Resorbable 3d-printed composite osteosynthetic plates for rib fracture repair

Resorbable 3D printed osteosynthetic fixation devices using fumarate-based ABA triblock copolyester composites address the limitations of metal plates by offering mechanical support and bone integration, reducing invasiveness and complications in rib fracture repair.

WO2026236550A1PCT designated stage Publication Date: 2026-11-12DUKE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/027179
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Current surgical stabilization of rib fractures using metal plates is invasive and has limitations, while existing resorbable polymer plates are not as effective in providing mechanical support and are prone to failure, leading to high morbidity and mortality rates in rib fracture patients.

Method used

Development of a resorbable 3D printed osteosynthetic fixation devices made from fumarate-based ABA triblock copolyester and star polymer composites, which are tunable for mechanical properties and degradation profiles, allowing for minimally invasive insertion and improved bone integration.

Benefits of technology

The composite plates provide mechanical support comparable to titanium, reduce inflammation and infection risk, and enhance bone mineralization, promoting better surgical outcomes and patient recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026027179_12112026_PF_FP_ABST
    Figure US2026027179_12112026_PF_FP_ABST
Patent Text Reader

Abstract

In various embodiments, the present invention is directed to a resorbable poly(propylene fumarate)-based 3D printable resin and resorbable 3D printed osteosynthetic apparatus for rib fracture repair comprising a linear or star-shaped poly(propylene fumarate)-based copolymer comprising at either an ABA block copolymer having a first and second poly(propylene fumarate) A blocks and a poly(propylene succinate) B block, a star-shaped poly(propylene fumarate) copolymer, or both; a multi-functional thiol-based crosslinker; and a plurality of filler nanoparticles.
Need to check novelty before this filing date? Find Prior Art

Description

RESORBABLE 3D-PRINTED COMPOSITE OSTEOSYNTHETIC PLATES FOR RIB FRACTURE REPAIR CROSS REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of U. S. provisional patent application serial number 63 / 801,510 entitled “Resorbable 3D-Printed Composite Osteosynthetic Plates For Rib Fracture Repair,” filed May 7, 2025, and incorporated herein by reference in its entirety.STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH OR DEVELOPMENT SUPPORT

[0002] This invention was made with government support under grant number 1 K08AR079609-1 awarded by the National Institutes of Health (N I H). The government has certain rights in the invention.FIELD OF THE INVENTION

[0003] One or more embodiments of the present invention relates to a plate for repair of rib fractures. In certain embodiments, resorbable, ABA triblock copolyester plate for repair of rib fractures.BACKGROUND OF THE INVENTION

[0004] Ribs are one of the most common bones to be fractured, with over 350,000 people in the United States alone sustaining rib injuries. Rib fractures are observed in roughly 40% of blunt chest trauma cases and account for approximately 10-15% of all trauma admissions. Moreover, multiple rib fractures are a marker for severe chest wall injury and are associated with high morbidity and mortality rates, particularly in patients with high-risk features such as age, pulmonary comorbidities, and polytrauma. Studies have shown that prognosis is worse in rib fracture patients with increasing age, number of rib fractures, and presence of flail chest. A majority of patients with isolated rib fractures (>60%) continue to experience prolonged chest wall pain and prolonged disability 2 months after injury. Despite the high incidence of rib fractures, outcomes remain poor and treatment options have not made significant improvements over the years.

[0005] The current standard of care for rib fractures is typically minimal, focusing on pain management and non-invasive respiratory assistance. Currently only 5% of patients with rib fractures undergo surgery, but this percentage is increasing for multiple reasons, including more minimally invasive surgical techniques that reduce morbidity of the surgery and evidence that shows surgery can improve outcomes. Surgical stabilization with a metal plate has been shown to decrease mortality, as well as shorten length of ventilator d ependence and decrease hospital length of stay in mechanically ventilated patients. Surgical stabilization of rib fractures (SSRF) relies on a metallic plate to promote across the fracture line. This improves both healing rates and clinical outcomes.

[0006] Current surgical techniques include an extra-thoracic approach, which means the surgeons remain outside of the thoracic cavity and an intra-thoracic cavity approach which means surgeons stabilize the ribs from the inside. Surgical intervention is most often reserved for severe cases, such as flail chest or other severe chest wall deformities. Currently, only metal alloys are used for rib fracture plating. In cases of flail chest, surgical stabilization of rib fractures (SSRF) with titanium plates has been shown to decrease intensive care unit (ICU) length of stay and rates of long-term complications such as pneumonia, respiratory infection, and chronic pain compared to non-operative management. Recent evidence suggests that SSRF also improves patient outcomes (e.g., pain control, respiratory disability) in cases of non-flail fracture patterns.

[0007] However, despite demonstrated success, the invasiveness of SSRF has limited its broader adoption. Potential drawbacks to rib fixation with metal hardware includes pain, scarring, bleeding, pneumothorax, infection, need for hardware removal, hardware failure and complications such as wound healing deficits, plate erosion, plate fractures, ''failures, and hardware infection. Moreover, many patients are sometimes intimidated by the prospect of a large surgery’ to place a permanent, metallic plate in their body. More recently, intrathoracic approaches have evolved to also place titanium plates on the inner surface of the thorax and in contact with the lung, furthering the need for resorbable hardware.

[0008] Accordingly, the development of new bioabsorbable fixation materials will be critical to the expansion of SSRF. Resorbable plates do not need to be removed, may reduce the incidence of hardware infections or complications, and the decreased fixation material rigidity may promote bone healing from reduced stress shielding of healing bone. (See, e.g., Zhang, Q.; Song. L.; Ning, S.; Xie, H.: Li, N.; Wang, Y. Recent Advances in Rib Fracture Fixation. J Thorac Dis 2019, 77(Suppl 8), S1070-S1077. https: / / doi.org / 10.21037 / jtd.2019.04.99; (15) Vu, K.-C.; Skourtis, M. E.; Gong, X.; Zhou, M.; Ozaki, W.; Winn, S. R. Reduction of Rib Fractures With a Bioresorbable Plating System: Preliminary Observations. Journal of Trauma and Acute Care Surgery 2008, 64 (5), 1264. https: / / doi.org / 10.1097 / TA.0b013e3180340e31; and (16) Pina, S.; Ferreira, J. M. F. Bioresorbable Plates and Screws for Clinical Applications: A Review. Journal of Healthcare Engineering 2012, 3 (2), 846435. https: / / doi. Org / 10.1260 / 2040-2295.3.2.243, the disclosures of which are incorporated herein by reference in their entirety).

[0009] However, commercially available resorbable plates have many limitations and have not yet proven to be as effective as titanium fixation in rib fracture repair. (See, e.g., Pontell, M. E.; Niklinska, E. B.: Braun, S. A.; Jaeger, N.; Kelly, K. J.; Golinko, M. S. Resorbable Versus Titanium Rigid Fixation for Pediatric Mandibular Fractures: A Systematic Review. Institutional Experience and Comparative Analysis. Craniomaxillofac Trauma Reconstr 2022, 15 (3), 189-200. https: / / doi. Org / 10.l 177 / 19433875211022573. (18) Ashley, D. W.; Christie, D. B. I.; Long, E. L.; Adiga, R.; Johns, T. J.; Fabico-Dulin, J.; Montgomery, A. Prospective Randomized Trial of Metal versus Resorbable Plates in Surgical Stabilization of Rib Fractures. Journal of Trauma and Acute Care Surgery 2022, 93 (2), 147, https: / / doi. Org / 10.1097 / TA.0000000000003642; Marasco, S. F.; Sutalo, I. D.; Bui, A. V. Mode of Failure of Rib Fixation With Absorbable Plates: A Clinical and Numerical Modeling Study, Journal of Trauma and Acute Care Surgery 2010, 68 (5), 1225. https: / / doi.org / 10.1097 / TA.0b013e3181d27cab; and Haslam, M.; Dentcheva, E.; Shafqat, M. S.; Petrov, R. Structural Failure of the BioBridge Rib Prosthesis After Chest Wall Reconstruction. The Annals of Thoracic Surgery 2022, 114 (4), e233-e235. https: / / doi.org / 10.1016 / j.athoracsur.2021.12.053, the disclosures of which are incorporated herein by reference in their entirety).

[0010] Hence, there is an ongoing need for improved materials and methods for rib stabilization. Ideally, a plate for rib stabilization would be resorbable and promote bone regrowth and repair, while avoiding the problems associated with metal alloy rib plates. Attempts have been made to fabricate rib stabilization plates using resorbable polymers, such as poly(lactides) and poly(caprolactones) but with little success. It would be made from a biocompatible material that can be adjusted for degradation and can be inserted via a minimally invasive, intrathoracic surgery approach. While patients may be intimidated by the prospect of a large surgery to place apermanent, metallic plate in their body, they likely be more comfortable agreeing to a small surgery that places a biodegradable plate that will resorb over time after the rib has fused.

[0011] Although work in resorbable polymers has been extensive, few materials have been utilized solely in FDA-approved orthopedic hardware. These have been primarily limited to well-characterized, hydrolytically degradable polyesters such as polylactides (PLGA, PLA) and carbonates (PTMC). (See, e.g., Pina, S.; Ferreira, J. M. F. Bioresorbable Plates and Screws for Clinical Applications: A Review. Journal of Healthcare Engineering 2012, 3 (2), 846435. https: / / doi. Org / 10.1260 / 2040-2295.3.2.243 and Böstman, O.; Pihlajamäki, H. Clinical Biocompatibility of Biodegradable Orthopaedic Implants for Internal Fixation: A Review. Biomaterials 2000, 21 (24), 2615-2621. https: / / doi.org / 10.1016 / S0142-9612(00)00129-0, the disclosures of which are incorporated herein by reference in their entirety). Resorbable fixation systems such as RAPIDSORB (PLLA / PLGA, DePuy Synthes) and Inion CPS (PLLA / PDLLA / PTMC, Inion) have been limited to craniomaxillofacial surgeries, where less mechanical strength is required to maintain unionization. In clinical trial rib fixation applications of these systems, high rates of postoperative fracture displacement were observed of 27.5% (see, Ashley, D. W.; Christie, D. B. I.; Long, E. L.; Adiga, R.; Johns, T. J.; Fabico-Dulin, J.; Montgomery, A. Prospective Randomized Trial of Metal versus Resorbable Plates in Surgical Stabilization of Rib Fractures. Journal of Trauma and Acute Care Surgery’ 2022, 93 (2), 147. https: / / doi.org / 10.1097 / TA.0000000000003642, the disclosure of which is incorporated herein by reference in its entirety) and 23% (see, Marasco, S. F.; Sutalo, I. D.; Bui, A. V. Mode of Failure of Rib Fixation With Absorbable Plates: A Clinical and Numerical Modeling Study. Journal of Trauma and Acute Care Surgery 2010, 68 (5), 1225. https: / / doi.org / 10.1097 / TA.0b013e3181d27cab, the disclosure of which is incorporated herein by reference in its entirety), respectively, especially in posterior fracture locations, despite similar outcomes in pain, narcotic use, and quality of life between titanium and resorbable treatment groups. RAPIDSORB and BioBridge (PLLA / PDLLA, Acumed) plates are also removed in a second surgery at a higher rate relative to titanium plates due to inflammation and infection. (See, e.g., Haslam, M.; Dentcheva, E.; Shafqat, M. S.; Petrov, R. Structural Failure of the BioBridge Rib Prosthesis After Chest Wall Reconstruction. The Annals of Thoracic Surgery 2022, 114 (4), e233- e235. https: / / doi. Org / 10.1016 / j.athoracsur.2021.12.053 and Miller, D. L.; Force, S. D.; Pickens, A.; Fernandez, F. G.; Luu, T.; Mansour, K. A. Chest Wall Reconstruction Using Biomaterials. TheAnnals of Thoracic Surgery 2013, 95 (3), 1050-1056. https: / / doi. Org / T0.1016 / j.athoracsur.2012.l 1.024, the disclosures of which arc incorporated herein by reference in their entirety). Clinical indications for use of BioBridge PLA bars remain limited to small to moderate sternal defects. (See, e.g., Miller, D. L.; Force, S. D.; Pickens, A.; Fernandez, F. G.; Luu, T.; Mansour, K. A. Chest Wall Reconstruction Using Biomaterials. The Annals of Thoracic Surgery 2013, 95 (3), 1050-1056. https: / / doi.org / 10.1016 / j.athoracsur.2012.11.024, the disclosure of which is incorporated herein by reference in its entirety). Thus, there remains an unmet material need for safe and effective resorbable plates for use in SSRF.

[0012] Additive manufacturing (AM), especially VAT photopolymerization, offers highly customizable parts and access to complex geometries that are difficult to achieve via traditional fabrication methods, (See, e.g., Placone, J. K.; Engler, A. J. Recent Advances in Extrusion-Based 3D Printing for Biomedical Applications. Advanced Healthcare Materials 2018, 7 (8), 1701161. https: / / doi.org / 10.1002 / adhni.201701161; Tetsuka, H.; Ryon Shin, S. Materials and Technical Innovations in 3D Printing in Biomedical Applications. Journal of Materials Chemistry B 2020, 8 (15), 2930-2950. https: / / doi.org / 10.1039 / D0TB00034E; and Kirillova, A.; Yeazel, T, R.; Asheghali, D.; Petersen, S. R.; Dort, S.; Gall, K.; Becker, M. L. Fabrication of Biomedical Scaffolds Using Biodegradable Polymers. Chem. Rev. 2021, 121 (18), 11238-11304. https: / / doi.org / 10.1021 / acs.chemrev.0c01200, the disclosures of which are incorporated herein by reference in their entirety).

[0013] The range of rib shapes, fracture sites, and cases of multiple fractures makes AM uniquely situated for the fabrication of resorbable orthopedic plates. The challenge has been the identification of resorbable resins possessing suitable properties. PLLA, poly(£-caprolactone) (PCL), (see, e.g., Yu, Y.-H.; Lin, Y.-T.; Hsu, Y.-H.; Chou, Y.-C.; Ueng, S. W.; Liu, S.-J. Biodegradable Antimicrobial Agent / Analgesic / Bone Morphogenetic Protein-Loaded Nanofibrous Fixators for Bone Fracture Repair. 1JN 2021, 16, 5357-5370. https: / / doi.org / 10.2147 / IJN. S325885 and Cheng, M. E.; Janzekovic, J.; Theile, H. J.; Rutherford- Heard, C.; Wille, M.-L.; Cole, C.; Lloyd, T. B.; Theile, R. J. W.; Wagels, M,; Hutmacher, D. W. Pectus Excavatum Camouflage: A New Technique Using a Tissue Engineered Scaffold. Eur J Plast Surg 2022, 45 (1), 177-182, https: / / doi.org / 10.1007 / s00238-021-01902-5, the disclosures of which are incorporated herein by reference in their entirety), poly(carbonates) (PC) (see, e.g., Brooks, S. L.; Amo, M. C.; Dove, A. P.; Weems, A. C. Postfabrication Functionalization of 4D-Printed Polycarbonate Photopolymer Scaffolds. ACS Appl. Polym. Mater. 2022, 4 (8), 5670-5679. https: / / doi.org / 10.1021 / acsapm.2c00648; Weems, A. C.; Amo, M. C.; Yu, W.; Huckstcpp, R. T. R.; Dove, A. P. 4D Polycarbonates via Stereolithography as Scaffolds for Soft Tissue Repair. Nat Commun 2021, 12 (1), 3771. https: / / doi.org / 10.1038 / s41467-021-23956-6; and Paul, S.; Zhu, Y.; Romain, C.; Brooks, R.; K. Saini, P.; K. Williams, C. Ring-Opening Copolymerization (ROCOP): Synthesis and Properties of Polyesters and Polycarbonates. Chemical Communications 2015, 51 (30), 6459-6479. https: / / doi.org / 10.1039 / C4CC10113H, the disclosures of which are incorporated herein by reference in their entirety) and polyfpropylene fumarate) (PPF) have each been used in Vat photopolymerization 3D printing. (See, e.g., Kirillova, A.; Yeazel, T. R.; Asheghali, D.; Petersen, S. R.; Dort, S.; Gall, K.; Becker, M. L. Fabrication of Biomedical Scaffolds Using Biodegradable Polymers. Chem. Rev. 2021, 121 (18), 11238-11304. https: / / doi.org / 10.1021 / acs.chemrev.0c01200. Paul, S.; Zhu, Y.; Romain, C.; Brooks, R.; K. Saini, P.; K. Williams, C. Ring-Opening Copolymerization (ROCOP): Synthesis and Properties of Polyesters and Polycarbonates. Chemical Communications 2015, 51 (30), 6459-6479. https: / / doi.org / 10.1039 / C4CC10113H: and Chyr, G.; M. DeSimone, J. Review of High-Performance Sustainable Polymers in Additive Manufacturing. Green Chemistry 2023, 25 (2), 453-466. https: / / doi.org / 10.1039 / D2GC03474C, the disclosures of which are incorporated herein by reference in their entirety). PCL has been used to 3D print patient-specific rib implants for large chest wall deformities. (See, Meng, Z.; Yang, Shangyuan; Yin, Feiyang; Liang, Xiao; Yan, Xiaolong; Li, Xinyu; He, Jiankang; Wang, Lei; and Li, D. 3D-Printed Biodegradable Polycaprolactone Rib Implants with Tissue-Specific Mechanical Properties Promote Chest Wall Recovery by Stimulating Tissue Fibrosis. Virtual and Physical Prototyping 2024, 19 (1), e2346816. https: / / doi.org / 10.1080 / 17452759.2024.2346816, the disclosure of which is incorporated herein by reference in its entirety). However, many of the PLA-, PC-, and PCL-based resins rely on acrylate or methacrylate end group functionalization that ultimately generate final products with non-degradable networks. (See, e.g., Bao, Y.; Paunovic, N.: Leroux, J.-C. Challenges and Opportunities in 3D Printing of Biodegradable Medical Devices by Emerging Photopolymerization Techniques. Advanced Functional Materials 2022, 32 (15), 2109864. https: / / doi.org / 10.1002 / adfm.202109864 and Voet, V. S. D.; Guit, J.; Loos, K. Sustainable Photopolymers in 3D Printing: A Review on Biobased, Biodegradable, and Recyclable Alternatives. Macromolecular Rapid Communications 2021, 42 (3), 2000475.https: / / doi.org / 10.1002 / marc.202000475, the disclosures of which are incorporated herein by reference in their entirety). Early generations of PPF co-crosslinked with diethyl fumarate also generated non-degradable carbon-carbon bonds. (See, e.g., Nettleton, K.; Luong, D.; Kleinfehn, A. P.; Savariau, L.; Premanandan, C.; Becker, M. L. Molecular Mass-Dependent Resorption and Bone Regeneration of 3D Printed PPF Scaffolds in a Critical -Sized Rat Cranial Defect Model. Advanced Healthcare Materials 2019, 8 (17), 1900646. https: / / doi.org / 10.1002 / adhm.201900646; Cai, Z.; Wan, Y.; Becker, M. L.; Long, Y.-Z.; Dean, D. Poly(Propylene Fumarate)-Based Materials: Synthesis, Functionalization, Properties, Device Fabrication and Biomedical Applications. Biomaterials 2019, 208, 45-71. https: / / doi. Org / 10.1016 / j.biomaterials.2019.0.3.038; and Kasper, F. K.; Tanahashi, K.; Fisher, J. P.; Mikos, A. G. Synthesis of Poly(Propylene Fumarate). Nat Protoc 2009, 4 (4), 518-525. https: / / doi.org / 10.1038 / nprot.2009.24, the disclosures of which are incorporated herein by reference in their entirety). However, more recent fumarate copolyesters crosslinked with ester containing thiols (see, e.g., Yu, Y.-H.; Lin, Y.-T.; Hsu, Y.-H.; Chou, Y.-C.; Ueng, S. W.; Liu, S.-J. Biodegradable Antimicrobial Agent / Analgesic / Bone Morphogenetic Protein-Loaded Nanofibrous Fixators for Bone Fracture Repair. N 2021, 16, 5357-5370. https: / / doi.org / 10.2147 / IJN. S325885, the disclosure of which is incorporated herein by reference in its entirety) and ceramic composite fillers (see, e.g., R. Klein, T.; Kirillova, A.; Gall, K.; L. Becker, M. Influence of Post- Processing on the Properties of 3D-Printed Poly(Propylene Fumarate) Star Polymer Hydroxyapatite Nanocomposites. RSC Applied Polymers 2023, 1 (1), 73-81. https: / / doi.org / 10.1039 / D3LP00013C, the disclosure of which is incorporated herein by reference in its entirety) have greatly expanded both the mechanical properties and degradability of the resulting resins.[0014| Fumarate-based copolyesters have been synthesized in various topologies and compositions (e.g., linear, ABA triblock, stars) to yield a range of mechanical properties in 3D- printed parts relevant for tissue engineering. (See, e.g., Kirillova, A.; Yeazel, T. R.; Gall, K.; Becker, M. L. Thiol-Based Three-Dimensional Printing of Fully Degradable Poly(Propylene Fumarate) Star Polymers. ACS Appl. Mater. Interfaces 2022, 14 (34), 38436-38447. https: / / doi.org / 10.1021 / acsami.2c06553; Yeazel-Klein, T. R.; Davis, A. G.: Becker, M. L. Thiol-Ene-Based 3D Printing of Bioresorbable Fumarate-Based ABA Triblock Copolyester Elastomers. Advanced Materials Technologies 2023, 8 (23), 2201904. https: / / doi.org / 10.1002 / admt.202201904: Bass, G. F.; Shin, Y.; Becker, M. L. Regio-RandomClemmensen Reduction of Biodegradable Polyesters for Photochemically Triggered 3D Printing. Macromolecules 2021, 54 (3), 1273-1280, https: / / doi.org / 10.1021 / acs.macromol.0c02729; Le Fer, G.; Dilla, R. A.; Wang, Z.; King, J.; Chuang, S. S. C.; Becker, M. L. Clustering and Hierarchical Organization of 3D Printed Poly(Propylene Fumarate)-Block-PEG-Block-Poly( Propylene Fumarate) ABA Triblock Copolymer Hydrogels. Macromolecules 2021, 54 (7), 3458-3468. https: / / doi.org / 10.1021 / acs.macromol.lc00132; and Petersen, S. R.; Yu, J.; Yeazel, T. R.; Bass, G.; Alamdari, A.; Becker, M. L. Degradable, Photochemically Printable Poly(Propylene Fumarate)-Based ABA Triblock Elastomers. Biomacromolecules 2022, 23 (6), 2388-2395. https: / / doi.org / 10.1021 / acs.biomac.2c00151, the disclosures of which are incorporated herein by reference in their entirety). Clinical success of 3D printed orthopedic rib fracture hardware will depend on fully degradable polymer networks that possess mechanical properties suitable for fixation and controlled degradation properties.

