Wire cable formed from anodized tungsten filaments and methods of anodizing tungsten wire filaments
Anodized tungsten wire cables address the challenges of high stress and wear in surgical instruments by maintaining anodized surfaces during cold drawing, resulting in enhanced fatigue life and durability, suitable for medical and other high-stress applications.
Patent Information
- Application Number
- PCT/US2026/027072
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing wire cables used in surgical instruments face challenges with high axial loads and torsion, leading to low cycle life and wear, particularly in small instruments where space is limited, and require materials with enhanced tensile strength and durability.
The development of wire cables made from anodized tungsten filaments, which are cold drawn to maintain an anodized outer surface of tungsten oxide, providing improved resistance to oxidation, corrosion, and wear, while maintaining high tensile strength.
The anodized tungsten wire cables exhibit significantly enhanced fatigue life and structural integrity, with up to 650% improvement in minimum and maximum fatigue life compared to non-anodized cables, suitable for applications in medical devices and other high-stress environments.
Smart Images

Figure US2026027072_12112026_PF_FP_ABST
Abstract
Description
WIRE CABLE FORMED FROM ANODIZED TUNGSTEN FILAMENTS AND METHODS OF ANODIZING TUNGSTEN WIRE FILAMENTSCROSS REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of U.S. Provisional Application No.63 / 802,070 filed May 8th, 2025, entitled “WIRE CABLE FORMED FROM ANODIZED TUNGSTEN FILAMENTS AND METHODS OF ANODIZING TUNGSTEN WIRE FILAMENTS’' which is herein incorporated by reference in its entirety.BACKGROUND1. Technical Field
[0002] The present disclosure pertains to wire products, including wire cables or ropes, made of a plurality of stranded individual tungsten filaments having an anodized outer surface of tungsten oxide, together with methods of producing anodized tungsten wire filaments and wire cables made of such filaments for use in applications such as surgical instruments, for example.2. Description of the Related Art
[0003] Wire ropes or multi-filament cables are commonly used in applications where axial and / or tensile loads are transmitted along a tortuous path, for example, around one or more pulleys or sheaves. One key application is in surgical instruments of the ty pe including manipulators actuated by wire cables for use in endoscopy, laparoscopy, and / or other surgeries such as neurosurgery, vascular surgery, or joint replacement surgery, for example.
[0004] The surgical instruments often include end effectors and may be controlled manually or by robotic manipulator technology7, for example. In the robotic and surgical instrument endoscopy markets, reduction in the size of endoscopes and the components that articulate the endoscopes is desirable. However, the loads required for the application typically do not decrease with instrument size. On the contrary, smaller instruments demand smaller moment arms for manipulation, and consequently7higher forces.
[0005] In modem surgical instruments, it is common that axial loads combined w ith bending over pulleys as small as 2-3 mm in diameter, for example, place very7high stresses on the cables. Under high axial loads, for example, greater than 50% of axial breaking load.known wire rope or cable constructs typically exhibit low cycle life. In addition, considerable torsion of the wire rope may occur as the helical winding of the cable attempts to “unwind” under high tensile loads.
[0006] In some surgical instruments used in minimally invasive surgical procedures, for example, the total size of the instrument is limited by the human body. Such instruments may have a maximum transverse dimension of about 7-8 mm, and this dimension may preferably be smaller and may not be larger. This small maximum dimension is imposed by human physiology, i.e., the spaces between tissues and bones which cannot be violated by the surgical instrument.
[0007] Wire cables used in such surgical instruments may be made of tungsten filaments having a polished outer surface in which any oxide layer formed on the wire filament has been removed by electropolishing or chemical polishing.
[0008] It is desired to provide a wire cable formed of a plurality' of individual tungsten filaments which is an improvement over the foregoing.SUMMARY
[0009] The present disclosure provides a wire cable made from anodized tungsten filaments designed to exploit the high tensile strength of tungsten while enhancing the performance and durability of the tungsten cable by anodizing the outer surfaces of the individual tungsten filaments. The filaments may also be cold drawn to provide high strength tungsten monofilament wires with anodized outer surfaces that are integrated into final cable assemblies, addressing the challenges of high wear applications in fields such as medical devices, aerospace, and military equipment, for example.
[0010] In one form thereof, the present invention provides a wire cable, including a plurality of individual wire filaments stranded to form the cable, at least some of the wire filaments made of tungsten, the tungsten wire filaments each having a core and an anodized outer surface of tungsten oxide.
[0011] In another form thereof, the present invention provides a method of forming anodized tungsten wire filaments, including anodizing the surface of wire filaments each made of tungsten and having a round cross-section with a first diameter to form the wire filaments with an anodized outer surface of tungsten oxide; and drawing the wire filaments through a die to reduce the cross section of the wire filaments to a second diameter less than the first diameter.BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The above mentioned and other features and objects of this invention, and the manner of attaining them, will become more apparent and the invention itself will be better understood by reference to the following description of embodiments of the invention taken in conjunction with the accompanying drawings, wherein:
[0013] Fig. 1 is a cross-sectional view of a tungsten wire filament including a core and an anodized outer surface of tungsten oxide.
[0014] Fig. 2 is a schematic view of an exemplary continuous anodizing apparatus.
[0015] Fig. 3 is a wire cable formed of a plurality of anodized tungsten wire filaments.
