Thin-film transistor with metal-alloy gate-electrode for increased channel mobility
By employing a metal-alloy gate-electrode with optimized surface roughness and correlation length, the mobility of charge-carriers in thin-film transistors is enhanced, improving display performance in OLED and LCD panels.
Patent Information
- Application Number
- PCT/US2026/027162
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing thin-film transistors face challenges in achieving desired transistor conduction characteristics due to difficulties in reducing surface roughness and correlation length of gate-electrodes, which affect charge-carrier mobility.
Utilizing a metal-alloy gate-electrode with a specific composition, such as Ti and Al, to minimize the product of surface roughness and correlation length, thereby improving field-effect mobility of charge-carriers.
The solution results in increased charge-carrier mobility and reduced ON resistance, leading to higher refresh rates and lower switching delays in displays, particularly in OLED and LCD panels.
Smart Images

Figure US2026027162_12112026_PF_FP_ABST
Abstract
Description
[0001] THIN-FILM TRANSISTOR WITH METAL-ALLOY GATE-ELECTRODE FOR INCREASED CHANNEL MOBILITY BACKGROUND
[0002] Technical Field
[0003] The present disclosure relates to thin-film transistors.
[0004] Description of the Related Art
[0005] Thin-film transistors (TFTs) are typically formed on non-conducting substrates. Thin-film transistors may be formed using processes that are different than traditional CMOS processes. Because thin-film transistors are not bound by some process constraints of traditional CMOS transistors, thin-film transistors can be utilized in various applications in which it may be difficult to utilize traditional CMOS transistors. These applications can include OLED displays and other types of displays. In spite of the various advantages of thin-film transistors, it can still be difficult to achieve desired transistor conduction characteristics within-film transistors.
[0006] BRIEF SUMMARY
[0007] Embodiments of the present disclosure provide thin-film transistors with high carrier mobility. This is accomplished, at least in part, by utilizing metal-alloy gate-electrodes with selected compositions. In some embodiments, the composition of gate-electrode is selected to reduce the product of the height correlation length L and the root mean square (RMS) surface roughness Rq of the gate-electrode. A reduction in the product L*Rq results in improved fieldeffect mobility of charge-carriers.
[0008] In some embodiments, the gate metal is an alloy of Ti and Al. In some embodiments, the alloy of Ti and Al includes an atomic percentage of Al between 45% and 55%. In some embodiments, the alloy of Ti and Al includes an atomic percentage of Al of 50%.
[0009] In some embodiments, a device includes a non-conducting substrate and a thin-film transistor on the substrate. The thin-film transistor includes a gate-electrode including a metalalloy, a layer of semiconductor material, and a gate dielectric between the gate-electrode and the layer of semiconductor material. A product of correlation length L and surface roughness Rq of the gate-electrode is less than 10 nm2.
[0010] In one embodiment, a device includes a non-conducting substrate and a thin-film transistor on the substrate. The thin-film transistor includes a gate-electrode including a metalalloy of Al and Ti, a layer of semiconductor material including a channel region, and a gate dielectric between the gate-electrode and the channel.In one embodiment, a method includes forming, over non-conductive substrate, a gateelectrode of a thin-film transistor including a metal-alloy. The method includes forming a gate dielectric of the thin-film transistor and forming a layer of semiconductor material including a channel region of the thin-film transistor. The gate insulator is between the channel region and the gate-electrode. A product of correlation length and surface roughness Rq of the gateelectrode is less than 10 nm2.
[0011] In one embodiment, a method includes forming, over non-conductive substrate, a gateelectrode including a metal-alloy of Al and Ti and forming a gate dielectric of the thin-film transistor. The method includes forming a layer of semiconductor material including a channel region of the thin-film transistor, wherein the gate insulator is between the channel region and the gate-electrode.
[0012] BRIEF DESCRIPTION OF THE SEVERAL VIEWS OF THE DRAWINGS
[0013] The detailed description is described with reference to the accompanying figures. The sizes and relative positions of elements in the figures are not necessarily drawn to scale. For example, the shapes of various elements and angles are not drawn to scale and some of these elements are enlarged and positioned to improve figure legibility. As is understood by one of skill in the art, the shape of a particular element may be modified (e.g., rounded, thinned, elongated, etc.) to suit a particular application.
[0014] Figure 1 A is a cross-sectional view of a thin-film transistor, in accordance with some embodiments.
[0015] Figure IB is a top view of the thin-film transistor of Figure 1 A, in accordance with some embodiments.
[0016] Figures 2A and 2B are graphs illustrating principles of charge-carrier scattering, in accordance with some embodiments.
[0017] Figures 3 A is a graph illustrating carrier mobility for various metal-alloys of a gateelectrode, in accordance with some embodiments.
[0018] Figures 3B is a graph illustrating the square of the product of surface roughness and correlation length various metal-alloys of a gate-electrode, in accordance with some embodiments.
[0019] Figures 4 is a graph illustrating resistivity for various metal-alloys of a gate-electrode, in accordance with some embodiments.
[0020] Figure 5 is a graph illustrating switching refresh rates displays of various resolution and the composition thin-film transistors utilized in the displays, in accordance with some embodiments.Figures 6A and 6B are graphs illustrating features of gate-electrodes of polycrystalline Ti, in accordance with some embodiments.
[0021] Figures 7A and 7B are graphs illustrating features of gate-electrodes of polycrystalline Al, in accordance with some embodiments.
[0022] Figures 8A and 8B are graphs illustrating features of gate-electrodes of amorphous alloy of Ti and Al, in accordance with some embodiments.
