiloxane, as described above; optionally b) a hydrosilylation reaction catalyst; and c) a reactive species having an average, per molecule, an anhydride moiety and at least one aliphatically unsaturated group capable of undergoing an addition reaction with a silicon bonded hydrogen atom of starting material a) the organohydrogensiloxane; thereby preparing a second hydrosilylation reaction product comprising a’) the organosiloxane.

[0030] Briefly stated, this method may be performed by modifying the method described in US Patent 9593209. The first hydrosilylation reaction product or a) the organohydrogensiloxane described hereinabove may be combined with the reactive species and optionally the hydrosilylation reaction catalyst (described as components c) and d), respectively) in the amounts and under conditions described in US Patent 9593209 at col. 8, line 44 to col. 10, line 47. The hydrosilylation reaction may be carried out batchwise or continuous in any suitable equipment, such as a jacketed reactor with agitation means such as an impeller or baffles.

[0031] In the method to form a’) the organosiloxane described herein, the hydrosilylationreaction may be performed by optionally dissolving or dispersing b) the hydrosilylation reaction catalyst (as described above for starting material A)) in d) a solvent (such as that described above as starting material D)) to facilitate mixing. Starting materials comprising a) the organohydrogensiloxane and c) the reactive species may be placed in the reactor with b) the hydrosilylation reaction catalyst, and the other of c) the reactive species and a) the organohydrogensiloxane may be fed into the reactor continuously or intermittently to control any exotherm. The reactor may be heated or cooled, such that the reaction mixture may be maintained a temperature of 50 °C to 150 °C, alternatively 60 °C to 100 °C, alternatively 70 °C to 90 °C. The same reactor used to prepare the first hydrosilylation reaction product may be used herein to prepare the second hydrosilylation reaction product comprising a’) the organosiloxane. Alternatively, a different reactor may be used.

[0032] Alternatively, the method for functionalizing a) the organohydrogensiloxane to form a’) the organosiloxane may optionally further comprise an additional step. For example, this method may further comprise iii) adding e) a hydrosilylation reaction inhibitor to the hydrosilylation reaction product; and / or iv) recovering the organosiloxane from the hydrosilylation reaction product. Recovering may be performed by any convenient means, such as stripping and / or distillation with heating, and optionally under vacuum.

[0033] Hydrosilylation reaction catalysts suitable for starting material b) in the method for functionalizing the organohydrogensiloxane as described and exemplified above for starting material A) in the method for preparing the first hydrosilylation reaction product comprising the organohydrogensiloxane. Starting material b) is optional, for example, additional hydrosilylation reaction catalyst may not be needed if starting material A) is present in the first hydrosilylation reaction product or if said catalyst is not inhibited, deactivated, or removed from the organohydrogensiloxane of formula a-1). Alternatively, starting material b) may be added when A) the hydrosilylation reaction catalyst used to make the organohydrogensiloxane is a platinum hydrosilylation reaction catalyst that is complexed with F) the thiuram disulfide in the method as described above. Alternatively, starting material b) may not be needed even if A) the platinum hydrosilylation reaction catalyst is complexed with F) the thiuram disulfide in the first hydrosilylation reaction product if the conditions (e.g., temperature) selected for the method for functionalizing the organohydrogensiloxane are sufficient to decomplex starting materials A) and F). Starting material b) may be the same or a different species as that selected for use above to make the first hydrosilylation reaction product comprising organohydrogensiloxane. For example, starting material b) may be a hydrosilylation reaction catalyst comprising a platinum group metal other than platinum, e.g., a rhodium catalyst. However, the amount of the hydrosilylation reaction catalyst used in this method to functionalize theorganohydrogensiloxane may be sufficient to provide 1 ppm to 1,000 ppm of platinum group metal based on combined weights of starting materials a), b), and c). Alternatively, when starting material b) is used, it may be added at a concentration of 1 ppm or more, alternatively 10 ppm or more, alternatively 20 ppm or more, alternatively 30 ppm or more, alternatively 40 ppm or more, alternatively 50 ppm or more, alternatively 60 ppm or more, alternatively 70 ppm or more, alternatively 80 ppm or more, alternatively 90 ppm or more, alternatively 100 ppm or more, alternatively 120 ppm or more, alternatively 140 ppm or more, alternatively 160 ppm or more, alternatively 180 ppm or more; while at the same time starting material b) may be added at a concentration of 200 ppm or less, alternatively 180 ppm or less, alternatively 160 ppm or less, alternatively 140 ppm or less, alternatively 120 ppm or less, alternatively 110 ppm or less, alternatively 100 ppm or less, alternatively 80 ppm or less, on the same basis above.