[0016] Fig. 4 is a partial sectional view of a pulley.
[0017] Fig. 5 is a view of the pulley of Fig. 4, carrying the cable of Fig. 3.
[0018] Corresponding reference characters indicate corresponding parts throughout the several views. Although the exemplifications set out herein illustrate embodiments of the invention, the embodiments disclosed below are not intended to be exhaustive or to be construed as limiting the scope of the invention to the precise form disclosed.DETAILED DESCRIPTION
[0019] 1. Introduction.
[0020] Referring to Fig. 1, a cross-sectional view of a wire filament 10 is shown, which is made of tungsten and generally includes a core 12 and an anodized layer of tungsten oxide (WO3) 14 formed on the outer surface of the wire filament 10 to a given depth Di as discussed in further detail below.
[0021] The w ire filament may be formed of tungsten having a purity of at least 99.0%. at least 99.5%. at least 99.95%, or at least 99.995%. for example, together with trace impurities, prior to being subjected to the anodizing process by which the anodized layer of tungsten oxide (WOs) 14 is formed.
[0022] Wire filament 10 may have a final diameter, after the anodizing and cold working processes described herein, of as little as 0.001 mm, 0.01 mm. or 0.10 mm, or as great as 0.50 mm, 1.0 mm, or 1.5 mm, or within any range using any two of the foregoing values as end points, for example, from 0.001 mm to 1.5 mm, from 0.01 mm to 1.0 mm, or from 0.10 mm to 0.50 mm, for example.
[0023] Wire filament 10 is shown having a round cross-section, though this is not critical, and the filament may alternatively have a square or rectangular cross-section, for example. As discussed in detail below, wire filament 10 is subjected to cold work, such as wire cold drawing, to progressively reduce the outer diameter of filament 10 while also maintaining the continuous, uninterrupted anodized layer 14 which is imparted via anodizing as discussed below.
[0024] Advantageously, it has been found that the anodizing conditions may be tailored to anodize the surface of the wire filaments to an extent by which the wire filaments may be subsequently draw n to reduce their diameter without adversely affecting the anodized surface. In this manner, following one or more drawing steps, the anodized surface is maintained continuously along the length of the wire filaments.
[0025] As used herein, "wire" or "wire product" encompasses continuous wire and wire products which may be continuously produced and wound onto a spool for later dispensation and use, such as wire having a round cross section and wire having a non-round cross section, including flat wire or ribbon. "Wire" or "wire product" also encompasses other wire-based products such as strands, cables, coil, and tubing, which may be produced at a particular length depending on a particular application. In some exemplary embodiments, a wire or wire product in accordance with the present disclosure may have a diameter up to 2.5 mm.
[0026] '“Impurities,” “incidental impurities” and ““trace impurities” and “‘unavoidable impurities” are material constituents present in a material at less than 500 parts per million or 0.05 wt. %.
[0027] 2. Anodizing process.
[0028] As discussed below; the wire filaments are subjected to a continuous anodization process to form a tungsten oxide layer on the surface of the wire filaments.
[0029] Referring to Fig. 2, an exemplary anodizing apparatus 18 as shown, which includes a spool 20 which wire 10 is taken, following by passing wire 10 through anodizing tank 22 including first and second chambers 22a and 22b separated by a bridge 24. A power source 26 is electrically connected to tank 22 via anode 28 and cathode 30. The apparatus 18 further includes a rinse bath 32 and one or more drawing dies 34 in a lubricant bath 36. Wire 10 is taken onto take-up spool 38 after drawing.
[0030] The anodizing bath may be an electrolytic solution of water and an electrolyte such as phosphoric acid, sulfuric acid, or ammonium titrate, for example.
[0031] The concentration of the electrolyte in the anodizing bath may be as little as 1 wt.%, 2 wt.%, or 3 wt.%, or as great as 8 wt.%, 9 wt.%. or 10 wt.%, based on a total weight of the electrolytic solution, or may be within any range including any two of the foregoing values as endpoints, such as from 1 wt.% to 10 wt.%, from 2 wt.% to 9 wt.%, or from 3 wt.% to 8 wt.%, for example.
[0032] The applied anodizing voltage may be as little as 10 volts (V). 20 volts (V), or 30 volts (V), or as great as 70 volts (V), 80 volts (V), or 90 volts (V), or may be within any range including any two of the foregoing values as endpoints, such as from 10 to 90 volts (V), from 20 to 80 volts (V), or from 30 to 70 volts (V), for example.
[0033] The wire filaments may be exposed to the anodizing bath for a dwell time of as little as 0.5, 1.0 or 1.5 seconds, or as great as 6. 8, or 10 seconds, or within any range including any two of the foregoing values as endpoints, such as from 0.5 to 10 seconds, from 1.0 to 8 seconds, or from 1.5 to 6 seconds, for example.
[0034] Referring again to Figs. 1, the anodizing process described above produces an anodized layer 14 of tungsten oxide at the outer surface of the wire, which extends to a depth Di of as little as 0.25 microns, 0.50 microns or 0.75 microns, or as great as 1.0 micron, 1.25 microns, or 1.5 microns from the surface of the wire filament 10, based on the anodizing conditions, or within any range using any two of the foregoing values as endpoints, for example, the depth Di may be from 0.25 microns to 1.5 microns, 0.50 microns to 1.25 microns, or from 0.75 microns to 1.0 micron, for example.. The variables that can affect the extent or depth of the anodized layer 14 include the voltage applied during anodizing, the amount of time the wire filament is exposed to the anodizing process, and the nature of the electrolyte solution, for example.