[0015] Unfortunately for patients, however, a prospective randomized study suggests that current resorbable polymers are inferior to standard rib plating strategy. Specifically, the metal plates were found to provided better initial alignment with no displacement over time compared to resorbable polymer plates which had worse initial alignment with subsequently worsened displacement at 3-6 month follow up. See, Ashley DW, Christie DB 3rd, Long EL, Adiga R, Johns TJ, Fabico-Dulin J, Montgomery A. “Prospective randomized trial of metal versus resorbable plates in surgical stabilization of rib fractures.” J Trauma Acute CareSurg. 2022 Aug 1;93(2): 147-156. doi: 10.1097 / TA.0000000000003642. Epub 2022 Apr 8. PMID: 35393383, the disclosure of which is incorporated herein by reference in its entirety.

[0016] Accordingly, what is needed in the art is a tunable, resorbable, and 3D printable platform of osteoconductive polymer composite osteosynthetic plates designed to reduce the cost and invasiveness associated with SSRF while providing sufficient mechanical support for rib unionization and simultaneously reducing inflammation and infection risk and improving bone mineralization compared to titanium implants.SUMMARY OF THE INVENTION

[0017] The Summary is provided to introduce a selection of concepts that are further described below in the Detailed Description. This Summary is not intended to identify key or essentialfeatures of the claimed subject matter, nor is it intended to be used as an aid in limiting the scope of the claimed subject matter.

[0018] As set forth above, Rib fractures are common among blunt chest trauma patients and are a hallmark of severe thoracic injury with high morbidity and mortality rates. The standard treatment of most rib fracture cases is limited to pain control and respiratory support, with the surgical stabilization of rib fractures (SSRF) using titanium plates reserved for severely injured patients. Although SSRF has been shown to improve long-term patient outcomes, its expanded use has been limited by the invasiveness of the procedure and a lack of safe and effective resorbable fixation materials. While resorbable metal and polymeric plates have each been used in the clinic, many failures have been reported and challenges remain to control the mechanical properties of the plate during the degradation process,

[0019] In various aspects of the present invention provides a resorbable 3D printed osteosynthetic fixation devices for rib fracture repair. In another aspect, the present invention provides resins for making the resorbable 3D printed osteosynthetic fixation devices for rib fracture repair. Another aspect of the present invention provides a method for repairing fractures using fixation devices as prescribed herein. In another aspect of the present invention provides a method of using copolymer materials as prescribed herein. Yet another aspect of the present disclosure provides a method of bone repair using a rib fixation device as prescribed herein. Other aspects of the present disclosure provides all that is described and illustrated herein.

[0020] In various embodiments, the present invention provides a series of tunable, resorbable, and 3D printable platforms of osteoconductive fumarate-based polymer composite osteosynthetic plates designed to reduce the cost and invasiveness associated with SSRF, while providing sufficient mechanical support for rib unionization and simultaneously reducing inflammation and infection risk and improving bone mineralization compared to titanium implants.

[0021] These resorbable polymer rib plates with performance comparable to current metal alloy plating systems and can be adjusted for various degradation profiles and inserted using a minimally invasive, intrathoracic surgery approach. Advantageously, the resorbable plates of the present invention comprise a fumarate-based ABA triblock copolyester or fumarate-based star polymer which forms rib plate devices that are not overly stiff, allowing for better surgical handling and compatibility with rib curvature and plates that are, otherwise, believed overcome the limitations of previous resorbable polymers. Compared to rigid titanium fixation plates, ribs fixed with 3Dprinted composite plates of the present invention have been found to elicit fracture calluses with decreased inflammatory response, enhanced osseointegration, and bone morphometry at 2- and 4-weeks post-fracture comparable to clinically used titanium plates.[0022 j In a first aspect, the present invention is directed to a resin for use in a resorbable 3D printed osteosynthetic apparatus for rib fracture repair comprising: a linear or star-shaped polypropylene fumarate)-based copolymer comprising at least one of an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block and a star-shaped polypropylene fumarate) copolymer; a thiol-based crosslinker; and a plurality of filler nanoparticles. In one or more of these embodiments, the resin further comprises a diluent and a photoinitiator. In some of these embodiments, the resin further comprises a photoinhibitor,

[0023] In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the linear or star-shaped polypropylene fumarate) -based copolymer is an ABA block copolymer having a first and second polyfpropylene fumarate) A blocks and a polypropylene succinate) B block comprising the residue of a difunctional alcohol initiator. In certain embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention comprising an ABA block copolymer having a formula selected from:where each n is an integer from about 1 to about 20, each m is an integer from about 2 to about 70, and I is the residue of an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups.

[0024] In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the linear or star-shaped polypropylene fumarate)-based copolymer is a star-shaped polyfpropylene fumarate) copolymer comprising 3 or 4 polypropylene fumarate) arms extending from a multi¬ functional alcohol initiator. In particular embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention comprising a star-shaped polyfpropylene fumarate) copolymer having the formula:DUK. P W00012where each m is an integer from about 10 to about 50.

[0025] In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the ABA block copolymer has a degree of polymerization of from about 10 to about 100. In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the star-shaped polypropylene fumarate) copolymer has a degree of polymerization of from about 40 to about 200. In various embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein each arm of the 3 or 4 polypropylene fumarate) arms extending from a multi-functional alcohol initiator copolymer has a degree of polymerization of from about 10 to about 50.

[0026] In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the linear or star-shaped polypropylene fumarate)-based copolymer comprises from about 50 wt.% to about 90 wt.% of the resin. In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the linear or star-shaped polypropylene fumarate)-based copolymer comprises about 70 wt.% of the resin. In one or more embodiments, the resin of the present invention includes any oneor more of the above referenced embodiments of the first aspect of the present invention wherein the thiol-based crosslinkcr is a molecule having 3 available thiol functional groups.

[0027] In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the thiol-based crosslinker comprises trimethylolpropane tris(3-mercaptopropionate), trimethylolpropanetris(3-mercaptopropionate), Thiocure 332 and Thiocure 333, ETTMP-700, ETTMP-1300, and combinations thereof. In various embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the thiol-based crosslinker has a formula selected from:In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the thiol-based crosslinker comprises from about 0.5 to about 10 mole percent of the resin.

[0028] In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the ratio of available alkene groups in the linear or star-shaped polypropylene fumarate)-based copolymer to available thiol groups in the thiol-based crosslinker in the resin is from about 3:1 to about 40:1. Inother embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the ratio of available alkene groups in the linear or star-shaped polyfpropylene fumarate)-based copolymer to available thiol groups in the thiol-based crosslinker in the resin is about 20:1.[0029} In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the plurality of filler nanoparticles comprises are selected from hydroxyapatite (HAp), strontium carbonate, tricalcium phosphate, barium phosphate and combinations thereof. In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the plurality of filler nanoparticles comprises from about I to about 20 weight percent of the resin. In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the plurality of filler nanoparticles comprise about 10 weight percent of the resin.

[0030] In various embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the plurality of filler nanoparticles have a mean particle size of from about 100 nm to about 1000 nm. In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the plurality of filler nanoparticles are hydroxyapatite (HAp) nanoparticles having a mean particle size of from about 100 nm to about 500 nm.

[0031] In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention having a complex viscosity of less than 50 Pa- sec. In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention having a complex viscosity of from about 5 to about 15 Pa- sec.

[0032] In various embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention having a complex viscosity suitable for 3D printing by Continuous Liquid Interface Production (CLIP) photochemical printing.

[0033] In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the diluent comprises from about 10 wt.% to about 50 wt.% of the resin. In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the diluent comprises from about 30 wt.% of the resin. In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the diluent is selected from the group ethyl acetate, acetone, dioxane, and combinations thereof.In one or more embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the photoinitiator is selected from the group consisting of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO). In some embodiments, the resin of the present invention includes any one or more of the above referenced embodiments of the first aspect of the present invention wherein the photoinhibitor is selected from the group consisting of oxybenzone (HMB).

[0034] In a second aspect, the present invention is directed to a 3D printed osteosynthetic composite material comprising any one of the resins described above. In some of these embodiments, the 3D printed osteosynthetic composite material comprises: a linear or star-shaped polypropylene fumarate)-based copolymer comprising at least one of an ABA block copolymer having a first and second polyfpropylene fumarate) A blocks and a polypropylene succinate) B block and a star-shaped polypropylene fumarate) copolymer; a thiol-based crosslinker; and a plurality of filler nanoparticles.

[0035] In a third aspect, the present invention is directed to a 3D printed osteosynthetic apparatus for rib fracture repair comprising the 3D printed osteosynthetic composite material described above. In some of these embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer comprises a resorbable ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block, wherein the first and second polypropylene fumarate) A blocks are each bonded covalently to an end of the polypropylene succinate) B polymer block to form an ABA block copolymer.

[0036] In some embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer of the present invention includes any one or more of the above referenced embodimentsof the third aspect of the present invention wherein the linear or star-shaped poly(propylene fumarate)-based copolymer comprises a resorbable star-shaped poly(propylene fumarate) copolymer comprising 3 or 4 poly(propylene fumarate) arms extending from a multi-functional alcohol initiator.[0037} In various embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer of the present invention includes any one or more of the above referenced embodiments of the third aspect of the present invention, further comprising a filler material to promote bone repair and / or regrowth. In certain embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer of the present invention includes any one or more of the above referenced embodiments of the third aspect of the present invention wherein the filler material is hydroxyapatite. In some embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer of the present invention includes any one or more of the above referenced embodiments of the third aspect of the present invention comprising from 1 wt.% to 20 wt.% hydroxyapatite.[0038| In particular embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer of the present invention includes any one or more of the above referenced embodiments of the third aspect of the present invention wherein the apparatus is a plate. In one or more embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer of the present invention includes any one or more of the above referenced embodiments of the third aspect of the present invention further comprising a plurality of openings sized to receive surgical screws.

[0039] In a fourth aspect, the present invention is directed to a method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair comprising: measuring and / or imaging a rib fracture on a subject having a rib fracture; generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in the subject, based upon the measurements and or images taken of the rib fracture; preparing a 3D printable resin described above and loading the resin mixture into a suitable 3D printer; 3D printing the resorbable 3D printed osteosynthetic apparatus for rib fracture repair based upon the 3D printable file. In various embodiments, the method further comprises post curing the resorbable 3D printed osteosynthetic apparatus for rib fracture repair with ultraviolet light

[0040] In one or more embodiments, the method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of the present invention includes any one or more of the above referenced embodiments of the fourth aspect of the present invention wherein the stepof preparing a 3D printable resin described above comprises: dissolving a linear or star-shaped polyfpropylcnc fumaratc)-bascd copolymer comprising at least one of an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block and a star-shaped poly (propylene fumarate) copolymer in a suitable diluent; adding a plurality of filler nanoparticles to the solution; adding the photoinitiator to the ABA block copolymer; adding a thiol-based crosslinker and mixing to form the 3D printable resin. In one or more embodiments, the method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of the present invention includes any one or more of the above referenced embodiments of the fourth aspect of the present invention wherein the step of adding a thiol-based crosslinker does not take place until immediately before less than 30 minutes before the step of 3D printing the resorbable 3D printed osteosynthetic apparatus.

[0041] In one or more embodiments, the method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of the present invention includes any one or more of the above referenced embodiments of the fourth aspect of the present invention wherein the step of preparing a 3D printable resin described above further comprises adding radical scavenger or photoinhibitor to the solution. In one or more embodiments, the method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of the present invention includes any one or more of the above referenced embodiments of the fourth aspect of the present invention wherein the 3D printable resin of step A wherein the filler nanoparticles promote bone repair and / or regrowth. In one or more embodiments, the method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of the present invention includes any one or more of the above referenced embodiments of the fourth aspect of the present invention wherein the filler nanoparticles to promote bone repair and / or regrowth are selected from the group consisting of hydroxyapatite, strontium carbonate, b-tricalcium phosphate, and combinations thereof.

[0042] In one or more embodiments, the method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of the present invention includes any one or more of the above referenced embodiments of the fourth aspect of the present invention wherein the molar ratio of the 3D printable resin to the thiol-based crosslinker in the crosslinker / resin mixture of step D is from about 3: 1 to about 40: 1. In one or more embodiments, the method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of the present invention includes any one or more of the above referenced embodiments of the fourth aspect of the presentinvention wherein the thiol-based crosslinker comprises trimethylolpropane tris(3-mercaptopropionate), Thiocure 332, and Thiocure 333, respectively.

[0043] In a fifth aspect, the present invention is directed to a method for treating a rib fracture in a subject comprising: preparing a 3D printed composite plate for rib fracture repair described above, wherein the 3D printable composite plate is sized for use in repairing a rib fracture at a rib fracture site in a subject; and surgically inserting the 3D printed composite plate into the subject and securing it across the rib fracture site such that the 3D printed composite plate is mechanically secured to the rib on either side of the rib fracture.

[0044] In some embodiments, the method for treating a rib fracture of the present invention includes any one or more of the above referenced embodiments of the fifth aspect of the present invention wherein the step of preparing a 3D printed composite plate for rib fracture repair comprises: preparing a 3D printable resin comprising an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block, wherein the first and second polypropylene fumarate) A blocks are each bonded covalently to an end of the polypropylene succinate) B polymer block to form an ABA block copolymer; a filler material; and a photoinitiator; measuring and / or imaging a rib fracture on a subject having a rib fracture; generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in the subject, based upon the measurements and or images taken of the rib fracture; adding a thiol-based crosslinker to 3D printable resin and loading the crosslinker / resin mixture into a suitable 3D printer; and 3D printing the 3D printable resin composite based upon the 3D printable file to produce a 3D printed composite plate for rib fracture repair.

[0045] In some other embodiments, the method for treating a rib fracture of the present invention includes any one or more of the above referenced embodiments of the fifth aspect of the present invention wherein the step of preparing a 3D printed composite plate for rib fracture repair comprises: preparing a 3D printable resin comprising a star-shaped PPF copolymer having 3 or 4 arm s, a filler material, and a photoinitiator; measuring and / or imaging a rib fracture on a subject having a rib fracture; generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in the subject, based upon the measurements and or images taken of the rib fracture; adding a thiol-based crosslinker to 3D printable resin and loading the crosslinker / resin mixture into a suitable 3D printer; and 3D printing the 3D printableresin composite based upon the 3D printable file to produce a 3D printed composite plate for rib fracture repair. In some of these embodiments, the 3 D printed composite plate comprises one or more openings sized to receive and retain a surgical screw. In one or more embodiments, the method for treating a rib fracture of the present invention includes any one or more of the above referenced embodiments of the fifth aspect of the present invention wherein the step of mechanically securing the 3D printed composite plate to the rib on either side of the rib fracture is performed using two or more screws running through the 3D printed composite plate.

[0046] As set forth above, the resorbable rib plates of the present invention not only avoids the prospect of a large surgery to place a permanent, metallic plate in the patient’s body, only a small minimally invasive surgery is required to install a resorbable rib plate. There is no metallic plate in the patient’s body that will be permanent if not subsequently removed, since the rib plates of the present invention will be resorbed into the body over time after the rib has fused. As it can be installed using new minimally invasive techniques, it is believed that the resorbable rib plate of the present invention provides an attractive option for both surgeons and patients. Other aspects of the present disclosure provides all that is described and illustrated herein.BRIEF DESCRIPTION OF THE DRAWINGS

[0047] For a more complete understanding of the features and advantages of the present invention, reference is now made to the detailed description of the invention along with the accompanying figures. The accompanying Figures are provided by way of illustration and not by way of limitation. The foregoing aspects and other features of the disclosure are explained in the following description, taken in connection with the accompanying example figures (also “FIG.”) relating to one or more embodiments.10048] FIG. 1A are images of showing effects of ri b plate material type on callus size and callus index.

[0049] FIG. I B is a graph showing the effects of rib plate material type on callus index,

[0050] FIG. 1C is a graph showing the effects of rib plate material type on callus size.

[0051] FIG. 2 are images showing effects of rib plate material type on calcium deposition.

[0052] FIG. 2B is a graph showing the effect of rib plate material type on total bone deposition.

[0053] FIG. 2C is a graph show ing the effect of rib plate material type on cortical deposition.

[0054] FIG. 2D is a graph showing the effect of rib plate material type on callus deposition.

[0055] FIG. 3A is a graph showing the effect of rib plate type on callus endochondral ossification.

[0056] FIG. 3B are images showing the effect of rib plate type on callus endochondral ossification.

[0057] FIGS. 4A-B are a reaction mechanism and schematic diagram showing polymer synthesis and 3D printing of fumarate -based star copolyesters and copolyester-composite rib fracture plates. FIG. 4A is a reaction mechanism showing ring-opening copolymerization of propylene oxide and maleic anhydride followed by an isomerization reaction to yield poly(propylene fumarate) star copolyesters. FIG. 4B is a schematic showing Continuous Liquid Interface Production (CLIP) photochemical printing of a one pot resin containing polypropylene fumarate) star copolyesters, trimethylolpropanetris(3 -mercaptopropionate) (thiol crosslinker) in a 20:1 (alkenerthiol) ratio, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO) and oxybenzone (HMB) were dissolved in ethyl acetate (70 wt.% polymer). Hydroxyapatite nanoparticles (10 wt.%) were added to the resin prior to printing to yield composite rib plates.

[0058] FIGS. 5A-D are graphs showing the mechanical properties of 3D printed fumarate-based copolyester star polymers and copolyester-hydroxyapatite composites and rib fracture plates. Tensile bars, fumarate-based copolyester and composite rib fracture plates were 3D printed at a 20: 1 alkene-to-thiol crosslink ratio. FIG. 5A is a graph showing representative fumarate-based copolyester, composite, and PLA stress-strain curves from uniaxial tension tests collected at 25 °C and 37 °C in lx PBS. PLA curves shown in inset for clarity. FIG. 5B is a graph showing stressstrain curves from three-point bend tests of 3D printed fumarate-based copolyester and composite plates, (n = 3) FIG. 5C is a graph showing box plots of copolyester and composite tensile modulus (n = 5) determined from stress-strain curves shown in FIG. 5A. The modulus of fumarate-based copolyester-HAp composite plates is more than two-fold greater than unfilled fumarate-based copolyester rib fracture plates. FIG. 5D is a graph showing stress-strain curves from three-point bend tests of PLA plates (n 3).

[0059] FIGS. 6A-B are images and a schematic drawing showing rabbit rib fracture surgical model and subsequent fixation with various osteosynthetic plates. FIG. 6A is a schematic diagram and images showing rib fixation using titanium and resorbable osteosynthetic plates. The 4thand 6thribs of New Zealand white rabbits were cut and immediately stabilized with eithercommercially available titanium or 3D printed, resorbable PLA, fumarate-based copolyester, or fumarate-based copolyester-HAp composite osteosynthetic plates. Radiographs show fixation at 4 weeks post-surgery. FIG. 6B is an image showing rib fixation with a composite plate, centered at the site of fracture with one screw on either end.[0060} FIGS. 7A-C are an image and two graphs showing the results of three-point bend mechanical testing of explanted rib callus at 2- and 4-weeks post-fracture. FIG. 7A is an image showing a representative three-point bend test of explanted rabbit rib. The applied force is centered at the site of fracture. Flexural strength, modulus, and toughness were determined from resulting stress-strain curves. FIG. 7B is a graph showing representative stress-strain curves obtained from three-point bend tests at 2 and 4 weeks (n = 3-4). Ribs stabilized with titanium plates and composite plates show increased callus modulus at 4 weeks compared to ribs stabilized with PLA and fumarate-based copolyester plates. FIG. 7C is a graph showing flexural modulus of stabilized rib fractures, obtained from curves in (FIG. 7B) (n = 3-4). The flexural modulus of the callus increases from 2 to 4 weeks across all groups. Means ± SD. *p < 0.05, **p < 0.01, ***p < 0.001, ns = not significant.10061] FIG. 8 are images showing radiography and histological staining of explanted rib callus at 2- and 4-weeks post-fracture. µCT and x-ray scans of explanted rib calluses at 2 and 4 weeks were obtained, followed by decalcification and cross-sectional histological characterization. Sections were visualized using Hematoxylin and Eosin (H& E) and Alcian Blue-Picrosirius Red staining (shown). Ribs stabilized with fumarate-based copolyester and fumarate-based copolyester-HAp composite plates exhibit decreased irritancy and greater osseointegration compared to ribs stabilized with PLA or titanium plates. Scale bar = I mm.

[0062] FIGS. 9A-E are micro-computed tomography (µCT) of explanted rib callus at 2- and 4-weeks post-fracture and related graphs reporting bone volume, structural model index, Trabecular thickness and surface area to volume ratio. FIG. 9A shows representative CT scans of rib fracture callus 4 weeks post-fracture. Non-union is observed in rib fractures without plate fixation and in fractures stabilized with PLA and fumarate-based copolyester plates (n 3-5 per group). FIG. 9B is a graph showing total bone volume (BV) of the region of interest (fracture site callus) increases across all groups from 2 to 4 weeks. FIG. 9C is a graph showing structure model index (SMI) differentiates between plate-like and rod-like structures in trabecular bone. Lower values indicate more plate-like, stronger structures. Decreases in SMI are observed across alltreatment groups from 2 to 4 weeks. FIG. 9D is a graph showing average thickness of trabeculae, reported as an inverse. Trabecular thickness increases from 2 to 4 weeks most significantly in control ribs and fumarate-based copolyester- and composite-stabilized ribs. FIG. 9E is a graph showing surface area of bone relative to its total volume. Means ± SD, *p < 0.05, **p < 0.01, ***p < 0.001, ns = not significant.

[0063] FIGS. 10A-C are images showing CLIP photochemical 3D printing of orthopedic plates. FIG. 10A is an image showing sample build tray from Carbon AO Suite software of fumarate-based copolyester star and copolyester-HAp composite prints. PLA plates were printed separately using a Dremel FDM printer. FIG. 10B is an image showing sample STL file of orthopedic plates. FIG. 10C is an image showing post-cured 3D printed plates, from left to right: PLA, fumarate-based copolyester, fumarate-based copolyester-HAp composite. Inset scale bar::::1 cm.

[0064] FIGS. 11 A-B are graphs showing the mechanical characterization of 3D printed tensile bars via uniaxial tensile testing (FIG. 11A) and orthopedic rib plates via 3-point bend flexural testing (FIG. 11B). Representative curves of fumarate-based copolyester-HAp composite samples, printed at a 20:1 alkene:thiol ratio, are shown.

