Phthalonitrile and polyimide-based compositions

A curable composition of phenol-containing and phthalonitrile-containing compounds with polyimide additives addresses the limitations of existing coatings by achieving high thermal stability and mechanical strength for aerospace applications.

WO2026236462A1PCT designated stage Publication Date: 2026-11-12CAMBIUM BIOMATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/027061
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing organic-based protective coatings for aircraft and missiles cannot withstand high in-flight temperatures and are difficult to apply and repair, leading to increased cost and weight.

Method used

A curable composition comprising phenol-containing and phthalonitrile-containing compounds with a thermoplastic additive, such as polyimide, which forms a crosslinked network with enhanced thermal stability and mechanical performance, suitable for high-temperature applications.

Benefits of technology

The composition achieves a glass transition temperature of at least 280°C, a char yield of at least 60%, and a lap shear strength of at least 650 psi at 315°C, providing effective thermal protection and mechanical integrity for aerospace applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026027061_12112026_PF_FP_ABST
    Figure US2026027061_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A composition includes a curable component and a thermoplastic additive. The curable component includes a reaction product of one or more phenol-containing compounds and one or more phthalonitrile-containing compounds, wherein each of the one or more phenol-containing compounds includes one or more phenolic hydroxyl groups, and each of the one or more phthalonitrile-containing compounds includes a phthalonitrile group and a substituent group attached to a benzene ring of the phthalonitrile group. A method of applying the composition and articles formed therefrom are also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No.: 0637-000020-WO-POAPHTHALONITRILE AND POLYIMIDE-BASED COMPOSITIONSCROSS-REFERENCE TO RELATED APPLICATION

[0001] This application claims priority to and the benefit of U.S. Provisional Application No. 63 / 801,557, filed on May 7, 2025, the disclosure of which is incorporated herein by reference in its entirety.FIELD

[0002] The present disclosure relates to phthalonitrile and polyimide-based compositions, and more particularly to high temperature polymeric materials for aerospace applications.BACKGROUND

[0003] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.

[0004] Many aircraft, missiles, and other air vehicles travel at high velocities and thus generate elevated temperatures on their exterior surfaces and associated materials during flight. Various material systems are used in such environments to provide thermal protection and to meet other functional specifications. Protective coatings are one example of such material systems and are often used to shield the exterior surfaces from friction and heat, as well as to meet other functional specifications. Organic-based protective coatings such as silicone-based coatings often cannot withstand these high in-flight temperatures (e.g., 343-427°C for 10 to 20 seconds), as their glass transition temperatures are typically equal to or below 260°C. In addition, the protective coatings are often difficult to apply and / or repair, and their application may lead to increased cost and weight of the air vehicles, which are undesirable.

[0005] These issues related to materials for use in high-temperature applications are addressed by the present disclosure.SUMMARY

[0006] This section provides a general summary of the disclosure and is not a comprehensive disclosure of its full scope or all of its features.

[0007] In one form, a composition comprises a curable componentAttorney Docket No.: 0637-000020-WO-POAcomprising a reaction product of reactants, wherein the reactants comprise one or more phenol-containing compounds, wherein each of the one or more phenol-containing compounds comprises one or more phenolic hydroxyl groups; and one or more phthalonitrile-containing compounds, wherein each of the one or more phthalonitrile-containing compounds comprises a phthalonitrile group and a substituent group attached to a benzene ring of the phthalonitrile group; and a thermoplastic additive.

[0008] In variations of this composition, which may be implemented individually or in any combination: the composition further comprises a solvent; the solvent is a polar aprotic solvent; the solvent is selected from the group consisting of methylene chloride, ethylene chloride, chloroform, tetrachloroethane, tetrahydrofuran (THF), dioxane, acetophenone, cyclohexanone, m-cresol, g-butyrolactone, dimethylformamide (DMF), dimethylacetamide (DMAC), and N-methylpyrrolidone (NMP), and combinations thereof; the solvent comprises tetrahydrofuran (THF); a total amount of the curable component and the thermoplastic additive in the composition is about 5 wt.% to about 40 wt.%; a total amount of the curable component and the thermoplastic additive is about 20 wt.% to about 30 wt.%; the one or more phenol-containing compounds and the one or more phthalonitrile-containing compounds are present such that a molar ratio of phenolic hydroxyl groups of the one or more phenol-containing compounds to substituent groups of the one or more phthalonitrile-containing compounds is about 0.9:1 to about 2:1; the one or more phenol-containing compounds comprise diallyl bisphenol A (DABPA), diallyl bisphenol S (DABPS), or a combination thereof; the one or more phthalonitrile-containing compounds comprise 3-substituted phthalonitrile, 4-substituted phthalonitrile, or a combination thereof; at least one of the one or more phenol-containing compounds comprises one or more substituents selected from the group consisting of alkyl group, allyl group, alkenyl group, alkynyl group, cycloaliphatic group, aromatic group, and combinations thereof; the curable component further comprises a curable resin component selected from a propargyl ether component, a benzoxazine component, an epoxy component, a bismaleimide component, a cyanate ester component, and combinations thereof; the thermoplastic additive comprises a soluble polyimide; the soluble polyimide is partially imidized or fully imidized; the soluble polyimide has a number average molecular weight of no more than 5 kDa; the thermoplastic additive has a number average molecular weight of no more than 10 kDa; the thermoplastic additive has a glassAttorney Docket No.: 0637-000020-WO-POAtransition temperature of at least about 250°C; the thermoplastic additive comprises polyimide, polyetherimide, or a combination thereof; the thermoplastic additive is present in an amount of about 1 wt.% to about 40 wt.% based on total solids of the composition; the composition comprises an additive selected from the group consisting of a curing agent, a catalyst, a surfactant, a filler, a viscosity modifier, an adhesion promoter, and combinations thereof; the composition further comprises an additive selected from the group consisting of a chain extender, a polymerization reaction control agent, a diluent, a reactive diluent, an appearance modifier, and combinations thereof; the filler is selected from the group consisting of carbon black, graphite, silica particles, fumed silica particles, alumina particles, titanium dioxide particles, clay particles, boron nitride particles, boron carbide particles, silicon carbide particles, and combinations thereof; the composition has a Brookfield viscosity of about 50 cP to about 5000 cP at 25°C; the curable component and the thermoplastic additive are miscible in a cast state; the composition, in a cured state, exhibits a glass transition temperature of at least about 280°C; the composition, in a cured state, exhibits a char yield of at least about 60%; the composition, in a cured state, exhibits a lap shear strength at least about 650 psi at a temperature of about 315°C as measured in accordance with ASTM D1002; the composition, in a cured, state, exhibits a lap shear strength at least about 900 psi at room temperature as measured in accordance with ASTM D1002; the composition is a sprayable composition having a Brookfield viscosity of no greater than about 300 cP at 25°C; and the composition is a paste having a Brookfield viscosity of about 300 cP to about 5000 cP at 25°C.

[0009] In another form, a product is formed from the composition described above.

[0010] In variations of this product, which may be implemented individually or in any combination: the product is uncured, partially cured or fully cured; and the product exhibits a glass transition temperature of at least about 280°C, a lap shear strength of at least about 650 psi at about 315°C in a cured state.