[0035] The anodizing process significantly enhances resistance of the wire cable to oxidation, corrosion, and chemical attack. Further, anodization provides improved surface properties, such as reduced friction, improving the interaction between the individual monofilaments within the cable assembly by reduced inter-filament wear. Still further, the anodized tungsten wire cable exhibits external and internal wear resistance as well as resistance to fretting or gall.
[0036] 3. Cold working.
[0037] Before and / or after anodizing, the wire filament is subjected to cold work to reduce its diameter, such as via wire drawing through one or more drawing dies. The end ofthe wire filament protruding through the drawing die is gripped and pulled through the die to reduce the diameter / cross-sectional area of the wire construct. For purposes of the present disclosure, cold-working methods effect material deformation at or near room temperature, e.g., 20-30 °C. Drawing imparts cold work, resulting in concomitant reduction in the cross-sectional area. The total cold work imparted to the wire during drawing can be characterized by the following formula (I):cw = l- x 100% (I)wherein “cw’’ is cold work defined by reduction of the original material area, "D2" is the outer cross-sectional diameter of the wire after the draw or draws, and "Di" is the outer cross-sectional diameter of the wire prior to the same draw or draws.
[0038] The cold work step may be performed by drawing the wire through a lubricated die having an output diameter D2, which is less than diameter Di of the wire prior to the drawing step. The outer diameter of the wire is accordingly reduced from pre-drawing diameter Di to drawn diameter D2, thereby imparting cold work (cw).
[0039] Alternatively, net cold work may be accumulated in the wire by other processes such as cold swaging, rolling the wire (e.g., into a flat ribbon or into other shapes), extrusion, bending, flow forming, severe plastic deformation, or pilgering. Cold work may also be imparted by any combination of techniques including the techniques described here, for example, cold swaging followed by drawing through a lubricated die finished by cold rolling into a ribbon or sheet form or other shaped wire forms. In one exemplary embodiment, the cold work step by which the diameter of the wire is reduced from Di to D2 is performed in a single draw and, in another embodiment, the cold work step by which the diameter of the wire is reduced from Di to D2 is performed in multiple draws which are performed sequentially without any annealing step therebetween. When calculating cold work cw using formula (I) above, it is assumed that no anneal has been performed subsequent to the process of imparting cold work to the material.
[0040] For processes where the drawing process is repeated without an intervening anneal of the wire, each subsequent drawing step further reduces the cross-sectional area of wire proportionately. Thermal stress relieving, otherwise known in the art as annealing, at a nominal temperature not exceeding the melting point of the wire material is used to improve the ductility of the fully dense composite between drawing steps, thereby allowing further plastic deformation by subsequent drawing steps.
[0041] Heating the wire to a temperature sufficient to cause recovery and recrystallization of grains eliminates accumulated cold work. The cold work imparted by each iterative cold work process is relieved by fully annealing the material between draws, thereby enabling the next iterative cold working process. In full annealing, the cold worked material is heated to a temperature sufficient to substantially relieve the internal stresses stored in the material, thereby relieving the stored cold work and “resetting” cold work to zero.
[0042] On the other hand, wires subject to drawing or other mechanical processing without a subsequent annealing process retain an amount of cold work. The amount of retained work depends upon the overall reduction in diameter from Di to D2 and may be quantified by individual grain deformation within the material resulting from the cold work imparted.
[0043] As a result of the deformation and annealing processes, the cross-sectional area of the preform may be reduced, as compared with the initial cross-sectional area of the preform formed by the additive manufacturing process described previously, by as little as 5%, 15%, 25%, 35%, or 45%. or as much as 55%. 65%. 75%. or even 90%, 95%, or 99.9%, or within any range using any of the two foregoing values used as endpoints, such as 5% to 99.0%, 15% to 95%, or 25% to 90%, for example.
[0044] It has been found that the cold working steps do not interrupt or otherwise compromise the anodized layer formed on the wire filaments. In other words, the anodized layer remains present as a continuous, uninterrupted layer on the wire filaments following each cold working step, wherein the anodized layer itself elongates with the underlying core of the wire filaments during cold drawing.
[0045] To some extent, a thicker anodized layer formed in one or more anodizing steps prior to a cold working step may allow a greater degree of cold work in a single or multiple draws following the anodizing step or steps.
[0046] The anodizing and drawings steps may be repeated, for example, following an initial step of anodizing followed by drawing, the wire may be subjected to an additional anodizing step followed by an additional drawing step. This process may be iteratively repeated to achieve the desired diameter reduction for the wire filaments. Additionally, these steps need not necessarily alternate with one another, for example, multiple passes through the anodizing process may be conducted before the wire is drawn and / or after a final drawing step, and multiple drawing steps may be conducted as desired between each anodizing step or after a final anodizing step.
[0047] 4. Stranding to form wire cables.
[0048] A plurality of wire filaments may be stranded to form a wire cable. Referring to Fig. 3, cable 50 may include several strands 52 with each strand 52 including a plurality of individual wire filaments 10.