[0034] Starting material c) the reactive species introduced above for functionalizing a) the organohydrogensiloxane is an unsaturated anhydride. The unsaturated anhydride is any suitable compound that can produce the anhydride group described herein via hydrosilylation reaction with a silicon bonded hydrogen atom. By the term “anhydride functionality” it is meant that the anhydride group for R2comprises the following structure: -C(=O)O-C(=O)-. Unsaturated anhydrides include maleic anhydride, alkenyl succinic anhydrides such as allyl succinic anhydride (CAS # 7539-12-0), polyisobutylenylsuccinic anhydride, bromomaleic anhydride, crotonic anhydride (CAS # 623-68-7), itaconic anhydride (CAS # 2170-03-8), nadic anhydride (CAS # 25134-21-8), and cis-1,2,3,6- tetrahydrophthalic anhydride (CAS # 935-79-5), all of which are commercially available from sources such as Sigma-Aldrich, Inc. of St. Louis, Missouri, USA, or TCI America. The anhydride functionality may also be formed from unsaturated anhydrides featuring bridged heterocyclic structures, such as bicyclooctenedicarboxylic anhydrides such as CAS # 6708-37-8, carbic anhydrides (CAS # 129-64- 6), bicyclooctenetetracarboxylic dianhydrides such as bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (CAS # 1719-83-1), ethenocyclobutabenzofuran-triones such as CAS # 55054-47-2, and ethenocycloheptafuran-diones such as CAS # 5650-01-1 and their isomeric variants. For example, the anhydride functionality in the anhydride group for R2can be, and alternatively is, a cyclic anhydride i.e., in a five-membered or six membered ring.Alternatively, c) the unsaturated anhydride may comprise one or more of allyl succinic anhydride (CAS # 7539-12-0): allyl maleic anhydride; allyl phthalic anhydride; 3-(2-methallyl)succinic anhydride); dihydro-3-(l,l,2-trimethyl-2-propen-l-yl)-2,5-furandione; 3-(l,2-dimethyl-2-propen-l-yl)dihydro-2,5-Furandione; and 3-(2-neopentylallyl)tetrahydrofuran-2,5-dione.

[0035] The amount of c) the unsaturated anhydride depends on various factors including thedesired degree of substitution of the organosiloxane. For example, the amount of c) the unsaturated anhydride may be sufficient to react all silicon bonded hydrogen atoms in a) the organosiloxane or an excess, e.g., a molar ratio of silicon bonded hydrogen atoms from a) the organosiloxane to aliphatically unsaturated groups from c) the unsaturated anhydride (SiH:vinyl ratio) may be < 1 : 1 to 1 : 1. Alternatively, it may be desirable for the organosiloxane to have both silicon bonded hydrogen atoms and anhydride-functional groups derived from c c) the unsaturated anhydride. In this instance, SiH:Vi ratio may be > 1:1. Alternatively, starting materials a) and c) may be used in amounts such that an average of two silicon bonded hydrogen atoms per molecule are replaced with functional groups derived from c) the unsaturated anhydride via the hydrosilylation reaction.

[0036] Starting material e) the hydrosilylation reaction inhibitor may be as described and exemplified above for starting material E) in the method for preparing the first hydrosilylation reaction product comprising a) the organohydrogensiloxane. The amount of e) inhibitor selected for use in this method for preparing the second hydrosilylation reaction product comprising a’) the organosiloxane depends on various factors including the type and amount of catalyst and inhibitor selected, however, the amount may be 0.00001 to 3 parts by weight, per 100 parts by weight of c) the reactive species.

[0037] The starting materials used in the method for functionalizing the organohydrogensiloxane may optionally further comprise one or more additional starting materials. The additional starting materials may be those additional ingredients disclosed in US Patent 9593209 at col. 10, line 48 to col. 16, line 17. The additional starting materials selected from the group consisting of filler, with or without treating agent, non-reactive resin, chain extender, endcapper, and hydrosilylation reaction catalyst inhibitor as described above.

[0038] The method described above produces the second hydrosilylation reaction product comprising a’) the organosiloxane. The organosiloxane comprises formula a’-l):as described above, each D is an independently selected divalent hydrocarbyl group of 2 to 6 carbon atoms, and each R2is independently selected from the group consisting of H and an anhydride functional group (which is derived from c) the unsaturated anhydride viahydrosilylation reaction of the alkenyl group in the alkenyl-functional anhydride), with the proviso that at least one R2per molecule is the anhydride -functional group (z.e., at least one instance of R2per molecule is not hydrogen). Alternatively, 1 to 4 instances of R2per molecule are functional groups (i.e., other than hydrogen). Alternatively 1 to 3, alternatively 1 to 2, and alternatively an average of two instances of R2per molecule are the anhydride-functional groups (other than hydrogen). Alternatively, one instance of R2on each cyclic siloxane ring may be the anhydride -functional group and the other instances of R2may be H. Alternatively, two instances of R2on each cyclic siloxane ring may be the anhydride -functional group and the other instances of R2may be H. Alternatively, three instances of R2on each cyclic siloxane ring may be the anhydride-functional group and the other instances of R2may be H. Alternatively, a’) may be fully functionalized, wherein each instance of R2on each cyclic siloxane ring is the functional group (with no instances of R2being H). The anhydride-functional group for R2is derived from starting material c) the unsaturated anhydride described above. Alternatively, in formula a’-l) each subscript n may independently have an average value of 2 to 4, alternatively > 2 to 4, alternatively 2 to 3, alternatively > 2 to 3, alternatively 2, and alternatively 3.