[0065] FIGS. 12A-B are1H NMR spectra of polypropylene maleate) star copolyester (FIG.12A) and isomerized polypropylene fumarate) star copolyester (FIG. 12B). Full conversion of the cis alkene to the trans alkene is observed.

[0066] FIG. 13 is a13C NMR spectrum of polypropylene fumarate) star copolymer.

[0067] FIG. 14 is a Size Exclusion Chromatography (SEC) (THF, based on PS standards) chromatogram of polypropylene fumarate) star copolymer. Mn= 4.2 kDa,= 6.9 kDa, DM = 1.65.

[0068] FIG. 15 are frequency sweeps of PPF star polymers with and without 10 wt.% HAp, dissolved in ethyl acetate (70 / 30 w / w). HAp moderately increases the resin viscosity. Both resins are below the CLIP printable limit of 10 Pa-s.

[0069] FIGS. 16A-C are representative fluorescence images of live / dead staining of control glass coverslips, fumarate-based star copolyester, and copolyester-composite coated coverslips (FIG. 16A); quantification of live / dead staining(FIG. 16B); and cell viability at 24 and 72 hours (FIG. 16C).

[0070] FIGS. 17A-B are μCT reconstructions of 3D printed resorbable osteosynthetic plates where the layer lines and lower resolution features are visible on PLA plates printed via FDM and small surface defects are visible on fumarate-based copolyester and composite plates printed via CLIP (FIG. 17A); internal cross sections of 3D printed plates show minimal internal defects (FIG.17B). Moderate inconsistencies in wall thickness arise from the printing process. HAp nanoparticles are visible within composite plates.

[0071] FIGS. 18A-B are graphs showing the results of thermal characterizations of 3D printed fumarate-based copolyester star polymers and copolyester-HAp composite. FIG. 18A is a graph showing thermogravimetric analysis (TGA) curves. FIG. 18B is a graph showing differential scanning calorimetry (DSC) curves from a second heating cycle with the glass transition temperature (Tg) marked by vertical lines, Tg(star copolyester) = 28 °C. Tg(composite)::::35 °C.

[0072] FIGS. 19A-B are graphs showing the results of dynamic mechanical analysis (DMA) three-point bend temperature sweeps of 3D printed fumarate-based copolyester star polymers (FIG. 19A) and copolyester-composite (FIG. 19B). Tgwas determined from the maximum of the tan(delta) curve. Tg(star copolyester) = 57 °C. Tg(composite) = 48 °C,

[0073] FIG. 20 is a graph showing the results of a degradation study of fumarate-based star polymers 3D printed discs in 0.25 N potassium hydroxide (aq.) at 37 °C with constant agitation. Samples are fully degraded after 11 days.

[0074] FIGS. 21A-B are annotated mass spectrometry7spectra of star copolyester (FIG. 21 A) and copolyester-composite (FIG. 21 B) plate samples, degraded fully in 10 M NaOH. Small molecule degradation products (i.e., propylene glycol and fumaric acid) are present in both degradation solutions. A higher concentration of these lower molecular weight products is present in the composite plate degradation solution, attributed to increased water penetration into the network in the presence of ceramic.

[0075] FIGS. 22A-D are tensile stress vs. strain curves of 3D printed fumarate-based copolyester stars and copolyester-composite printed at a 20:1 alkene:thiol ratio, performed at ambient conditions (FIGS. 22A-B) and in 1x PBS at 37 °C (FIGS 22C-D).

[0076] FIG. 23 are hematoxylin and eosin (H& E) stained sections of explanted rib callus at site of plate implant at 2- and 4-weeks post-fracture. Implant indicated with star. Inset scale bar = 300 pm.

[0077] FIG. 24 are hematoxylin and eosin (H& E) stained sections of explanted callus at 2-and 4-weeks post-fracture. Inset scale bar = 1 mm,

[0078] FIGS. 25A-F are graphs showing results of histological evaluation and ISO scoring of H& E stained slides of fracture calluses. ISO scoring was performed on 2-3 sites per animal at different areas of the device and then scores averaged for final analysis. Irritancy scores were calculated from scoring of different cell types (FIG. 25A-B) and neovascularization, fibrosis, and fatty infiltrates (FIG. 25C-D). Scoring of additional features including necrosis, mineralization, granulomas, and hemorrhage is shown in FIG. 25E-F.

[0079] FIGS. 26 A-B are graphs showing the results of additional CT quantification of rib fracture callus at 2- and 4-weeks post-fracture. FIG. 26A is a graph showing bone volume (BV) over total volume (TV), a metric for bone density (n = 3-5). There is little variation in BV / TV between 2- and 4-weeks or between treatment groups post-fracture. FIG. 26B is a graph showing connectivity density of the trabecular network. Means ± SD. ns = not significant.DETAILED DESCRIPTION OF THE ILLUSTRATIVE EMBODIMENTS

[0080] The following is a detailed description of the disclosure provided to aid those skilled in the art in practicing the present disclosure. Those of ordinary skill in the art may make modifications and variations in the embodiments described herein without departing from the spirit or scope of the present disclosure. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. The terminology used in the description of the disclosure herein is for describing particular embodiments only and is not intended to be limiting of the disclosure.

[0081] As set forth above, there is a dearth of solid curing, yet resorbable, biocompatible polymers with appropriate degradation and resorption times to serve as a tissue substitute that are photo-cross-linkable (i.e., 3D printable). Materials explored to date include polylactides, poly(s-caprolactone) (PCL), and PPF. With regard to resorption profiles, polylactides, including PLGA, have been found to resorb in 1-2 months (too early for orthopedic applications) and may undergo rapid bulk degradation leading to a localized acidosis and inflammation. PCL is known to degrade very slowly, sometimes over years, thereby preventing the remodeling and vascularization necessary for neo-tissue persistence. When used in photochemical 3D printing, nearly all ofpolyesters rely on methacrylate end group functionalization which generate a non -degradable network during the 3D printing process, limiting the biorcsorption process.

[0082] The resins used in the present disclosure are based on polypropylene fumarate) (PPF). PPF, first reported in 1994, was driven by the need for a degradable material that would be useful for tissue engineering. PPF has been crosslinked into mechanically strong scaffolds using a photoinitiator and light source. ISO- 10993-5 compliant toxicity testing has consistently found 3D printed PPF implants to be biocompatible with useful mechanical and osteoconductive properties. However, like the methacrylate scaffolds noted above, PPF has been co-crosslinked with diethyl fumarate (DEF) which serves as a reactive diluent. Unfortunately, previous reports of photochemical crosslinking of PPF with DEF during 3D printing results in a non-degradable carbon-carbon bond network. The present invention outlines a solution to this translational barrier.

[0083] PPF resins possess a wide variation in molecular composition, topology, architectures, copolymerization ratios and new, degradable crosslinking methodology which converge to offer an unprecedented range in material properties that can be applied to scaffolds for soft tissue engineering. These materials are different than PPF generated using step-growth polymerization, demonstrated by many groups for scaffold fabrication. PPF with narrow molecular mass distributions have been used to 3D print scaffolds (i.e., 75-100 um features) with precise mechanical properties and resorption profiles that correlate with molecular mass and surface area. The incorporation of functional epoxides into the PPF facilitates post-printing functionalization, and the use of star polymer architectures significantly reduce resin viscosity further define the translational pathway.

[0084] In an example embodiment, the rib fixation device is a conventional rib plate design that is made from a resin as disclosed herein. In another embodiment, the rib plate is a design that is patient-specific, customized to match a patient's anatomy, The customization can be based on 2D or 3D patient images (e.g., OCT, MRI, etc.) for example, and it can optionally be 3D printed. Additional details are described in the accompanying appendix.

[0085] In some embodiments, the rib fixation devices of the present invention comprises a class of biocompatible, resorbable ABA triblock copolyesters of polyfpropylene fumarate) (PPF)- b-poly(propylene succinate) (PPS)-b-poly(propylene fumarate) elastomers. In some other embodiments, the rib fixation devices of the present invention comprises a class of biocompatible, resorbable PPF-based star polymers. In either case, these elastomers are well suited to thedisclosed application and have not been previously applied in the fracture repair space. Unlike previously printed PPF-based materials that were co-crosslinked with non-degradable diethyl fumarate (DEF), the thiol-based crosslinkers used in the present invention control both network density (crosslinking) and elasticity (stoichiometry), which collectively govern degradation timelines and mechanical properties of the rib fixation apparatus. These elastomeric materials can advantageously avoid overly stiff devices and allow for surgical handling and compatibility with rib curvature. Studies using these materials show a gradual loss of mechanical properties with time, and the post mortem histology show that neither the device nor its degradation products induce an acute inflammatory response.

[0086] Further, to improve the mechanical properties of the PPF-based polymers used and / or improve healing and bone growth, filler nanoparticles are added to the resin, as described below.

[0087] In various embodiments, the rib plates according to present invention can facilitate a clinical departure from current standards of care, including surgical stabilization of rib fractures (SSRF), allowing for a minimally invasive approach to rib fixation through video -assisted thoracoscopic (VATS) SSRF. As another advantage, the disclosed rib plating device can seamlessly fit into current clinical workflows. SSRF has shown to be beneficial in the treatment of patients with severe rib fractures. Because of the maximally invasive nature of the operative VATS, approaches have been developed. Yet, these approaches lack optimized plate design and resorbability. Intra-thoracic fixation has the benefits of minimally invasive approaches to reduce pain, hospital LOS. and wound complications.

[0088] In order to realize the benefits of VATS-SSRF, patient risk must be minimized. While extrathoracially placed plates have acceptably low rates of infection, intra-thoracic plates are subject to a life-long risk for infection or pulmonary complication such as erosion. A resorbable plate can address this risk. Further, plate design and manufacturing has been adapted from long bone surgical implants, which requires intraoperative customization and significant preoperative planning to ensure a proper fit and dimension. The option of on-demand construction, such as additive manufacturing, holds the promise to address this costly and time-consuming approach through the personalization of plate design.

[0089] The following terms may have meanings ascribed to them below, unless specified otherwise. As used herein, the terms "comprising" "to comprise" and the like do not exclude the presence of further elements or steps in addition to those listed in a claim. Similarly, the terms “a,”“an” or “the” before an element or feature does not exclude the presence of a plurality of these elements or features, unless the context clearly dictates otherwise. Further, the term "means" used many times in a claim does not exclude the possibility that two or more of these means are actuated through a single element or component.[0090} Unless specifically stated or obvious from context, as used herein, the term "about" is understood as within a range of normal tolerance in the art, for example within 2 standard deviations of the mean. " About" can be understood as within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05%, or 0.01% of the stated value. Unless otherwise clear from context, all numerical values provided herein in the specification and the claim can be modified by the term "about."

[0091] It should be also understood that the ranges provided herein are a shorthand for all of the values within the range and, further, that the individual range values presented herein can be combined to form additional non-disclosed ranges. For example, a range of 1 to 50 is understood to include any number, combination of numbers, or sub-range from the group consisting 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43. 44, 45, 46, 47, 48, 49, or 50.

[0092] Further, as used herein, the term “callus” refers to the bony healing tissue which forms around the ends of broken bone, more specifically, a mass of exudate and connective tissue that forms around a break in a bone and is converted into bone in healing.

[0093] All publications, patent applications, patents, and other references mentioned herein are expressly incorporated by reference in their entirety, which means that they should be read and considered by the reader as part of this text. That the document, reference, patent application, or patent cited in this text is not repeated in this text is merely for reasons of conciseness. In the case of conflict, the present disclosure, including definitions, will control. All technical and scientific terms used herein have the same meaning, unless otherwise indicated.

[0094] Further, any compositions or methods provided herein can be combined with one or more of any of the other compositions and methods provided herein. The fact that given features, elements or components are cited in different dependent claims does not exclude that at least some of these features, elements or components maybe used in combination together.10095] In a first aspect, the present invention is directed to a rib fixation device for rib fracture repair, as described below. In various embodiments, the present invention is directed to aresorbable 3D printed osteosynthetic apparatus for rib fracture repair comprising a linear or star¬ shaped poly(propylene fumarate)-based copolymer comprising at either an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block, a star-shaped polypropylene fumarate) copolymer, or both; a multi-functional thiol-based crosslinker; and a plurality of filler nanoparticles.

[0096] As set forth above, in various embodiments, the rib plate comprises a degradable, 3D printable ABA triblock copolyester resin system that is viable for scale-up and translation into defined pre-clinical applications. Some examples of suitable copolymers for the disclosed device are described in patent application publication US 2024 / 0182747 Al, the disclosure of which is incorporated by reference herein in its entirety.

[0097] These biocompatible, resorbable ABA triblock copolyesters of polypropylene fumarate) (PPF)-b-polypropylene succinate) (PPS)-b-polypropylene fumarate) crosslink to form elastomers. These elastomers are well suited to the disclosed application and have not been previously applied in the fracture repair space. Unlike previously printed PPF materials that were co-crosslinked with non-degradable diethyl fumarate (DEF), recent advances in degradable, thiol-based crosslinkers control both network density (crosslinking) and elasticity (stoichiometry), which collectively govern degradation timelines and mechanical properties. Elastomeric materials can advantageously avoid overly stiff devices and allow for surgical handling and compatibility with rib curvature. Studies using these materials show a gradual loss of mechanical properties with time, and the post mortem histology show the device nor the degradation products induce an acute inflammatory response.

[0098] In one or more embodiments, the ABA triblock copolymer has the formula:orwhere each n is an integer from about 1 to about 20, each m is an integer from about 2 to about 70, and I is the residue of an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups.

[0099] In one or more embodiments, the ABA triblock copolymer may have the formula:where each n is an integer from about 1 to about 20, and each m is an integer from about 2 to about 70.

[0100] In one or more embodiments, the ABA triblock copolymer may have the formula:where each n is an integer from about 1 to about 20, each m is an integer from about 2 to about 70, and I is the residue of an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups.

[0101] In some other embodiments, the ABA triblock copolymer may have the formula:where each n is an integer from about 1 to about 20, each m is an integer from about 2 to about 70, and I is the residue of an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups.

[0102] In yet other embodiments, the ABA triblock copolymer may have the formula:In one or more embodiments, each n is an integer from about 1 to about 18, preferably an integer from about 1 to about 10, and more preferably an integer from about 1 to about 5 In some embodiments, each n is an integer from about 1 to about 15, in other embodiments, from about 3 to about 20, in other embodiments, from about 5 to about 20, in other embodiments, from about 8 to about 20, in other embodiments, from about 10 to about 20, in other embodiments, from about 12 to about 20, in other embodiments, from about 15 to about 20, and in other embodiments, from about 18 to about 20. In some embodiments, each n is 3. In some embodiments, each n is 5.

[0103] In various embodiments, each m is an integer from about 1 to about 70, preferably between 10 and 50, and more preferably between 10 and 30. In some embodiments, each m is an integer from about 1 to about 65, in other embodiments, from about 1 to about 50, in other embodiments, from about 1 to about 40, in other embodiments, from about 1 to about 30, in other embodiments, from about 1 to about 20, in other embodiments, from about 5 to about 70, in other embodiments, from about 15 to about 70, in other embodiments, from about 25 to about 70, in other embodiments, from about 35 to about 70, and in other embodiments, from about 50 to about 70. In some embodiments, each m is an integer from between 10 and 40. In some embodiments, each m is an integer from 10 and 25. In some embodiments, each m is an integer from 10 and 20.DUK.p.woooi2

[0104] In some of these embodiments, I is one or more C2 to C20 diol, C2 to C20 dithiol, ( '; to C20 dicarboxylic acid, or a combination thereof. In some other embodiments, I will comprise a C? to C20 alkyl or aryl group having one or more terminal hydroxyl group and one or more terminal carboxyl groups or thiol groups. In some other embodiments, I will comprise a C > to C20 alkyl or aryl group having one or more terminal carboxyl group and one or more terminal thiol groups. In some embodiments, I is the residue of an initiator selected from fumaric acid (FmA), succinic acid, 1,4-cyclohexanedicarboxylic acid (CHDA), cyclohexane dimethanol (CH DM), benzene dimethanol (BDM), cis-butane-2-diol (cis-BD), butyn-2-diol (2BD), 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol (HD), 1,8-octanediol. 1,10-decanediol, 1,12-dodecandiol (DD), or a combination thereof. In some embodiments, I is the residue of fumaric acid (FmA). In some other embodiments, I is the residue of 1,4-cyclohexanedicarboxylic acid (CHDA). In some other embodiments, I is the residue of cyclohexane dimethanol (CHDM). In some other embodiments, I is the residue of benzene dimethanol (BDM) In some other embodiments, I is the resid ue of cis-butane-2-diol (cis-BD). In some other embodiments, I is the residue of butyn-2-diol (2BD). In some other embodiments, I is the residue of hexanediol (HD). In some other embodiments, I is the residue of 1,12-dodecandiol (DD).

[0105] In various embodiments, the ratio of the degree of polymerization of said first A polymer block to the B polymer block to the second A polymer block is from 1:100:1 to 1:2:1, preferably from about 1:50:1 to about 1:2:1, and more preferably from about 1: 10: 1 to about 1:2:1. In some embodiments, the ratio of the degree of polymerization of the first A polymer block to the B polymer block to the second A polymer block is from about 1:30:1 to about 1:2:1. In some embodiments, the ratio of the degree of polymerization of the first A polymer block to the B polymer block to the second A polymer block is from about 1:20:1 to about 1:2:1. In some embodiments, the ratio of the degree of polymerization of the first A polymer block to the B polymer block to the second A polymer block is 1:5:1,

[0106] In various embodiments, the ABA triblock copolymer will contain from about 5 mol% to about 50 mol% fumarate units, in other embodiments from about 10 mol% to about 40 mol% fumarate units, and in other embodiments, from about 10 mol% to about 30 mol% fumarate units.

[0107] In some embodiments, the ABA block copolymer has a degree of polymerization of from about 10 to about 100.

[0108] In one or more embodiments, the ABA triblock copolymers will have a glass transition temperature (Tg) of from about-50 °C to about 10 °C (below 10 °C), preferably from about -40 °C to about 5 °C (below 5 °C), and more preferably from about -35 °C to about 0 °C (below 0 °C).

[0109] In one or more embodiments, the ABA triblock copolymers of the present invention will have a degradation temperature (Ta) of from about 100 °C to about 500 °C (above 100 °C), preferably from about 150 °C to about 450 °C (above 150 °C), and more preferably from about 200 °C to about 400 °C (above 200 °C).

[0110] In one or more embodiments, the ABA triblock copolymers will have a number average molecular mass ( i) of from about 500 Da to about 30000 Da, preferably from about 800 Da to about 25,000 Da, and more preferably from about 1000 Da to about 20000 Da.

[0111] In various embodiments, the ABA triblock copolymers will have a molecular mass distribution (Đm) of from about 1.01 to about 5.00, preferably from about 1.02 to about 4.50, and more preferably from about 1.03 to about 4.00.

[0112] Because the polymer making up the B block is saturated and does not provide an alkene unit for crosslinking, it is and will remain less stiff and more flexible than the PPF A blocks. As a result, the ABA triblock co-polymers of the present invention will have a lower viscosity that a PPF polymer of comparable size. In various embodiments, the ABA triblock co-polymers of the present invention will have a complex viscosity of from about 0.001 Pa-s to 20 Pa-s, preferably from about 0.01 Pa-s to about 10 Pa-s, and more preferably from about 0.05 Pa-s to about 5 Pa s.

[0113] In one or more of these embodiments, the ABA triblock copolymers may be formed as shown in Scheme 1 below:Scheme 1ROCOP of SA, MA and PO to form polypropylene fumarate) -b-polypropylene succinatefb-polypropylene fumarate) (PPF-b -PPSu-b-PPF) with fumaric acid (FmA), 1,4 -cyclohexanedicarboxylic acid (CHDA), cyclohexane dimethanol (CHDM), benzene dimethanol (BDM), cis-butene-2-diol (cBD), butyn-2-diol (BYD). hexanediol (HDO) a d decanediol (DD) as initiators.Reaction 1

[0114] In a first reaction, the selected acid anhydride is reacted with propylene oxide by ring opening polymerization in the presence of an initiator and a catalyst to form the B polymer block. In these embodiments, a selected acid anhydride, a first quantity of propylene oxide, an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups, a catalyst and a suitable solvent are added to a suitable reaction vessel under an inert atmosphere. While the first reaction may occur at ambient temperature, the vessel is preferably heated to a temperature of from about 40 °C to about 150 °C, preferably from about 50 °C to about 140 °C, and more preferably from about 60 °C to about 130 °C to facilitate the reaction. As will be apparent, the reaction vessel should not be heated to a temperature at or above the degradation temperature (Td) of the polymer being formed or any of the reagents. In some of these embodiments, the vessel is heated to a temperature of about 80 °C to facilitate the reaction.

[0115] The acid anhydride selected is not particularly limited provided that it will polymerize with propylene oxide by ring opening polymerization and docs not contain a cross-linkable alkene group. Suitable acid anhydrides may include, without limitation, succinic anhydride, glutaric anhydride (pentandioic anhydride), adaptic anhydride, pimelic anhydride, citraconic anhydride, itaconic anhydride, methyl itaconic anhydride, phenyl itaconic anhydride, phthalic anhydride, cyclohexane anhydride, cyclopropane anhydride, cyclopentane anhydride, cyclohexane anhydride, diglyolic anhydride and combinations thereof. As will be apparent, the selected acid anhydride should not be maleic anhydride, as that anhydride will be used to form the A blocks and, as set forth above, contains a cross-linkable alkene group. In one or more embodiments, the acid anhydride is succinic anhydride.

[0116] The initiator chosen is not particularly limited provided that it has at least two reactive hydroxyl, thiol or carboxylic acid groups and does not otherwise interfere with the reaction. In one or more embodiments, initiators may include C2 to C20 diols, C2 to C20 dithiols, and C2 to C20 dicarboxylic acids. Suitable initiators may include, without limitation, fumaric acid (FmA), succinic acid, 1,4-cyclohexnadicarboxylic acid (CHDA), cyclohexane dimethanol (CHDM), benzene dimethanol (BDM), cis-butane-2-diol (cis-BD), butyn-2-diol (BYD), 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol (HD), 1,8-octanediol, 1,10-decanediol, 1,12-dodecandiol (DD), or a combination thereof. In one or more embodiments, the initiator may have one or more of the following formulas:HDO DD

[0117] The versatility of the various potential initiators is an important advantage of the present invention. In some embodiments, the relatively higher portion of initiator residue compared to low molecular weight copolymer means that the initiator can significantly impactDUK. P. WOOOI2polymer properties, and, in turn, the 3D printed product. In some embodiments, orthogonal reactions, such as azidc-alkync click reaction in the case of butynediol, may be utilized to enable the post-polymerization modification of the ABA triblock copolymer to endow additional functionality before or after 3D printing.