[0049] For purposes of the present disclosure, a cable construction is represented according to the nomenclature ”| number of strands in the cable] x [number of wire filaments per strand],” where a wire filament (also known as a filar) is a single, monolithic drawn wire and a strand is a collection of wire filaments twisted or wound together. Cable 50 show n in Figs. 3 is referred to as a “37 x 7” cable 10, meaning that cable 50 has thirty -seven strands 52, with each strand 52 including seven wire filaments 10.
[0050] In some designs, a central cable construct may be sheathed within another, outer cable construct. For purposes of the present disclosure, these designs are represented as “[number of strands in the central cable] x [number of wire filaments per strand in the central cable] + ([number of strands in the outer cable] x [number of wire filaments per strand in the outer cable])”. Thus, a “7 x 7 + (8 x 19)” cable construct has a 7 x 7 construct forming a central cable, which is sheathed by eight strands each including 19 wire filaments forming an outer cable.
[0051] However, the cable configuration shown in Fig. 3 is not critical and merely one representative cable construction. Cables 50 of the present disclosure may include a total of at least 75, at least 100, at least 125, at least 150 or at least 175 or more individual wire filaments 10.
[0052] Referring again to Fig. 3, the strands 52 of the are arranged in first, second, third, and fourth layers 52a, 52b, 52c and 52d and may be wound in alternating, sequentially opposite helical directions. For example, the strands 52 of second layer 52b may be wound in a first helical direction, the strands 52 of third layer 52c in a second, opposite helical direction, and the strands 52 of fourth layer 52d in the same helical direction as strands 52 of second layer 52b.
[0053] Advantageously, with the strands 52 of adjacent layers wound in opposite helical directions, when cable 50 is subjected to axial / tensile loading to generate an unwinding force, because the layers are wound in opposite helical directions the unwinding forces of the layers tend to act opposite one another and thereby maintain the winding integrity of the cable layers. In this manner, the overall cable 50 has a high tensile stability and resistance to unwinding and may be referred to as a “non-rotating” cable. Thus, cable 50provides a high axial and torsional load carry ing capability without inducing torque or “spin" within cable 50 itself or within the device in which cable 10 is incorporated.
[0054] Further, cable 50 may be assembled in a “regular lay” construction, in which the wire fdaments 10 of each strand 52 are wound in a first helical direction, with the strands 52 themselves wound in a second, opposite helical direction. The foregoing discussion of cable 50 assumes a “regular lay” construction. Alternatively, cable 50 may be made in a “Lang’s lay” construction, in which filaments 10 of each strand 52 are wound in a first helical direction, with the strands 52 themselves wound in the same first helical direction. In the case of a Lang's lay configuration, adjacent layers 52a, 52b, 52c, 52d may be wound in the same helical direction, rather than an opposite helical direction as described above.
[0055] The final cable 50 may itself be swaged, drawn, heat treated (annealed), and / or coated or over-braided as desired.
[0056] 5. Physical properties.
[0057] Wire filaments and wire cables made in accordance with the present disclosure, and particularly section 4 above, provide excellent performance in terms of structural fatigue and mechanical strength.
[0058] In rotary7beam fatigue testing in accordance with the Examples herein, a wire cable formed of the plurality of wire filaments in accordance with Section 4 above, is cut to a length of approximately about 118 mm (e.g., for a 0.33 mm diameter wire), then secured at its axial ends to rotatable jaws. The free portion of the wire between the jaws is bent to introduce a desired tensile strain at the “peak” or outermost portion of the bend. Directly opposite this peak of the bend, the wire experiences a compressive strain equal to the tensile strain, with the nominal value of both the tensile and compressive strains referred to herein as the “strain amplitude.” The jaws are then rotated in concert (i.e., each jaw rotated with the same speed and in the same direction), such that the area of maximum tensile strain is rotated around the wire “peak” and transitioned to the area of maximum compressive strain with each 180-degree rotation of the jaws and wire. Rotary beam fatigue testing is further described in ASTM E2948-14, the entire disclosure of which is hereby expressly incorporated herein by reference.
[0059] The fatigue strength and endurance of wire cables formed from anodized tungsten, as performed on the rotary beam described previously, outperforms wire cables formed from otherwise identical unanodized tungsten material. Said another way, theanodization process results in a wire cable with increased strength and endurance over wire cables that do not undergo anodization.
[0060] For example, a wire cable formed from non-anodized tungsten wire may exhibit an average fatigue life of about 1,200 cycles, about 1,500 cycles, or about 2,000 cycles before failure when tested under combined bending and wear conditions at a strain amplitude of approximately 12-13% at room temperature. A wire cable formed from anodized tungsten wire in accordance with the present disclosure, however, may exhibit an average fatigue life of about 10,000 cycles, about 11,000 cycles, or about 12,000 cycles before failure, substantially exceeding the average cycles-to-failure of an otherwise identical wire cable formed from non-anodized tungsten wire. Stated another way, the anodized tungsten wire may provide about 550% greater, about 600% greater, or about 650% greater average fatigue life than a wire cable formed from non-anodized tungsten wire.