[0011] In another form, a coated substrate comprises the product described above, wherein the product is a coating.

[0012] In another form, a bonded article comprises the product described above, wherein the product is an adhesive disposed between two substrates.

[0013] In variations of this bonded article, which may be implemented individually or in any combination: the adhesive is a free-standing film; and theAttorney Docket No.: 0637-000020-WO-POAadhesive is supported on a scrim.

[0014] In another form, a composite comprises the product described above, wherein the product is a binder or a matrix material.

[0015] In a variation of this composite, the composite further comprises a reinforcement selected from the group consisting of fibers, fabrics, particulates, and combinations thereof.

[0016] In another form, a method of forming a coating on a substrate comprises forming the composition described above, the composition having a total solids content of about 10 wt.% to about 30 wt.%; adjusting the total solids content of the composition to have a Brookfield viscosity of no greater than about 300 cP at 25°C; spraying the composition on at least a portion of a surface of the substrate to form a deposited layer; and curing the deposited layer to form the coating.

[0017] In variations of this method, which may be implemented individually or in any combination: the composition is sprayed to the surface of the substrate by high-volume low-pressure (HVLP), airless, air-assist airless, or electrostatic spray equipment; the composition is sprayed onto the surface of the substrate with a nozzle orifice size of about 0.3 mm to about 1.5 mm, an atomizing pressure of about 0.5 bar to about 3.5 bar, and a spray distance of about 10 cm to about 30 cm; the deposited layer is cured at a temperature of about 120°C to about 300°C for about 10 minutes to about 4 hours; the deposited layer is further cured at about 200°C to about 425°C for about 30 minutes to about 6 hours; the method comprises pre-treating the surface of the substrate prior to spraying by at least one of solvent wipe, abrasion, plasma treatment, and application of a silane adhesion promoter; and the method comprises multi-pass spraying to build thickness, wherein about 2 to about 50 passes are applied with about 1 to about 5 minutes between passes.

[0018] In another form, a coating is formed by the method described above.

[0019] In variations of this coating, which may be implemented individually or in any combination: the coating has a dry thickness of about 0.5 pm to about 1 mm; and the coating exhibits adhesion of greater than 4B as measured in accordance with ASTM D3359.

[0020] In another form, a coated substrate comprises a coating on at least a portion of a surface of a substrate, wherein the coating is formed using theAttorney Docket No.: 0637-000020-WO-POAmethod described above.

[0021] In variations of this coated substrate, which may be implemented individually or in any combination: the substrate comprises titanium or aluminum; the coating exhibits a glass transition temperature of at least about 280°C; the coating exhibits a lap shear strength of at least about 650 psi at about 315°C as measured in accordance with ASTM D1002; and the coating exhibits a lap shear strength of at least about 900 psi at room temperature as measured in accordance with ASTM D1002.

[0022] Further areas of applicability will become apparent from the description provided herein. It should be understood that the description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.DRAWINGS

[0023] In order that the disclosure may be well understood, there will now be described various forms thereof, given by way of example, reference being made to the accompanying drawings, in which:

[0024] FIG. 1 is a schematic illustration of a composition according to the teachings of the present disclosure.

[0025] FIG. 2 is a schematic illustration of a curable component according to the teachings of the present disclosure.

[0026] FIG. 3 shows chemical structures of phenol-containing components according to the teachings of the present disclosure.

[0027] FIG. 4 shows chemical structures of phthalonitrile-containing components according to the teachings of the present disclosure.

[0028] FIG. 5A is a schematic illustration of forming a curable component according to the teachings of the present disclosure.

[0029] FIG. 5B shows chemical structures of curing components according to the teachings of the present disclosure.

[0030] FIG. 6 shows chemical structure of a thermoplastic additive according to the teachings of the present disclosure.

[0031] FIG. 7 is a schematic illustration of a method of coating a substrate according to the teachings of the present disclosure.

[0032] FIG. 8 is a flowchart illustrating a method of forming a coating on a substrate according to the teachings of the present disclosure.

[0033] The drawings described herein are for illustration purposes onlyAttorney Docket No.: 0637-000020-WO-POAand are not intended to limit the scope of the present disclosure in any way.DETAILED DESCRIPTION

[0034] The following description is merely exemplary in nature and is not intended to limit the present disclosure, application, or uses. It should be understood that throughout the drawings, corresponding reference numerals indicate like or corresponding parts and features.

[0035] The present disclosure provides compositions for forming materials, such as coatings, adhesives, and composites, suitable for high temperature applications. The compositions comprise phthalonitrile-based curable components and thermoplastic additives, such as polyimides, which together provide enhanced thermal stability, mechanical performance, and processing advantages. The present disclosure further provides methods of applying such compositions as well as articles formed therefrom.

[0036] Referring to FIG. 1, an exemplary composition according to the teachings of the present disclosure is shown. The composition 100 in one form generally comprises a curable component 110, a thermoplastic additive 120, and optionally a solvent 130.

[0037] In some forms, the curable component 110 undergoes a curing reaction to form a crosslinked network. Referring to FIG. 2, in some forms, the curable component 110 comprises a reaction product of reactants, wherein the reactants comprise (i) one or more phenol-containing compounds 112, wherein each of the one or more phenol-containing compounds 112 comprises one or more phenolic hydroxyl groups; and (ii) one or more phthalonitrile-containing compounds 114, wherein each of the one or more phthalonitrile-containing compounds 114 comprises a phthalonitrile group and a substituent group bonded to a benzene ring of the phthalonitrile group. As used herein, the term “phthalonitrile group” refers to a functional group comprising a benzene ring substituted with two nitrile groups in ortho positions. As used herein, the term “substituent group” refers to a functional group bonded to the benzene ring of the phthalonitrile group that is capable of reacting with phenolic hydroxyl groups, including, but not limited to, nitro (-NO2) groups and halogen (e.g., fluoro, chloro, bromo, or iodo) groups. The curable component 110 may further comprise one or more curable resin components, such as a benzoxazine component, bismaleimideAttorney Docket No.: 0637-000020-WO-POAcomponent, an epoxy component, a propargyl ether component and a cyanate ester component.

[0038] In some forms, the one or more phenol-containing compounds 112 are monofunctional or multifunctional and include one or more phenolic hydroxyl groups per molecule. The one or more phenol-containing compounds 112 may include, without limitation, phenol, substituted phenols, bisphenols, diallyl bisphenol A (BPA), diallyl bisphenol S (BPS), polyhydric phenols, oligomeric or polymeric species containing phenolic hydroxyl groups, and combinations thereof. The one or more phenol-containing compound 112 may further comprise one or more substituents, such as alkyl group, allyl group, alkenyl group, alkynyl group, cycloaliphatic group, and aromatic group, wherein the one or more substituents are functional groups attached to the aromatic ring of the phenol-containing compound 112, the functional groups being capable of modifying one or more properties of product formed from the composition 100 and / or participating in further reactions, including chemical modification or crosslinking. Referring to FIG. 3, examples of the one or more phenol-containing compound 112 (112a and 112b) are shown. In some forms, the one or more phenol-containing compounds 112 comprise diallyl bisphenol A (DABPA) (112a) or diallyl bisphenol S (DABPS) (112b). These compounds may be used individually or in any combination thereof.