[0118] The reaction solvent chosen should be a solvent for all of the reagents in the first reaction at the selected operating conditions, but the reaction solvent used is not otherwise limited, provided that the solvent chosen does not react with any of the reagents or inhibit the ring-opening polymerization reaction or denature the catalyst. In one or more embodiments, the reaction solvent will be an organic solvent. Suitable solvents may include, without limitation, toluene, hexane, heptane CH2CI2, CCI3, CCI4, and combinations thereof. In one or more embodiments, the reaction solvent for the first reaction is toluene.

[0119] The catalyst is not particularly limited provided that it will catalyze the ring opening polymerization of acid anhydrides and propylene oxide. Suitable catalysts include magnesium catalysts, including Mg! A and Mg(BHT) (THF), but Mg(BHT)2(THF)2 is preferred. In most embodiments, the quantity of catalyst added is sufficient to catalyze both the first and the second reaction. (See Scheme I, above).

[0120] The first reaction is allowed to proceed until substantially all (approximately 99%) of the selected acid anhydride has reacted and the allowed to cool to ambient temperature. The reaction should not, however, be allowed to consume 100% of the available acid anhydride and run to completion, as it may become difficult to restart the reaction to add the A blocks as described below. As would be apparent to those of skill in the art, the amount of time required for substantially all of the selected acid anhydride to react will depend, upon, among other things, the acid anhydride selected, the quantity of reactants, the reaction temperature, the reactivity of the initiator, the type and quantity of catalyst used and the re ction conversion.

[0121] As will be apparent and can be seen in scheme 1, the bifunctional initiators will initiate the ring opening polymerization of the acid anhydride and propylene oxide in two directions to form a B block intermediate polymer having two reactive ends capable continuing ring opening polymerization. In some embodiments, the acid anhydride is succinic anhydride as shown in Scheme 1, above, and B block intermediate polymer formed in the first reaction has the formula:where I is the residue of the divalent initiator used and each m is a number propylene succinate repeating units. In various embodiments, I can be the residue of any of the initiators described above and m can be as described above.

[0122] In some other embodiments, the B block intermediate polymer formed in the first reaction has the formula:where I is the residue of the divalent initiator used and each m is a number propylene succinate repeating units. In various embodiments, I can be the residue of any of the initiators described above and m can be as described above.

[0123] In some other embodiments, the B block intermediate polymer formed in the first reaction has the formula:100124] In still other embodiments, the B block intermediate polymer formed in the first reaction has the formula:where each m is a number propylene succinate repeating units. In various embodiments, m can be as described above.

[0125] In a second reaction, polypropylene maleate) is added to the ends of the B block intermediate polymer. (See, Scheme 1, above). In this reaction a second quantity of propylene oxide and maleic anhydride are added to the reaction vessel, which is then preferably again heated as set forth in the first reaction. The molar ratio of maleic anhydride to propylene oxide added to the vessel is preferably 1:1. Depending upon the type and quantity of catalyst used, it may be necessary to add additional catalyst in the second reaction, but this is not ordinarily required. In various embodiments, the catalyst for the second reaction is Mg(BHT)2(THF)2.

[0126] As can be seen in Scheme 1, both ends of the B block intermediate polymer have terminal carboxyl groups capable of initiating additional ring opening polymerization of the maleic anhydride and propylene oxide to form propylene maleate repeating units. The second reaction is allowed to proceed until substantially all (>99%) of the maleic anhydride has reacted. The polymer mixture is then quenched according to known methods and precipitated into a non-solvent to produce an ABA triblock copolymer intermediate having two poly(propylene maleate) A blocks. In some embodiments, the second reaction is quenched in chloroform and precipitated twice from hexanes. In the embodiments shown in Scheme 1, the selected anhydride is succinic anhydride and the resulting ABA triblock copolymer intermediate is a poly(propylene maleate-A-propylene succinate-h-propylene maleate) ABA triblock copolymer having the formula:where each n is an integer from about 1 to about 20, each m is an integer from about 2 to about 70, and I is the residue of an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups, as set forth above.

[0127] In some other embodiments, the resulting ABA triblock copolymer intermediate is an ABA triblock copolymer having the formula:where each n is an integer from about 1 to about 20, each m is an integer from about 2 to about 70, and I is the residue of an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups, as set forth above.

[0128] In some embodiments, I is the residue of an initiator selected from fumaric acid (FmA), succinic acid, 1,4-cyclohexanedicarboxylic acid (CHDA), cyclohexane dimethanol (CHDM), benzene dimethanol (BDM), cis-butane-2-diol (cis-BD), butyn-2-diol (2BD), 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol (HD), 1,8-octanediol, 1,10-decanediol, 1,12-dodecandiol (DD), and combinations thereof. In some embodiments, each n is an integer from about 1 to about 18, preferably an integer from about 1 to about 10, and more preferably an integer from about 1 to about 5 In some embodiments, each n is an integer from about 1 to about 15, in other embodiments, from about 3 to about 20, in other embodiments, from about 5 to about 20, in other embodiments, from about 8 to about 20, in other embodiments, from about 10 to about 20, in other embodiments, from about 12 to about 20, in other embodiments, from about 15 to about 20, and in other embodiments, from about 18 to about 20. In some embodiments, each n is 3. In some embodiments, each n is 5.

[0129] In these embodiments, the structure of the ABA triblock copolymer intermediate will, of course, depend upon the B block used to form the polymer. In some embodiments, the ABA triblock copolymer intermediate will have the formula:where each n is an integer from about 1 to about 20. each m is an integer from about 2 to about 70, as set forth above. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional non-disclosed ranges.

[0130] In some other embodiments, the ABA triblock copolymer intermediate will have the formula:where each n is an integer from about 1 to about 20, each m is an integer from about 2 to about 70, and I is the residue of an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups, as set forth above. In one or more of these embodiments, the variables m, n, and I may have any of the values described above for that variable.

[0131] Finally, in a third reaction, the ABA triblock copolymer intermediate described above is isomerized with an organic base, such as diethylamine (HNEt?), to form the corresponding fumarate polymer. In these embodiments, the BA triblock copolymer intermediate described above is dissolved in a suitable solvent and the organic base added. The solution is then refluxed under an inert atmosphere until the ABA triblock copolymer intermediate is completely isomerized. In the embodiments, shown in Scheme 1, above, the poly(propylene maleate -b-propylene succinate-b-propylene maleate) ABA triblock copolymer is isomerized to form the corresponding polypropylene fumarate-b-propylene succinate-b-propylene fumarate) ABA triblock copolymer having the formula:where each n, m, and I are as set forth above. In one or more of these embodiments, the mole ratio of maleic anhydride to succinic anhydride is from about 0.025 to about 15, preferably from about 0.05 to about 10, and more preferably from about 0,1 to about 2.

[0132] Once isomerization is complete, the ABA triblock copolymer may be recovered and purified using conventional methods known to those of skill in the art for this purpose.In some embodiments, the organic layer is washed with an aqueous monosodium phosphate solution and the polymer was recovered after drying under vacuum overnight (45 °C, 10 mTorr). One of ordinary skill in the art will be able to recover and purify the ABA triblock copolymer produced without undue experimentation.

[0133] In one or more embodiments, the ABA triblock copolymer as described above may be formed by reacting succinic anhydride, a first quantity of propylene oxide, an initiator selected from the group consisting of selected from the group consisting of fumaric acid (FmA), succinic acid, 1,4-cyclohexanedicarboxylic acid (CH DA), cyclohexane dimethanol (CHDM), benzene dimethanol (BDM), cis-butane-2-diol (cis-BD), bui.yn-2.~dio! (BYD), 1,4-butanediol, 1,5- pentanediol, 1,6-hexanediol (HD), 1,8-octanediol, 1,10-decanediol, 1,12-dodecandiol (DD), or acombination thereof and Mg(BHT 2 THF 2 catalyst to form a polypropylene succinate) polymer B block having a reactive first and second end; then reacting the polypropylene succinate) polymer B block with maleic anhydride, a second quantity of propylene oxide, and a catalyst to form a first and second polypropylene maleate) polymer A blocks covalently bonded to the first and second ends of said polypropylene succinate) B polymer block to form a polypropylene maleate-b-propylene succinate-b-propylene maleate) ABA triblock copolymer intermediate; and then isomerizing said polypropylene maleate-b-propylene succinate-b-propylene maleate) ABA block copolymer to form a polypropylene fumarate-b-propylene succinate-b-propylene fumarate) ABA triblock copolymer,

[0134] As set forth above, in some embodiments the linear or star-shaped polypropylene fumarate)-based copolymer used in the present invention will be a star-shaped PPF-based 3D printable copolymer having from 3 or 4 PPF arms connected to and extending outward from a central core. In the context of a polymer or copolymer, the terms “star polymer,” “star-shaped,” and “multi-arm” are used herein interchangeably to refer to a polymer or co polymer having 3 or more arms extending outward from a central core. As used herein, the term “arm” refers to a substantially linear polymer or copolymer chain that is bonded at one end to a central core and extends outward therefrom. As follows from this, the term “PPF ami” is used herein to refer to an arm, as defined above, comprising PPF and the term “PPM arm” is used herein to refer to an arm comprising PPM. As used herein, the temi “3D printable,” as applied to a polymer or copolymer, refers to a polymer or copolymer that can be used alone or with other ingredients such as a diluent, crosslinkers, diluents, photoinitiators, dyes, light attenuating agents, dispersants, emulsifiers, ceramics, BIOGLASS™, hydroxyapatite, p-tricalcium phosphate, and / or solvents to form a resin capable of be printed into a 3 dimensional structure using conventional additive manufacturing (3D printing) technologies. In one or more embodiments, the PPF-based star polymer may be any of those disclosed in US Patent No. 1 1,661,477, the disclosure of which is incorporated herein by reference in its entirety.

[0135] The star PPF copolymers of the present invention will, in various embodiments, have a substantially higher number average molecular mass (Mn) at printable viscosities when compared to linear PPF polymers and will also crosslink more quickly than a comparable linear PPF. As a result, the star PPF copolymers of the present invention allow for the formulation of 3D printableresins having less diluent, higher Mnand faster printing times than 3D printable resins prepared with conventional linear PPF polymers.

[0136] In various embodiments, these star-shaped PPF-based co polymers of the present invention may have from 3 to 6 arms, but will preferably have 3 or 4 arms. While the star-shaped PPF-based 3D printable copolymers of the present invention may in some embodiments have more than 6 arms, this is not preferred as it may create additional difficulties with crosslinking the polymer. In some embodiments, the star-shaped PPF-based co polymers of the present invention will have 3 arms. In other embodiments, the star-shaped PPF-based co polymers of the present invention will have 4 arms.

[0137] As will be apparent, the central core of the star-shaped PPF-based 3D printable copolymers of the present invention will comprise the residue of the multi-functional alcohol used to as the initiator and the number of arms on these polymers is likewise controlled by the number of alcohol (i.e. hydroxyl) functional groups present on the multi-functional alcohol initiator. As used herein, the term “residue(s)” is used to refer generally to the portion of a monomer or other chemical unit that has been incorporated into a polymer or other large molecule. By way of example, in one or more embodiments, the terms “4-arm star” and “4-arm star-shaped” are used to refer to PPF copolymers with 4 arms derived from the ROCOP of MAn with PO initiated by an alcohol having four available hydroxyl groups, such as meso-erythritol, with each of the four hydroxyl groups initiating ROCOP of one ami of the 4-arm star polymer and the remainder of the alcohol molecule forming the core. Similarly', the terms “5-arm star” and “5-arm star-shaped” refer to PPF copolymers with 5 arms derived from the ROCOP of MAn with PO initiated by an alcohol having five available hydroxyl groups, such as adonitol, with each of the five hydroxyl groups initiating ROCOP of one arm of the 5-ami star polymer and the remainder of the alcohol molecule forming the core.

[0138] As set forth above, it has been found that multi-functional alcohol molecules can be used to initiate of ROCOP of MAn with PO in the presence of a magnesium catalyst, thereby forming the star-shaped PPF-based 3D printable copolymers of the present invention. The initiating alcohol forming the core of the star-shaped PPF-based 3D printable copolymers of the present invention is not particularly limited provided that it has three or more available hydroxyl functional groups and is capable of initiating ROCOP of maleic anhydride (MAn) monomers, with propylene oxide (PO) monomers, in the presence of a magnesium catalyst. Suitable multi-functional alcohol initiators, may include, without limitation, glycerol (propane- 1,2,3-triol), meso-crythritol ((2 / ?,35’)-butanc-l,2,3,4-tctrol), pcntacrythritol (2,2-bis(hydroxymcthyl)propanc-l,3-diol), theitol ((2J?,37?)-Butane-l,2,3,4-tetrol), arabitol ((22?,4J?)-pentane-l,2,3,4,5-pentol) xilitol ((2J?,3r,4S)-pentane-l, 2.3,4, 5-pentol), adonitol ((27?, 3.y,46)-pentane-l, 2,3, 4, 5-pentol), fucitol ((2 / ?,3S,4J?,55)-hexane-l,2,3,4,5-pentol), and sorbitol ((2S,3R,4R,5 )-hexane-l,2,3,4,5,6-hexol). In some embodiments, the multi-functional alcohol initiator may be a sugar based alcohol. In one or more embodiments, the multi-functional alcohol initiator may be selected from the family of sugar based alcohols that includes meso-erythritol and adonitol. As set forth above, the meso-erythritol molecule bears four hydroxyl functional groups and it has been found that all hydroxyl groups of we o-erythritol are able to initiate the ROCOP of MAn with PO with a controlled manner to produce defined 4-arm star-shaped PPF copolymer. Similarly, the adonitol molecule bears five alcohol moieties and it has likewise been found that all hydroxyl groups of adonitol are able to initiate the copolymerization of MAn with PO with a controlled manner to produce defined 5 -ami star-shaped PPF copolymer.

[0139] In one or more embodiments, the multi-functional alcohol initiator may include one or more other functional groups for post polymerization functionalization as described in international application publication number WO 2018 / 144849, the disclosure of which is incorporated herein by reference in its entirety,

[0140] In various embodiments, the magnesium catalyst may be Mg(BHT)2 THF)2 or MgEt2, but is preferably Mg(BHT)?(THF)2.

[0141] In one or more embodiments, the arms of the PPF-based 3D printable star-shaped polymers of the present invention will comprise the isomerized residues a maleic anhydride monomer and residues of propylene oxide monomer. As follows, the terms “residues of propylene oxide monomer,” “residues of propylene oxide” and “propylene oxide residue(s)” are all used herein to refer to the portion(s) of propylene oxide monomer incorporated into the poly(propylene fumarate) copolymers. Similarly, the terms “isomerized residue of a maleic anhydride monomer,” “isomerized residues of maleic anhydride monomer,” “isomerized residues of a maleic anhydride,” “isomerized residues of maleic anhydride,” and “isomerized maleic anhydride residues” are used interchangeably to refer to residues of the maleic anhydride monomer incorporated into the polypropylene fumarate) copolymer of the present invention in which the carbon-carbon double bond has subsequently been isomerized from the cis (maleate) configuration to the trans (fumarate)configuration during formation of the polypropylene fumarate) copolymer from the polypropylene maleate) copolymer intermediate.

[0142] In some embodiments, the arms of the PPF-based 3D printable star-shaped polymers used in the present invention may further comprise succinic anhydride residues as described in U. S. Patent No. 12,258,443, the disclosure of which is incorporated herein by reference in its entirety. In some embodiments, the arms of the PPF-based 3D printable star-shaped polymers of the present invention may further comprise residues of functionalized propylene oxide monomers as described in US Patent No. 11,499,008, the disclosure of which is incorporated herein by reference in its entirety.

[0143] In some other embodiments, the arms of the multi-aim PPF copolymers used in the present invention may comprise block copolymers of lactones and PPF as described in US Patent No. 12, 187,844, the disclosure of which is incorporated herein by reference in its entirety. In these embodiments, the magnesium catalyst is first used to catalyze the formation a lactone block by ring opening polymerization of one or more lactone, and then to catalyze formation of a PPF block by ROCOP of MAn with PO as described above. It has been found that multi-arm PPF copolymers have a lower viscosity and comparable absorption than linear PPF copolymer.

[0144] As set forth above, the degree of polymerization and dispersity of the star-shaped PPF polymers used in the present invention must be carefully controlled to obtain polymers having the desired viscosity. As will be understood by those of ordinary skill in the art, the “degree of polymerization” (DP) generally refers to the number of monomer units in a macromolecule, polymer or oligomer molecule. As used herein, the degree of polymerization refers to the total number of propylene maleate or propylene fumarate units, respectively, forming the star-shaped PPM copolymer intermediate or star-shaped PPF copolymer of the present invention. As will be apparent, the DP of any one of the arms of the star-shaped PPF copolymer of the present invention (the “degree of polymerization by arm” “DP by arm” or “number of repetitive units by arm”) will be the total DP for the star copolymer divided by the number of amis. So, by way of example, a 4- ann shaped PPF copolymer of the present invention having a total DP of 40, would have a DP by arm of 10. In some embodiments, each polylpropydene fumarate) arm extending from a multifunctional alcohol initiator copolymer has a degree of polymerization of from about 10 to about 50.

[0145] In one or more of embodiments, the copolymers used in the present invention have total DPs from about 3 to about 650, preferably from about 3 to about 325, and more preferably from about 3 to about 200. In some embodiments, the copolymers of the present invention will have a total DP of from about 3 to 5. in other embodiments, from about 3 to 10, in other embodiments, from about 3 to 15, in other embodiments, from about 3 to 20, in other embodiments, from about 3 to 30, in other embodiments, from about 3 to 50, in other embodiments, from about 3 to 100, in other embodiments, from about 3 to 200, in other embodiments, from about 10 to 200, in other embodiments, from about 20 to 200, in other embodiments, from about 40 to 200, in other embodiments, from about 80 to 200. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional non-disclosed ranges.

[0146] In one or more embodiments, the star-shaped PPF copolymer composition used in the present invention will have a number average molecular weight (Mn) of from about 0.5 kDa to about 100 kDa, preferably from about 0.5 kDa to about 50 kDa, and more preferably from about 0.5 kDa to about 30 kDa, as calculated from NMR spectroscopy or measured by size exclusion chromatography (SEC) or gel penneation chromatography (GPC). In some embodiments, the starshaped PPF copolymer composition used in the present invention will have a number average molecular weight (Mn) of from about 0.5 kDa to about 80 kDa, in other embodiments, from about 0.5 kDa to about 60 kDa, in other embodiments, from about 0.5 kDa to about 40 kDa, in other embodiments, from about 0.5 kDa to about 20 kDa, in other embodiments, from about 5 kDa to about 100 kDa, in other embodiments, from about 10 kDa to about 100 kDa, in other embodiments, from about 20 kDa to about 100 kDa, in other embodiments, from about 30 kDa to about 100 kDa, and in other embodiments, from about 50 kDa to about 100 kDa, as calculated from NMR spectroscopy or measured by size exclusion chromatography (SEC) or gel permeation chromatography (GPC).

[0147] In one or more of these embodiments, the star copolymer used in the present invention will have a molecular mass distribution (£)m) of from about 1 to about 2, preferably from about 1 to about 1.7, and more preferably from about 1 to about 1.4. In some embodiments, the star copolymer composition of the present invention will have a D,„ of from about 1.0 to about 2.0, in other embodiments, from about 1.2 to about 2.0, in other embodiments, from about 1.4 to about 2.0, in other embodiments, from about 1.6 to about 2.0, in other embodiments, from about 1.8 to about 2.0, in other embodiments, from about 1.0 to about 1.9, in other embodiments, from about1.0 to about 1.7, in other embodiments, from about 1.0 to about 1.5, and in other embodiments, from about 1.0 to about 1.3. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional non-disclosed ranges. As used herein, the terms “dispersity,” “polydispersity,” “molecular mass distribution,” and “molecular weight distribution” are used interchangeably to refer to the ratio of the weight average molecular weight to the number a verage molecular weightof a material.1001481 In one or more embodiments, the star-shaped PPF copolymer used in the present invention have an average complex viscosity of from about 0.1 Pa-s to about 10.0 Pa-s, preferably from about 1.0 Pa-s to about 5.0 Pa-s, and more preferably from about 3.0 Pa-s to about 5.0 Pa-s, as measured by a rheometer. In some embodiments, the star-shaped PPF copolymer compositions of the present invention have an average complex viscosity of from about 0.5 Pa-s to about 10.0 Pa-s, in other embodiments, from about 1.0 Pa-s to about 10.0 Pa-s, in other embodiments, from about 2.0 Pa-s to about 10.0 Pa-s, in other embodiments, from about 3.0 Pa-s to about 10.0 Pa-s, in other embodiments, from about 5.0 Pa-s to about 10 Pa-s, in other embodiments, from about 0.1 Pa-s to about 8.0 Pa-s, in other embodiments, from about 0.1 Pa-s to about 6.0 Pa-s, in other embodiments, from about 0.1 Pa s to about 4.0 Pa s, in other embodiments, from about 0.1 Pa s to about 2.0 Pa-s, as measured by a rheometer. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional non-disclosed ranges.

[0149] In one or more embodiments, the star-shaped PPF copolymer composition used in the present invention may have the following formula:where m is the degree of polymerization by arm (also named number of repetitive units by arm) from about 1 to about 200, n is a number of arms greater than 2 and less than 6, and the “core” structure comprises the residue of the multi-functionalized alcohol initiator used to form the polymer. In some embodiments, n is from 3 or 4. In some embodiments, n is 3. In some embodiments, n is 4. In some embodiments, the core comprises the residue of meso-erythritol and n is 4.

[0150] In one or more embodiments, the star-shaped PPF polymer used in the present invention has the formula:here each m is an integer from about 10 to about 50.

[0151] In various embodiments, the the multi-arm PPF star polymers may be formed as shown in Scheme 2, below.Scheme 2Star-shaped polypropylene maleate)IsomerizationStar-shaped polypropylene fumarate)

[0152] As will be apparent to those of skill in the art, the degree of polymerization may be controlled by controlling the available moles of initiator and / or the time and temperature of thepolymerization reaction. In embodiments where the polymerization reaction is allowed to go to completion (where substantially all of the monomers have been reacted), the degree of polymerization may be controlled by controlling the available moles of initiating alcohol as a function of the total moles of available monomer. In some other embodiments, the degree of polymerization may be controlled by controlling ratio of the moles of initiating alcohol functions to both the moles of propylene oxide and the moles of maleic anhydride used to form the copolymer. In one or more of these embodiments, the maleic anhydride and propylene oxide are combined, with a 1:1 molar ratio, in a suitable sealed reaction vessel with an initiating alcohol, MgCBHThfTHF)?., and a suitable solvent. One of ordinary skill in the art will be able to select, configure, or create a suitable reaction vessel without undue experimentation. In one or more of these embodiments, maleic anhydride, propylene oxide and initiator are combined at a molar ratio of maleic anhydride to propylene oxide to alcohol initiating function of from about 200:200:1 to about 3:3:1.