[0023] Figures 9A-9I are cross-sectional views and top views of an electronic device at various stages of formation of a thin-film transistor, in accordance with some embodiments.
[0024] Figure 10 is a flow-diagram of a method for forming a thin-film transistor, according to one embodiment.
[0025] Figure 11 is a flow-diagram of a method for forming a thin-film transistor, according to one embodiment.
[0026] DETAILED DESCRIPTION
[0027] It will be appreciated that, although specific embodiments of the present disclosure are described for purposes of illustration, various modifications may be made without departing from the spirit and scope of the present disclosure.
[0028] In this description, certain specific details are set forth in order to provide a thorough understanding of various aspects of the disclosed subject matter. However, the disclosed subject matter may be practiced without these specific details. In some instances, well-known structures and methods of semiconductor processing comprising embodiments of the subject matter disclosed herein have not been described in detail to avoid obscuring the descriptions of other aspects of the present disclosure.
[0029] Reference throughout the specification to “one embodiment” or “an embodiment” means that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment. Thus, the appearance of the phrases “in one embodiment” or “in an embodiment” in various places throughout the specification are not necessarily all referring to the same aspect. Furthermore, the particular features, structures, or characteristics may be combined in any suitable manner in one or more aspects of the present disclosure.
[0030] The present disclosure is directed to various implementations of a transistor that incorporates amorphous metal thin-films. Amorphous metal thin-films, used in conjunction with an insulating layer perform transistor functions without the complexity of standard, silicon-based transistors. Such amorphous metal transistors can be formed on any number of support substrates, giving flexibility to designers with regard to the types of materials and products thatcan incorporate transistors, i.e., active circuitry. These amorphous-metal transistors can be formed on flexible substrate as they can bend and change shapes without damage to the circuitry. These flexible substrates may be polymers, glass or other materials.
[0031] Many aspects of our lives are benefited by utilizing ever smaller electronic devices.
[0032] These include televisions, mobile electronic devices, like cellular phones, smart phones, tablet computers, and wearable electronics, like smart watches and pedometers. The transistors built on semiconductor substrates are limited by the materials used to form these circuits, i.e., silicon or other semiconductor wafers. With flexible transistors, the potential uses of electronic devices can be further expanded and improved, such as lighter and faster displays, wearable displays, mobile or easily movable displays, integrated into internet-of-things applications, or be integrated into medical devices.
[0033] These transistor structures can be used to form high-performance analog devices or digital devices as the end application dictates.
[0034] Figure 1 A is a cross-sectional view of a thin-film electronic device 100 and an intermediate stage of processing, according to one embodiment. The thin-film electronic device includes a thin-film transistor 101 on a substrate 102. As will be set forth in more detail below, the composition of the thin-film transistor 101 helps to ensure high carrier mobility with a channel region of the transistor 101.
[0035] The thin-film electronic device 100 includes a substrate 102. The substrate 102 corresponds to a support substrate on which a thin-film transistor will be formed. The thin-film transistor may include many materials and structures that are nontraditional with respect to traditional complimentary metal-oxide-semiconductor (CMOS) transistors. Accordingly, the substrate 102 may include nontraditional materials and characteristics with respect to CMOS transistors. For example, traditional CMOS transistors typically performed on a monocrystalline semiconductor substrate. However, the substrate 102 may include materials other than monocrystalline semiconductors, though monocrystalline semiconductors can be used in some embodiments. The ability to use materials other than monocrystalline semiconductors can greatly simplify the manufacturing process and reduce the manufacturing cost.
[0036] The substrate 102 can include a substantially nonconductive material. The substrate can be glass, a polymer, plastic, or other materials. In some embodiments, the substrate is glass, a polymer, plastic, or other material. In other embodiments, the substrate is a rubber. As used herein, “rubber” includes polymers of isoprene as well as forms of polyisoprene. In some such embodiments, the substrate is a plastic. Any suitable plastic may be used. In some embodiments, the plastic is a polyimide, an arylamide, acrylamide, polybenzimidazole (PBI), polyetherimide, polyetherketoneketone (PEKK), polyether ether ketone (PEEK), polyamide,polyimide, polyamide-imides, polystyrene (PS), polyphenylene oxide (PPO), polyphthalamide (PPA), polyvinyl alcohol (PVA), acrylonitrile butadiene styrene (ABS), polycarbonate (PC), thermoset, PBI-PEEK, urea, epoxies, polyurethanes, or any combination thereof. In some embodiments, the plastic is a polyethylene. In particular embodiments, the plastic is a high density polyethylene.
[0037] In further embodiments, the flexible substrate can be deformed (e.g., bowed, rolled, etc.) to form a curve having a central angle of at least about 5 degrees. In some embodiments, the flexible substrate can be deformed (e.g., bowed, rolled, etc.) to form a curve having a central angle of at least about 10 degrees. Unless otherwise specified, the central angle is measured for a curve in relation to an apex of the curve.
[0038] The materials of the support substrate can be selected by the manufacturer based on the end application of the transistor structure and the ultimate device being manufactured. For example, if the transistor structure is incorporated with an array of transistor structures, the array could be implemented within a liquid crystal display. Other end applications include wearable electronics. The support substrate can be transparent or non-transparent, such as those that can be used in some reflective displays.
[0039] Manufacturing on non-conducting flexible support substrates can reduce manufacturing costs significantly. Such substrates can enable roll-to-roll manufacturing of transistors. Such manufacturing changes can redefine the electronic supply chain.