[0039] In some forms, the one or more phthalonitrile-containing compounds 114 are 3-substituted phthalonitrile, such as 3-nitrophthalonitrile, 4-substituted phthalonitrile, such as 4-nitrophthalonitrile, or combinations thereof. Referring to FIG. 4, examples of the one or more phthalonitrile-containing compounds 114 (114a and 114b) are shown. In some forms, the one or more phthalonitrile-containing compounds 114 comprises 3-nitrophthalonitrile (114a) or 4-nitrophthalonitrile (114b). In some forms, the one or more phthalonitrile-containing compounds 114 comprises 3-halo substituted phthalonitrile, 4-halo substituted phthalonitrile, or combinations thereof. In some forms, the one or more phthalonitrile-containing compounds 114 are selected from 3-iodo substituted phthalonitrile, 4-iodo substituted phthalonitrile, 3-bromo substituted phthalonitrile, 4-bromo substituted phthalonitrile, 3-chloro substituted phthalonitrile, 4-chloro substituted phthalonitrile, 3-fluoro substituted phthalonitrile, 4-fluoro substituted phthalonitrile, and combinations thereof. These compounds may be used individually or in any combination thereof.Attorney Docket No.: 0637-000020-WO-POA

[0040] In some forms, the one or more phenol-containing compound 112 and the one or more phthalonitrile-containing compound 114 are reacted to form a reaction product (the curable component 110) via a nucleophilic aromatic substitution reaction. Without being bound by theory, the phenolic hydroxyl groups of the one or more phenol-containing compound 112 may be deprotonated under basic conditions to form phenoxide species, which act as nucleophiles and react with electron-deficient aromatic rings of the one or more phthalonitrile-containing compound 114, particularly when the one or more phthalonitrile-containing compound 114 comprises a leaving group such as nitro (-NO2) or halogen (e.g., fluoro, chloro, bromo, or iodo) at the 3-and / or 4-position. Referring to FIG. 5A, an exemplary reaction scheme between the phenol-containing compound 112a and the phthalonitrile-containing compound 114b is shown, the nucleophilic substitution results in displacement of the leaving group (-NO2 of 114b) and formation of an aryl ether linkage (dashed box) between the phenol-containing compound 112a and the phthalonitrile-containing compound 114b, generating a curable component 110a. In some forms, the curable component 110 comprises one or more reaction products in which the one or more phenol-containing compound 112 is covalently bonded to the one or more phthalonitrile-containing compound 114 through one or more aryl ether linkages, while retaining the phthalonitrile groups. Referring to FIG. 5B, examples of the curable component 110 (110a, 110b, 110c, and 110d) are shown. In some forms, the curable component 110 comprises one or more molecules formed by reacting diallyl bisphenol A (DABPA) with 3-substituted phthalonitrile (110b: Ri=CN, R2=CN, Rs=H) or 4-substituted phthalonitrile (110a: Ri=H, R2=CN, Rs=CN), and by reacting diallyl bisphenol S (DABPS) with 3-substituted phthalonitrile (110d: Ri=CN, R2=CN, Rs=H) or 4-substituted phthalonitrile (110c: Ri=H, R2=CN, Rs=CN). The phthalonitrile groups may undergo thermal curing to form a crosslinked network, such as through cyclotrimerization or related reactions of the nitrile groups, thereby providing a thermally stable polymeric structure.

[0041] In some forms, the thermoplastic additive 120 is a polymeric or oligomeric material that softens upon heating and hardens upon cooling without undergoing irreversible chemical crosslinking, and is incorporated into the composition 100 to enhance one or more properties of the products formed from the composition 100, such as strength, toughness, adhesion, cure shrinkage, crack resistance, thermal stability, impact resistance, or scratch resistance. In some forms, the thermoplasticAttorney Docket No.: 0637-000020-WO-POAadditive 120 is physically dispersed in the composition 100. In some forms, the thermoplastic additive 120 is partially miscible, or fully miscible with the curable component 110 in a cast state (e.g., before curing) or in a cured state (e.g., after curing), as determined by optical microscopy and / or differential scanning calorimetry. In some forms, compositions exhibiting partial or full miscibility between the thermoplastic additive 120 and the curable component 110 further exhibit enhanced performance characteristics, such as mechanical properties, in the cured state.

[0042] Suitable thermoplastic additive 120 includes, without limitation, polyimide, polyetherimide, and a combination thereof. In some forms, the thermoplastic additive 120 comprises a polyimide. Referring to FIG. 6, an exemplary structure of the polyimide is shown, which is formed from benzophenone tetracarboxylic dianhydride (BTDA) and p-phenylenediamine (PDA). The polyimide may also be formed from other dianhydrides, such as pyromellitic dianhydride (PMDA), 4,4'-oxydiphthalic anhydride (ODPA) and biphenyltetracarboxylic dianhydride (BPDA), and other diamines, such as 4,4'-oxydianiline (ODA), 4,4'-diaminodiphenyl sulfone (DDS), diaminophenylindane (DAPI) and methylenedianiline (MDA). In some forms, the polyimide or polyetherimide is partially imidized, fully imidized, or a combination thereof. In some forms, the thermoplastic additive 120 comprises a soluble thermoplastic additive. As used herein, the term “soluble” refers to the ability of the thermoplastic additive 120 to dissolve or be molecularly dispersed in one or more organic solvents to form a substantially homogeneous solution suitable for processing prior to curing. In some forms, the thermoplastic additive 120 is soluble in one or more polar aprotic solvents. In some form, the thermoplastic additive 120 is a fully imidized polyimide. In some forms, the thermoplastic additive 120 exhibits a glass transition temperature of at least about 250°C.

[0043] In some forms, the thermoplastic additive 120 has a number-average molecular weight (Mn), as measured by refractive index gel permeation chromatography (GPC) in tetrahydrofuran relative to polystyrene standards, of less than about 15,000. In some forms, the thermoplastic additive 120 has an Mn, as so measured, of less than about 10,000. In some forms, the thermoplastic additive 120 has an Mn, as so measured, of less than about 5,000. In some forms, the thermoplastic additive 120 has a weight-average molecular weight (Mw), as so measured, of less than about 120,000. In some forms, the thermoplasticAttorney Docket No.: 0637-000020-WO-POAadditive 120 has an Mw, as so measured, of less than about 100,000. In some forms, the thermoplastic additive 120 has an Mw, as so measured, of less than about 85,000.

[0044] In some forms, the thermoplastic additive 120 is about 1 wt.% to about 40 wt.% based on total solids. In some forms, the thermoplastic additive 120 is about 10 wt.% to about 30 wt.% based on total solids. In some forms, the thermoplastic additive 120 is about 20 wt.% to about 30 wt.% based on total solids. In some forms, the thermoplastic additive 120 is about 8 wt.% to about 12 wt.% based on total solids.