[0153] Suitable solvents for this purpose are not particularly limited provided that the reaction proceeds and may include, without limitation, toluene, pentane, hexane, heptane, octane, THF, or a combination thereof. One of ordinary skill in the art will be able to select a suitable reaction solvent without undue experimentation.

[0154] In these embodiments, the combination of reactive species is heated until substantially all of the maleic anhydride and propylene oxide have reacted to form the star-shaped polypropylene maleate) copolymer intermediate. In one or more embodiments, the star-shaped polypropylene maleate) copolymer intermediate may have the following formula:where m is the degree of polymerization by arm (also named number of repetitive units by arm) from about 1 to about 200, n is a number of anus greater than 2 and less than 6, and the core comprises the residue of the multi-functionalized initiator used to form the copolymer. In some embodiments, n is from 3 to 5. In some embodiments, n is 3. In some embodiments, n is 4. In some embodiments, the core comprises the residue of meso-erythritol and n is 4.

[0155] In some embodiments, star-shaped polypropylene fumarate) copol ymer has a degree of polymerization of from about 40 to about 200.

[0156] In one or more of these embodiments, the sealed reaction vessel containing the reactive mixture is heated to a temperature of from about 40°C to about 80°C for from about 1 hour to about 200 hours (or until essentially all of the monomer is consumed) to produce a star-shaped cis-isomer polypropylene maleate) intermediate of the star-shaped hwx-isomer polypropylene fumarate) copolymer composition of the present invention. In some embodiments, the sealed reaction vessel is heated to a temperature of from about 40°C to about 75°C, in other embodiments, from about 40°C to about 70°C, in other embodiments, from about 40°C to about 65°C, in other embodiments, from about 40°C to about 60°C, in other embodiments, from about 50°C to about 80°C, in other embodiments, from about 60°C to about 90°C, and in other embodiments, from about 70°C to about 100°C. In some embodiments, the sealed reaction vessel is heated for from about 1 hour to about 200 hours, in other embodiments, in other embodiments from about 1 hour to about 150 hours, from about 1 hour to about 100 hours, in other embodiments, from about 1 hour to about 48 hours, in other embodiments, from about 1 hour to about 24 hours. In other embodiments, from about 24 hours to about 200 hours, in other embodiments, from about 48 hours to about 200 hours, in other embodiments, from about 150 hours to about 200 hours, and in other embodiments, from about 100 hours to about 200 hours.

[0157] The star-shaped polypropylene maleate) copolymer intermediate may be recovered by any suitable method known in the art for that purpose. In some embodiments, the star-shaped polypropylene maleate) copolymer intermediate maybe recovered by precipitation into an excess of a non-solvent for the star-shaped polypropylene maleate) copolymer intermediate such as diethyl ether, isopropyl alcohol, ethyl alcohol (also named ethanol), hexane, or a combination thereof.

[0158] The recovered star-shaped polypropylene maleate) copolymer intermediate is then dried to remove remaining solvent. The star-shaped polypropylene maleate) copolymer intermediate may be dried using any suitable method known in the art including, but not limited to vacuum evaporation, air drying, rotary evaporation, or a combination thereof.

[0159] As set forth above, the cis double bonds in the maleic anhydride residues of the starshaped polypropylene maleate) copolymer intermediate are next isomerized to arrive the star¬ shaped polypropylene fumarate) copolymer described above. As used herein, the terms“isomerize” and “isomerization” refer broadly to the conversion of the cfr-isomer (PPM) to its frnns-isomcr (PPF) form or, in the context of a chemical reaction or process (an “isomerization reaction”) to a reaction or process that converts the czs-isomer (PPM) to its rra s-isomer (PPF) form. And as set forth above, the terms “isomerized residue of a maleic anhydride monomer,” “isomerized residues of maleic anhydride monomer,” “isomerized residue of a maleic anhydride” and “isomerized residues of maleic anhydride” specifically refers to one or more residues of the maleic anhydride monomer used to form the star-shaped PPF-based 3D printable polymer composition of the present invention wherein the double bond has been isomerized from the cis (maleate) configuration to the trans (fumarate) configuration during formation of the polypropylene fumarate) copolymer from the star-shaped polypropylene maleate) copolymer intermediate, as described below. While the isomerization of the star-shaped polypropylene maleate) copolymer intermediate does result in some other changes to the polymer, it should be understood that most general characteristics of the star-shaped PPF-based 3D printable polymer composition of the present invention, such as the approximate Mn, Đm, and Tgranges, are determined in the initial ROCOP reaction and do not change during the isomerization reaction.

[0160] In one or more of these embodiments, the star-shaped polypropylene maleate) copolymer intermediate is first dissolved in a suitable organic solvent. Suitable solvents for this purpose are not particularly limited provided that the reaction proceeds and may include, without limitation, chloroform, dichloromethane or a combination thereof. In one or more embodiments, the star-shaped polypropylene maleate) copolymer intermediate is dissolved in chloroform. Next, a quantity of an organic base, such as diethylamine or pyridine, is added to the solution and it is heated to reflux temperature under an inert atmosphere to produce the star-shaped polypropylene fumarate) copolymer of the present invention.

[0161] In some of these embodiments, the solution is heated to a reflux temperature under an inert atmosphere for from about 1 to about 48 hours (or until substantially all of star-shaped polypropylene maleate) copolymer intermediate has isomerized) to produce the star-shaped polypropylene fumarate) copolymer of the present invention. In some embodiments, the solution is refluxed for from about 1 hours to about 48 hours, in other embodiments, from about 1 hours to about 36 hours, in other embodiments, from about 1 hours to about 30 hours, in other embodiments, from about 1 hours to about 24 hours, in other embodiments, from about 6 hours to about 48 hours, in other embodiments, from about 12 hours to about 48 hours, in other embodiments, from about18 hours to about 48 hours, in other embodiments, from about 24 hours to about 48 hours, and in other embodiments, from about 36 hours to about 48 hours to produce the star-shaped polypropylene fumarate) copolymer of the present invention.

[0162] Finally, the star-shaped polypropylene fumarate) produced may be washed with a sodium phosphate aqueous solution to remove residual monomers and base, and then dried to recover the star-shaped polypropylene fumarate) copolymer. Finally, the star-shaped polypropylene fumarate) copolymer may be purified by any suitable method known in the art for that purpose. In some of these embodiments, the star-shaped polypropylene fumarate) copolymer is purified by repeated washing in an excess of sodium phosphate aqueous solution or a suitable acid solution, combining the organic layers, and drying the resulting polymer under vacuum to produce the purified polymer.

[0163] As set forth above, 3D printable PPF-based polymer resin further comprises a multifunctional thiol crosslinker. As will be apparent, the thiol functional groups on the multi-functional thiol crosslinker will, under the proper conditions, react with the alkene fumarate double bonds to crosslink the polymer.

[0164] In various embodiments, the multi-functional thiol crosslinker will have from 2 to 5 reactive thiol groups. In some embodiments, the multi-thiol crosslinker will have from 2 reactive thiol groups. In other embodiments, the multi-thiol crosslinker will have from 3 reactive thiol groups. In some embodiments, the 3D printable polymer resin may contain two or more different multi-thiol crosslinkers. Suitable multi-functional thiol crosslinkers may include, without limitation, ethylene glycole bis-mercaptoacetate, 3,6-dioxa-l,8-octanedithiol, pentaerythritol tetrakis(3 -mercaptopropionate), trimethylolpropane tris(3 -mercaptopropionate), 2,2 ’-thiodiethanethiol, ethyleneglycol dithiol, tetra(ethylene glycol) dithiol, hexapthylene glycol) dithiol, poly(ethylene glycole) dithiol, 1,6-hexanedithiol, 1,8-oxtanedithiol, 1,9-nonanedi thiol, 1,11 -undecan edithol, 1,16-hexandecanedithiol. and combinations thereof.

[0165] In one or more of these embodiments, the 3D printable polymer resin of the present invention will comprise a polypropylene fumarate-b-propylene succinate-b-propylene fumarate) ABA triblock copolymer and at least one multi-thiol crosslinker having three reactive thiol groups. In some other embodiments, the 3D printable polymer resin of the present invention will comprise a star-shaped PPF copolymer, as described above, and at least one multi-thiol crosslinker having three reactive thiol groups.

[0166] In some embodiments, the thiol-based crosslinker comprises trimethylolpropane tris(3-mercaptopropionate), trimcthylolpropanctTis(3-mcrcaptopropionatc), 2-[2,2-Bis[2-(3-sulfanylpropanoyloxy)ethoxymethyl] butoxy] ethyl 3 -sulfanylpropanoate, THIOCURE™ 332 (CAS:674786-83-5) and THIOCURE™ 333 (CAS:345352-19-4), for the 700 and 1300 molecular weights, respectively. Alternative names for THIOCURE™ 332 and 333 are ETTMP-700 and ETTMP-1300, respectively, and combinations thereof. In one or more embodiments, the thiol-based crosslinker has a formula selected from:

[0167] In some embodiments, the 3D printable PPF-based copolymer resin of the present invention will have a ratio of fumarate groups in the PPF-based copolymer to reactive thiol groups on said multi-thiol crosslinker of from about 50 to about 1, in other embodiments, from about 30 to about 1, in other embodiments, from about 20 to about 1, in other embodiments, from about 10 to about 1, in other embodiments, from about 5 to about 1, and in other embodiments, from about 2 to about 1. In some embodiments, the ratio of available alkene groups in said linear or star¬ shaped poly(propylene fumarate)-based copolymer to available thiol groups in said thiol-based crosslinker in said resin is from about 3:1 to about 40:1. In some embodiments, the ratio of available alkene groups in said linear or star-shaped polypropylene fumarate)-based copolymer to available thiol groups in said thiol-based crosslinker in said resin is about 20:1.

[0168] In some embodiments, the thiol-based crosslinker comprises from about 0.5 to about 10 mole percent of said resin. In sonic embodiments, the thiol-based crosslinkcr comprises from about 1 to about 10 mole percent, in other embodiments, from about 2 to about 10 mole percent, in other embodiments, from about 4 to about 10 mole percent, in other embodiments, from about 6 to about 10 mole percent, in other embodiments, from about 0.5 to about 8 mole percent, in other embodiments, from about 0.5 to about 6 mole percent, in other embodiments, from about 0.5 to about 4 mole percent, and in other embodiments, from about 0.5 to about 2 mole percent of said resin

[0169] In various embodiments, the 3D printable resin will also include an organic solvent or diluent and a pho to initiator to facilitate crosslinking the polymer during the printing process. The choice of organic solvent is not particularly limited provided, of course, that it does not react with or damage the PPF-based polymer or crosslinker being used. One of ordinary skill in the art will be able to select a suitable diluent without undue experimentation. Suitable diluents may include, without limitation, ethyl acetate, acetone, dioxane, and combinations thereof.

[0170] To make the 3D printable resin, the PPF based copolymer being used is diluted copolymer described above is first dissolved in a suitable solvent until the resulting solution has a complex viscosity of from about 0.001 Pa sec to about 10 Pa-sec as measured by shear rheology. In these embodiments, the multi-thiol crosslinker or crosslinkers and photoinitiator are then added to form the resin. The final resin must have a complex viscosity within the specifications of the specific 3D printer being used. It may be necessary in some embodiments to add additional solvent to obtain the recommended viscosity for the particular 3D printer being used.

[0171] In one or more embodiments, the diluent comprises from about 10 wt.% to about 50 wt.% of said resin. In some embodiments, the diluent comprises from about 30 wt.% of said resin. In various embodiments, the diluent is selected from the group ethyl acetate, acetone, dioxane, and combinations thereof,

[0172] In one or more embodiments, the 3D printable resin of the present invention will comprise one or more of the star PPF copolymers described above and ethyl acetate as a diluent. In some embodiments, the 3D printable resin of the present invention will comprise two or more different star PPF copolymers. In some embodiments, the photo-crosslinkable 3D printable resin of the present invention may also comprise one or more linear PPF. In various embodiments, the 3D printable resin of the present invention will comprise from about 50 wt.% to about 70% of thestar PPF copolymers described above. In some embodiments, 3D printable resin of the present invention will comprise from about 55 wt.% to about 70%, in other embodiments, from about 60 wt.% to about 70 %wt.%, in other embodiments, from about 65 wt.% to about 70 %wt.%, in other embodiments, from about 50 wt.% to about 65 %wt.%, in other embodiments, from about 50 wt.% to about 60 %wt.%, and in other embodiments, from about 50 wt.% to about 55 %wt.% of the star PPF copolymers described above.100173] In one or more embodiments, the 3D printable resins of the present invention having from about 30% to about 50% of diluent by weight will have an average complex viscosity of from about 0.01 Pa-s to about 25.0 Pa-s, preferably from about 2.0 Pa-s to about 5.0 Pa-s, and more preferably from about 0.1 Pa-s to about 1.5 Pa-s, as measured by a rheometer. In some embodiments, these photo-crosslinkable 3D printable resins (comprising from about 30% to about 50% of diluent by weight) will have an average complex viscosity of from about 0.5 Pa-s to about 25.0 Pa-s, in other embodiments, from about 1.0 Pa-s to about 25.0 Pa-s, in other embodiments, from about 2.0 Pa-s to about 25.0 Pa s, in other embodiments, from about 4.0 Pa-s to about 25.0 Pa-s, in other embodiments, from about 8.0 Pa-s to about 25 Pa s, in other embodiments, from about 0.1 Pa-s to about 20.0 Pa-s, in other embodiments, from about 0.1 Pa-s to about 15.0 Pa-s, in other embodiments, from about 0.1 Pa-s to about 10.0 Pa s, in other embodiments, from about 0.1 Pa-s to about 4.0 Pa-s, as measured by a rheometer. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional nondisclosed ranges.

[0174] The photoinitiators are not particularly limited but must be: capable of generating radicles at the wavelengths of light used by the 3D-printing device (ordinarily 254-450 nm) being used, soluble in the resin being used, and compatible with the both the 3D printed PPF matrix and its component parts at the concentrations to be used. As will be appreciated by those of skill in the art, the choice of pho to initiator is often dictated by the requirements of the 3D printer being used. Suitable photoinitators may include, without limitation, phenylbis(2,4,6-trimethylbenzoyljphosphine oxide (BAPO), IRGACURE™ 819 / BAPO (BASF, Florham Park, NJ), IRGACURE™ 784 (BASF, Florham Park, NJ), IRGACURE™ 2959 (BASF, Florham Park, NJ), and combinations thereof. In some embodiments, the photoinitiator is selected from the group consisting of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO).

[0175] As set forth above, the resin may also comprise a photoinhibitor to prevent unwanted side reactions. The photoinhibitor is not particularly limited and any suitable photoinitiator may be used provided that it does not it does not react with or damage the PPF-based polymer or crosslinker being used. In some embodiments, the photoinhibitor oxybenzone (HMB).

[0176] As set forth above, the resin of the present invention will contain one or more filler nanoparticles to improve the physical properties of the 3D printed resin and / or stimulate bone growth and / or regrowth. In various embodiments, filler nanoparticles are selected from hydroxyapatite (HAp), strontium carbonate, tricalcium phosphate, barium phosphate and combinations thereof.

[0177] In some embodiments, the filler nanoparticles comprises from about 1 to about 20 weight percent of said resin. In some embodiments, the filler nanoparticles comprises from about 2 to about 20 wt.%, in other embodiments, from about 4 wt. % to about 20 wrt. %, in other embodiments, from about 6 wt. % to about 20 wt. %, in other embodiments, from about 8 wt.% to about 20 wt. %, in other embodiments, from about 10 wt. % to about 20 wt. %, in other embodiments, from about 15 wt. % to about 20 wt. %, in other embodiments, from about I wt.% to about 15 wt.%, in other embodiments, from about 1 wt. % to about 10 wt. %, and in other embodiments, from about 1 wt. % to about 5 wt. % of said resin. In some of these embodiments, the filler nanoparticles will comprise about 10 weight percent of said resin. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional non-disclosed ranges.

[0178] In various embodiments, the plurality of filler nanoparticles have a mean particle size of from about 100 nm to about 1000 nm. In some embodiments, the plurality of filler nanoparticles have a mean particle size of from about 200 nm to about 1000 nm, in other embodiments, from about 300 pm to about 1000 uni, in other embodiments, from about 400 pm to about 1000 pm, in other embodiments, from about 600 pm to about 1000 pm, in other embodiments, from about 700 pm to about 1000 pm, in other embodiments, from about 100 pm to about 800 pm, in other embodiments, from about 100 pm to about 600 pm, in other embodiments, from about 100 pm to about 400 pm, in other embodiments, from about 100 pm to about 300 pm, and in other embodiments, from about 100 pm to about 200 pm. In some embodiments, the plurality of filler nanoparticles are hydroxyapatite (HAp) nanoparticles having a mean particle size of from about100 nm to about 500 nm. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional non-discloscd ranges.

[0179] In some embodiments, the 3D printable PPF-based copolymer resin of the present invention may also include additives commonly used in 3D printing resins including, but not limited to, such things as dyes, light attenuating agents, radical scavengers, dispersants, emulsifiers, ceramics, (bioglass) hydroxyapatite, [3-tricalcium phosphate, and combinations thereof. The additives are not particularly limited provided that they do not quench the radicals needed for crosslinking of the 3-D printable resin.

[0180] In some embodiments, the resin for use in a resorbable 3D printed osteosynthetic apparatus for rib fracture repair comprising: a linear or star-shaped poly(propylene fumarate)-based copolymer comprising at least one of an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block and a star-shaped polypropylene fumarate) copolymer; a thiol-based crosslinker; and a plurality of filler nanoparticles. In some embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer comprises from about 50 wt.% to about 90 wt.% of said resin. In some of these embodiments, the linear or star-shaped poly(propylene fumarate)-based copolymer comprises from about 50 wt.% to about 90 wt.%, in other embodiments, from about 60 wt. % to about 90 wt. %, in other embodiments, from about 70 wt. % to about 90 wt. %, in other embodiments, from about 80 wt.% to about 90 wt. %, in other embodiments, from about 50 wt. % to about 80 wt. %, in other embodiments, from about 50 wt. % to about 70 wt. %, and in other embodiments, from about 50 wt.% to about 60 wt.% of said resin. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional non-disclosed ranges.

[0181] In some embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer comprises about 70 wt.% of said resin. In various embodiments, the resin has a complex viscosity of less than 50 Pa- sec. In some of these embodiments, the resin of the present invention has a complex viscosity of from about 5 Pa- sec to about 15 P -sec. In some embodiments, the resin of the present invention has a complex viscosity of from about 6 Pa -sec to about 15 Pa- sec, in other embodiments, from about 7 Pa-s to about 15 Pa s, in other embodiments, from about 8 Pa-s to about 15 Pa-s, in other embodiments, from about 9 Pa s to about 15 Pa-s, in other embodiments, from about 10 Pa-s to about 15 Pa-s, in other embodiments, from about 5 Pa-s to about 13 Pa s, in other embodiments, from about 5 Pa-s to about 11 Pa-s, in other embodiments, from about 5 Pa-sto about 10 Pa s, and in other embodiments, from about 5 Pa s to about 8 Pa-s. Here, as well as elsewhere in the specification and claims, individual range values can be combined to form additional non-disclosed ranges. In some embodiments, the resin has a complex viscosity suitable for 3D printing by Continuous Liquid Interface Production (CLIP) photochemical printing.

[0182] In one or more embodiments, the photo-crosslinkable 3D printable resins are formed by dissolving one or more of the star PPF copolymers described above in from about 30 wt.% to about 50wt% diluent to form a PPF solution containing from about 50 wt.% to about 70 wt.% of the star PPF copolymers described above. The various other resin components described above (e.g. photoinitiators, dyes, light attenuating agents, dispersants, emulsifiers, ceramics, bioglass, hydroxyapatite, p-tricalcium phosphate, crosslinkers and / or solvents) may be added to the 3-D printable resin at any time prior to crosslinking of the PPF polymer and are mixed evenly throughout the resin, as is known in the art. In some embodiments, a PPF solution having from about 50 wt.% to about 70 wt.% of the star PPF copolymers described above is first prepared. Next, two photoinitiators, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO) and IRGACURE™ 784, and a radical scavenger oxybenzone (HMB) are added to the PPF solutions at 3 %, 0.4 % and 0.7 % by weight, respectively and mixed evenly throughout the resin, following a previously reported protocol with modification in the mixing ratio of copolymer and a diluent to obtain a 3D printable star PPF resin. See, J. P, Fisher, D. Dean and A. G. Mikos, Biomaterials, 2002, 23, 4333-4343 and Y. Luo, C. K. Dolder, J. M. Walker, R. Mishra, D. Dean and M. L. Becker, Biomacromolecules, 2016, 17, 690-697. the disclosures of which are incorporated herein in their entirety.

[0183] The photo-crosslinkable 3-D printable resins of the present invention be printed using conventional additive manufacturing (3D printing) techniques, such as stereolithography or continuous digital light processing (cDLP) techniques and photocrosslinked to form 3D printed structures having virtually any shape. Any suitable light-based 3D printer may be used. Suitable 3-D printers may include, without limitation, Carbon3D printers (CARBON3D™, Redwood City, CA), PERFACTORY™ P3 3D printer (EnvisionTEC, Dearborn, Ml), Micro HR 279 printer EnvisionTEC (Dearborn. MI. USA), photocentric stereolithographic or photochemical 3D printers. In some embodiments, photo-crosslinkable 3-D printable resins of the present invention be printed using Micro HR 279 (EnvisionTEC, Dearborn, MI, USA) printer using a 405 nni LED UV light projector with an irradiance of 225 mW dm⁻².

[0184] In various embodiments, the star PPF printed structure may be formed by first generating a set of instructions for 3-D printing a desired structure and sending those instructions to a suitable 3-D printer. In some of these embodiments, the set of instructions may comprise a computer assisted design (CAD) file generated using suitable computer software that are readable by the 3D printer to be used. In some embodiments, the design files may be created using SolidWorks software (Dassault Systems SolidWorks Corp., Waltham, MA). In some embodiments, the CAD models were sliced digitally into layers using the Perfactory software suite prior to manufacturing. The Perfactory P3 is an inverted system that projects upward through a transparent glass plate into a reservoir containing the resin. In one or more embodiments, the CAD or other computer file containing instructions for printing the star PPF printed structure may be generated as set forth in U. S. Patent Nos. 6,849,223, 7,702,380, 7,747,305, 8,781,557. 9,208,558, 9,275,191, 9,292,920, 9,330,206, 9,626,756, 9,672,302, 9,672,617, and 9,688,023, the disclosures of which are incorporated herein by reference in their entirety.