[0061] A wire cable formed from non-anodized tungsten wire may exhibit a minimum fatigue life of about 1,000 cycles, about 1,200 cycles, or about 1,500 cycles before failure, when tested under combined bending and wear conditions at a strain amplitude of approximately 12-13% at room temperature. A wire cable formed from anodized tungsten wire in accordance with the present disclosure, however, may exhibit a minimum fatigue life of about 7,000 cycles, about 7,500 cycles, or about 8,000 cycles before failure under similar test conditions. Stated another way, the anodized tungsten wire cable may exhibit greater than about 500%, greater than about 550%. or greater than about 600% improvement in minimum fatigue life relative to an otherwise identical wire cable formed from non-anodized tungsten wire. This improvement in minimum fatigue life is particularly relevant as the minimum cycles-to-failure value defines a conservative design limit for high-reliability applications.
[0062] In another example, a wire cable formed from non-anodized tungsten wire strands may exhibit a maximum fatigue life of about 1,900 cycles, about 2,000 cycles, or about 2,100 cycles before failure when tested under combined bending and wear conditions at a strain amplitude of approximately 12-13% at room temperature. A wire cable formed from anodized tungsten wire strands in accordance with the present disclosure, however, may exhibit a maximum fatigue life of about 15,000 cycles, about 16,000 cycles, or about 17,000 cycles before failure under similar test conditions. Said another way, the anodized tungsten wire cable may exhibit about 650% greater, about 700% greater, or about 750% greater maximum fatigue life than an otherwise identical wire cable formed from non-anodized tungsten wire strands.
[0063] Said another way, the fatigue life of the wire cable formed from anodized tungsten wire filaments may outperform the minimum performing non-anodized wire (e.g., the non-anodized wire exhibiting the minimum performance of 1195 cycles) by as little as about 563%, about 564%, about 567%, about 568%, about 757%, or about 849%, or by as much as about 864%, about 913%, about 963%, about 1047%, about 1156%, about 1191%, or about 1315%, or between any of the foregoing values used as endpoints, such as about 563% to about 1315%.
[0064] The fatigue life of the wire cable formed from anodized tungsten wire filaments also may outperform the maximum performing non-anodized wire (e.g., the non-anodized wire exhibiting the maximum performance of 2062 cy cles) by as little as about 284%, about 285%, about 286%, about 287%. about 397%. or about 450%, and by as much as about 459%, about 487%, about 516%, about 565%, about 628%, about 648%, or about 720%, or between any of the foregoing values used as endpoints, such as about 284% to about 720%. This demonstrates that the improvement in fatigue performance is maintained even relative to either the lowest or highest-performing non-anodized wires, and reflects a consistent and significant enhancement of the wire cable formed from anodized tungsten wire filaments.
[0065] A wire cable formed from anodized tungsten wire filaments in accordance with the present disclosure may also have a breaking strength of at least 4500 MPa, at least 5500 MPa. or at least 6500 MPa, as determined by ASTM F288 using an Instron twin screw tensile tester utilizing 10 to 1000 N load cells depending on wire size and strength level and using flat face pneumatic grips and fine emery to avoid slipping.
[0066] This enhanced fatigue endurance of the wire filaments allows wire cables formed from the filaments to be well suited for use in many medical and non-medical applications as set forth below.
[0067] 6. Medical device applications.
[0068] Cable 50 will be further described below with reference to an exemplary- medical device application in which cable 50 may be used, such as an endoscope device which includes a relatively small diameter pulley 54, shown in Fig. 4. Pulley 54 defines a root diameter, shown as dimension RD in Fig. 4, which may be as little as 1 mm, 2 mm, or 3 mm or as great as 4 mm, 5 mm or 6 mm, for example. Referring to Fig. 5, when disposed around pulley 54, due to the small diameter of pulley 54, cable 50 will need to accommodate a very high amount of bending strain for cable 50 to remain properly seated within the pulleyspace 56 defined within the root diameter RD of pulley 54 while cable 50 is subjected to tensile loading.
[0069] In this connection, one typical problem with existing cables is that the individual wire filaments of the cables are too large in diameter to accommodate the bending stresses imposed by such small pulleys. In addition, because the cables are subjected to relatively high tensile loads, the use of relatively larger diameter wire filaments minimizes the contact points or total contact area, between the outermost periphery of the cable with the pulley, thereby leading to potential disengagement of the cable from the pulley.
[0070] In many industrial, large-scale applications, pulleys will typically have a root diameter which is much larger than the diameter of an associated cable, such as 15, 20, 25, or 40 times the diameter of the cable. However, in the present medical device application, the root diameter RD of pulley 54 may be between 3 and 6 times the outer diameter of cable 50, such as 3, 4, 5, or 6 times the diameter of cable 50.
[0071] Advantageously, cable 50 provides good resistance to bending stress in that the outer diameter of the individual wire filaments 10 is minimized such that the wire filament count, or ‘'filar” count, of cable 50 is high to provide reduced bending strain. As may be seen in Fig. 5, the minimized outer diameter of the wire filaments 10 of cable 50, as well as the relatively small number of wire filaments 10 in each strand 52 with the number of strands 52 being high in the outermost layer 52d of cable 50, the outmost periphery of cable 50 closely approximates a cylinder, such that cable 50 will maintain substantial area contact with the adjacent (generally cylindrical) surface of pulley 54.
[0072] Cable 50 further exhibits resistance to crushing or flattening when used in a system of pulleys or sheaves or other guiding surfaces of the type shown in Fig. 5, such as pulley surfaces of small diameter as in surgical instruments or robotic systems. Cable 50 has a greater surface area in contact with the pulley 54 therefore distributing normal forces and resulting in lower contact stress.