[0040] The thin-film transistor 101 includes a gate-electrode 104. In some embodiments, the gate-electrode 104 includes an amorphous metal-alloy. The composition of the gate-electrode is selected to help ensure high carrier mobility with the channel region, as will be set forth in more detail below. Further details regarding the composition of the gate-electrode and its effect on the function of the thin-film transistor 101 will be provided after discussing the other components of the thin-film transistor.
[0041] The thin-film transistor 101 includes a gate insulator 106 on the top surface of the gateelectrode 104 and on exposed portions of the substrate 102. The gate insulator 106 has a material and thickness selected to enable the gate insulator 106 to electrically insulate the gateelectrode 104 from the semiconductor channel region, described further below.
[0042] The gate insulator 106 can have a thickness between 5 nm and 25 nm, though other thicknesses can be utilized without departing from the scope of the present disclosure. The gate insulator 106 can include AI2O3, hafnium oxide, silicon nitride, silicon oxide, or other suitable materials. The thickness and deposition process utilized for the gate insulator 106 can be selected based on the material and thickness of the gate-electrode 104. The gate insulator 106 can be deposited by a PVD process, a CVD process, such as PECVD, or an ALD process.The thin-film transistor 101 a source electrode 110 and a drain electrode 112. The source electrode 110 and the drain electrode 112 overlie the substrate 102, the gate dielectric layer 106, and the gate-electrode 104. The gate dielectric layer 106 is positioned between the source / drain electrodes 110 / 112 and the substrate 102. The gate dielectric layer 106 is positioned between the source / drain electrodes 110 / 112 and the gate-electrode 104. The source electrode 110 and the drain electrode 112 are separated from each other by a gap over the top surface of the gateelectrode 104.
[0043] In some embodiments, the source electrode 110 the drain electrode 112 are formed of a layer of conductive material. After deposition of the layer of conductive material on the gate dielectric layer 106, the layer of conductive material is patterned to form the source / drain electrodes 110 / 112 as shown. The source / drain electrodes 110 / 112 can have a thickness between 50 nm and 100 nm. The source / drain electrodes 110 / 112 can include a metal. The metal can include one or more of Cu, Al, Ti, W, or other suitable metals.
[0044] In some embodiments, the thin-film transistor 101 includes a layer of semiconductor material 108 overlying the source / drain electrodes 110 / 112 and the gate dielectric layer 106. The layer semiconductor material 108 is positioned directly on the gate dielectric layer 106 over the top surface of the gate-electrode 104 between the source / drain electrodes 110 / 112.
[0045] The semiconductor material 108 can include one or more of IGZO (compositions of In, Ga, Zn, and O), low temperature polycrystalline silicon (LTPS), amorphous silicon, or other suitable semiconducting materials. The layer of semiconductor material 108 can include IGZO between 30 nm and 50 nm in thickness, formed with a PVD process, though other thicknesses can be utilized without departing from the scope of the present disclosure. In some embodiments, IGZO may correspond to amorphous In-Ga-Zn-0 compositions, also referred to as a-IGZO. In other embodiments, IGZO may include crystalline materials, referred to as c-IGZO or c-axis aligned IGZO. Crystalline IGZO materials may include, for example,
[0046] InGaZnO4, InGaO3(ZnO)s, or In2Ga2ZnO?. The portion of the layer of semiconductor material 108 over gate-electrode 104 corresponds to the channel region of the thin-film transistor 101.
[0047] In some embodiments, the thin-film transistor 101 includes a passivation layer 114 on the semiconductor material 108 and exposed portions of the source electrode 110 and drain electrode 112. The passivation layer 114 can include a dielectric material with a thickness between 50 nm and 500 nm though other thicknesses can be utilized without departing from the scope of the present disclosure. The passivation layer 114 can include one or more of silicon dioxide, silicon nitride, or other dielectric materials.
[0048] The thin-film transistor 101 includes the gate-electrode 104, the gate insulator 106, the source electrode 110, the drain electrode 112, and the semiconductor material 108. Thesemiconductor material 108 includes a channel region 109. The channel region 109 corresponds to the portion of the semiconductor material 108 between the source and drain electrodes 110, 112 and the above the gate-electrode 104. The gate insulator 106 separates the channel region 109 of the semiconductor material 108 from the gate-electrode 104.
[0049] The thin-film transistor 101 can operate by selectively applying voltages to the gateelectrode 104, the source electrode 110, and the drain electrode 112. In one example, thin-film transistor 101 is turned on by applying a gate to source voltage and a drain to source voltage of about 4 V. The thin-film transistor 101 can be turned off by applying a gate to source voltage of 0 V. Other voltages can be utilized without departing from the scope of the present disclosure.
[0050] Figure IB is a top view of the thin-film transistor 101 of Figure IB. The gate insulator 106 and the passivation layer 114 are not shown. Figure IB illustrates that the semiconductor material 108 is positioned over portions of the gate-electrode 104, the source electrode 110, and the drain electrode 112. The various components of the thin-film transistor 101 can have other shapes and arrangements without departing from the scope of the present disclosure.
[0051] Figures 2A and 2B are enlarged cross-sectional views of portions of a gate-electrode, a gate insulator, and a semiconductor layer (channel) of a thin-film transistor, in accordance with some embodiments. The views of Figures 2A and 2B are helpful in illustrating scattering effects that can affect the mobility of charge-carriers (e.g., electrons) in the channel of the thin-film transistor.