[0039] Divalent hydrocarbon group D has 2 to 6, alternatively 2, 3, or 6 carbon atoms. D may be linear or branched and may be an alkane-diyl group. Examples of D include, -CH2-CH2-, -CH (CH3)-, -CH2-CH(CHS)-, -CH2-CH2-CH2-, and combinations thereof. Alternatively, each D may be selected from , -CH2-CH2- and -CH (CH3)-. Alternatively, each D may be , -CH2-CH2-.

[0040] Alternatively, the organosiloxane may comprise formula a’ -2):subscript n, D, R3, and RA|are as described and exemplified above. Alternatively, the organosiloxane may comprise formula a’ -3):subscript n has an average value of 2 to 4, each D1is independently selected from the group consisting of -CH2CH2- and -CH(CH3)-, Ph means phenyl, and each R2is H or a propyl succinic anhydride group, with the proviso that at least one instance of R2per molecule is the propyl succinic anhydride group.

[0041] Alternatively, the organosiloxane may comprise formula a’ -4):n, D, R3, and R^ are as described and exemplified above. Alternatively, the organosiloxane maywhere each subscript n has an average value of 2 to 4, each D1is independently selected from the group consisting of -CH2CH2- and -CH(CH )-, Ph means phenyl, and each R2is H or a propyl succinic anhydride group, with the proviso that at least one instance of R2per molecule is the propyl succinic anhydride group. One skilled in the art would recognize that the formulas shown above are not limiting. In addition to the species with the formulas shown above, one skilled in the art would recognize that the second hydrosilylation reaction reaction product may further comprise additional species that may have more than two cyclic groups per molecule and more than one linear group L bonded to a cyclic group via the divalent hydrocarbyl group D. For example, a group R2may optionally be replaced with a group of formulawhere D, R1, R2, and subscript n are as describedabove. In addition, a side product may be present, such asR1R1R2- Si — O R1R1O - Si - R2, where R1, R2, and subscript n are as described above, e.g„ as an impurity in the cyclic siloxane starting material or when water is present during the second hydrosilylation reaction.

[0042] The organosiloxane of formula a’ -2), a’ -3), a’ -4), and / or a’ -5) described above may be used as an adhesion promoter in a curable silicone composition, such as a liquid silicone rubber composition. The organosiloxane of formulae a’ -2), a’ -3), a’ -4), and a’-5) are useful in curable silicone compositions as adhesion promoters.

[0043] A curable silicone composition may comprise: (I) the organosiloxane of formulae a’-2), a' -3), a’ -4), and / or a’ -5); and (II) a silicone composition. The organosiloxane may be added to the silicone composition as an adhesion promoter, i.e., that increases adhesion of a cured silicone (prepared by curing the curable silicone composition) as compared to a cured silicone prepared from the same silicone composition, but that does not contain the above described I) organosiloxane as adhesion promoter.

[0044] The curable silicone composition may comprise:the organosiloxane of formulae a’ -2), a’ -3), a’ -4), and / or a’ -5);a divinyl-terminated polyphenylsiloxane;a vinyl-terminated polyphenylsiloxane resin;a hydrogenphenylsiloxane; anda hydrosilylation catalyst.

[0045] The term “divinyl-terminated polyphenylsiloxane” is preferably a compound of Formula 5:Ph \ MeS Ii - O I — ) — S1i_Formula 5where Ph is phenyl; each R' is independently Ci-Ce-alkyl or phenyl; and n is from 1 or from 5 or from 10 to 500 or to 200 or to 100. Preferred Ci-Ce-alkyl groups are methyl groups. Preferably,each R' is methyl. Preferably, the concentration of the divinyl-terminated polyphenylsiloxane, is in the range of from 1 or from 2 or from 4 weight percent, to 30 or to 10 or to 8 weight percent, based on the weight of the composition.

[0046] The vinyl-terminated polyphenylsiloxane resin is conveniently prepared by reacting together a tri-C i-Ce-alkoxyphenylsilane and a compound of Formula 6:Formula 6where n' is from 1 to 20, preferably to 10, and more preferably to 5; most preferably, n' is 1 and each R' is methyl. This most preferred vinyl-terminated polyphenylsiloxane resin, MMePhV1aTPhb, where a and b are mole fractions, wherein a + b = 1, can be conveniently prepared by contacting trimethoxyphenylsilane with l,3-dimethyl-l,3-diphenyl-l,3-divinyldisiloxane in the presence of an acid catalyst. Mole fraction a is preferably in the range of from 0.10 to 0.40 and mole fraction b is preferably in the range of from 0.60 to 0.90. MMePhV1is represented by the following fragment:Meand Tphis represented by the following fragment:PhIO - Si - O / I \O'.where the dotted lines represent bonds to other silicon atoms in the vinyl-terminated polyphenylsiloxane resin. Preferably, the concentration of the vinyl-terminated polyphenylsiloxane resin is in the range of from 50 to 80 weight percent, based on the weight of the composition.