[0073] In the above manner, in the field of medical devices such as endoscopes, cable 10 provides increased design flexibility due to its superior bending stress characteristics for a given tensile load rating. Similarly, cable 50 provides a high-performance, long-lasting replacement for cables used in existing medical device designs.
[0074] Potential applications of cable 50 include continuum robots / endoscopes, “snake-like” robots / endoscopes, high precision linear / cable extensometers, cerclage systems, catheter and delivery systems (which maintain planarity when deflected), electrophysiology catheters, prosthetics (which benefit from quiet running due to smooth surface in conduits).
[0075] 7. Other applications.
[0076] Non-medical device applications for cable 50 include aerospace, for example, durable wiring and structural components for spacecraft and high-altitude aircraft and in the military industry, for example, reinforced cables for military -grade equipment operating in extreme conditions. Further applications include safety lock wires (which benefit from not untwisting when tensioned), antennae arrays, mechanical drive systems, cable extension position sensors, and mechatronic applications.EXAMPLES
[0077] The following non-limiting Examples illustrate various features and characteristics of the present invention, which is not to be construed as limited thereto.Example 1Production of anodized tungsten wires and cables
[0078] Tungsten wire was received in diameters ranging from 0.010” (0.254 mm) to 0.005” (0.127 mm), and the wire was cleaned to remove any existing foreign material and / or oxidation layers in preparation of the surface for anodization. The wire w as passed through the inline anodizing system including an anodizing tank with two chambers separated by a bridge with each chamber containing a stainless-steel cathode plate. The anodizing bath included 4 wt.% sulfuric acid in water that was purified by reverse osmosis.
[0079] The applied voltage was between 10 and 90 volts, typically 40-50 volts, and the dwell time of the wire in the anodizing tank was about 2 seconds, forming an anodized oxide layer of approximately 60 microinches (pin). Anodized and drawn tungsten wire is continuously wound onto a take-up spool with effective tensioning control to maintain consistent wire quality and prevent back tension damage.
[0080] After anodizing and rinsing, the wire enters a drawing die with oil lubricant to enhance lubricity and reduce die wear for cold drawing in multiple stages, wherein each stage reduces the wire diameter incrementally w hile repeating the anodizing and rinsing steps inline. The monofilament wire is then stranded to form a cable.
[0081] While this invention has been described as having an exemplary' design, the present invention may be further modified w ithin the spirit and scope of this disclosure. This application is therefore intended to cover any variations, uses, or adaptations of the invention using its general principles. Further, this application is intended to cover such departuresfrom the present disclosure as come within known or customary practice in the art to which this invention pertains.Example 2Production and Fatigue Evaluation of Anodized Tungsten Wires and Cables
[0082] Wire cables formed in accordance with Example 1 were evaluated to determine fatigue performance under cyclic loading conditions representative of high-contact, high-cycle applications, including cable-driven medical and robotic actuation systems.Comparative fatigue testing was conducted using tw o cable configurations: a standard cable formed from non-anodized tungsten wire strands and an otherwise identical cable formed from anodized tungsten wire strands produced as described in Example 1. All other variables, including cable geometry, construction, filament count, and base material composition, were held constant betw een test groups.
[0083] Fatigue testing was performed using a Blockwise Engineering FTX Wire Rotary Beam Fatigue Tester modified to introduce accelerated wear conditions. Portions of ASTM E2948-14 were used in the testing. The tester was configured with a wear pin positioned at the apex of cable deflection on the compression side such that the cable experienced localized contact and sliding interaction at a fixed point during cyclic loading. A spring-loaded hinge mechanism applied a substantially constant normal force to the cable against the wear pin throughout testing, thereby subjecting the cable to combined bending fatigue and surface wear.
[0084] All cable specimens w ere tested at room temperature with a calculated strain amplitude of approximately 12.8%. Cyclic loading was applied until failure, which w as defined as fracture of one or more load-bearing filaments resulting in loss of structural integrity of the cable. The number of cycles to failure was recorded for each specimen.
[0085] The measured cycles to failure for the standard cables and the anodized cables are summarized in Tables 1 and 2 below, respectively.Table 1 — Cycles to Failure Under Combined Bending and Wear Conditions for Standard Cable:StandardSample Cable(cycles)1 18752 15723 14734 151 15 13776 18747 20628 14229 160110 151211 119512 173813 2010Average 1589Maximum 2062Minimum 1195Table 2 — Cycles to Failure Under Combined Bending and Wear Conditions for Anodized Cable:% Increase in % Increase in Anodized Cycles vs. Cycles vs.Sample Cable Minimum Maximum(cycles) Standard Cable Standard Cable Cycles (1195) Cycles (2062)1 13708 1047 565 2 7987 568 287 3 15006 1156 628 4 12108 913 487 5 7921 563 284 6 16905 1315 720 7 7939 564 285 8 7967 567 286 9 10247 757 397 10 11335 849 450 11 15424 1191 648 12 11518 864 459 13 12703 963 516Average 11504 863 458Maximum 16905 1315 720Minimum 7921 563 284
[0086] As based on the data in Tables 1 and 2, the wire cables formed from anodized tungsten wire strands demonstrated a substantial improvement in fatigue performance relative to the wire cables formed from non-anodized tungsten wire strands. The average fatigue life of the anodized cable population was approximately 11,504 cycles, compared to approximately 1589 cycles for the non-anodized cable population, representing an improvement of approximately 6.2-fold (e.g., 624 %). The minimum observed fatigue life increased from 1195 cycles for the non-anodized cables to 7,921 cycles for the anodized cables, corresponding to approximately 5.6 fold (e.g., 563%) improvement in minimum fatigue performance. The maximum observed fatigue life increased from 2,062 cycles to 16, 905 cycles, indicating an improvement of approximately 7.2-fold (e.g., 720%).