[0045] In some forms, the solvent 130 is a liquid medium capable of dissolving, dispersing, or otherwise facilitating uniform mixing of the curable component 110 and the thermoplastic additive 120 of the composition 100. The solvent 130 is substantially non-reactive with the curable component 110 and the thermoplastic additive 120 in the composition 100 under storage and application conditions, and is present primarily to adjust viscosity, solids content, and application properties of the composition 100. The solvent 130 may be removed at least in part, prior to or during curing of the composition 100. Suitable solvent 130 includes, without limitation, methylene chloride, ethylene chloride, chloroform, tetrachloroethane, tetrahydrofuran (THF), dioxane, acetophenone, cyclohexanone, m-cresol, g-butyrolactone, dimethylformamide (DMF), dimethylacetamide (DMAC), and N-methylpyrrolidone (NMP), and combinations thereof. In some forms, the solvent 130 comprises a polar aprotic solvent. In some forms, the solvent 130 comprises THF.

[0046] In some forms, the curable component 110 and the thermoplastic additive 120 are dissolved in the solvent 130 at a total concentration of about 10 wt.% to about 40 wt.%, and in some forms, about 15 wt.% to about 35 wt.%, and in some forms, about 20 wt.% to about 30 wt.%, and in some forms, about 20 wt.% to about 25 wt.%, and in some form, about 25 wt.% to about 30 wt.%.

[0047] In some forms, the phenol-containing compound 112 and the phthalonitrile-containing compound 114 are present such that a molar ratio of the phenolic hydroxyl groups to the substituent groups is about 0.9:1 to about 2:1 , in some forms, about 1 :1 to about 1.5:1, in some forms, about 1.05:1 to about 1.1:1, in some forms, at least about 0.9:1, in some forms, at least about 1:1, in some forms, at least about 1.05:1 , in some forms, no greater than about 2:1 , in some forms, no greater than about 1.5:1 , and in some forms, no greater than about 1.1:1.

[0048] In some forms, the composition 100 further comprises other additives selected from the group consisting of curing agent, catalyst, surfactant, filler,Attorney Docket No.: 0637-000020-WO-POAa chain extender, a polymerization reaction control agent, a diluent, a reactive diluent, an appearance modifier, a viscosity modifier, an adhesion promoter, and combinations thereof.

[0049] In some forms, the composition 100 further comprises a curing agent in addition to the curable component 110. In some forms, the curing agent comprises a phenol, an amine, an organic acid, and / or an organometallic compound. In some forms, the curing agent is in an amount of at least about 0.1 wt.%, in some forms, at least about 1 wt.%, in some forms, at least about 5 wt.%, in some forms, no greater than about 50 wt.%, in some forms, no greater than about 45 wt.%, in some forms, about 1 wt.% to about 50 wt.%, and in some forms, about 5 wt.% to about 45 wt.% based on total weight of the composition 100. In some forms, the composition 100 is substantially free, essentially free, or completely free of curing agent.

[0050] In some forms, the composition 100 further comprises a catalyst to facilitate or accelerate curing of the curable component 110. In some forms, the catalyst comprises a transition metal. In some forms, the catalyst is in an amount of at least about 0.1 wt.%, in some forms, at least about 1 wt.%, in some forms, no greater than about 10 wt.%, in some forms, no greater than about 5 wt.%, in some forms, about 0.1 wt.% to about 10 wt.%, and in some forms, about 1 wt.% to about 5 wt.% based on total weight of the composition 100.

[0051] In some forms, the surfactant is incorporated into the composition 100 to enhance wetting, dispersion, or surface uniformity of the composition 100 and facilitate application processes. In some forms, the surfactant comprises a carbonbased surfactant, a silicone-based surfactant, or a combination thereof. In some forms, the surfactant is in an amount of at least about 0.01 wt.%, in some forms, at least about 0.05 wt.%, in some forms, no greater than about 10 wt.%, in some forms, no greater than about 5 wt.%, in some forms, about 0.01 wt.% to about 10 wt.%, and in some forms, about 0.5 wt.% to about 5 wt.% based on total weight of the composition 100. In some forms, the composition 100 is substantially free, essentially free, or completely free of surfactant.

[0052] In some forms, the filler is incorporated into the composition 100 to function as one or more, without limitation, of a reinforcement, a viscosity modifier, a surface modifier, a processing aid, a fire retardant, a thermal stability enhancer, a pyrolysis aid, or a graphitization aid. The filler may enhance performance properties of the composition 100, such as mechanical properties, thermal properties, orAttorney Docket No.: 0637-000020-WO-POAprocessing characteristics of the composition 100 and products formed from the composition 100. In some forms, the filler comprises one or more materials selected from carbon-based and / or inorganic microstructures and / or nanostructures, silsesquioxane compounds, bio-derived polymers, thermosetting polymer additives, thermoplastic polymer additives, fibers, and combinations thereof. Suitable filler includes, without limitation, carbon black, graphite, silica particles, fumed silica particles, alumina particles, titanium dioxide particles, clay particles, boron nitride particles, boron carbide particles, silicon carbide particles, polyhedral oligomeric silsesquioxanes (POSS), and combinations thereof.

[0053] In some forms, the filler is in an amount of at least about 0.1 wt.%, in some forms, at least about 1 wt.%, in some forms, no greater than about 50 wt.%, in some forms, no greater than about 40 wt.%, in some forms, about 0.1 wt.% to about 50 wt.%, and in some forms, about 5 wt.% to about 40 wt.% based on total weight of the composition 100. In some forms, the composition 100 is substantially free, essentially free, or completely free of filler.

[0054] In some forms, the composition 100 exhibits a Brookfield viscosity of about 1 cP to about 5000 cP at 25°C, and in some forms, about 2 cP to about 120 cP, and in some forms, about 100 cP to about 4000 cP, and in some forms, about 200 cP to about 3000 cP, and in some forms, about 1 to about 2000 cP, and in some forms, about 300 cP to about 2000 cP, and in some forms, 400 cP to about 1000 cP, and in some forms, about 100 to about 200 cP, and in some forms, about 500 cP to about 800 cP. Unless otherwise stated, the Brookfield viscosity described in the present application is measured at 25°C using a Brookfield viscometer equipped with Spindle #2 at a spindle speed of about 6 rpm to about 60 rpm.

[0055] In some forms, the composition 100 is in a form selected from a liquid, a paste, or a solid powder. In some forms, the composition 100 is a sprayable composition having a Brookfield viscosity of no greater than about 300 cP at 25 °C. In some forms, the composition 100 is a paste having a Brookfield viscosity of about 300 cP to about 5000 cP at 25 °C. In some forms, the composition 100 is formulated to form a coating, an adhesive, ora composite. In some forms, the composition 100, after curing, exhibits a glass transition temperature of at least about 280 °C, a char yield of at least about 60%, and a lap shear strength of at least about 300 psi at a temperature of about 315°C. In some forms, the adhesive formed from the composition 100 is provided as a free-standing film or is supported on a scrim.Attorney Docket No.: 0637-000020-WO-POA

[0056] In some forms, the composition 100 is in a cured or partially cured state, wherein the composition 100 has been subjected to staged curing, multi-step curing, or post-curing. In some forms, the composition 100 is optionally B-staged prior to final curing. In some forms, the composition 100 that is cured or partially cured exhibits a char yield of at least about 50%, at least about 60%, or at least about 70%, as determined by thermogravimetric analysis under a nitrogen atmosphere at 1000 °C. In some forms, the composition 100, in an as-prepared (uncured), cured, or partially cured state, is configured for use as a coating, an adhesive, or a matrix material in a composite. In some forms, the composition 100 is disposed on, applied to, or bonded to a substrate. In some forms, the substrate comprises a metal, metal alloy, composite material, polymeric material, ceramic material, glass, fiber-reinforced fabric, or another solid material capable of receiving and supporting the composition.