[0052] Figure 2A illustrates a scattering mechanism called surface roughness scattering, in accordance with some embodiments. In the view of Figure 2A, the interface between the gate insulator and the semiconductor layer is quite rough. More particularly, the top surface of the gate insulator is quite rough, resulting in peaks and valleys at the interface. This scattering process is local. By local, the spatial position of charge-carriers (e.g., electrons) in the semiconductor layer and the scattering center are coincident. Herein, a charge carrier within the semiconductor layer is scattered due to fluctuations in the intensity of the transverse electric field. Fluctuations are caused by the surface roughness of the interface between the gate insulator and semiconductor.
[0053] Figure 2B illustrates a scattering mechanism called remote surface roughness scattering, in accordance with some embodiments. As can be seen in Figure 2B, the surface of the gateelectrode is quite rough. This scattering process is nonlocal. By nonlocal, the spatial position of charge-carriers (e.g., electrons) in the semiconductor and the scattering center are not coincident, being separated by a distance. Nonlocal scattering is also referred to as 'remote’ for the same reason. Essentially, a charge carrier within the semiconductor is scattered due to fluctuations in the intensity of the transverse electric field from positive charges on the gate-electrode’s surface.Fluctuations are caused by height variation, quantified by the surface roughness of the gateelectrode. As positive charges accumulate along the gate-electrode’s surface, the electric field “seen” by an electron in the channel will vary. This can have the effect of causing upward or downward tilt in the electrons path of travel as the electron travels from left to right. These path changes correspond to a type of charge-carrier scattering. This scattering effectively reduces the mobility of the electrons in the channel, and the field-effect mobility of the thin-film transistor.
[0054] Returning now to the composition of the gate-electrode 104 of Figure 1 A, the composition of the gate-electrode 104 can have a strong impact on the scattering mechanisms of the charge-carriers (electrons) in the channel 111 of the thin-film transistor 101, in accordance with some embodiments. In some embodiments, a metal-alloy is utilized as the gate-electrode with chemical composition that minimizes surface roughness. Use of metal-alloys facilitates composition-based improvement of surface roughness. Lower surface roughness of the gateelectrode results in lower charge-carrier scattering rates, thereby increasing charge carrier mobility.
[0055] In some embodiments, the metal-alloy of the gate-electrode 104 is selected so that each constituent of the alloy has a similar work function to within 0.1 - 0.3 eV. This ensures a very small change in work function as the chemical composition of the metal-alloy is varied. The work function of the gate-electrode 104 is a parameter influencing the threshold voltage in a thin-film transistor. Generally, a higher work function corresponds to a higher threshold voltage and a lower ON resistance of the thin-film transistor. In embodiments in which the electronic device 100 is a display (such as a high definition television) made up of a large number of thin-film transistors 101, a lower ON resistance results in a higher refresh rate of the display.
[0056] In some embodiments, the metal-alloy may consist of any number of constituents (e.g., binary, ternary, quaternary, etc.). In some embodiments, the metal-alloy of the gate-electrode 104 is a binary metal-alloy of Ti and Al. The alloy can be deposited by sputtering a fixed composition target; or co-sputtering of several targets equal to the number of constituents. In some embodiments, the metal-alloy of the gate-electrode 104 is Ti Al with an atomic percentage of Al between 40% and 60%. In some embodiments, the concentration of Al is between 45% and 55%. In some embodiments, the concentration of Al is 50%. In other words, in some embodiments, the gate metal 104 is TiAl, rather than TiA13, or another composition of Ti Al. In some embodiments, the gate metal 104 is an amorphous alloy of Ti Al.
[0057] In some embodiments, the mobility of charge-carriers in the channel Ill is inversely proportional to the square of the product of surface roughness Rq and height correlation length L of the gate-electrode 104. Accordingly, a high mobility of charge-carriers in the channel can be promoted by forming the gate-electrode 104 with a composition that results in a very low valueof the product of the height correlation length L and the surface roughness Rq. In some embodiments, the product of L and Rq is less than 10 nm2(or less than 100 nm4), though other values can be utilized without departing from the scope of the present disclosure.
[0058] In some embodiments, the height correlation length L is determined by
[0059] letting the surface height be given by h(x, y) over a lateral area. For a line scan along x, denote t he height as h(x). The mean height is
[0060] _ 1 fD
[0061] h = — I h(x) dx
[0062]
[0063] D Jo
[0064] for a total length D. The height fluctuation is
[0065] <5 / i(x) = h(x) — h.
[0066] The Height-Height Autocorrelation Function is then computed. The autocorrelation function C(r) is defined as:
[0067] 1 rD-r
[0068] C(r) = (<5 / i(x) 8h(x + r)) = — - I <5 / i(x) 8h(x + r) dx,
[0069]
[0070] D — T Jo
[0071] where r is the lateral distance and (•) denotes averaging over positions.
[0072] A normalized autocorrelation function can also be used, in some embodiments:
[0073] C fr')
[0074] = 7^.C(0) = = Rq2.
[0075]
[0076] where Rq is the root-mean-square (rms) roughness.
[0077] The height correlation length (also termed simply correlation length) L is the characteristic decay length of the autocorrelation function. For many surfaces, C(r) decays approximately exponentially:
[0078] C(r) = Rq2exp (-y),
[0079] or for some self-affine surfaces, as a Gaussian:
[0080] C(r) = Rq2exp [-(y)2].