[0047] The term “hydrogenphenylsiloxane” refers to a compound of Formula 7:where each R" is independently phenyl or Ci-Ce-alkyl, with the proviso that at least one of the R" groups is a phenyl group; c, d, e, and f are mole fractions wherein c + d + e + f = 1; wherein c is from 0.01 to 0.75; d is from 0 to 0.4; e is from 0 to 0.96; and f is from 0 to 0.6;wherein M1®"2, DHR", DR 2and, TR" are defined as follows:R" R" R" oH - S Ii - O— w. — O - Sli - O — — O - Sli - 0 — — O - Sii - O —R I" H I R I" R I"M1®"2D1®" DR 2TR"

[0048] An example of a hydrogenphenylsiloxane is a compound of Formula 7a:Formula 7 awhere m is from 1 to 50 or to 20 or to 10. Preferably m is 1. Preferred Ci-Ce-alkyl groups are methyl groups. Preferably, each R is phenyl. Preferably, the concentration of the hydrogenphenylsiloxane is in the range of from 10 to 30 weight percent.

[0049] The hydrosilylation catalyst is a catalyst that promotes hydrosilylation, such as those described above as starting material A). Alternatively, the hydrosilylation catalyst in the curable silicone composition may be selected from the group consisting of platinum(II) acetoacetonate, platinum(O) l,3-divinyl-l,l,3,3-tetramethyldisiloxane complex and trimethyl(methylcyclopentadienyl)platinum (IV) .

[0050] The curable silicone composition may optionally further comprise one or more additional starting materials. For example, the curable silicone composition may further comprise a filler, such as fumed silica. Alternatively, the composition may optionally further comprise an alkoxysilane, e.g., methyltrimethoxysilane. The curable silicone composition may further contain an inhibitor for the hydrosilylation catalyst may be as described above, alternatively the inhibitor may be selected from phenylbutynol or methyl (tris( 1,1 -dimethyl-2-propynyl) oxy) silane. The curable silicone composition may optionally further comprise a pigment such as STAN-TONE 40SP03 Blue pigment.

[0051] Alternatively, the curable silicone composition of the present invention may form a coating for a variety of substrates such as paper, metal, plastic, and glass. Said coating may have one or more of the following properties: optically clear, hard, and / or non-delaminating coatings.

[0052] A method of preparing an article with the curable silicone composition comprises 1 ) disposing the curable silicone composition on the substrate. The method further comprises 2) curing the curable silicone composition on the substrate. Curing may be performed by any convenient means. For example, the curable silicone composition may cure by exposure toultraviolet radiation, heating at an elevated temperature, e.g., 50 °C to 180 °C, alternatively 50 °C to 120 °C, and alternatively 50 °C to 90 °C, or both to give the article, which comprises a cured silicone (product prepared by curing the curable silicone composition) adhered to the substrate. One skilled in the art would be able to select exposure dose depending on various factors including the type and amount of catalyst in the curable silicone composition. One skilled in the art would be able to select an appropriate temperature depending on various factors including the selection of optional starting materials in the curable silicone composition and the substrate material of construction.

[0053] The curable silicone composition may be disposed or dispensed on the substrate in any suitable manner. Typically, the curable composition is applied in wet form via a wet coating technique. The curable silicone composition may be applied by i) spin coating; ii) brush coating; iii) drop coating; iv) spray coating; v) dip coating; vi) roll coating; vii) flow coating; viii) slot coating; ix) gravure coating; x) Meyer bar coating; or xi) a combination of any two or more of i) to x). Typically, disposing the curable silicone composition on the substrate results in a wet deposit on the substrate, which is subsequently cured to give the article, which comprises a cured silicone (e.g., coating or elastomer) formed from the curable silicone composition on the substrate.

[0054] The substrate is not limited and may be any substrate. The substrate may have an integrated hot plate or an integrated or stand-alone furnace for curing the wet deposit. The substrate may optionally have a continuous or non-continuous shape, size, dimension, surface roughness, and other characteristics. The substrate may comprise a plastic, which may be a thermosetting and / or thermoplastic. However, the substrate may alternatively be glass, metal (e.g., aluminum or steel), paper, wood, cardboard, paperboard, a silicone, or polymeric materials, or a combination thereof. Specific examples of suitable substrates include paper substrates such as Kraft paper, polyethylene coated Kraft paper (PEK coated paper), and regular papers; polymeric substrates such polyamides (PA); polyesters such as polyethylene terephthalates (PET), polybutylene terephthalates (PET), polytrimethylene terephthalates (PTT), polyethylene naphthalates (PEN), and liquid crystalline polyesters; polyolefins such as polyethylenes (PE), polypropylenes (PP), and polybutylenes; styrenic resins; polyoxymethylenes (POM); polycarbonates (PC); polymethylenemethacrylates (PMMA); polyvinyl chlorides (PVC); polyphenylene sulfides (PPS); polyphenylene ethers (PPE); polyimides (PI); polyamideimides (PAI); polyetherimides (PEI); polysulfones (PSU); polyethersulfones; polyketones (PK); polyetherketones; polyvinyl alcohols (PVA); polyetheretherketones (PEEK); polyetherketoneketones (PEKK); polyarylates (PAR); polyethernitriles (PEN); phenolic resins; phenoxy resins; celluloses such as triacetylcellulose, diacetylcellulose, and cellophane:fluorinated resins, such as polytetrafluoroethylenes; thermoplastic elastomers, such as polystyrene types, polyolefin types, polyurethane types, polyester types, polyamide types, polybutadiene types, polyisoprene types, and fluoro types; and copolymers, and combinations thereof. Alternatively, the substrate may be a substrate useful in the electronics industry, such as metal (e.g., aluminum), glass, or a plastic such as polybutylene terephthalate (PBT), polyamide (PA), or polycarbonate (PC).