[0185] In some embodiments, the present invention is directed to a 3D printed osteosynthetic composite material formed from the resins described above. In one or more of these embodiments, the 3D printed osteosynthetic composite material comprises: a linear or star-shaped poly(propylene fumarate)-based copolymer comprising at least one of an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block and a starshaped polypropylene fumarate) copolymer; a thiol-based crosslinker; and a plurality of filler nanoparticles.

[0186] In some embodiments, the present invention is directed to a 3D printed osteosynthetic apparatus for rib fracture repair comprising the 3D printed osteosynthetic composite material described above.

[0187] In some of these embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer comprises a resorbable ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block, wherein said first and second polypropylene fumarate) A blocks are each bonded covalently to an end of said polypropylene succinate) B polymer block to form an ABA block copolymer. In some other embodiments, the linear or star-shaped polypropylene fumarate)-based copolymer comprises a resorbable star-shaped polypropylene fumarate) copolymer comprising 3 or 4 polypropylene fumarate) arms extending from a multi-functional alcohol initiator. In some embodiments, the 3Dprinted osteosynthetic apparatus for rib fracture repair, further comprising a filler material to promote bone repair and / or regrowth.

[0188] In some of these embodiments, said filler material is hydroxyapatite. In certain embodiments, the resorbable 3D printed osteosynthetic apparatus for rib fracture repair comprised from 1 wt.% to 20 wt.% hydroxyapatite. In various embodiments, the resorbable 3D printed osteosynthetic apparatus for rib fracture repair is a plate. In some embodiments, the plates will comprise a plurali ty of openings sized to received surgical screws.

[0189] In certain embodiments, the present invention is directed to a method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair comprising: measuring and / or imaging a rib fracture on a subject having a rib fracture; generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in said subject, based upon the measurements and or images taken of the rib fracture; preparing a 3D printable resin as described in detail above and loading the resin mixture into a suitable 3D printer; 3D printing the resorbable 3D printed osteosynthetic apparatus for rib fracture repair based upon said 3D printable file. In some of these embodiments, the method further comprising post curing the resorbable 3D printed osteosynthetic apparatus for rib fracture repair with ultraviolet light

[0190] In some embodiments, the step of preparing a 3D printable resin comprises: dissolving a linear or star-shaped poly(propylene fumarate)-based copolymer comprising at least one of an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block and a star-shaped polypropylene fumarate) copolymer in a suitable diluent; adding a plurality of filler nanoparticles to the solution of Cl; adding said photoinitiator to said ABA block copolymer; adding a thiol-based crosslinker and mixing to form said 3D printable resin. In some of these embodiments, the step of adding a thiol-based crosslinker does not take place until immediately before less than 30 minutes before the step of 3D printing the resorbable 3D printed osteosynthetic apparatus. In various embodiments, the step of preparing a 3D printable resin further comprises adding radical scavenger or photoinhibitor to the solution.

[0191] In some embodiment, the filler nanoparticles promote bone repair and / or regrowth. Suitable filler nanoparticles for promote bone repair and / or regrowth include but are not limited to hydroxyapatite, strontium carbonate, b-tricalcium phosphate, and combinations thereof.

[0192] In one or more embodiments, the thiol-based crosslinker will comprise trimethylolpropane tris(3-mercaptopropionate), Thiocure 332 and 333, for the 700 and 1300 molecular weights, respectively. Alternative names for Thiocure 332 and 333 are ETTMP-700 and ETTMP-1300, respectively. In one or more of these embodiments, the molar ratio of said 3D printable resin to said thiol-based crosslinker in the crosslinker / resin mixture of is from about 3:1 to about 40: 1.

[0193] In various embodiments, the present invention also includes a method for treating a rib fracture in a subject comprising; preparing a 3D printed composite plate for rib fracture repair as described above, wherein said 3D printable composite plate is sized for use in repairing a rib fracture at a rib fracture site in a subject: surgically inserting said 3D printed composite plate into the subject and securing it across said rib fracture site such that said 3D printed composite plate is mechanically secured to the rib on either side of said rib fracture.

[0194] In some of these embodiments, the step of preparing a 3D printed composite plate for rib fracture repair comprises: preparing a 3D printable resin comprising an ABA block copolymer having a first and second polyfpropylene fumarate) A blocks and a polyfpropylene succinate) B block, wherein said first and second polyfpropylene fumarate) A blocks are each bonded covalently to an end of said polyfpropylene succinate) B polymer block to form an ABA block copolymer; a filler material; and a photoinitiator; measuring and / or imaging a rib fracture on a subject having a rib fracture; generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in said subject, based upon the measurements and or images taken of the rib fracture; adding a thiol-based crosslinker to 3D printable resin and loading the crosslinker / resin mixture into a suitable 3D printer; and 3D printing the 3D printable resin composite based upon said 3D printable file to produce a 3D printed composite plate for rib fracture repair.

[0195] In other embodiments, the step of preparing a 3D printed composite plate for rib fracture repair comprises: preparing a 3D printable resin comprising a star-shaped PPF copolymer having 3 or 4 arms; a filler material; and a photoinitiator measuring and / or imaging a rib fracture on a subject having a rib fracture generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in said subject, based upon the measurements and or images taken of the rib fracture; adding a thiol-based crosslinker to 3D printable resin and loading the crosslinker / resin mixture into a suitable 3D printer; and 3D printingthe 3D printable resin composite based upon said 3D printable file to produce a 3D printed composite plate for rib fracture repair.

[0196] In some embodiments, the 3D printed composite plate comprises one or more openings sized to receive and retain a surgical screw. In certain embodiments, the step of mechanically securing said 3D printed composite plate to the rib on either side of said rib fracture is performed using two or more screws running through said 3D printed composite plate.EXPERIMENTAL

[0197] To more fully illustrate and reduce the invention to practice, the effects of using PPF-based materials for rib fracture plating on rib fracture healing were investigated in a rabbit model using radiographic, mechanical, and histologic evaluation.

[0198] ABA block copolymer embodiments

[0199] In these experiments, rib fracture plating was prepared from resins containing the PPF based ABA block copolymers described above, with and without hydroxyapatite nanoparticles, and their efficacy evaluated in a rabbit rib fracture model relative to untreated ribs, commercially available PLA, and clinical standard titanium pla te fixation. The abilit y of these resorbable fixation materials to provide sufficient mechanical support for rib unionization and simultaneously reduce inflammation and infection risk and improve bone mineralization compared to titanium implants was evaluated.

[0200] Radiographically, the plates with the hydroxyapatite nanoparticles (PPF+HAnp plates) results in more robust calluses with more calcium deposition compared to titanium plates. With mechanical testing, showed that PPF+HAnp plates results in increased elasticity of calluses, but titanium plates still yield calluses with the highest modulus. Histologically, titanium plates resulted in the most mature calluses with higher endochondral ossification, but of the biomaterials, PPF+HAnp resulted in the most mature calluses on histology. Altogether, these findings support the hypothesis that PPF+HAnp plates accelerate rib fracture healing and result in more mature calluses. Using multimodal approaches of evaluating the resulting rib fracture calluses because no single method of evaluating a callus will give useful translational data. It is only in conjunction that these multiple points of data will give a thorough picture of whether these biomaterials have the potential to improve rib fracture plating.DUK. P W00012

[0201] The underlying mechanism by which PPF+HAnp plates accelerate rib fracture healing in this model may be increased cell adhesion and proliferation, While it would be outside the scope of this study to evaluate the granular biochemical underpinnings of the effects of PPF+HAnp on callus formation, other in vitro studies have shown that PPF+HAnp scaffolds seeded with bone marrow-derived stem cells result in increased cell adhesion and subsequent cell proliferation. The incorporation of HA into the PPF likely stimulates bone regrowth.Effects of pla te material type on rib fracture callus size and composition

[0202] Compared to titanium, both PPF+HAnp (5.91mm vs 3.63 mm, p = 0.01) and PPF (8.25mm vs 3.63mm, p = 0.02) plates increased rib fracture callus diameter after four weeks. Only PPF plates increased rib fractured callus index compared to titanium at four weeks (2.26 vs 1.77, p = 0.02). (FIG. 1A-C) PPF+HAnp plates had equivalent callus calcium deposition as measured by mineralized volume fraction on microCT to titanium plates (0.075 vs 0.071, p = 0.80), and increased calcium deposition compared to both PPF (0.075 vs 0.042, p = 0.04) and PLA (0.075 vs 0.057, / ?=0.02). (FIGS. 2A-D) There were no differences in callus calcium deposition between PLA and PPF (0.042 vs 0.057, p = 0.23). There were no differences in cortical bone calcium deposition between plate types.Effects of plate material type on rib fracture callus endochondral ossification

[0203] Alcian blue straining showed that rib fracture calluses from titanium resulted in the most endochondral ossification on histology with cartilage to bone ratio of 0.071 compared to PPF+HAnp (0.150, p = 0.03), PPF (0.354, p < 0.01), and PLA (0.702, p < 0.01). (FIGS. 3A-B ) PPF+HAnp plates resulted in significantly more endochondral ossification than PPF (0.150 vs 0.354, p = 0.01) and PLA (0.150 vs 0.702, p < 0.01) plates with PLA showing the least endochondral ossification of all the plate materials.Effects of plate material type on rib fracture callus mechanical characteristics

[0204] Plating with PPF+HAnp resulted in increased elastic modulus compared to PPF (6.12 MPa vs 0.962 MPa), PLA (6.12 MPa vs 1.43 MPa), and non-stabilized fracture (6.12 MPa vs 1.36MPa). Titanium stabilized ribs showed highest modulus (19.7 MPa). PPF+HAnp had 100% reduction while PPF and PLA plates lead to 25% incidence of fracture non-reduction at 4 weeks. (FIGS. 7B-C)Star polymer embodimentsPolymer synthesis and 3D printing

[0205] Four-arm star polypropylene fumarate) copolyesters were synthesized via a ring¬ opening copolymerization (ROCOP) as reported previously (See, e.g., Kirillova, A.; Yeazel, T. R.: Gall, K.: Becker, M. L. Thiol-Based Three-Dimensional Printing of Fully Degradable Poly(Propylene Fumarate) Star Polymers. ACS Appl. Mater. Interfaces 2022. 14 (34). 38436- 38447. https: / / doi.org / 10.1021 / acsami.2c06553 and Fer, G. L.; Luo, Y.; Becker, M. L. Polypropylene Fumarate) Stars. Using Architecture to Reduce the Viscosity of 3D Printable Resins. Polymer Chemistry 2019, 10 (34), 4655-4664. https: / / doi.org / 10.1039 / C9PY00738E, the disclosures of which are incorporated herein by reference in their entirety). Polypropylene maleate) (PPM) was first polymerized via ROCOP of maleic anhydride (MAn) and propylene oxide (PO) using Mg(BHT)2(THF)2 as a catalyst and meso-erythritol as a tetrafunctional initiator. A degree of polymerization (DPn) of 30 was targeted for each arm, corresponding to a total DPnof 120. Four-arm star PPM was then converted to fumarate-based copolyester through a base-catalyzed isomerization using diethylamine. Isomerization of -alkenes to / raws-alkenes was monitored by protonnuclear magnetic resonance (NMR) spectroscopy, and full conversion was confirmed after 18 h (FIGS. 12A-B). Fumarate-based copolyester star copolymers were obtained with a number-average molecular mass (Mᴿ) of 4.2 kDa as determined by size-exclusion chromatography (SEC) (FIG. 14).

[0206] FIGS. 4A-B show a reaction mechanism and schematic diagram of polymer synthesis and 3D printing of fumarate-based star copolyesters and copolyester-composite rib fracture plates. FIG. 4A is a reaction mechanism showing ring-opening copolymerization of propylene oxide and maleic anhydride followed by an isomerization reaction to yield polypropylene fumarate) star copolyesters. FIG. 4B is a schematic showing Continuous Liquid Interface Production (CLIP) photochemical printing of a one pot resin containing polypropylene fumarate) star copolyesters, trimethylolpropanetris(3-mercaptopropionate) (thiol crosslinker) in a 20:1 (alkene: thiol) ratio, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO) and oxybenzone (HMB) were dissolved in ethyl acetate (70 wt.% polymer). Hydroxyapatite nanoparticles (10 wt.%) were added to the resin prior to printing to yield composite rib plates.

[0207] Synthesized four-arm star fumarate-based copolyesters were 3D printed via continuous liquid interface production (CLIP) on a Carbon M2 printer at 70 wt.% in ethyl acetate with 0.6 wt.% photoinitiator (phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, BAPO) and 0.4 wt.% oxybenzone (HMB), a photoinhibitor. Table 1 details the appropriate print parameters for both star copolyester and composite resins. In fumarate-based copolyester-HAp composite resins, 10 wt.% hydroxyapatite nanoparticles (<200 nm) relative to polymer, crosslinker, and photoactive additives mass were added to the resin prior to printing. Hydroxyapatite is a bioactive ceramic that resembles the calcium phosphate of bone apatite and has demonstrated osteoconductivity. (See, e.g., Wang, M. Developing Bioactive Composite Materials for Tissue Replacement. Biomaterials 2003, 24 (13), 2133-2151. https: / / doi.org / 10.1016 / S0142-9612(03)00037-l and Woodard, J. R.; Hilldore, A. J.; Lan, S. K.; Park, C. J.; Morgan, A. W.; Eurell, J. A. C.; Clark, S. G.: Wheeler, M. B.; Jamison, R. D.; Wagoner Johnson, A. J. The Mechanical Properties and Osteoconductivity of Hydroxyapatite Bone Scaffolds with Multi-Scale Porosity. Biomaterials 2007, 28 (1), 45-54. https: / / doi. Org / 10.1016 / j.biomaterials.2006.08.021, the disclosures of which are incorporated herein by reference in their entirety). However, the poor mechanical properties of calcium phosphates prevent clinical translation on their own. See, e.g., Pina. S.; Ferreira, J. M. F. Bioresorbable Plates and Screws for Clinical Applications: A Review. Journal of Healthcare Engineering 2012, 3 (2), 846435. https: / / doi. Org / 10.1260 / 2040-2295.3.2.243, the disclosure of which is incorporated herein by reference in its entirety). Previous work has shown polymer-HAp composites to enhance calcification and bone regeneration within 8 weeks compared to unfilled controls, (see, e.g., Kuss, M. A.; Wu, S.; Wang, Y.; Untrauer, J. B.; Li, W.; Lim, J. Y.; Duan, B. Prevascularization of 3D Printed Bone Scaffolds by Bioactive Hydrogels and Cell Co-Culture. Journal of Biomedical Materials Research Part B: Applied Biomaterials 2018, 106 (5), 1788- 1798. https: / / doi. Org / 10.1002 / jbm.b.33994, the disclosure of which is incorporated herein by reference in its entirety) but these systems either have slow degradation profiles (e.g., PLA-PEG) or are difficult to process (e.g., chitin). (See, e.g., Kaito, T.; Myoui, A.; Takaoka, K.; Saito, N.; Nishikawa, M,; Tamai, N.; Ohgushi, H.; Yoshikawa, H. Potentiation of the Activity of Bone Morphogenetic Protein-2 in Bone Regeneration by a PLA-PEG / Hydroxyapatite Composite. Biomaterials 2005, 26 (1), 73-79. https: / / doi. Org / 10.1016 / j.biomaterials.2004.02.010 and Ge, Z.; Baguenard, S.; Lim, L. Y.; Wee, A.; Khor, E. Hydroxyapatite-Chitin Materials as Potential Tissue Engineered Bone Substitutes. Biomaterials 2004, 25 (6), 1049-1058.https: / / doi.org / 10.1016 / S0142-9612(03)00612-4, the disclosures of which are incorporated herein by reference in their entirety).Table 1Print parameters on Carbon M2 printer for fumarate-basedcopolyester and copolyester-HAp composite resins.

[0208] Vat photopolymerization using CLIP typically requires polymer resins with viscosities below 10 Pa-s. (See, e.g., Tumbleston, J. R.; Shirvanyants, D.; Ermoshkin, N.; Janusziewicz. R.; Johnson, A. R.; Kelly, D.; Chen, K.; Pinschmidt, R.; Rolland, J. P.; Ermoshkin, A.; Samulski, E. T.; DeSimone, J. M. Continuous Liquid Interface Production of 3D Objects. Science 2015, 347 (6228), 1349-1352. https: / / doi.org / 10.1126 / science.aaa2397, the disclosure of which is incorporated herein by reference in its entirety). A formulation of 70 wt.% star polymer in ethyl acetate, with or without HAp, results in resin viscosities below this threshold (FIG. 15). HAp moderately increases the resin viscosity compared to unfilled resins. The nominal crosslink alkene-to-thiol ratio of 20:1 was determined stoichiometrically from the number of alkenes in the polymer backbone to the number of pendant thiol groups in the 3 -arm thiol crosslinker, trimethylolpropane tris(3-mercaptopropionate), which react via thiol-ene reactions. Live / dead and cell viability assays of fumarate-based copolyester and copolyester-composite materials show low cytotoxicity, comparable with glass co vers lip controls (FIGS. 16A-C). Rib fixation plates were designed to the size and shape specifications of commercially available titanium midface plates obtained from Synthes so they were compatible with existing surgical methods. Upon print completion, the osteosynthetic plates and control parts were washed sequentially with isopropanol and ethyl acetate to remove excess resin, followed by post-curing in a deionized (DI) water bath in a UV oven (λ = 385-410 nm) for 5 min. The parts were dried at 60 °C for 5 days to yield fumarate-based copolyester and HAp composite tensile bars and osteosynthetic rib plates (FIG. 4B). Separately, PLA plates were 3D printed via fused deposition modeling (FDM) using commercially availablePLA (FIG. 1 OC). Microcomputed tomography (pCT) scans of 3D printed plates reveal high feature resolution and minimal internal defects in fumarate-based copolyester and composite plates and higher surface roughness in PLA plates (FIGS. 17A-B).

[0209] HAp nanoparticles were suspended in the fumarate-based copolyester stars resin prior to printing and remained suspended throughout the duration of the print. The incorporation of 10 wt.% HAp into the osteosynthetic plates was confirmed by thermogravimetric analysis (TGA) (FIG. 18A). After heating to 600 °C, 24.6% of mass remains in the composite samples compared to 11.2% in the fumarate-based copolyester samples. Slight deviations from nominal HAp loadings suggests some heterogeneity in the distribution of the nanoparticles throughout the polymer matrix.3D printed fumarate -based copolyester samples had a slightly lower glass transition temperature (Tg) (28 °C) compared to 3D printed HAp composite samples (35 °C) by differential scanning calorimetry (DSC) (FIG. 18B). The opposite trend is observed, however, in Tsas determined by dynamic mechanical analysis (DMA) temperature sweeps (FIGS. 19A-B). 3D printed discs of fumarate -based copolyester star polymers were subjected to accelerated degradation conditions (aq. 0.25 N KOH) at physiological temperature with constant agitation, and complete degradation was achieved after 11 days (FIG. 20). Separately, to isolate the degradation products of the osteosynthetic plates, 3D printed plates were fully degraded in a strongly basic solution (aq. 10 M NaOH), and mass spectrometry was performed on the degradation solutions (FIGS. 20A-B). Monomeric subunits — propylene glycol and fumaric acid — are observed in both the star copolyester and composite plate degradation solutions. A higher concentration of low molecular weight species and oligomers in the composite plate degradation solution is attributed to increased water transport throughout the network resulting from ceramic loading.

[0210] Stress-strain curves obtained from uniaxial tension tests of 3D printed tensile bars (ASTM D638 Type V) (FIG. 5A) show an increase in Young’s modulus (£b) and ultimate tensile strength (UTS) with a corresponding decrease in elongation at break (Eᵇ) resulting from the HAp composite filler (Table 2). A greater than two-fold increase in Eᵇ is observed in fumarate-based copolyester-HAp composite (51.5 ± 5,0 MPa) compared to the fumarate-based copolyester (21.3 ± 0.9 MPa) at ambient conditions (FIG. 5C). HAp nanoparticles act as a toughening agent in the composite substrates, resulting in improved mechanical performance compared to fumarate-based copolyester star polymers alone. Eᵇ is reduced at physiological conditions within both fumarate- based copolyester (3.2 ± 0.6 MPa) and fumarate-based copolyester-HAp (4.6 ± 1.1 MPa) tensilebars. Flexural stress-strain curves of the PLA plates (FIG. 5D), 3D printed fumarate-based copolyester and composite plates (FIG. 5B) were obtained via DMA three-point bend testing at 25 °C and 37 °C. The PLA plates are considerably stiffer (91.7 ± 27.0 MPa) than fumarate-based copolyester (8.4 ± 1.4 MPa) and composite (27.7 ± 5.2 MPa) osteosynthetic plates at ambient conditions. This is also reflected in the higher tensile modulus of PLA at 25 °C (914.2 ± 105.1 MPa.) and 37 °C (765.3 ± 34.0 MPa). However, PLA is notably more brittle with an Eb of 6 ± 3 % compared to fumarate-based copolyester (244 ± 35 %) and fumarate-based copolyester-HAp composite (130 ± 34 %) materials at ambient conditions. Post-operative breakage of commercially available PLA fixation plates has been reported widely (see, e.g., Ashley, D. W.; Christie, D. B. I.; Long, E. L.: Adiga, R.; Johns, T. J.; Fabico-Dulin, J.; Montgomery, A. Prospective Randomized Trial of Metal versus Resorbable Plates in Surgical Stabilization of Rib Fractures, Journal of Trauma and Acute Care Surgery 2022, 93 (2), 147. https: / / doi.org / 10.1097 / TA.0000000000003642 and Miller, D. L.; Force, S. D.; Pickens, A.; Fernandez, F. G.; Luu, T.; Mansour, K. A. Chest Wall Reconstruction Using Biomaterials. The Annals of Thoracic Surgery 2013, 95 (3), 1050-1056. https: / / doi.org / 10.1016 / j.athoracsur.2012.11.024, the disclosures of which are incorporated herein by reference in their entirety), resulting in fracture displacement at early timepoints and over time. We hypothesize that tough, elastomeric materials such as the crosslinked fumarate-based copolyester star polymer composite plates described herein will reduce rates of post-operative plate failure, as well as allow for improved surgical handling and compatibility with rib curvature.