[0081] Lt
[0082] To extract L compute C(r) / C(0) versus r and fit the decay to either an exponential or Gaussian model. L is defined as the distance where: C(r) / C(0) = 1 / e for an exponential decay, or C(r) / C(0) = e-1for a Gaussian decay (the characteristic width. Mathematically:
[0083] Exponential: C(L) = C(0) / e => L
[0084] Gaussian: C(L) = C (O') / e => L
[0085] The choice of functional form depends on the surface morphology and empirical data. Other methods and procedures can be utilized to determine the correlation length L without departing from the scope of the present disclosure.Figure 3 A is a graph of measured field-effect mobility in the channel versus the composition of a gate-electrode, in accordance with some embodiments. In Figure 3 A the x-axis corresponds to the atomic percentage of Al in an alloy of Al and Ti. In some embodiments, a peak in the measure mobility occurs with a concentration of Al between 40% and 60%. In some embodiments, the peak in the measured mobility occurs with a concentration of Al between 45% and 55%. In some embodiments, a peak in the measure mobility occurs with a concentration of Al of about 50%.
[0086] Figure 3B illustrates the product of the correlation length L in the surface roughness R for various concentrations of Al in a metal-alloy of Ti Al of a gate-electrode, in accordance with some embodiments. As set forth previously, the mobility of charge-carriers in the channel is inversely proportional to the square of R*L. As can be seen in Figure 3B, the low point of C*L occurs between 40% and 70%. In Figure 3B the gate-electrode has a thickness of 50 nm.
[0087] In some embodiments, the composition of the gate-electrode 104 is selected to result in (L*R)A2 having a value less than 1E2, though other values can be utilized without departing from the scope of the present disclosure. Figure 4 is a graph illustrating the ON resistance R ON of a channel of the thin-film transistor versus the concentration of Al in a metal-alloy of Ti Al of a gate-electrode, in accordance with some embodiments. The ON resistance corresponds to the resistance in the channel when the transistor is turned on. As can be seen in Figure 4, the on resistance is lowest when the concentration of Al is between 40% and 60%. This low resistance corresponds to a very small switching delay of all of the switching transistors present in an LCD or OLED display panel. Accordingly, the smaller the resistance, the lower the switching delay. The lower the switching delay, the higher the frame rate of the panel.
[0088] Figure 5 is a graph illustrating the refresh rate or frame rate of displays of varying resolution versus concentration of Al in the metal-alloy of the gate-electrode, in accordance with some embodiments. The graph is shown for a display having 8k resolution, a display having 4k resolution, and a full HD display having 1080p resolution. For each of the types of displays, the highest refresh rate occurs when the concentration of Al is between 40% and 60%.
[0089] Figures 6A and 6B are graphs illustrating features of gate-electrodes of polycrystalline Ti, in accordance with some embodiments. In Figures 6A and 6B, the concentration of Al and the gate-electrode is 0.
[0090] Figures 7A and 7B are graphs illustrating features of gate-electrodes of polycrystalline Al, in accordance with some embodiments. In Figures 7A and 7B, the concentration of Al in the gate-electrode is 100%.Figures 8A and 8B are graphs illustrating features of gate-electrodes of amorphous alloy of Ti and Al, in accordance with some embodiments. In Figures 8A and 8B, the concentration of Al is 50%.
[0091] Figures 9A-9I are cross-sectional views and top views of an electronic device at various stages of formation of a thin-film transistor, in accordance with some embodiments. In Figure 9 A, a layer of conductive material 103 has been deposited on a nonconducting substrate 102. The layer of conductive material 103 corresponds to the material from which the gate-electrode 104 will be patterned. Accordingly, the layer of conductive material 103 can have compositions and thicknesses described previously for the gate-electrode 104. In one particular example, the layer of conductive material 103 is an amorphous metal-alloy of Ti and Al.
[0092] In some embodiments, the layer of conductive material 103 is deposited with the sputtering process. The sputtering process can include a single target of Ti and Al, or from multiple targets of Al and Ti. Other materials and sputtering processes can be utilized without departing from the scope of the present disclosure. In some embodiments, the layer of conductive material 103 has a surface roughness less than 0.5 nm.
[0093] In Figure 9B, the layer of conductive material 103 has been patterned to form a gateelectrode 104. The gate-electrode 104 can be formed from the layer of conductive material 103 by a photolithography process. The photolithography process can include patterning a mask on the layer of conductive material 103 and etching the layer of conductive material 103 in the presence of the mask. The etching process can include a wet etch or dry etch. The resulting gate-electrode 104 has a shape corresponding to the shape of the mask.
[0094] The gate-electrode 104 has a top surface 105. The roughness of the top surface 105 can affect the performance of the thin-film transistor in which the gate-electrode 104 will be part, as set forth previously. Furthermore, rougher top and bottom surfaces of a semiconductor layer can result in trap-states that can capture charge-carriers, such as electrons, reducing mobility. While trap-states can exist anywhere within a semiconductor material, trap-states are much more likely to occur at rough surfaces of a semiconductor material. The more charge-carriers that are trapped in trap-states at the surfaces of the semiconductor layer, the lower the conductivity of the semiconductor layer. Low conductivity in the semiconductor layer may correspond to poor performance of the thin-film transistor.
[0095] Accordingly, as the roughness of the surfaces of the semiconductor layer is influenced by the roughness of the gate-electrode 104, embodiments of the present disclosure provide a gateelectrode 104 having a top surface 105 with low roughness. In one embodiment, the top surface 105 of the gate-electrode 104 has a roughness less than 2 nm. Based on the material of the deposition process of the layer of conductive material 103, the top surface 105 of the gate-electrode 104 may have a roughness less than 1 nm. For example, a gate-electrode 104 of an amorphous alloy of TiAl may have a roughness less than 0.5 nm.