[0057] In some forms, the composition 100 in a cured or partially cured state exhibits a lap shear strength, as determined in accordance with ASTM D1002 using titanium substrates, of at least about 900 psi or at least 1100 psi at room temperature. In some forms, after thermal exposure at about 427 °C for about 2 hours, the composition 100 in a cured or partially cured state retains a lap shear strength at room temperature of at least about 300 psi or at least about 500 psi. In some forms, the composition 100 in a cured or partially cured state exhibits a lap shear strength of at least about 650 psi, at least about 850 psi, or at least about 1100 psi when measured at an elevated temperature of 315°C. In some forms, after thermal exposure at about 427 °C for about 2 hours, the composition 100 in a cured or partially cured state exhibits a lap shear strength of at least about 280 psi or of at least 350 psi when measured at about 315 °C. As used herein, the term “lap shear strength” refers to the shear strength measured using single-lap shear testing in accordance with ASTM D1002 on titanium substrates, unless otherwise specified.

[0058] In some forms, the composition 100 comprises the solvent 130 (e.g., a single solvent or a mixture of solvents) during formulation or application. In some forms, the solvent 130 is at least partially removed prior to curing, partial curing, or final use of the composition 100. In some forms, the composition 100 is dried or partially dried to reduce solvent content before or during staged curing, B-staging, or post-curing. In some forms, removal of the solvent 130 facilitates formation of a self-supporting coating, adhesive layer, or composite structure.Attorney Docket No.: 0637-000020-WO-POA

[0059] The following are examples (DABPA-3PN and DABPS-4PN) of forming the curable component 110, which are used to prepare the composition 100 in Examples 1-8 described later in the description.

[0060] DABPA-3PN: a mixture of 39.74 parts by weight (grams) of 2,2'-bis(3-allyl-4-hydroxyphenyl)isopropylidene (Diallyl bisphenol A, DABPA), 44.62 parts by weight (grams) of 3-nitrophthalonitrile, 39.46 parts by weight (grams) of potassium carbonate, and 110.5 parts by weight (grams) of acetonitrile was combined in a three-neck 500-milliliter flask equipped with a condenser, thermocouple, and rubber septum under a nitrogen atmosphere. The mixture was heated to 75 °C and maintained at that temperature with stirring for 8 hours. The reaction mixture was then cooled to 25 °C, and 165.75 parts by weight (grams) of deionized water was slowly added. The resulting solution was transferred to a separatory funnel and washed with water and ethyl acetate until a pH of 7 was achieved. The resulting resinous material was concentrated using a rotary evaporator to remove excess ethyl acetate and subsequently dried in a forced-air oven at 85 °C, yielding DABPA-3PN in 89% yield.

[0061] DABPS-4PN: a mixture of 35.07 parts by weight (grams) of 4,4'-sulfonylbis[2-(prop-2-en-1-yl)phenol] (Diallyl bisphenol S, DABS), 36.75 parts by weight (grams) of 4-nitrophthalonitrile, 32.50 parts by weight (grams) of potassium carbonate, and 97.5 parts by weight (grams) of acetonitrile was combined in a three-neck 500-milliliter flask equipped with a condenser, thermocouple, and rubber septum under a nitrogen atmosphere. The mixture was heated to 75 °C and maintained at that temperature with stirring for 8 hours. The reaction mixture was then cooled to 25 °C, and 200 parts by weight (grams) of deionized water was slowly added, resulting in the formation of a resinous precipitate. The precipitate was isolated by decanting the aqueous phase and washed with deionized water until a pH of 7 was achieved, and then dried in a forced-air oven at 85 °C, yielding DABS-4PN in 94.8% yield.

[0062] The following are general procedures and examples (Examples 1-8) for forming and curing the composition 100 and testing the product formed from the composition 100.

[0063] Coating composition preparation: high temperature coating compositions were prepared from a polyimide and a phthalonitrile monomer using tetrahydrofuran (THF) as solvent. In all compositions, the total mass of coating solution was maintained at 10.0 g. Solutions were formulated to desired solids contents byAttorney Docket No.: 0637-000020-WO-POAadjusting the relative masses of solids and solvent. The solid components were added to THF in a sealable vessel containing a magnetic stir bar. The vessel was sealed to limit solvent evaporation and stirred at ambient temperature until a homogeneous solution was obtained.

[0064] Soravable coating application: the coating solutions were transferred to a disposable spray cup liner system (3M™ PPS™ Spray Gun Cup Liner Kit, Model 26000) and applied using a gravity feed HVLP spray gun (Graco AirPro®, Model 289023) equipped with a 0.055 inch nozzle. These components are provided as representative examples, and equivalent spray systems may be used. Titanium substrates consisted of Ti 6AI 4V alloy (0.063 inch thickness, AMS 4911) prepared as lap shear panels. Prior to coating, the substrates were degreased with acetone and abrasive blasted to produce a uniformly roughened surface. Coatings were applied by spray deposition in successive passes, with approximately 5 minutes of ambient air drying between passes, until a dry coating thickness of approximately 0.005 inches was obtained for mechanical testing. In general, the spray process was utilized to produce coating thicknesses from about 0.002 to about 0.040 inches.

[0065] Thermal cure: after application, the coated substrates were cured in Yamato programmable ovens according to the following thermal profile: ramp from ambient temperature to 215 °C over approximately 1 hour; hold at 215 °C for approximately 8 hours; ramp to 250 °C over approximately 12 minutes; hold at 250 °C for approximately 6 hours; controlled cool down to ambient temperature over approximately 3 hours; post cure at 315 °C for approximately 4 hours.

[0066] Mechanical testing: mechanical performance was evaluated using single lap shear testing in accordance with ASTM D1002. Lap shear testing was employed to assess the mechanical integrity of the cured formulas, such as high temperature coatings or adhesives under both ambient and elevated temperature conditions.

[0067] Example 1 (0 wt.% Polvimide / DABPS-4PN): a coating composition was prepared from 2.0 g DABPS-4PN dissolved in 8.0 g THF, providing a solution containing 20 wt.% solids. The solution viscosity was 3.0 cP (Brookfield viscosity, using Spindle #2 with a spindle speed of 60 rpm at 25°C). The coating was applied, cured, and tested as described above. Lap shear testing yielded a shear strength of 705.8 psi at 315°C.Attorney Docket No.: 0637-000020-WO-POA

[0068] Example 2 (10 wt.% Polvimide / 90 wt.% DABPS-4PN): a coating composition was prepared from 0.20 g soluble polyimide and 1.80 g DABPS-4PN dissolved in 8.0 g THF, yielding a 20 wt.% solids solution. Lap shear testing yielded a shear strength of 696.8 psi at 315°C. A dynamic mechanical analysis (DMA) sample was prepared from this composition by dissolving the curable component and the thermoplastic component in dichloromethane (DCM). The solvent was removed by agitating the resulting mixture at approximately 60 °C, followed by heating at approximately 100 °C under vacuum for about 20 minutes. The dried material was then reduced to a particulate form, placed into a rectangular silicone mold, and subjected to a curing cycle. After curing, the sample was sanded to a planar surface and analyzed using a TA Instruments Discovery DMA 850. The cured composition exhibited a glass transition temperature (Tg) of 380.7 °C, as determined from the onset of the storage modulus.