[0087] In addition to improvements in minimum and average fatigue life values, the fatigue life of the anodized cable population was consistently and substantially greater than that of the non-anodized cable population across all samples. The non-anodized cables exhibited fatigue life values on the order of approximately 1,200 to 2,000 cycles, whereas all anodized cable samples exhibited markedly higher fatigue life, generally in the range of approximately 8,000 to 18,000 cycles. Notably, even the lowest-performing anodized cable exceeded the highest fatigue life observed for the non-anodized cables.
[0088] Specifically, the fatigue life of the anodized wire outperforms the minimum performing non-anodized wire (e.g., the non-anodized wire exhibiting the minimum performance of 1195 cycles) by as little as about 563%. about 564%, about 567%, about 568%, about 757%, or about 849%, or by as much as about 864%, about 913%, about 963%, about 1047%, about 1156%, about 1191%, or about 1315%, or between any of the foregoing values used as endpoints, such as about 563% to about 1315%. The fatigue life of the anodized wire also outperformed the maximum performing non-anodized wire (e.g., the non-anodized wire exhibiting the maximum performance of 2062 cycles) by as little as about 284%, about 285%, about 286%, about 287%, about 397%, or about 450%, and by as much as about 459%, about 487%, about 516%, about 565%, about 628%, about 648%, or about 720%, or between any of the foregoing values used as endpoints, such as about 284% to about 720%. This demonstrates that the improvement in fatigue performance is maintained even relative to the highest-performing non-anodized wires and reflects a consistent and significant enhancement across the tested cable population.
[0089] This demonstrated that the improvement in fatigue performance w as not limited to isolated cases but instead represented a consistent and significant enhancement across the tested cable population.
[0090] The fatigue performance improvements observed for the wire cables formed from anodized tungsten wire strands are believed to arise from modifications to the surface condition of the individual wires resulting from the anodization process. In particular, anodization is believed to reduce the incidence of surface-initiated crack formation under cyclic loading, improve resistance to wear and fretting at contact interfaces, including wire-to-wire and wire-to-counterface contact regions, and enhance durability under conditions involving simultaneous bending and surface interaction. These effects are especially relevant under the combined bending and wear conditions imposed during testing, which simulate dominant failure modes encountered in pulley-driven and cable-actuated systems.
[0091] The modified fatigue testing configuration, incorporating a wear pin positioned at the apex of cable deflection and a substantially constant normal force applied throughout cyclic loading, further emphasizes the ability of the anodized wire surface to withstand localized contact stresses and sliding interaction during repeated bending. The observed increases in minimum, average, and maximum cycles to failure, as well as the upward shift in the overall fatigue-life distribution of the anodized cable population, demonstrate that anodization provides a robust and repeatable improvement in fatigue performance across the tested cables.
[0092] In particular, the substantial increase in minimum fatigue life is significant for applications requiring high reliability and predictable failure thresholds, as the minimum cycles-to-failure value defines a conservative design limit. The improvement in maximum fatigue life further indicates enhanced endurance under demanding operating conditions. Taken together, the data demonstrate that anodization of individual tungsten wire strands prior to cabling produces a meaningful and population-wide enhancement in fatigue performance of the resulting wire cables, particularly under conditions involving combined bending and surface wear.ASPECTS
[0093] Aspect 1 is a wire cable, comprising a plurality of individual wire filaments stranded to form the cable, at least some of the wire filaments made of tungsten and having a round cross-section, the tungsten wire filaments each having a core and an anodized outer surface of tungsten oxide.
[0094] Aspect 2 is the wire cable of Aspect 1. wherein the wire filaments have a diameter of less than 1.5 mm.
[0095] Aspect 3 is the wire cable of Aspect 1 , wherein the wire filaments have a diameter of less than 1.0 mm.
[0096] Aspect 4 is the wire cable of Aspect 1, wherein the wire filaments have a diameter of less than 0.5 mm.
[0097] Aspect 5 is the wire cable of any one of Aspects 1-4, wherein the core of each of the tungsten wire filaments is made of tungsten having a purity of at least 99.0 wt.%.
[0098] Aspect 6 is the wire cable of any one of Aspects 1-5, wherein the core of each of the tungsten wire filaments is made of tungsten having a purity of at least 99.0 wt.%.
[0099] Aspect 7 is the wire cable of any one of Aspects 1 -6, wherein the anodized outer surface of tungsten oxide has a thickness of at least 0.25 microns.
[0100] Aspect 8 is the wire cable of any one of Aspects 1-7, wherein the anodized outer surface of tungsten oxide has a thickness of from 0.25 microns to 1.5 microns.
[0101] Aspect 9 is the wire cable of any one of Aspects 1-8, wherein each of the tungsten wire filaments has a breaking strength of at least 4500 MPa, as determined by ASTM F288.