[0096] Unless stated otherwise, as used herein, roughness values are given as root mean square (RMS) roughness values Rq, though other types of roughness values can be used. For example, roughness can be given as the arithmetical mean deviation of an assessed surface profile, as a maximum valley depth of the assessed surface profile, the maximum peak height of the assessed surface profile, the skewness of the assessed surface profile, the kurtosis of the assessed surface profile, or the average distance between the highest peak and lowest valley in each sampling length. Those of skill in the art will recognize, in light of the present disclosure, that while RMS roughness is used herein, various other surface roughness assessments can be utilized without departing from the scope of the present disclosure, such as Sq, a two-dimensional surface roughness measure. In RMS roughness, a mean line corresponds to the mean height of the top surface 105 when all peaks and valleys are taken into account along a sampling length.
[0097] Accordingly, the mean line is at a height between the highest peak and the lowest valley of the top surface 105 of the gate-electrode 104. The RMS roughness Rq is calculated by taking a number of height measurement samples relative to the mean line. In one embodiment, surface height is measured using atomic force microscopy (AFM). Surface heights greater than the mean line have a positive value. Surface heights that are lower than the mean line ML have a negative value. Each of the individual surface height measurements is squared. The squares of all the measurements are summed and divided by the number of samples. The square root of this value is the RMS roughness Rq and has units of distance. Accordingly, an RMS roughness of 2 nm means that the line Rq is 2 nm above the mean line ML. A larger RMS roughness value indicates a rougher surface. Height may be measured along a line or over an area without departing from the scope of the present disclosure. Unless specified otherwise, roughness values provided herein correspond to RMS roughness values.
[0098] With reference again to Figure 9B, after patterning the conductive material 103 to form the gate-electrode 104, one or more planarization processes may be performed on the gateelectrode 104. For example, a CMP process may be performed on the gate-electrode 104 to further reduce the roughness of the top surface 105 of the gate-electrode 104.
[0099] The gate-electrode 104 can be formed in ways other than those described above. For example, the gate-electrode 104 can be formed by depositing the gate-electrode metal in trench or gap formed in a dielectric layer formed on the substrate 102. This can be followed by a planarization process, such as a CMP process to remove excess metal and to reduce the roughness of the top surface 105 of the gate-electrode 104.In Figure 9C, the gate insulator 106 is formed on the top surface 105 of the gate-electrode 104 and on exposed portions of the substrate 102. The gate insulator 106 has a material and thickness described previously. The gate insulator 106 can be deposited by a PVD process, a CVD process, such as PECVD, or an ALD process.
[0100] In Figure 9D, a layer of conductive material 111 is deposited on the gate insulator 106. The layer of conductive material 111 can have a thickness between 50 nm and 100 nm though other thicknesses can be utilized without departing from the scope of the present disclosure. The layer of conductive material 111 can include a metal. The metal can include one or more of copper, Al, Ti, tungsten, or other suitable metals. The layer of conductive material 111 can be deposited by PVD, chemical vapor deposition (CVD), ALD, or other suitable deposition processes.
[0101] In Figure 9E, an opening 126 has been formed in the layer of conductive material 111. The opening 126 exposes portion of the top surface of the gate insulator 106. The opening 126 also defines a source electrode 110 and a drain electrode 112 from the layer of conductive material 111. The opening 126 can be formed by a photolithography process including forming a mask on the layer of conductive material 111 and etching exposed portions of the layer of conductive material 111
[0102] In Figure 9F, a layer of semiconductor material 108 has been deposited on the source electrode 110, the drain electrode 112, and the exposed portion of the gate insulator 106. The semiconductor material 108 can have a thickness between 15 nm and 55 nm. The semiconductor material 108 can be formed with a deposition process including PVD, plasma enhanced CVD (PECVD), and PECVD with Excimer laser annealing (ELA). The layer of semiconductor material 108 can have materials and thicknesses described previously.
[0103] In Figure 9G, the semiconductor material 108 has been etched so that the semiconductor material 108 terminates on the source electrode 110 and the drain electrode 112. The semiconductor material 108 can be patterned and etched with photolithographic masking process followed by a wet or a dry etch.
[0104] In Figure 9H, a passivation layer 114 has been formed on the semiconductor material 108 and exposed portions of the source electrode 110 and drain electrode 112. The passivation layer 114 can include a dielectric material with a thickness between 50 nm and 500 nm though other thicknesses can be utilized without departing from the scope of the present disclosure.. The passivation layer 114 can include one or more of silicon dioxide, silicon nitride, or other dielectric materials.
[0105] In Figure 9H, the formation of a thin-film transistor 101 is complete. The thin-film transistor 101 includes the gate-electrode 104, the gate insulator 106, the source electrode 110,the drain electrode 112, and the semiconductor material 108. The semiconductor material 108 includes a channel region 109. The channel region 109 corresponds to the portion of the semiconductor material 108 between the source and drain electrodes 110, 112 and the above the gate-electrode 104. The gate insulator 106 separates the channel region 109 of the semiconductor material 108 from the gate-electrode 104.
[0106] The thin-film transistor 101 can operate by selectively applying voltages to the gateelectrode 104, the source electrode 110, and the drain electrode 112. In one example, thin-film transistor 101 is turned on by applying a gate to source voltage and a drain to source voltage of about 4V. The thin-film transistor 101 can be turned off by applying a gate to source voltage of 0 V. Other voltages can be utilized without departing from the scope of the present disclosure.