[0069] Example 3 (20 wt.% Polvimide / 80 wt.% DABPS-4PN): a coating composition comprising 0.40 g soluble polyimide and 1.60 g DABPS-4PN in 8.0 g THF (20 wt.% solids) was applied and cured as described above. Lap shear testing produced a shear strength of 804.1 psi at 315°C.

[0070] Example 4 (30 wt.% Polvimide / 70 wt.% DABPS-4PN): a coating composition comprising 0.60 g soluble polyimide and 1.40 g DABPS-4PN dissolved in 8.0 g THF (20 wt.% solids) was spray applied and cured as described above. The solution viscosity was 115.5 cP (Brookfield viscosity, using Spindle #2 with a spindle speed of 6 rpm at 25°C). Lap shear testing yielded a shear strength of 1155.7 psi at 315 °C and 1207 psi at room temperature. After exposure to 427 °C for 2 hours, lap shear testing at 315°C yielded a shear strength of 385.00 psi, with the coating remaining adherent to the titanium substrates. The as-sprayed coating exhibited no phase separation as determined by visually and using optical microscopy (100-500x, Keyence digital microscope).

[0071] Example 5 (40 wt.% Polvimide / 60 wt.% DABPS-4PN): a coating composition containing 0.80 g soluble polyimide and 1.20 g DABPS-4PN in 8.0 g THF (20 wt.% solids) was applied and cured as described above. Lap shear testing yielded a shear strength of 1155.7 psi at 315 °C. After exposure to 427 °C for 2 hours, lap shear testing at 315°C yielded a shear strength of 266.60 psi, with the coating remaining adherent to the titanium substrates. Phase separation was visually in the as-sprayed coating.Attorney Docket No.: 0637-000020-WO-POA

[0072] Example 6 (0 wt.% Polvimide / DABPA-3PN): a coating composition was prepared using 2.00 g DABPA-3PN dissolved in 8.0 g THF, forming a solution containing 20 wt.% solids. The coating was applied and cured as described above. Lap shear testing yielded a shear strength of 903.5 psi at room temperature.

[0073] Example 7 (30 wt.% Polvimide / DABPA-3PN at Reduced Solids): A coating composition was prepared using 0.30 g soluble polyimide and 0.70 g DABPA-3PN dissolved in 9.0 g THF, forming a solution containing 10 wt.% solids. The coating was applied and cured as described above. Lap shear testing yielded a shear strength of 860.4 psi at 315°C and 1152 psi at room temperature. After exposure to 427 °C for 2 hours, the coating had a lap shear strength of 344.6 psi. The as-sprayed coating exhibited phase separation as observed utilizing optical microscopy (100-500x, Keyence digital microscope).

[0074] Example 8 (100 wt.% Polvimide): a coating composition was prepared using 2 g soluble polyimide was dissolved in 8.0 g THF, forming a viscous solution containing 20 wt.% solids. The coating was painted on a titanium substrate using an acid brush and subjected to cure cycle described above. After the cure, the coating delaminated from the titanium substrate during (the cutting of) lap shear sample preparation.

[0075] Table 1 below shows examples of the composition 100 according to the teachings of the present disclosure. Two different curable component 110 are used, including DABPS-4PN and DABPA-3PN, which refer to reaction products formed from diallyl bisphenol S (DABPS) and 4-nitrophthalonitrile, and diallyl bisphenol A (DABPA) and 3-nitrophthalonitrile, respectively. Polyimide is used as the thermoplastic additive 120 and THF is used as the solvent 130 in each example. Table 1 summarizes (i) the amounts (in grams) of the curable component 110, the thermoplastic additive 120 and the solvent 130; (ii) the concentration (wt.%) of the thermoplastic additive 120 based on total solids; (iii) the total solids content (wt.%) of the curable component 110 and the thermoplastic additive 120; and (iv) the Brookfield viscosity of the examples of the composition 100.Example 120 110 Solids 120 110 130 Viscosity (wt.%) Content (g) (g) (g) (cP)(wt.%)1 0 DABPS-4PN 20 0.00 2.00 8.0 3.0Attorney Docket No.: 0637-000020-WO-POA2 10 DABPS-4PN 20 0.20 1.80 8.0 —3 20 DABPS-4PN 20 0.40 1.60 8.0 —4 30 DABPS-4PN 20 0.60 1.40 8.0 115.5 5 40 DABPS-4PN 20 0.80 1.20 8.0 —6 0 DABPA-3PN 20 0.00 2.00 8.0 —7 30 DABPA-3PN 10 0.30 0.70 9.0 —8 100 — 20 2.00 0 8.0 —Table 1. Examples 1-8: Examples of the composition 100. The symbol indicates that the corresponding data was not measured.

[0076] Table 2 below summarizes lap shear performance of the composition 100 in a cured state (Examples 1-8). The lap shear performance is evaluated using single-lap shear testing in accordance with ASTM D1002. Table 2 summarizes lap shear strength measured at 315°C, lap shear strength measured at room temperature (RT), and lap shear strength measured at room temperature after exposure at 427 °C for 2 hours. As shown, Examples 4 and 5, comprising 30 wt.% and 40 wt.% of the thermoplastic additive 120, respectively, and DABPS-4PN as the curable component 110 with a total solids content of 20 wt.%, exhibit a lap shear strength of 1155.7 psi at 315°C. In addition, Example 4 (with 30 wt.% of the thermoplastic additive 120) exhibits a lap shear strength of 1208.8 psi at room temperature and a lap shear strength of 503.46 psi at room temperature after exposure at 427 °C for 2 h.Example Lap Shear Lap Lap Shear Lap Shear Lap shear Lap Strength at Shear Stre at RT After at 315°C at 315°C shear at 315°C ngth at RT Exposure After after expos 315°C after (Psi) (Psi) at 427 Exposure ure at 427 exposure at °C for 2 h at 315°C °C for 427 °C for (Psi) for 100 hrs 2 hrs (psi) 2 hours (Psi)1 705.8 — — — — — 2 696.8 — — — — — 3 804.1 — — — — — 4 1155.7 1208.8 503.46 1082.2 385 —5 1155.7 — — — — —Attorney Docket No.: 0637-000020-WO-POA6 — 903.53 — — — — 7 860.4 1152 344.6 640.8 299.6 249.5 8 — — Delaminate — — —dTable 2. Examples 1-8: Lap Shear Performance of the composition 100 in a cured state. The symbol indicates that the corresponding data was not measured.

[0077] Referring to FIG. 7, a schematic illustration of a method of forming a coating on a substrate is shown. As illustrated, the composition 100 is applied to a surface 220 of a substrate 210 to form a deposited layer 230. The deposited layer 230 is subjected to a curing process to form a coated substrate 200 comprising the substrate 210 and a coating 240 on the surface 220 of the substrate 210.