[0211] FIGS. 5A-D are graphs showing the mechanical properties of 3D printed fumarate-based copolyester star polymers and copolyester-hydroxyapatite composites and rib fracture plates. Tensile bars, fumarate-based copolyester and composite rib fracture plates were 3D printed at a 20: 1 alkene-to-thiol crosslink ratio. FIG. 5A is a graph showing representative fumarate-based copolyester, composite, and PLA stress-strain curves from uniaxial tension tests collected at 25 °C and 37 °C in lx PBS. PLA curves shown in inset for clarity. FIG. 5B is a graph showing stress-strain curves from three-point bend tests of 3D printed fumarate -based copolyester and composite plates, (n = 3) FIG. 5C is a graph showing box plots of copolyester and composite tensile modulus (n = 5) determined from stress-strain curves shown in FIG. 5A. The modulus of fumarate-based copolyester-HAp composite plates is more than two-fold greater than unfilled fumarate-basedcopolyester rib fracture plates. FIG. 5D is a graph showing stress-strain curves from three-point bend tests of PLA plates (n 3).Table 2Summary of Mechanical Properties of Rib Fracture Plates at 25 °C and 37 °C,Rabbit rib fracture model and stabilization with 3D printed plates

[0212] A New Zealand white rabbit rib fracture model was used to evaluate the performance of 3D printed orthopedic plates in rib fracture repair as a resorbable alternative to titanium SSRF. Of the rabbits that underwent treatment, fractured ribs were immediately stabilized with either commercial titanium midface plates (Synthes), 3D printed PLA plates, fumarate-based copolyester plates, or composite plates (FIGS. 6A-B). No major complications were observed among the animals that received treatment with fixation plates. Experimental controls included ribs without any fracture (Control Rib) and untreated ribs that were fractured without subsequent fixation (Fracture & No Plate). Fracture healing was assessed at 2- and 4-weeks post- fracture by fracture callus flexural strength and bone morphometry, and histological evaluation was used to assess bioabsorbable implant tolerance and inflammatory response.

[0213] FIGS. 6A-B show rabbit rib fracture surgical models and subsequent fixation with various osteosynthetic plates. FIG. 6A is a schematic diagram and images showing rib fixation using titanium and resorbable osteosynthetic plates. The 4* and 6taribs of New Zealand white rabbits were cut and immediately stabilized with either commercially available titanium or 3D printed, resorbable PLA, fumarate-based copolyester, or fumarate-based copolyester-HAp composite osteosynthetic plates. Radiographs show fixation at 4 weeks post-surgery. FIG, 6B isan image showing rib fixation with a composite plate, centered at the site of fracture with one screw on either end.Biomechanical characterization of explanted ribs1002141 Mechanical stability under load is a paramount function of bone and is thus an important assessment of healing, and various mechanical tests have been utilized ex vivo to this end. Four-point bending experiments have been used to biomechanically assess failure modes in various metal rib fixation systems in cadaver models. (See, e.g., Prins, J. T. H.; Van Wijck, S. F. M.; Leeflang, S. A,; Kleinrensink, G.-J.; Lottenberg, L.; de la Santa Barajas, P, M.; Van Huijstee, P. J.; Vermeulen, J.; Verhofstad, M. H. J.; Zadpoor, A. A.; Wijffels, M. M. E.; Van Lieshout, E. M. M. Biomechanical Characteristics of Rib Fracture Fixation Systems. Clinical Biomechanics 2023, 102, 105870. https: / / doi. Org / 10.1016 / j.clinbiomech.2023.105870, the disclosure of which is incorporated herein by reference in its entirety). Three-point bend and torsional testing are employed in small rodent animal models to evaluate tibia and femur strength, both with and without fractures. (See, e.g., Manigrasso, M. B.; O’Connor, J. P. Characterization of a Closed Femur Fracture Model in Mice. Journal of Orthopaedic Trauma 2004, 18 (10), 687; Prodinger, P. M.; Biirklein, D.; Foehr, P.; Kreutzer, K.; Pilge, H.; Schmitt, A.; Eisenhart-Rothe, R. V.; Burgkart, R.: Bissinger, O.; Tischer, T. Improving Results in Rat Fracture Models: Enhancing the Efficacy of Biomechanical Testing by a Modification of the Experimental Setup. BMC Musculoskelet Disord 2018, 19 (1), 243. https: / / doi.org / 10.1186 / s12891-018-2155-y; Deckard, C.; Walker, A.; Hill, B. J. F. Using Three-Point Bending to Evaluate Tibia Bone Strength in Ovariectomized Young Mice. J Biol Phys 2017, 43 (1), 139-148. https: / / doi.org / 10.1007 / s10867-016-9439-y; Camarena, A.; Kang, L.; Mirando, A. J.; Augustine, E.; McMillian, N. S.; Stinson, N. C.; Agarwal, S. M.; Becker, M. L.; Hilton, M. J.; Fernandez-Moure, J. S. Platelet-Rich Plasma Enhances Rib Fracture Strength and Callus Formation in Vivo. Journal of Trauma and Acute Care Surgery 2024, 97 (6), 884. https: / / doi.org / 10.1097 / TA.0000000000004441, the disclosures of which are incorporated herein by reference in their entirety). In this study, given the shape of the rib and directionality of blunt force trauma to the chest wall, the mechanical strength of the control and treated ribs at 2 and 4 weeks was assessed by three-point bend mechanical testing. Explanted rabbit ribs were subjected to three-point bend experiments, with the applied force centered at the site of the fracture callus (FIG. 7A). The slopes of the resultant flexural stress-strain curves highlight theincrease in flexural modulus, a marker for strength of healing bone, of ribs fixed with titanium and fumarate-based copolyester-HAp composite plates after 4 weeks compared to the no-plate condition, PLA, and fumarate -based copolyester plates (FIG. 7B). In all treatment groups, the fracture biomechanics are reproducible and low at 2 weeks. Flexural modulus and flexural strength of the fracture callus increases moderately from 2 to 4 weeks post-fracture in all fixation groups (FIG. 7C). The most significant increase in flexural modulus was observed in titanium-fixed ribs from 0.1 ± 0.1 MPa to 10.6 ± 9.1 MPa between 2 and 4 weeks (***p < 0.001), respectively. Of the ribs fixed with bioabsorbable plates (PLA, fumarate-based copolyester, fumarate-based copolyester-HAp), ribs stabilized with lumarate-based copolyester-HAp composite plates exhibit the greatest flexural modulus increase from 2 weeks (0.4 ± 0.4 MPa) to 4 weeks (4.1 ± 3.5 MPa) post-fracture. The flexural modulus of the control rib without any fracture (521.7 ± 168,8 MPa) is considerably higher than all ribs at 4 weeks post-fracture. The large difference in mechanical strength between the no-fracture and no-plate controls (Table 3) indicates that this characterization method is a reasonable, quantitative measure of bone strength that can be used to assess bone healing. Notably, fracture model mechanical testing is high variance in nature. (See, e.g., Manigrasso, M. B.; O’Connor, J. P. Characterization of a Closed Femur Fracture Model in Mice. Journal of Orthopaedic Trauma 2004, 18 (10), 687 and Hiltunen, A.; Vuorio, E.; Aro, H. T. A Standardized Experimental Fracture in the Mouse Tibi. Journal of Orthopaedic Research 1993, 11 (2), 305-312. https: / / doi. Org / 10.1002 / jor.1100110219: the disclosures of which are incorporated herein by reference in their entirety). However, ribs fixed with titanium plates exhibited the highest variation in flexural modulus at 4 weeks, suggesting an inconsistent binary of rib union / non-union. Although lower than the titanium clinical standard, the mechanical maturation of the fracture callus from 2 to 4 weeks in ribs treated with 3D printed fumarate-based copolyester-HAp plates suggests that optimization in this space (e.g., plate geometry, polymer mechanicals) may make viable a bioabsorbable orthopedic plate for SSRF.

[0215] FIGS. 7A-C show the results of three-point bend mechanical testing of explanted rib callus at 2- and 4-weeks post-fracture. FIG. 7 A is an image showing a representative three-point bend test of explanted rabbit rib. The applied force is centered at the site of fracture. Flexural strength, modulus, and toughness were determined from resulting stress-strain curves. FIG. 7B is a graph showing representative stress-strain curves obtained from three-point bend tests at 2 and 4 weeks (n = 3-4). Ribs stabilized with titanium plates and composite plates show increased callusmodulus at 4 weeks compared to ribs stabilized with PLA and fumarate -based copolyester plates. FIG. 7C is a graph showing flexural modulus of stabilized rib fractures, obtained from curves in (b) (n = 3-4). The flexural modulus of the callus increases from 2 to 4 weeks across all groups. Means ± SD. *p < 0.05, **p < 0.01, ***p < 0.001, ns = not significant.Table 3Summary of 3-Point Bend Mechanics of Explanted Rabbit Ribs.Histological evaluation of implant site and fracture callus

[0216] The tissue immune response is of interest for its influence on healing and vascular remodeling of the callus site (see, e.g., Baht, G. S.; Vi, L.; Alman, B. A. The Role of the Immune Cells in Fracture Healing. Curr Osteoporos Rep 2018, 16 (2), 138-145. https: / / doi.org / 10.1007 / s11914-018-0423-2 and Schmidt-Bleek, K.; Schell, H.; Schulz, N.; Hoff, P.; Perka, C.: Buttgereit, F.; Volk, H.-D.; Lienau, J.; Duda, G. N. Inflammatory Phase of Bone Healing Initiates the Regenerative Healing Cascade. Cell Tissue Res 2012, 347 (3), 567-573. https: / / doi. Org / 10.1007 / s00441-011-1205-7, the disclosures of which are incorporated herein by reference in their entirety), over which the implant material exerts significant control. We sought to investigate the role of plate mechanical properties and resorption effects on the inflammatory response during bone regeneration in rib fractures, Radiographs and pCT scans of explanted ribs were obtained, followed by decalcification and histological evaluation of the fracture callus. Explanted ribs were paraffin sectioned into 5 μm slices, and sections were stained with eitherDUK. P. WOOOI2hematoxylin & eosin (H& E) (FIG. 23, FIG. 24) or alcian blue and picrosirius red (FIG. 8). H& E-stained sections were evaluated by a veterinary pathologist using an International Organization for Standardization (ISO) scoring system for inflammation / irritancy, osseointegration, and fracture union (Table 4).

[0217] When compared to titanium at 2 weeks, the PLA implants displayed slight irritancy with a reactivity ranking score of 5.1. This appears primarily driven by slightly more mononuclear cell infiltrates compared to the examined areas of the titanium implants and slightly more necrosis present in each animal in this group compared to animals in the titanium group. Irritancy scores decreased across all bioabsorbable groups between the 2- and 4-week time points, with PLA and fumarate-based copolyester decreasing by more than 50%, and composite decreasing by 15.5% (Table 4). Titanium irritancy scores remained comparable at both time points. Qualitatively, titanium implants had consistently more remaining leukocytes of any category surrounding the implant location than any of the bioabsorbable groups. Fumara te-based copolyester and composite plates displayed overall lower amounts of inflammatory cell populations at both time points with lower numbers of individual cell populations.

[0218] FIG. 8 shows radiography and histological staining of explanted rib callus at 2- and 4-weeks post- fracture. μCT and x-ray scans of explanted rib calluses at 2 and 4 weeks were obtained, followed by decalcification and cross-sectional histological characterization. Sections were visualized using Hematoxylin and Eosin (H& E) and Alcian Blue-Picrosirius Red staining (shown). Ribs stabilized with fumarate-based copolyester and fumarate-based copolyester-HAp composite plates exhibit decreased irritancy and greater osseointegration compared to ribs stabilized with PLA or titanium plates. Scale bar = 1 mm.

[0219] All bioabsorbable plates (fumarate-based copolyester, fumarate-based copolyester-HAp composite) displayed some degree of osseointegration, defined as bone growth near and along the device / tissue interface, at the 2 -week time point while titanium implants displayed none. At 2 weeks, just 1 / 3 of the animals plated with composite materials displayed any degree of osseointegration, while 2 / 3 animals in the PLA group and all 4 animals in the fumarate-based copolyester plated group displayed at least a small amount of osseointegration. At 4 weeks, all groups displayed some degree of osseointegration with fumarate -based copolyester and composite plates showing the highest level of osseointegration, and with all animals in those groupsdisplaying this feature. 1 / 3 animals in the PLA group and 2 / 5 animals in the titanium group at the 4-week timepoint displayed no osseointegration.Table 4Summary of Rib Fracture Pathology ISO Scoring.

[0220] There was significant variability on fracture union scores within each group and the score appeared associated more with the degree of alignment of the cortices. Fracture union scores were positively associated with fracture alignment. On average, fracture union scores were the highest in the no plate and titanium groups. The low fracture union scores in the bioabsorbable implants suggest increased flexibility allowing for motion and alignment at the fracture site.

[0221] Overall, all test implants (PLA, fumarate-based copolyester, fumarate-based copolyester-HAp) qualify as biocompatible, with reduced irritancy compared to titanium implants by the 4-w'eek timepoint and on average, minimal inflammatory infiltrates (FIGS. 25A-F). The PLA implants did display slight irritancy at the 2-week timepoint. The implanted polymer plates on average result in more new bone growth around the implant than the titanium implants. However, the ability to evaluate the effect of the implants on fracture healing is hampered by the malalignment of several of the fractures across all implant categories. Progression of the callus to osseous union appears related in part to the degree of fracture alignment which is masking the role of the implanted plates.μCT and bone morphometry of explanted rib callus

[0222] Microcomputed tomography imaging is a non-destructive characterization method used widely in preclinical bone research to evaluate 3D bone microstructure (e.g., architecture, density) in animal models (see, e.g., Morgan, E. F.; Mason, Z. D.; Chien, K. B.; Pfeiffer, A. J.;Barnes, G. L.; Einhorn, T. A.; Gerstenfeld, L. C. Micro-Computed Tomography Assessment of Fracture Healing: Relationships among Callus Structure, Composition, and Mechanical Function. Bone 2009, 44 (2), 335-344. https: / / doi.org / 10.1016 / j.bone.2008.10.039 and Gabet, Y.; Muller, R.; Regev, E.; Sela, J.; Shteyer, A.; Salisbury, K.; Chorev, M.; Bab, I. Osteogenic Growth Peptide Modulates Fracture Callus Structural and Mechanical Properties. Bone 2004, 35 (1), 65-73. https: / / doi. Org / 10.1016 / j.bone.2004.03.025, the disclosures of which are incorporated herein by reference in their entirety), a marked improvement over 2D techniques such as radiography. Moreover, callus structure and mineralization have been shown to correlate with bone strength and stiffness that ultimately define healing. (See, e.g., Morgan, E. F.; Mason. Z. D.; Chien, K, B.; Pfeiffer, A. J.; Barnes, G. L.; Einhorn, T. A.; Gerstenfeld, L. C. Micro -Computed Tomography Assessment of Fracture Healing: Relationships among Callus Structure, Composition, and Mechanical Function. Bone 2009, 44 (2), 335-344. https: / / doi. Org / 10.1016 / j.bone.2008.10.039; (61) O’Neill, K. R.; Stutz, C. M.; Mignemi, N. A.: Burns, M. C.; Murry, M. R.; Nyman, J. S.; Schoenecker, J. G. Micro-Computed Tomography Assessment of the Progression of Fracture Healing in Mice. Bone 2012, 50 (6), 1357-1367. https: / / doi. Org / 10.1016 / j.bone.2012.03.008; and Shefelbine, S. J.; Simon, U.; Claes, L.; Gold, A.; Gabet, Y.; Bab, I.; Muller, R.; Augat, P. Prediction of Fracture Callus Mechanical Properties Using Micro-CT Images and Voxel-Based Finite Element Analysis. Bone 2005, 36 (3), 480-488. https: / / doi. Org / 10.1016 / j.bone.2004.11.007, the disclosures of which are incorporated herein by reference in their entirety).

[0223] Bone regeneration and morphometry of the rib fracture callus at 2- and 4-weeks postfracture were assessed by μCT imaging. Representative μCT constructions (FIG. 9A) of ribs explanted after 4 weeks show significant non-union in ribs fixed with PLA and fumarate-based copolyester plates. There was variation in fracture union in no-plate control ribs and those fixed with fumarate-based copolyester-HAp composite plates, which is consistent with pathological observations. Quantification of the μCT reconstructions show an increase in mineralized callus bone volume (BV) from 2 to 4 weeks within each experimental group (FIG. 9B). Normalization of BV with total volume (TV) of the callus (BV / TV), however, reveals little variation between populations at each time point (FIG. 26A). This is likely due to the large differences in callus size — with displaced ribs generating considerably larger calluses than fixed ribs — that produce an averaging effect. Modest increases in trabecular thickness (FIG. 9D) and trabecular connectivity density (FIG. 26B) are observed from 2 to 4 weeks. There is a significant difference in trabecularthickness (FIG. 9D) from 2 to 4 weeks in untreated ribs (***p < 0.0005) and ribs stabilized with fumarate-based copolyester (***p < 0.0005) or composite (*p < 0,05) plates, indicating stronger bone. The structure model index (SMI), a metric for quantifying plate-like and rod-like trabecular structure in bone, is significantly lower (*p < 0.05) in the titanium plated ribs compared to the noplate controls at 2 weeks, indicating more plate-like, stronger structures (FIG. 9C). SMI is also significantly lower from 2 to 4 weeks in the no-plate control and fumarate-based copolyester groups (**p < 0.005). Improvement in these metrics (bone volume, trabecular thickness, SMI) from 2 to 4 weeks in the plated treatment groups demonstrate improved formation of stronger trabecular bone relative to fractured, untreated control ribs, and resorbable plates are performing similarly to titanium.

[0224] FIGS. 9A-E Micro-computed tomography (uCT) of explanted rib callus at 2- and 4-weeks post-fracture and related graphs reporting bone volume, structural model index, Trabecular thickness and surface area to volume ratio are shown in FIGS. 9A-E. FIG. 9A shows representative μCT scans of rib fracture callus 4 weeks post-fracture. Non-union is observed in rib fractures without plate fixation and in fractures stabilized with PLA and fumarate-based copolyester plates (n = 3-5 per group). FIG. 9B is a graph showing total bone volume (BV ) of the region of interest (fracture site callus) increases across all groups from 2 to 4 weeks. FIG. 9C is a graph showing structure model index (SMI) differentiates between plate-like and rod-like structures in trabecular bone. Lower values indicate more plate-like, stronger structures. Decreases in SMI are observed across all treatment groups from 2 to 4 weeks. FIG. 9D is a graph showing average thickness of trabeculae, reported as an inverse. Trabecular thickness increases from 2 to 4 ’eeks most significantly in control ribs and fumarate-based copolyester- and composite-stabilized ribs. FIG.9E is a graph showing surface area of bone relative to its total volume. Means ± SD. *p < 0.05, **p < 0.01, ***p < 0.001, ns = not significant,Conclusion

[0225] Fumarate-based copolyester star copolymers were synthesized and 3D printed, both with and without HAp composite filler. The introduction of 10 wt.% HAp composite filler to printable fumarate-based copolyester stars resin significantly improved the tensile and flexural mechanical properties of printed parts, providing an additional route for tunability while also imparting osteoconductive functionality. 3D printed fumarate-based copolyester and composite osteosynthetic plates produced a demonstrably lower inflammatory response in vivo compared toDUK. P W00012both PLA and titanium fixation plates, as well as a corresponding increase in osseointegration immediately surrounding the implant. Although rigid rib fixation with titanium plates yielded the most significant callus maturation from 2 to 4 weeks, composite plates demonstrated improved callus maturation within the same timeframe compared to commercial PLA and unfilled fumarate-based copolyester plates. While the precise impact of inflammatory effects of the implant on callus formation and fracture healing remains unknown, enhanced callus maturations suggest an interplay between plate mechanicals and resorption profile at the fracture site may play a role. The relatively low fracture union scores across all bioabsorbable plates relative to titanium standards warrants stiffer plate mechanics in future studies.

[0226] Rib fracture fixation represents a unique biomechanical challenge arising from 12 unique rib geometries and continuous daily breathing movements. As such, an osteosynthetic stabilization plate needs to be rigid enough to maintain fixation, flexible to not inhibit daily activity, and tunable to a range of injury' geometries. The fumarate -based star copoly'ester composite plates detailed herein offer a range of tunability with respect to mechanical properties and degradation rates, allowing for tailored orthopedic plates which can match the nature of the patient bone and fracture severity. In particular, the ability to fabricate osteosynthetic plates via additive manufacturing methods is clinically significant for rapid patient customization, a requirement for the expansion of minimally invasive intrathoracic stabilizati on methods.EXAMPLES

[0227] The following examples are offered to more fully illustrate the invention, but are not to be construed as limiting the scope thereof. Further, while some of examples may include conclusions about the way the invention may function, the inventor do not intend to be bound by those conclusions, but put them forth only as possible explanations. Moreover, unless noted by use of past tense, presentation of an example does not imply that an experiment or procedure was, or was not, conducted, or that results were, or were not actually obtained. Efforts have been made to ensure accuracy with respect to numbers used (e.g., amounts, temperature), but some experimental errors and deviations may be present. Unless indicated otherwise, parts are parts by weight, molecular weight is weight average molecular weight, temperature is in degrees Centigrade, and pressure is at or near atmospheric.Example 1Polypropylene fumarate-b-propylene succinate-b-propylene fumarate) (PPFPSu 10-10-10) Synthesis1002281 PPFPSu triblock copolymers were synthesized by a ring-opening copolymerization reported previously. Under an inert atmosphere, succinic anhydride (100 g, 0.9993 mol, 1.0 eq.) and propylene oxide (69.9 ml, 0.9993 mol, 1.0 eq.) were added to a solution of initiator, fumaric acid, (11.6 g, 0.0999 mol, 0.1 eq.) and catalyst, Mg(BHT)2(THF)2, (6.23 g, 0.01 mol, 0.01 eq.) dissolved in 250 ml of anhydrous toluene. The solution was stirred at 80 °C for 10 days, at which point 99% conversion was achieved. The reaction was cooled to room temperature, and maleic anhydride (196.0 g, 1.9986 mol, 2.0 eq.) and propylene oxide (139.9 ml, 1.9986 mol, 2.0 eq.) were added. The solution was again heated to 80 °C to resume polymerization and stirred for 5 days, at which point 99% was achieved. The PPMPS copolymer was recovered by precipitation into hexanes twice and dried by rotary evaporation.