[0102] Aspect 10 is a wire cable of any one of Aspects 1-9, comprising a rotary beam fatigue life exceeding that of a corresponding cable formed from non-anodized wire filaments.
[0103] Aspect 11 is a wire cable of any one of Aspects 1-10, wherein the rotary beam fatigue life is at least 250% greater than that of a corresponding cable formed from nonanodized wire filaments.
[0104] Aspect 12 is a wire cable of any one of Aspects 1-11, comprising a rotary7beam fatigue strength exceeding 12,000 cycles at 12.8% strain.
[0105] Aspect 13 is the wire cable of any one of Aspects 1-12, wherein the cable comprises at least 100 of the wire filaments.
[0106] Aspect 14 is the wire cable of any one of Aspects 1-13, wherein the wire filaments each have a round cross-section.
[0107] Aspect 15 is a method of forming anodized tungsten w ire filaments, comprising anodizing the surface of wire filaments each made of tungsten and having a round cross-section with a first diameter to form the wire filaments with an anodized outer surface of tungsten oxide; and drawing the wire filaments through a die to reduce the cross section of the wire filaments to a second diameter less than the first diameter.
[0108] Aspect 16 is the method of Aspect 15, further comprising the step of stranding a plurality of the wire filaments to form a wire cable.
[0109] Aspect 17 is the method of Aspect 15 or Aspect 16, wherein the anodizing step further comprises use of at least one of an applied anodizing voltage of from 10 to 90 volts (V); an anodizing electrolyte comprising sulfuric acid; an electrolyte concentration from 1 to 10 wt.%, based on a total weight of the electrolytic solution; and a dwell time of the wire fdaments in an anodizing bath of from 0.5 to 10 seconds.
[0110] Aspect 18 is the method of any one of Aspects 15-17, wherein the drawing step achieves a diameter reduction of the wire filaments from the first diameter to the second diameter of at least 5 %.
[0111] Aspect 19 is the method of any one of Aspects 15-18, wherein the draw ing step achieves a diameter reduction of the wire filaments from the first diameter to the second diameter of at least 10 %.
[0112] Aspect 20 is the method of any one of Aspects 15-19, further comprising repeating the anodizing and drawing steps at least three times.
Claims
CLAIMSWhat is claimed is:
1. A wire cable, comprising:a pl urality of individual wire filaments stranded to form the cable, at least some of the wire filaments made of tungsten, the tungsten wire filaments each having a core and an anodized outer surface of tungsten oxide.
2. The wire cable of claim 1, wherein the w ire filaments have a diameter of less than 1.5 mm.
3. The wire cable of claim 1, wherein the wire filaments have a diameter of less than 1.0 mm.
4. The wire cable of claim 1, wherein the wire filaments have a diameter of less than 0.5 mm.
5. The w ire cable of any one of claims 1-4, w herein the core of each of the tungsten wire filaments is made of tungsten having a purity of at least 99.0 wl.%.
6. The wire cable of any one of claims 1 -5, wherein the core of each of the tungsten wire filaments is made of tungsten having a purity of at least 99.0 wt.%.
7. The wire cable of any one of claims 1-6. wherein the anodized outer surface of tungsten oxide has a thickness of at least 0.25 microns.
8. The wire cable of any one of claims 1-7, wherein the anodized outer surface of tungsten oxide has a thickness of from 0.25 microns to 1.5 microns.
9. The wire cable of any one of claims 1-8, wiierein each of the tungsten wire filaments has a breaking strength of at least 4500 MPa, as determined by ASTM F288.
10. The wire cable of any one of claims 1-9. comprising a rotary beam fatigue life exceeding that of a corresponding cable formed from non-anodized wire filaments.
11. The wire cable of any one of claims 1-10, wherein the rotary beam fatigue life is at least 250% greater than that of a corresponding cable formed from non-anodized wire filaments.
12. The wire cable of any one of claims 1-11, comprising a rotary beam fatigue strength exceeding 12,000 cycles at 12.8% strain.
13. The wire cable of any one of claims 1-12, wherein the cable comprises at least 100 of the wire filaments.
14. The wire cable of any one of claims 1-13, wherein the wire filaments each have a round cross-section.
15. A method of forming anodized tungsten wire filaments, comprising:anodizing the surface of wire filaments each made of tungsten and having a round cross-section with a first diameter to form the wire filaments with an anodized outer surface of tungsten oxide; anddrawing the wire filaments through a die to reduce the cross section of the wire filaments to a second diameter less than the first diameter.
16. The method of claim 15, further comprising the step of stranding a plurality of the wire filaments to form a wire cable.
17. The method of claim 15 or claim 16, wherein the anodizing step further comprises use of at least one of:an applied anodizing voltage of from 10 to 90 volts (V);an anodizing electrolyte comprising sulfuric acid;an electrolyte concentration from 1 to 10 wt.%, based on a total weight of the electrolytic solution; anda dwell time of the wire filaments in an anodizing bath of from 0.5 to 10 seconds.
18. The method of any one of claims 15-17, wherein the drawing step achieves a diameter reduction of the wire filaments from the first diameter to the second diameter of at least 5 %.
19. The method of any one of claims 15-18, wherein the drawing step achieves a diameter reduction of the wire filaments from the first diameter to the second diameter of at least 10 %.
20. The method of any one of claims 15-19, further comprising repeating the anodizing and drawing steps at least three times.