[0055] The article may be utilized in diverse end use applications. For example, the article may be utilized in coating applications, packaging applications, adhesive applications, fiber applications, fabric or textile applications, construction applications, transportation applications, electronics applications, or electrical applications. However, the curable composition may be utilized in other applications, e.g. in the preparation of electronic devices.

[0056] The method of use of the curable silicone composition may further comprise; 3) treating the substrate before disposing the curable silicone composition on the substrate.Treating the substrate may be performed by any convenient means such as a plasma treatment or a corona discharge treatment. Alternatively, the substrate may be treated by applying a primer. In certain instances anchorage of the cured silicone may be improved if the substrate is treated before disposing the curable silicone composition thereon.

[0057] When the curable silicone composition includes a solvent, the method may further comprise: 4) removing solvent, which may be performed by any conventional means, such as heating at 50 °C to 100 °C for a time sufficient to remove all or a portion of the solvent. The method may further comprise 5) curing the curable silicone composition to form a cured silicone on a surface of the substrate, as described above.EXAMPLES

[0058] These examples are intended to illustrate the invention and should not be interpreted as limiting the scope of the invention set forth in the claims. The starting materials in Table 1 were used in the examples herein.Table 1 - Starting MaterialsName Chemical Description Supplier C1) DOWSIL™ cyclic polymethylhydrogensiloxane mixture having Dow MH- 1109, stripped DP = 4 to 6, stripped (to remove impurities afterproduction) ((CHs)HsiO2 / 2)v, where v = 4 to 6Bl) MV1DPh2MV11 ,5-divinyL 1 , 1 ,5,5-tetramethyl-3 ,3- Synthesized diphenyltrisiloxane at Dow B2) MV1PhMV1Ph1 , 3 -di vinyl- 1 , 3 -dimethyl- 1 , 3 -diphenyldi siloxane Synthesized at Dow Al) Pt Karstedt’ s catalyst DowHydrosilylationReaction CatalystName Chemical Description Supplier A2) Pt Hexachloroplatinic acid hexahydrate Sigma- Hydrosilylation (hexachloroplatinic acid : 6 H2O) Aldrich Reaction CatalystStabilizer 1 Tetra-n-butyl thiuram disulfide Fisher Hydrosilylation 1 -Ethynyl- 1 -cyclohexanol additive Sigma- Reaction Inhibitor, Aldrich ETCHSolvent 1 Toluene Sigma- Aldrich Solvent 2 IPA Isopropyl alcohol Sigma- AldrichASA Allyl succinic anhydrideExample 1 - Preparation of Compound of Formula a’ -3)A. Preparation of Intermediate AMH- 1109 VT 'rCAC Intermediate A The formula for Intermediate A in the scheme shown above is exemplary, not limiting.

[0059] A 3L 4-neck round bottom flask equipped with a dropping funnel, a multiport with 2 inlets for dry N2 and dry air, a temperature controller, a reflux condenser, and a magnetic stir bar, was placed on a hot plate. Toluene (400 g) and chloroplatinic acid hexahydrate (1 wt.% in isopropanol, 0.18 g) were added to the flask, and a mixture of DOWS IL™ MH-1109, stripped (v = 1, 2, and 3; 938 g) and MV1DPh2MV1(500 g) was loaded into the dropping funnel. The mixture in the flask was heated to 75 °C with stirring and dry air flow, followed by dropwise addition of the mixture from the dropping funnel. After addition was completed, the reaction mixture was stirred for 1 h at 75 °C. An aliquot of the reaction mixture was removed forJH NMR spectroscopic analysis to verify that the vinyl groups were fully consumed. The reaction mixture was cooled to 60 °C, at which temperature tetra-n-butyl thiuram disulfide (1 wt.% in toluene solution, 0.64 g) was added. The reaction mixture was stirred for an additional 3 h, cooled to room temperature, then transferred to another flask. The volatile materials were removed in vacuo at 95 °C and 0.1 mbar for 2 h, and the residue liquid (1014g) was transferred into a Nalgene bottle and kept under N2. The product was characterized by1H,13C, and29Si NMR spectroscopies.B. Preparation of Compound of Formula a’ -3)allyl succinic anhydride Formula a-j)

[0060] One skilled in the art would recognize that the product of Formula a’ -3) shown is representative, not limiting in that the propyl succinic anhydride groups may be bonded to different silicon atoms in the cyclic moieties, and the C2H4 groups are predominantly linear and may include some branched groups.