[0107] Figure 91 is a top view of the thin-film transistor 101 of Figure 9H. The gate insulator 106 and the passivation layer 114 are not shown. Figure 91 illustrates that the semiconductor material 108 is positioned over portions of the gate-electrode 104, the source electrode 110, and the drain electrode 112. The various components of the thin-film transistor 101 can have other shapes and arrangements without departing from the scope of the present disclosure.
[0108] While the description of Figures 9A-9H has primarily described formation of a thin-film transistor 101 including a gate-electrode 104 having a top surface 105 with low roughness, principles of the present disclosure can extend to other structures formed in the thin-film electronic device 100. For example, the layer of conductive material 103 can be patterned to form various types of metal structures on the substrate 102 in addition to the gate-electrode 104. These other metal structures will also have top surfaces with the low roughness of the top surface 105. Accordingly, these other metal structures, and the structures formed over them, may also benefit from the low roughness top surface. The other metal structures can include metal lines, contacts, plugs, or types of metal structures that may be formed with the metal of the gateelectrode 104.
[0109] Figure 10 is a flow-diagram of a method 1000 for forming a thin-film transistor, in accordance with some embodiments. The method 1000 can utilize processes, materials, and components described in relation to Figures 1 A-9I. At 1002, the method 1000 includes forming, over non-conductive substrate, a gate-electrode including a metal-alloy. At 1004, the method 1000 includes forming a gate dielectric of the thin-film transistor. At 1006, the method 1000 includes forming a layer of semiconductor material including a channel region of the thin-film transistor, wherein the gate insulator is between the channel region and the gate-electrode, wherein a product of correlation length and surface roughness Rq of the gate-electrode is less than 10.Figure 11 is a flow-diagram of a method 1100 for forming a thin-film transistor, in accordance with some embodiments. The method 1100 can utilize processes, materials, and components described in relation to Figures 1 A-9I. At 1102, the method 1100 includes forming, over non-conductive substrate, a gate-electrode including a metal-alloy of Al and Ti. At 1104, the method 1100 includes forming a gate dielectric of the thin-film transistor. At 1106, the method 1100 includes forming a layer of semiconductor material including a channel region of the thin-film transistor, wherein the gate insulator is between the channel region and the gateelectrode.
[0110] In some embodiments, a device includes a non-conducting substrate and a thin-film transistor on the substrate. The thin-film transistor includes a gate-electrode including a metalalloy, a layer of semiconductor material, and a gate dielectric between the gate-electrode and the layer of semiconductor material. A product of correlation length L and surface roughness (Rq) of the gate-electrode is less than 10 nm2.
[0111] In one embodiment, Rq is less than 0.5 nm.
[0112] In one embodiment, the metal-alloy is an alloy of Ti and Al.
[0113] In one embodiment, an atomic percentage of Al in the metal-alloy is between 40% and 60%.
[0114] In one embodiment, the atomic percentage of Al in the metal-alloy is between and 45% and 55%.
[0115] In one embodiment, the atomic percentage of Al in the metal-alloy is 50%.
[0116] In one embodiment, the alloy is an amorphous material.
[0117] In one embodiment, the layer of semiconductor material includes a channel region, wherein the gate insulator is positioned between the channel region and the gate-electrode.
[0118] In one embodiment, the thin-film transistor includes a source electrode and a drain electrode in contact with the channel region.
[0119] In one embodiment, the layer of semiconductor material includes InGaZnO.
[0120] In one embodiment, a device includes a non-conducting substrate and a thin-film transistor on the substrate. The thin-film transistor includes a gate-electrode including a metalalloy of Al and Ti, a layer of semiconductor material including a channel region, and a gate dielectric between the gate-electrode and the channel.
[0121] In one embodiment, the metal-alloy include Ti Al.
[0122] In one embodiment, a concentration of Al in the metal-alloy is between 40% and 60%. In one embodiment, the concentration of Al in the metal-alloy is between 45% and 55%. In one embodiment, a concentration of Al in the metal-alloy is 50%.
[0123] In one embodiment, the gate dielectric includes AI2O3.In one embodiment, the gate dielectric includes Hf.
[0124] In one embodiment, the channel region has a thickness less than 50 nm though other thicknesses can be utilized without departing from the scope of the present disclosure.
[0125] In one embodiment, the semiconductor material includes low temperature polysilicon. In one embodiment, the semiconductor material includes amorphous silicon.
[0126] In one embodiment, the source and drain electrodes are positioned above the semiconductor material.
[0127] In one embodiment, the source and drain electrodes are positioned below the semiconductor material.
[0128] In one embodiment, the substrate includes glass.
[0129] In one embodiment, the substrate includes a polymer.
[0130] In one embodiment, a method includes forming, over non-conductive substrate, a gateelectrode of a thin-film transistor including a metal-alloy. The method includes forming a gate dielectric of the thin-film transistor and forming a layer of semiconductor material including a channel region of the thin-film transistor. The gate insulator is between the channel region and the gate-electrode. A product of correlation length L and surface roughness (Rq) of the gateelectrode is less than 10 nm2.
[0131] In one embodiment, the metal-alloy include Ti Al.
[0132] In one embodiment, an atomic percentage of Al in the metal-alloy is between 40% and 60%.
[0133] In one embodiment, the atomic percentage of Al in the metal-alloy is between 45% and 55%.
[0134] In one embodiment, the atomic percentage of Al in the metal-alloy is 50%.
[0135] In one embodiment, forming the gate-electrode includes performing a sputtering process. In one embodiment, the gate-electrode is below the channel region.
[0136] In one embodiment, the gate-electrode is above the channel region.