[0078] In some forms, the composition 100 is formulated to a desired solids content by adjusting the relative amounts of the curable component 110, the thermoplastic additive 120, and the solvent 130. In some forms, the composition 100 is prepared by forming a stock solution of the composition 100 and diluting the stock solution with the solvent 130. In some forms, the stock solution has a concentration of about 10 wt.% to about 30 wt.%, and in some forms, about 2 wt.% to about 50 wt.%, and in some forms, about 5 wt.% to about 40 wt.%, and in some forms, about 20 wt.% to about 30 wt.%. In some forms, the composition 100 has a Brookfield viscosity of no greater than about 300 cP at 25°C, and in some forms, about 50 cP to about 5000 cP at 25°C, and in some forms, about 100 cP to about 200 cP at 25°C, and in some forms, about 1 cP to about 2000 cP at 25°C. In some forms, the curable component 110 and the thermoplastic additive 120 are mixed with the solvent 130 in a sealable vessel containing a magnetic stir bar. The vessel is sealed to limit solvent evaporation and the mixture is stirred at ambient temperature until a homogeneous solution of the composition 100 is obtained.

[0079] In some forms, the substrate 210 provides mechanical support and defines the surface 220 upon which the composition 100 is applied to form a deposited layer 230 and cured to form the coating 240. In some forms, the substrate 210 comprises a metal, metal alloy, composite, polymeric material, ceramic, glass, fiber-reinforced fabric, or other solid material capable of receiving and supporting the coating 240. In some forms, the substrate 210 comprises titanium, aluminum, or alloys thereof. In some forms, the substrate 210 comprises a Ti-6AI-4V alloy.Attorney Docket No.: 0637-000020-WO-POA

[0080] In some forms, the composition 100 is applied to the surface 220 by spraying, rolling, brushing, dip coating, or dispensing. In some forms, the composition 100 is sprayed to the surface 220 by high-volume low-pressure (HVLP), airless, air-assist airless, or electrostatic spray equipment. In some forms, the composition 100 is sprayed onto the surface 220 with a nozzle orifice size of about 0.3 mm to about 1.5 mm, an atomizing pressure of about 0.5 bar to about 3.5 bar, and a spray distance of about 10 cm to about 30 cm. In some forms, the composition 100 is transferred to a disposable spray cup liner system and sprayed using a gravity-feed HVLP spray gun equipped with a 0.055-inch nozzle. In some forms, the surface 220 is pre-treated by at least one of solvent wipe, abrasion, plasma treatment, and application of a silane adhesion promoter. In some forms, the surface 220 is degreased with acetone and abrasive blasted to produce a uniformly roughened surface. In some forms, the composition 100 is applied to the surface 220 by spraying in successive passes, wherein about 2 to about 50 passes are applied with about 1 to about 5 minutes between passes. In some forms, the composition 100 is sprayed on at least a portion of the surface 220 of the substrate 210.

[0081] In some forms, the deposited layer 230 is cured at a temperature of about 120°C to about 300°C for about 10 minutes to about 4 hours, optionally followed by post-curing at about 200°C to about 325°C for about 30 minutes to about 6 hours. In some forms, the deposited layer 230 is cured by a thermal curing process comprising ramping from ambient temperature to about 215°C over about 1 hour, holding at about 215 °C for about 8 hours, ramping to about 250°C over about 12 minutes, holding at about 250 °C for about 6 hours, cooling to ambient temperature in a controlled manner over about 3 hours, and post-curing at about 315°C for about 4 hours. In some forms, the coating 240 has a dry thickness of about 0.005 inches. In some forms, the coating 240 is about 0.002 to about 0.040 inches. In some forms, the coating 240 has a dry thickness of about 0.5 pm to about 1 mm. In some forms, the coating 240 exhibits adhesion of greater than 4B according to ASTM D3359. In some forms, the coating 240 exhibits a glass transition temperature of at least about 280°C and a lap shear strength of at least about 650 psi at about 315°C.

[0082] Referring to FIG. 8, a method for forming the coating 230 on the substrate 210 is schematically shown and indicated by reference numeral 300. The method 300 begins at operation 302 with forming the composition 100, wherein the composition 100 has a total solids content (the curable component 112, theAttorney Docket No.: 0637-000020-WO-POAthermoplastic additive 114, and other additives) of about 10 wt.% to about 30 wt.%. At operation 304, the method 300 includes adjusting the total solids content of the composition 100 (e.g., by increasing the amount of the solvent 130) to have a Brookfield viscosity of no greater than about 300 cP at 25°C. At operation 306, the method 300 includes spraying the composition 100 on at least a portion of the surface 220 of the substrate 210 to form the deposited layer 230. At operation 308, the method 300 includes curing the deposited layer 230 to form the coating 240.

[0083] Unless otherwise expressly indicated herein, all numerical values indicating mechanical / thermal properties, compositional percentages, dimensions and / or tolerances, or other characteristics are to be understood as modified by the word “about” or "approximately" in describing the scope of the present disclosure. This modification is desired for various reasons including industrial practice, material, manufacturing, and assembly tolerances, and testing capability.

[0084] As used herein, the phrase at least one of A, B, and C should be construed to mean a logical (A OR B OR C), using a non-exclusive logical OR, and should not be construed to mean “at least one of A, at least one of B, and at least one of C.”

[0085] The description of the disclosure is merely exemplary in nature and, thus, variations that do not depart from the substance of the disclosure are intended to be within the scope of the disclosure. Such variations are not to be regarded as a departure from the spirit and scope of the disclosure.

Claims

Attorney Docket No.: 0637-000020-WO-POACLAIMSWhat is claimed is:

1. A composition comprising:a curable component comprising a reaction product of reactants, wherein the reactants comprise:one or more phenol-containing compounds, wherein each of the one or more phenol-containing compounds comprises one or more phenolic hydroxyl groups; andone or more phthalonitrile-containing compounds, wherein each of the one or more phthalonitrile-containing compounds comprises a phthalonitrile group and a substituent group attached to a benzene ring of the phthalonitrile group; anda thermoplastic additive.

2. The composition of Claim 1, wherein the composition further comprises a solvent.

3. The composition of Claim 2, wherein the solvent is a polar aprotic solvent.

4. The composition of Claim 2, wherein the solvent is selected from the group consisting of methylene chloride, ethylene chloride, chloroform, tetrachloroethane, tetrahydrofuran (THF), dioxane, acetophenone, cyclohexanone, m-cresol, g-butyrolactone, dimethylformamide (DMF), dimethylacetamide (DMAC), and N-methylpyrrolidone (NMP), and combinations thereof.

5. The composition of Claim 2, wherein the solvent comprises tetrahydrofuran (THF).

6. The composition of Claim 2, wherein a total amount of the curable component and the thermoplastic additive in the composition is about 5 wt.% to about 40 wt.%.Attorney Docket No.: 0637-000020-WO-POA7. The composition of Claim 2, wherein a total amount of the curable component and the thermoplastic additive in the composition is about 20 wt.% to about 30 wt.%.

8. The composition of Claim 2, wherein the composition has a Brookfield viscosity of about 50 cP to about 5000 cP at 25°C.