[0061] A 4-neck round bottom flask was charged with Intermediate A (94.1 g). The flask was equipped with a glass stir rod with a Teflon stir paddle, a cooled condenser equipped with an outlet leading to a bubbler, a thermocouple fitted with a nitrogen inlet, and an addition funnel, which was charged with allyl succinic anhydride (ASA, 26.5 g). Intermediate A was heated to 50-75 °C and stirred. A portion of ASA (1.3 g) was then added to the flask from the addition funnel, followed by addition of Karstedt’s catalyst (1 wt% solution in toluene, 0.024 g) with a micropipette. The remainder of the ASA was added slowly to ensure that the reaction temperature remained below 90 °C. After ASA addition was completed, additional Karstedt’s catalyst (1 wt% solution in toluene, 0.024 g) was added, and the reaction mixture was stirred at 80 °C for another 30 min. The reaction mixture was cooled to ambient temperature, then charged with 1-ethynyl-l -cyclohexanol (ETCH, 0.204 g), before being transferred to a Nalgene bottle. The product was characterized by1H,13C and29Si NMR spectroscopy, as well as by FTIR spectroscopy.Example 2 - Preparation of Compound of Formula a’ -5)A. Preparation of Intermediate BMH-1109 MVIP11MV1PI1Intermediate B

[0062] The formula for Intermediate B in the scheme shown above is exemplary, not limiting.

[0063] A 3L 4-neck round bottom flask equipped with a dropping funnel, a multiport with 2 inlets for dry N2 and dry air, a temperature controller, a reflux condenser, and a magnetic stir bar, was placed on a hot plate. Toluene (217 g) and chloroplatinic acid hexahydrate (1 wt.% in isopropanol, 0.10 g) were added to the flask, and a mixture of MH-1109 (v = 1, 2, and 3; 577 g)and MV1PhMV1P11(248 g) was loaded into the dropping funnel. The mixture in the flask was heated to 75 °C with stirring and dry air flow, followed by dropwise addition of the mixture from the dropping funnel. After addition was completed, the reaction mixture was stirred for 1 h at 75 °C. An aliquot of the reaction mixture was removed for 'H NMR spectroscopic analysis to verify that the vinyl groups were fully consumed. The reaction mixture was cooled to 60 °C, at which temperature tetra-ra-butyl thiuram disulfide (1 wt% in toluene solution, 0.36 g) was added. The reaction mixture was stirred for an additional 3 h, cooled to room temperature, then transferred to another flask. The volatile materials were removed in vacuo at 95 °C and 0.1 mbar for 2 h, and the residue liquid (585g) was transferred into a Nalgene bottle and kept under N2. The product was characterized byXH,13C, and29Si NMR spectroscopies.B. Preparation of the Compound of Formula a’ -5)

[0064] One skilled in the art would recognize that the product of Formula a’ -5) shown is representative, not limiting in that the propyl succinic anhydride groups may be bonded to different silicon atoms in the cyclic moieties, and the C2H4 groups are predominantly linear and may include some branched groups.

[0065] A 4-neck round bottom flask was charged with Intermediate B (173.3 g). The flask was equipped with a Teflon coated magnetic stir bar, a cooled condenser equipped with an outlet leading to a bubbler, a thermocouple fitted with a nitrogen inlet, and an addition funnel which was charged with allyl succinic anhydride (ASA, 57.4 g). Intermediate B was heated to 80 °C, followed by the addition of ca. 2.9 g ASA upon stirring. Karstedt’s catalyst (1 wt% solution in toluene, 0.030 g) was added via micropipette. Exotherm was observed immediately. ASA was added gradually at a rate to keep the reaction temperature below 100°C. After the addition of ASA was complete, additional Karstedt’s catalyst (1 wt% solution in toluene, 0.060 g) was added in two aliquots and the reaction mixture was stirred at 80 °C for another 30 minutes. The SiH consumption was monitored by a Perkin Elmer FTIR fitted with an ATR plate. After cooled to ambient temperature, the reaction mixture was charged and mixed with ETCH (0.358 g), before being transferred to a Nalgene bottle. The product was characterized by1H,13C and29Si NMR as well as FTIR and GPC.Example 3 - Preparation of UV-Heat Curable Organosiloxane Composition with Formula a’ -5) Adhesion Promoter

[0066] A curable organopoly siloxane composition was prepared by blending MV'DP1123MV1(6.5 pbw), MPhV1o.23TPho.77 (68.1 pbw), MHDPh2MH(20.4 pbw); methyl(tris(l,l-dimethyl-2-propynyl) oxy) silane (0.001 pbw); and the compound of Formula a’ -5) (1.0 pbw). The mixture was blended for 2 min at 1,500 rpm, after which time Reolsil DM-30S fumed silica (3 pbw) was added. The composition was further blended for 2 min at 2,000 rpm, then for another 2 min at 2000 rpm. 1 %-Trimethyl(methylcyclopentadienyl)platinum (IV) in methyltrimethoxysilane (1 pbw) was then added to the mixture, and blending was reinitiated for 2 min at 1,500 rpm. The sample was packaged in 30-mL syringes and vacuum sealed. The syringes were stored in an aluminum bag -5 °C. The sample was cured first by exposing it to LED UV (Firejet FJ800) at 365 nm and a UVA dosage of 5,000 mJ / cm2; the cure was completed by storing the sample in an oven at 70 °C for 30 min.Example 4 - Preparation of Pt -Catalyzed Heat Curable Organosiloxane Composition with the Compound of Formula a’ -5)

[0067] A curable organopoly siloxane composition was prepared by blending MV1Dph23MV1(6.5 pbw), MphV1o.2 Tpho.77 (68.8 pbw), MHDP112MH(20.6 pbw); methyl(tris(l,l-dimethyl-2-propynyl) oxy) silane (0.001 pbw); and the compound of Formula a’ -5)