[0137] In one embodiment, a method includes forming, over non-conductive substrate, a gateelectrode including a metal-alloy of Al and Ti and forming a gate dielectric of the thin-film transistor. The method includes forming a layer of semiconductor material including a channel region of the thin-film transistor, wherein the gate insulator is between the channel region and the gate-electrode.
[0138] In one embodiment, a square of the product of surface roughness and correlation length of the gate-electrode is less than 10.
[0139] In one embodiment, an atomic percentage of Al in the metal-alloy is between 40% and 60%.In one embodiment, the atomic percentage of Al in the metal-alloy is between 45% and 55%.
[0140] In one embodiment, the atomic percentage of Al in the metal-alloy is 50%.
[0141] In one embodiment, forming the gate-electrode includes performing a sputtering process. In one embodiment, the gate-electrode is below the channel region.
[0142] In one embodiment, the gate-electrode is above the channel region.
[0143] These and other changes can be made to the embodiments in light of the above-detailed description. In general, in the following claims, the terms used should not be construed to limit the claims to the specific embodiments disclosed in the specification and the claims but should be construed to include all possible embodiments along with the full scope of equivalents to which such claims are entitled. Accordingly, the claims are not limited by the disclosure.
Claims
CLAIMS1. A device, comprising:a non-conducting substrate;a thin-film transistor on the substrate and including:a gate-electrode including a metal-alloy;a layer of semiconductor material;a gate dielectric between the gate-electrode and the layer of semiconductor material, wherein the product of correlation length L and surface roughness (Rq) of the gateelectrode is less than 10 nm2.
2. The device of claim 1, wherein Rq is less than .5 nm.
3. The device of claim 1, wherein the metal-alloy is an alloy of Ti and Al.
4. The device of claim 3, wherein an atomic percentage of Al in the metal-alloy is between 40% and 60%.
5. The device of claim 4, wherein the atomic percentage of Al in the metal-alloy is between and 45% and 55%.
6. The device of claim 5, wherein the atomic percentage of Al in the metal-alloy is 50%.
7. The device of claim 1, wherein the alloy is an amorphous material.
8. The device of claim 1, wherein the layer of semiconductor material includes a channel region, wherein the gate insulator is positioned between the channel region and the gateelectrode.
9. The device of claim 8, wherein the thin-film transistor includes a source electrode and a drain electrode in contact with the channel region.
10. The device of claim 1, wherein the layer of semiconductor material includes InGaZnO.
11. A device, comprising:a non-conducting substrate;a thin-film transistor on the substrate and including:a gate-electrode including a metal-alloy of Al and Ti;a layer of semiconductor material including a channel region;a gate dielectric between the gate-electrode and the channel.
12. The device of claim 11, wherein the metal-alloy include Ti Al.
13. The device of claim 12, wherein a concentration of Al in the metal-alloy is between 40% and 60%.
14. The device of claim 13, wherein the concentration of Al in the metal-alloy is between 45% and 55%.
15. The device of claim 14, wherein a concentration of Al in the metal-alloy is 50%.
16. The device of claim 11, wherein the gate dielectric includes AI2O3.
17. The device of claim 11, wherein the gate dielectric includes Hf.
18. The device of claim 17, wherein the channel region has a thickness less than 50 nm.
19. The device of claim 11, wherein the semiconductor material includes low temperature polysilicon.
20. The device of claim 11, wherein the semiconductor material includes amorphous silicon.
21. The device of claim 20, wherein the source and drain electrodes are positioned above the semiconductor material.
22. The device of claim 21, wherein the source and drain electrodes are positioned below the semiconductor material.
23. The device of claim 11, wherein the substrate includes glass.
24. The device of claim 11, wherein the substrate includes a polymer.
25. A method, comprising:forming, over non-conductive substrate, a gate-electrode including a metal-alloy; forming a gate dielectric of the thin-film transistor;forming a layer of semiconductor material including a channel region of the thin-film transistor, wherein the gate insulator is between the channel region and the gate-electrode, wherein the product of correlation length L and surface roughness (Rq) of the gate-electrode is less than 10 nm2.
26. The method of claim 25, wherein the metal-alloy include Ti Al.
27. The method of claim 26, wherein an atomic percentage of Al in the metal-alloy is between 40% and 60%.
28. The method of claim 27, wherein the atomic percentage of Al in the metal-alloy is between 45% and 55%.
29. The method of claim 26, wherein the atomic percentage of Al in the metal-alloy is 50%.
30. The method of claim 25, wherein forming the gate-electrode includes performing a sputtering process.
31. The method of claim 25, wherein gate-electrode is below the channel region.
32. The method of claim 25, wherein the gate-electrode is above the channel region.
33. A method, comprising:forming, over non-conductive substrate, a gate-electrode including a metal-alloy of Al and Ti;forming a gate dielectric of the thin-film transistor;forming a layer of semiconductor material including a channel region of the thin-film transistor, wherein the gate insulator is between the channel region and the gate-electrode.
34. The method of claim 33, wherein the product of correlation length L and surface roughness (Rq) of the gate-electrode is less than 10 nm2.
35. The method of claim 33, wherein an atomic percentage of Al in the metal-alloy is between 40% and 60%.
36. The method of claim 35, wherein the atomic percentage of Al in the metal-alloy is between 45% and 55%.
37. The method of claim 33, wherein the atomic percentage of Al in the metal-alloy is 50%.
38. The method of claim 33, wherein forming the gate-electrode includes performing a sputtering process.
39. The method of claim 33, wherein gate-electrode is below the channel region.