9. The composition of Claim 2, wherein the composition is a sprayable composition having a Brookfield viscosity of no greater than about 300 cP at 25°C.

10. The composition of Claim 1 or 2, wherein the composition is a paste having a Brookfield viscosity of about 300 cP to about 5000 cP at 25°C.

11. The composition of Claim 1 , wherein the one or more phenol-containing compounds and the one or more phthalonitrile-containing compounds are present such that a molar ratio of phenolic hydroxyl groups of the one or more phenol-containing compounds to substituent groups of the one or more phthalonitrile-containing compounds is about 0.9:1 to about 2:1.

12. The composition of Claim 1, wherein the one or more phenol-containing compounds comprise diallyl bisphenol A (DABPA), diallyl bisphenol S (DABPS), or a combination thereof.

13. The composition of Claim 1, wherein the one or more phthalonitrile-containing compounds comprise 3-substituted phthalonitrile, 4-substituted phthalonitrile, or a combination thereof.

14. The composition of Claim 1, wherein at least one of the one or more phenol-containing compounds comprises one or more substituents selected from the group consisting of alkyl group, allyl group, alkenyl group, alkynyl group, cycloaliphatic group, aromatic group, and combinations thereof.

15. The composition of Claim 1, wherein the curable component further comprises a curable resin component selected from a propargyl ether component, aAttorney Docket No.: 0637-000020-WO-POAbenzoxazine component, an epoxy component, a bismaleimide component, a cyanate ester component, and combinations thereof.

16. The composition of Claim 1, wherein the thermoplastic additive comprises a soluble polyimide.

17. The composition of Claim 16, wherein the soluble polyimide has a number average molecular weight of no more than 5 kDa.

18. The composition of Claim 16, wherein the soluble polyimide is partially imidized, fully imidized, or a combination thereof.

19. The composition of Claim 1, wherein the thermoplastic additive has a number average molecular weight of no more than 10 kDa.

20. The composition of Claim 1, wherein the thermoplastic additive has a glass transition temperature of at least about 250°C.

21. The composition of Claim 1, wherein the thermoplastic additive comprises polyimide, polyetherimide, or a combination thereof.

22. The composition of Claim 21, wherein the thermoplastic additive is fully or partially imidized.

23. The composition of Claim 1, wherein the thermoplastic additive is present in an amount of about 1 wt.% to about 40 wt.% based on total solids of the composition.

24. The composition of Claim 1, wherein the composition comprises an additive selected from the group consisting of a curing agent, a catalyst, a surfactant, a filler, a viscosity modifier, an adhesion promoter, and combinations thereof.

25. The composition of Claim 24, wherein the filler is selected from the group consisting of carbon black, graphite, silica particles, fumed silica particles, aluminaAttorney Docket No.: 0637-000020-WO-POAparticles, titanium dioxide particles, clay particles, boron nitride particles, boron carbide particles, silicon carbide particles, and combinations thereof.

26. The composition of Claim 1, wherein the composition further comprises an additive selected from the group consisting of a chain extender, a polymerization reaction control agent, a diluent, a reactive diluent, an appearance modifier, and combinations thereof.

27. The composition of Claim 1, wherein the curable component and the thermoplastic additive are miscible in a cast state.

28. The composition of Claim 1, wherein the composition, in a cured state, exhibits a glass transition temperature of at least about 280°C.

29. The composition of Claim 1, wherein the composition, in a cured state, exhibits a char yield of at least about 60%.

30. The composition of Claim 1, wherein the composition, in a cured state, exhibits a lap shear strength at least about 650 psi at a temperature of about 315°C as measured in accordance with ASTM D1002.

31. The composition of Claim 1, wherein the composition, in a cured, state, exhibits a lap shear strength at least about 900 psi at room temperature as measured in accordance with ASTM D1002.

32. A product formed from the composition of Claim 1.

33. The product of Claim 32, wherein the product is uncured, partially cured or fully cured.

34. The product of Claim 32, wherein the product exhibits a glass transition temperature of at least about 280°C, a lap shear strength of at least about 650 psi at about 315°C in a cured state.Attorney Docket No.: 0637-000020-WO-POA35. A coated substrate comprising the product of Claim 32, wherein the product is a coating.

36. A bonded article comprising the product of Claim 32, wherein the product is an adhesive disposed between two substrates.

37. The adhesive of Claim 36, wherein the adhesive is a free-standing film.

38. The adhesive of Claim 36, wherein the adhesive is supported on a scrim.

39. A composite comprising the product of Claim 32, wherein the product is a binder or a matrix material.

40. The composite of Claim 39, wherein the composite further comprises a reinforcement selected from the group consisting of fibers, fabrics, particulates, and combinations thereof.

41. A method of forming a coating on a substrate, the method comprising:forming the composition according to Claim 2, the composition having a total solids content of about 10 wt.% to about 30 wt.%;adjusting the total solids content of the composition to have a Brookfield viscosity of no greater than about 300 cP at 25°C;spraying the composition on at least a portion of a surface of the substrate to form a deposited layer; andcuring the deposited layer to form the coating.

42. The method of Claim 41, wherein the composition is sprayed to the surface of the substrate by high-volume low-pressure (HVLP), airless, air-assist airless, or electrostatic spray equipment.

43. The method of Claim 42, wherein the composition is sprayed onto the surface of the substrate with a nozzle orifice size of about 0.3 mm to about 1.5 mm, an atomizing pressure of about 0.5 bar to about 3.5 bar, and a spray distance of about 10 cm to about 30 cm.Attorney Docket No.: 0637-000020-WO-POA44. The method of Claim 41, wherein the deposited layer is cured at a temperature of about 120°C to about 300°C for about 10 minutes to about 4 hours.

45. The method of Claim 44, wherein the deposited layer is further cured at about 200°C to about 325°C for about 30 minutes to about 6 hours.

46. The method of Claim 41 , wherein the method comprises pre-treating the surface of the substrate prior to spraying by at least one of solvent wipe, abrasion, plasma treatment, and application of a silane adhesion promoter.

47. The method of Claim 41, wherein the method comprises multi-pass spraying to build thickness, wherein about 2 to about 50 passes are applied with about 1 to about 5 minutes between passes.

48. A coating formed by the method of Claim 41.

49. The coating of Claim 48, wherein the coating has a dry thickness of about 0.5 pm to about 1 mm.

50. The coating of Claim 48, wherein the coating exhibits adhesion of greater than 4B as measured in accordance with ASTM D3359.

51. A coated substrate comprising a coating on at least a portion of a surface of a substrate, wherein the coating is formed using the method of Claim 41.

52. The coated substrate of Claim 51, wherein the substrate comprises titanium or aluminum.

53. The coated substrate of Claim 51, wherein the coating exhibits a glass transition temperature of at least about 280°C.

54. The coated substrate of Claim 51, wherein the coating exhibits a lap shear strength of at least about 650 psi at about 315°C as measured in accordance with ASTM D1002.Attorney Docket No.: 0637-000020-WO-POA55. The coated substrate of Claim 51, wherein the coating exhibits a lap shear strength of at least about 900 psi at room temperature as measured in accordance with ASTM D1002.