[0068] (1.0 pbw). The mixture was blended for 2 min at 1,500 rpm, after which time Reolsil DM-30S fumed silica (3 pbw) was added. The composition was further blended for 2 min at 2,000 rpm, then for another 2 min at 2000 rpm. 0.5%- Platinum, 1,3-diethenyl-l, 1,3,3-tetramethyldisiloxane complexes in Methyltrimethoxysilane (0.04 pbw) was then added to the mixture, and blending was reinitiated for 2 min at 1,500 rpm. The sample was packaged in 30-mL syringes and vacuum sealed. The syringes were stored in an aluminum bag -5 °C. The sample was heat cured at 150 °C for 1 h.Example 5 - Preparation of UV-Heat Curable Organosiloxane Composition with the Compound of Formula a’ -3)

[0069] The composition was prepared and cured substantially as described in Example 3, except that the compound of Formula a' -3) (1.0 pbw) was used instead of the compound of Formula a’ -5).Example 6 - Preparation of Pt -Catalyzed Heat Curable Organosiloxane Composition with the Compound of Formula a’ -3)

[0070] The composition was prepared substantially and cured as described in Example 4, except that the compound of Formula a’ -3) ( 1.0 pbw) was used instead of the compound of Formula a’ -5).Comparative Example 1 - Preparation of UV-Heat Curable Organosiloxane Composition with no Adhesion Promoter

[0071] The composition was prepared substantially as described in Example 3 without the inclusion of the compound of Formula a’-5). MphV1o.23Tpho.77 was increased to 68.8 pbw and MHDP112MHwas increased to 20.7 pbw.Comparative Example 2 - Preparation of Pt -Catalyzed Heat Curable Organosiloxane Composition with no Adhesion Promoter

[0072] The composition was prepared substantially as described in Example 4 without the inclusion of the compound of Formula a’ -3). MphV1o.23Tpho.77 was increased to 69.6 pbw and MHDph2MHwas increased to 20.9 pbw.Crosshatch Procedure

[0073] ASTM D3359 was used to measure the area removed on a coated glass slide. The coated surface was etched in a crosshatched fashion and tested. The crosshatch test classifications are illustrated in Table 2.Table 2 - Crosshatch Test ClassificationsClassification % Area Removed0B > 65%IB 35-65%2B 15-35%3B 5-15%4B < 5%5B 0%Adhesion Lap Shear Testing

[0074] Lap shear testing was carried out using an Instron 3366 mechanical testing system. The cured samples (10-mm thick) were sandwiched between two 0.5-mm thick glass or aluminum (Al) substrates; each substrate was pulled and pushed parallel to the sample until breakageoccurred due to adhesive failure (AF), cohesive failure (CF), or substrate failure (SF). The results of the adhesion lap shear, crosshatch testing, and failure modes of the samples are illustrated in Table 3.

[0075] Table 3 illustrates adhesion lap shear and crosshatch classification for aluminum and glass substrates, and failure mode for glass substrates. Lap shear is measured in MPa. CF refers to cohesive failure, and AF refers to adhesion failure. For glass substrates, the minimum requirement for adhesion lap shear was > 4 MPa; for aluminum substrates, the minimum requirement for adhesion lap shear was > 3 MPa. CF and a crosshatch classification of 4B or 5B were also required.Table 3 - Failure Mode and Crosshatch EvaluationEx. 3 Ex. 4 Ex. 5 Ex. 6 CEx. 1 CEx 2 Adhesion lap shear - Glass > 5.50 > 5.50 > 5.50 > 5.50 3.86 > 5.50 Failure mode - Glass CF CF CF CF AF CF Adhesion lap shear - Al 3.80 10.69 4.30 10.16 2.49 1.70Crosshatch Classification 5B 5B 5B 5B 0B 5B

[0076] The data show that heat cured samples containing the compounds of Formulas a’ -5) and a’ -3) (Examples 4 and 6) gave superior adhesion strength for aluminum substrates as compared with Comparative Example 2, which contained no adhesion promoter. The data further show that the properties of the UV-heat cured samples containing the compounds of Formulas a’ -5) and a’ -3) (Examples 3 and 5) are superior in all respects to Comparative Example 1 , which contained no adhesion promoter.

[0077] Abbreviations used in the specification have the definitions in Table A, below.Table A - AbbreviationsAbbreviation Definition°C degrees CelsiusDP degree of polymerizationDph Difunctional siloxane unit of formula (MePhSiCFc)Dph2Difunctional siloxane unit of formula (Ph2SiO2 / 2)CT gramGC gas chromatographyGPC gel permeation chromatographyLC-MS liquid chromatography-mass spectrometryMV1Monofunctional siloxane unit of formula (ViMe2SiOi / 2)Me methylmg milligrammJ mi Hi JoulemL millilitermm millimetermPa-s milli-Pascal secondMn Number average molecular weight measured by GPCMw Weight average molecular weight measured by GPCAbbreviation DefinitionMz Z average molecular weight measured by GPCNMR nuclear magnetic resonancepbw parts by weightPh phenylPPm part per millionRT room temperature of 23 °C ± 3 °Cs secondSiH content hydrogen, as silicon bonded hydrogenpL microliterpm micrometerVi vinyl

[0078] All amounts, ratios, and percentages are by weight unless otherwise indicated. The amounts of all starting materials in a composition total 100% by weight. The SUMMARY and ABSTRACT are hereby incorporated by reference. The articles ‘a’, ‘an’, and ‘the’ each refer to one or more, unless otherwise indicated by the context of specification. The singular includes the plural unless otherwise indicated. The disclosure of ranges includes the range itself and also anything subsumed therein, as well as endpoints. Similarly, the disclosure of Markush groups includes the entire group and also any individual members and subgroups subsumed therein.

Claims

CLAIMS:

1. An organosiloxane comprising formula:each subscript n independently has a value of 2 to 18;each R1is an independently selected monovalent hydrocarbyl group;each R2is independently selected from the group consisting of H and an anhydride-functional group; with the proviso that at least one instance of R2per molecule is the anhydride-functional group;each D is independently a divalent hydrocarbyl group of 2 to 6 carbon atoms;R3R3| R^ | .PArL is a divalent linking moiety selected from the group consistingof O R3RArR3| R3| _RAr| R3^Si\ / S'\and O O , wherein each RA1is an independently selected monovalent aromatic group and each R3is an independently selected alkyl group.

2. The organosiloxane of claim 1 , whereineach subscript n independently has an average value of 2 to 4,each R1is methyl or ethyl;each R3is methyl or ethyl;each RAIis selected from the group consisting of phenyl, tolyl, and xylyl; andan average of two to four instances of R2per molecule are the anhydride-functional group.

3. The organosiloxane of claim 2 or claim 3, whereineach subscript n has an average value of 2 to 3,each R1is methyl,R3is methyl,RA1is phenyl, andeach R2is selected from H, and a propyl-succinic anhydride group.

4. The organosiloxane of claim 1, wherein the organosiloxane comprises formula:subscript n, D, R3, and R^ are as described above5. The organosiloxane of claim 1, wherein the organosiloxane comprises formula:each subscript n has an average value of 2 to 4,each D1is independently selected from the group consisting of -CH2CH2- and -CH(CHs), Ph means phenyl, andeach R2is H or a propyl succinic anhydride group, with the proviso that at least one instance of R2per molecule is the propyl succinic anhydride group.

6. The organosiloxane of claim 1, wherein the organosiloxane comprises formula:n, D, R3, and RA|are as described above.

7. The organosiloxane of claim 1, wherein the organosiloxane comprises formula:each subscript n has an average value of 2 to 4,each D1is independently selected from the group consisting of -CH2CH2- and -CH(CH3)- Ph means phenyl, andeach R2is H or a propyl succinic anhydride group, with the proviso that at least one instance of R2per molecule is the propyl succinic anhydride group.

8. A composition comprising: the organosiloxane of any one of claims 1 to 7 and a thiuram disulfide.

9. A method for preparing the organosiloxane of any one of claims 1 to 7, wherein the method comprises:1) combining, under conditions to effect a first hydrosilylation reaction, starting materials comprising:A) a hydrosilylation reaction catalyst;B) an alkenyl-functional siloxane selected from the group consisting ofR3R3R3RArR3| RAr| RAr| R3| RAr| R3RVlO RV1and RV1O O RV1, wherein R3and RArare as described above, and each RV1is an independently selected alkenyl group;C) a cyclic polyorganohydrogensiloxane of unit formula (R1HSiO2 / 2)v, wherein subscript v has an average value of 4 to 20 (v = n-2), and each R1is as described above;optionally E) a hydrosilylation reaction inhibitor;optionally D) a solvent; andoptionally all or a portion of F) a thiuram disulfide; thereby preparing a first hydrosilylation reaction product comprising a) an organohydrogensiloxane and the hydrosilylation reactioncatalyst, and, when present the hydrosilylation reaction inhibitor and / or the solvent; and optionally 2) combining the hydrosilylation reaction product or a) the organohydrogensiloxane and all or a portion of F) the thiuram disulfide; andoptionally 3) purifying the organohydrogensiloxane.4) combining, under conditions to effect a second hydrosilylation reaction, starting materials comprisingthe first hydrosilylation reaction product or a) the organohydrogensiloxane, optionally b) a second hydrosilylation reaction catalyst, andc) an unsaturated anhydride having, per molecule at least one aliphatically unsaturated group capable of undergoing an addition reaction with a silicon bonded hydrogen atom of a) the organohydrogensiloxane and further comprising a moiety comprising an anhydride-functional group;thereby preparing a second hydrosilylation reaction product comprising the organosiloxane;optionally 5) adding a thiuram disulfide to the second hydrosilylation reaction product; and optionally 6) recovering the organosiloxane.

10. The method of claim 9, wherein B) the alkenyl-functional siloxane is selected from the group consisting of l,5-divinyl-l,l,5,5-tetramethyl-3,3-diphenyltrisiloxane and l,3-divinyl-l,3-dimethyl- 1 ,3 -diphenyldisiloxane11. The method of claim 9 or claim 10, wherein c) the unsaturated anhydride comprises allyl succinic anhydride.

12. Use of the organosiloxane of any one of claims 1 to 7 or the composition of claim 8, as an adhesion promoter in a curable silicone composition.