[0229] To isomerize to the trans copolymer PPFPSu, the PPMPSu was dissolved in chloroform. Diethylamine (46.5 ml, 0.4497 mol, 0.45 eq.) was added to the solution, which was stirred under reflux for 24 hours. Following complete isomerization, the product was washed three times with a 1.0 M solution of monosodium phosphate. The organic layer was collected and dried with sodium sulfate. The polymer was dried by rotary evaporation, followed by high vacuum for four days.Example 2Plate 3D Printing

[0230] All samples were fabricated using a Carbon (Redwood, CA) M2 printer (1= 385 nm). The polymer was dissolved in ethyl acetate (7:3 w / w), to which 0.6 wt.% phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO) and 0.4 wt.% of oxybenzone (OB) were added and shaken overnight to form a resin. Immediately before printing, trimethylolpropane tris(3-mercaptopropionate) was added to the resin to achieve the desired crosslinking ratios of 20: 1, 10:1, and 5: 1 of polymer alkene to thiol crosslinker (mol / mol). In resins containing hydroxyapatite (HA), wt.% of HA was added immediately before printing, with respect to the total mass of polymer, BAPO, OB, and thiol crosslinker. Cure tests were performed to determine optimal photocuring conditions.

[0231] The STL files were obtained from open-source locations or created using AutoCAD. For the tensile measurements, ASTM D638 Type V tensile bars were printed. (See, e.g., FIG. 10B).The photochemically printed products were washed with ethyl acetate and isopropyl alcohol (IP A), placed in a deionized water bath, and then post-cured in a B9 Model Cure UV oven (B9Creations, 70W, 55Hz, X λ = 390-420 nm) for 5 minutes. Post-cured products were dried under vacuum at 60 °C for 5 days prior to further analysis.Example 3Plate Characterization

[0232] Uniaxial tensile tests were conducted using an Instron 5800 Series Universal Testing System (Instron, Norwood, MA). The force was measured with a 100 N load cell at room temperature with a crosshead speed of 10 mm min-1. The elastic modulus was determined from the slope of the initial linear region (0-3%), with a sample size of n=5. (See, e.g.. FIGS. 7B-C).Example 4Rib Fracture Surgery

[0233] Pre-operative analgesic in the form of Buprenorphine (0.05mg / kg) and Carprofen (5mg / kg) was administered prior to anesthesia. After appropriate anesthesia was induced with isoflurane as described above, rabbits were placed in left or right lateral decubitus position, and the contralateral lateral chest was clipped of hair, prepared, and draped in standard fashion. A 3 cm skin incision is made longitudinally along the fifth rib and chest wall muscles are bluntly separated to achieve adequate exposure of both the fourth and sixth rib without violating the underlying pleura. The fourth rib plate is first partially fixated with one 4 or 5mm titanium self-tapping screw (Synthes; West Chester, Pennsylvania). The position of the second screw is determined using the plate, and the hole for the second screw is made. The rib is then sharply divided with wire clippers at the midpoint of the plate, and the rib plate is fully fixated with the second screw. This is repeated with the sixth rib. Titanium plates were 1.5mm craniofacial midface plates (Synthes; West Chester, Pennsylvania),

[0234] A 6-0 Prolene horizontal mattress stitch is placed in the external oblique muscle, and the skin incision is closed with interrupted 5-0 Prolene deep dermal suture and surgical staples. Local anesthesia is then administered via injection of 25% bupivacaine along the incision. Postoperative analgesia was achieved with administration of Buprenorphine (0.03mg / kg) and Carprofen (5mg / kg), which was also administered daily until post-operative day three, Throughout postoperative week one, the rabbits were weighed and examined daily for any signs of hypoxia, bleeding, infection, hematoma / seroma formation, and incision dehiscence. Animals who lost morethan 10% weight were given saline injections and moist pellets. On post-operative day seven, surgical clips were removed under anesthesia.Example 5Radiologic Evaluation

[0235] Explanted ribs were radiographed with the MultiFocus X-Ray Imaging System (Faxitron; Tuscon, Arizona). Callus diameter was measured from radiographs, and callus index was calculated by dividing callus diameter by unaffected rib diameter. Rib fracture samples were assessed prior to decalcification with a VivaCT 80 scanner (Scanco Medical; Brüttisellen, Switzerland) using a 55-kVp source. Mineralized volume fraction (BV / TV) was used to quantify callus volume. The point of maximal callus diameter was selected as the callus midpoint and the midpoint allowed for 300 slices to be selected before and after that point for a total of 600 slices. One threshold value in the system included all original bone and newly formed from the callus. Another threshold value was used to include only the original bone. The BV / TV values from these two analyses then calculated the callus BV / TV. (See, e.g. FIGS, 26A-B)Example 6Mechanical Testing

[0236] For ribs fixated with biomaterial plates, 3-point bending tests were conducted using an Instron 5800 Series Universal Testing System (Instron, Norwood, MA). Ribs were placed on the stage with the midpoint of the attachment at the site of fracture. The ribs were placed concave for testing and stabilized by rubber bands on both ends.

[0237] The specimen was stressed at a rate of 5 mm min-1 until failure. Flexural modulus of the sample was obtained from the slope of the stress-strain curve at the initial strain values (0 - 3% strain). Flexural strength values were obtained from the point of the inflexion on the stressstrain graphs. This was assumed to be where the rib broke, and the values after this point was where the sample was held together by residual tissue. (See, e.g. FIGS. 7A-C).Example 7Histology and Quantification

[0238] After radiographs and micro-CTs were obtained, titanium screws were removed, and fracture calluses were formaldehyde-fixed for 1-3 days, decalcified with EDTA and processed for paraffin sectioning using an automated tissue processor. Serial sections (5uM) were collected witha microtome (Leica) for hematoxylin and eosin staining and immunohistochemical analyses. In order to quantify cellularization, cellular nuclei were stained with DAPI (1:1000) and quantified using Image!. Five fields of view (FoV) were taken and then each measured five times to generate 25 independent quantifications for each callus. These were then averaged to determine callus cellularization. In order to quantify callus cartilage content, calluses were stained with Alcian blue (Sigma- Aldrich) and quantified using ImageJ. Image color channels were split, and the red channel selected. Identical image thresholds were set to highlight the Alcian blue stain within the callus alone excluding both soft tissue and bone. Particles were then analyzed and the percentage area staining positive was recorded. (See, e.g., FIGS 3 A-B, 8).Example 8Statistics

[0239] Measurements were compared with paired t tests and ANOVA using Prism 9 as appropriate.Example 9Synthesis of 4-arm star polypropylene maleate) of a total DP20 with a meso-erythritol core

[0240] Meso-erythritol (112.12 g.mol"1, 249.1 mg, 2.04 mmol), Mg(BHT)2(THF)2(604.95 g.mol"1, 246.8 mg, 4.08×10-1mmol), anhydrous toluene (10.2 mL), MAn (98.06 g.mol'1, 4.0 g, 40.8 mmol) and PO (58.08 g.mol"1, 2.85 mL, 40.8 mmol) were introduced in a flame-dried schlenk, in this order. The schlenk was sealed with a PTFE plug and removed from the glovebox. The solution was stirred at 80 °C for 24 hrs. The resultant copolymer was recovered by precipitation in diethyl ether and then dried under vacuum to afford a sticky beige powder. Yield: 88 %.

[0241] The resulting 4-arm star polypropylene maleate) copolymer was characterized bylH NMR (500 MHz, 298 K, CDCh): 6.42-6.18 (m, 42.1 FI, C^OCHCHC^O), 5.44 (m, 2 H, C7 / (OR)CH2OR), 5.36-5.17 (m, 21.2 H, CH2C CH3O), 4.55-4.47 (d, 1.7 H, CH(OR)CH OR), 4.45-4.00 (m, 44.9 H, OC / / 2CHCH3), 1.41-1.23 (m, 54.3 H, CH(Cft)O), 1.23-1.0 (m, 12.1 H, CH(CTC)OH). A1H NMR spectrum of 4-arm star polypropylene maleate) of a total DP20 with a meso-erythritol core is shown in FIG. 17A. The degree of polymerization and the resulting molecular weight (Mn) were confirmed byNMR calculations. The molecular mass distribution (dispersity) (£>,„) was determined by size exclusion chromatography (SEC), and the trace is shown in FIG. 14. The results are reported on Table 5, below.DUK.p.woooi2Example 10Synthesis of 4-arm star polypropylene maleate) of a total DP40 with a meso-erythritol core

[0242] Meso-erythritol (112.12 g.mol"1, 124.5 mg, 1.02 mmol), Mg(BHT)2(THF)2 (604.95 g.mol'1, 123.4 mg, 2.04×10-1mmol), anhydrous toluene (10.2 mL), MAn (98.06 g.mol'1, 4.0 g, 40.8 mmol) and PO (58.08 g.mol'1, 2.85 mL, 40.8 mmol) were introduced in a flame-dried schlenk, in this order. The schlenk was sealed with a PTFE plug and removed from the glovebox. The solution was stirred at 80 °C for 48 hrs. The resultant copolymer was recovered by precipitation in diethyl ether and then dried under vacuum to afford a sticky beige powder. Yield: 78 %

[0243] The resulting 4-arm star polypropylene maleate) copolymer was characterized by NMR (500 MHz, 298 K, CDCI3): 6.42-6.18 (m, 79.3 H, C=OC / / CMC=O), 5.44 (m, 2 H, C / Z(OR)CH2OR), 5.36-5.17 (m, 37.5 H, CH2CY / CH3O), 4.55-4.47 (d, 2.1 H, CH(OR)CH / / OR), 4.45-4.00 (m, 86.5 H, OC / Z2CHCH3), 1.41-1.25 (m, 130.2 H, CH(CH O), 1.25-1.0 (m, 11.8 H, CH(CZ / 3)OH). A!H NMR spectrum of 4-arm star polypropylene maleate) of a total DP40 with a meso-erythritol core is shown in FIG. 12A. The degree of polymerization and the resulting molecular weight (Mn) were confirmed byfH NMR calculations. The dispersity (Dm) was determined by size exclusion chromatography (SEC), and the trace is shown in FIG. 14. The results are reported on Table 5, below.Example 11Synthesis of 4-arm star polypropylene maleate) of a total DP80 with a meso-erythritol core

[0244] Meso-erythritol (112.12 g.mol'1, 62.3 mg, 5.10×10-1mmol), Mg(BHT)2(THF)2 (604.95 g.mol'1, 61.7 mg, 1.02×10-1mmol), anhydrous toluene (10.2 mL), MAn (98.06 g.mol'1, 4.0 g, 40.8 mmol) and PO (58.08 g.mol'1, 2.85 mL, 40.8 mmol) were introduced in a flame-dried schlenk, in this order. The schlenk was sealed with a PTFE plug and removed from the glovebox. The solution was stirred at 80 °C for 100 hrs. The resultant copolymer was recovered by precipitation in diethyl ether and then dried under vacuum to afford a sticky beige powder. Yield: 82 %

[0245] The resulting 4-arm star polypropylene maleate) copolymer was characterized by NMR (500 MHz, 298 K, CDCI3): 6.47-6.18 (m, 161.3 H, C=OCMCMC=O), 5.44 (m, 2 H, CJ7(OR)CH> OR), 5.37-5.05 (m, 82.2 H, CH2C / ZCH3O), 4.58-4.46 (d, 2.4 H, CH(OR)CHFZOR), 4.45-3.98 (m, 194.8 H, OCM2CHCH3), 1.51-1.25 (m, 251.4 H, CH(CH?)O), 1.21-1.0 (m, 13.6 H,NMR spectrum of 4-arm star polypropylene maleate) with a meso-erythritolcore is shown in FIG. 12A The degree of polymerization and the resulting molecular weight (Mn) were confirmed by3H NMR calculations. The dispersity (Dm) was determined by size exclusion chromatography (SEC), and the trace is shown in FIG. 14. The results are reported on Table 5.Example 12Synthesis of 4-arm star polypropylene maleate) of a total DP 120with a meso-erythritol core

[0246] Meso-erythritol (112.12 g.mol-1, 31.1 mg, 2.55×10-3mmol), Mg(BHT)2(THF)2(604.95 g.mol"1, 30.8 mg, 5.10×10-2mmol), anhydrous toluene (7.6 mL), MAn (98.06 g.mol"1, 3.0 g, 30.6 mmol) and PO (58.08 g.mol-1, 2.14 mL, 30.6 mmol) were introduced in a flame-dried schlenk, in this order. The schlenk was sealed with PTFE plug and removed from the glovebox. The solution was stirred at 80 °C for 150 hrs. The resultant copolymer was recovered by precipitation in diethyl ether and then dried under vacuum to afford a sticky beige powder. Yield: 72 %

[0247] The resulting copolymer was characterized by *H NMR (500 MHz, 298 K, CDCh): 6.50-6.18 (m, 239.9 H, C=OC / / CHC=O), 5.44 (m, 2 H, C / / (OR)CH2OR), 5.37-4.96 (m, 113.2 H, CH2CI7CH3O), 4.58-4.46 (d, 2.1 H, CH(OR)CHHOR), 4.45-3.94 (m, 232.8 H, OC / / 2CHCH3), 1.49-1.22 (m, 318.5 H, CH(Cft)O), 1.22-1.0 (m, 14.9 H, CH(Cft)OH). A!H NMR spectrum of 4-arm star poly(propylene maleate) with a meso-erythritol core is shown in FIG. 12A. The degree of polymerization and the resulting molecular weight (Mn) were confirmed by1H NMR calculations. The dispersity Đm) was determined by size exclusion chromatography (SEC), the trace is shown in FIG. 14. The results are reported on Table 5, below.Table 5Molecular characteristics of 4-arm star-shaped PPCopolymer Target DP „MAn,0 / . DP (fH NMR)! J cConversion (%)7Example! 20 (4 x 5) 99 21 3,400 1.45 Example 2 40 (4 x 10) 95 40 6,300 1.44 Example 3 80 (4 x 20) 99 82 12,900 1.48 Example 4 120 (4 x 30) 82 120 18,800 1.35Example 13Synthesis of 5-arm star polypropylene maleate) of a total DP4C) with an adonitol core

[0248] Adonitol (152.15 g.mol"1, 116.3 mg, 7.65x10"’ mmol), Mg(BHT)2(THF)2 (604.95 g.mol"1, 92.5 mg, 1.53x1 O’1mmol), anhydrous toluene (7.6 ml), MAn (98.06 g.mol'1, 3.0 g, 30.6 mmol) and PO (58.08 g.mol"1, 2.14 mL, 30.6 mmol) were introduced in a flame-dried schlenk, in this order. The schlenk was sealed with a PTFE plug and removed from the glovebox. The solution was stirred at 80 °C for 48 hrs. The resultant copolymer was recovered by precipitation in diethyl ether and then dried under vacuum to afford a sticky beige powder. Yield: 85 %

[0249] The resulting 5-arm star polypropylene maleate) copolymer was characterized by ’H NMR (500 MHz, 298 K, CDCI3): 6.47-6.16 (m, 79.8 H, C=OC / / C7 / C=O), 5.64-5.43 (m, 3 H, ORCH2CZ / (OR)C / Z(OR)CJ / (OR)CH2OR), 5.40-5.00 (m, 36.7 H, CH2C / / CH3O), 4.61-4.45 (d, 2.3 H, CH(OR)CHZZOR), 4.45-3.95 (m, 78.1 H, OCZACHCH3), 1.44-1.22 (m, 119.1 H, CH(Cft)O), I.22-1.0 (m, 14.18 H, CH(C / / ?)OH). The degree of polymerization and the resulting molecular weight (Mn) were confirmed byN MR calculations. The dispersity (£>,„) was determined by size exclusion chromatography (SEC). The results are reported on Table 6, below.Table 6Molecular characteristics of 5-arm star-shaped PPM.Copolymer Target DPMAnDP ([HNMR)conversion (%) (g.mol )Example 5 40 (5 x 8) 97 44 7,000 1.72Isomerization of the star-shaped PPM into a star-shaped PPF[1)0250] The general procedures for the isomerization reaction are as follows: the multi -arm PPM copolymer was dissolved in chloroform, to reach a concentration of 0.5 mol. L"’ of MAn residues. Diethylamine (DEA) (0.15 eq / MAn residue) was added and the solution was refluxed for 24 hrs under inert atmosphere. The organic layer was washed with 1 M sodium phosphate aqueous solution and the copolymer was recovered by evaporation under vacuum to afford a sticky beige powder.Example 14Isomerization of 4-arm star PPM of a total DP20 with a meso-erythritol coreinto the corresponding star-shaped PPF

[0251] 6 g of the star-shaped PPM (1.79 mmol, 37.1 mmol of MAn residue) recovered from Example 9 were dissolved in 74 mL of chloroform and 0.58 mL of diethylamine (5.57 mmol) was added to the solution. The solution was heated to reflux under inert atmosphere for 24 hours. The organic solution was then washed with a sodium phosphate aqueous solution, chloroform removed by evaporation under vacuum to afford a sticky beige powder. Yield; 93 %.

[0252] The resulting copolymer was characterized by1H NMR (500 MHz, 298 K, CDCh) a!H NMR spectrum of 4-arm star poly(propylene fumarate) of a total DP20 with a meso-erythritol core is shown in FIG. 17 (bottom).NMR spectra performed before and after isomerization reaction attests that the 4-arm star PPM of Example 1 was successfully isomerized to form the corresponding 4-arm star PPF by showing a disappearance of the proton resonance signal corresponding to cw-alkene protons (5 6.2 ppm) and an appearance of the new proton resonance signal corresponding to / rans-alkene protons (6 = 6.7 ppm).Example 15Isomerization of 4-arm star PPM of a total DP 40 with a meso-erythritol coreinto the corresponding star-shaped PPF

[0253] 4.8 g of the star-shaped PPM (7.62 x 10~!mmol, 30.5 mmol of MAn residue) recovered from Example 10 were dissolved in 61 mL of chloroform and 0.47 mL of diethylamine (4.57 mmol) was added to the solution. The solution was heated to reflux under inert atmosphere for 24 hours. The organic solution as then washed with an aqueous sodium phosphate solution, and the chloroform removed by evaporation under vacuum to afford a sticky beige powder. Yield: 95 %

[0254] The resulting copolymer was characterized by!H NMR (500 MHz, 298 K, CDCh) a!H NMR spectrum of 4-arm star poly(propylene fumarate) of a total DP40 with a mexo-erythritol core is shown in FIG. 19 (bottom), 'll NMR spectra performed before and after isomerization reaction attested that star PPM of Example 2 was successfully isomerized to form the corresponding star PPF by showing the disappearance of the proton resonance signal corresponding to cis-alkene protons (5::::6.2 ppm) and the appearance of the new proton resonance signal corresponding to ira / ?x-alkene protons (8 = 6.7 ppm).Example 16Isomerization of 4-arm star PPM of a total DP80 with a meso-erythritol coreinto the corresponding star-shaped PPF

[0255] 5.5 g of the star-shaped PPM (4.26×10-1mmol, 35.0 mmol of MAn residue) recovered from Example 11 were dissolved in 70 mL of chloroform and 0.54 ml of diethylamine (5.24 mmol) was added to the solution. The solution was heated to reflux under inert atmosphere for 24 hours. The organic solution was then washed with a sodium phosphate aqueous solution, chloroform removed by evaporation under vacuum to afford a sticky beige powder. Yield: 91 %. The resulting copolymer was characterized byNMR (500 MHz, 298 K, CDCh) aiH NMR spectrum of 4-ann star polypropylene fumarate) of a total DP80 with a w o-erythritol core is shown in FIG. 21 (bottom).1H NMR spectra performed before and after isomerization reaction attested that star PPM of Example 3 was successfully isomerized into the corresponding star PPF by showing the disappearance of the proton resonance signal corresponding to c? -alkene protons (S = 6.2 ppm) and the appearance of the new proton resonance signal corresponding to fraws-alkene protons (8 = 6.7 ppm).Example 17Isomerization of 4-arm star PPM of a total DP 120 with a meso-erythritol coreinto the corresponding star-shaped PPF

[0256] 3.5 g of the star-shaped PPM (1.86 x 10-1mmol, 23.2 mmol of MAn residue) recovered from Example 12 were dissolved in 46 mL of chloroform and 0.36 mL of diethylamine (3.48 mmol) was added to the solution. The solution was heated to reflux under inert atmosphere for 24 hours. The organic solution was then washed with a sodium phosphate aqueous solution, chloroform removed by evaporation under vacuum to afford a sticky beige powder. Yield: 95 % 100257] The resulting copolymer was characterized by H NMR (500 MHz, 298 K, CDCls), a ‘H NMR spectrum of 4-arm star poly(propylene fumarate) of a total DP 120 with a meso-erythritol core is shown in FIG. 23 (bottom).1H NMR spectra performed before and after isomerization reaction attested that star PPM of Example 5 was successfully isomerized to form the corresponding star PPF by showing the disappearance of the proton resonance signal corresponding to ci -alkene protons (8 = 6.2 ppm) and the appearance of the new proton resonance signal corresponding to / ra y-alkene protons (8::::6,7 ppm).Example 18Isomerization of5-arm star PPM of a total DP40 with an adonitol coreinto the corresponding star-shaped PPF

[0258] 3.6 g of the star-shaped PPM (5.14×10-1mmol, 23.1 mmol of MAn residue) recovered from Example 13 were dissolved in 46 mL of chloroform and 0.36 mL of diethylamine (3.47 mmol) was added to the solution. The solution was heated to reflux under inert atmosphere for 24 hours. The organic solution was then washed with a sodium phosphate aqueous solution, chloroform removed by evaporation under vacuum to afford a sticky beige powder. Yield: 97 %

[0259] The resulting copolymer was characterized bylH NMR (500 MHz, 298 K, CDCk)lH NMR spectra performed before and after isomerization reaction attested that star PPM of Example 5 was successfully isomerized to the corresponding star PPF by showing the disappearance of the proton resonance signal corresponding to cri-alkene protons (6 = 6.2 ppm) and the appearance of the new proton resonance signal corresponding to frz -alkene protons (8::::6.7 ppm).Example 19Synthesis of star-shaped polypropylene maleate) (PPM).

[0260] Four-arm star-shaped polypropylene maleate) (PPM) copolymers were synthesized by ring-opening copolymerization (ROCOP) of maleic anhydride (MAn) and propylene oxide (PO) using weso-erythritol as an initiator. Various [monomers] / [initiator] molar ratios were used to obtain copolymers with different PPM arm lengths and consequently various degrees of polymerization (DPs). For instance, four-arm star PPM with target a degree of polymerization (DP) 40, was prepared as follows: in a glovebox, meso-erythritol (112.12 g-mol'1, 124.5 mg, 1.02 mmol), Mg(BHT)2(THF)2 (604.95 g mol"1, 123.4 mg, 2.04x10'’ mmol), anhydrous toluene (10.2 mL), MAn (98.06 g-mol'1, 4.0 g, 40.8 mmol) and PO (58.08 g-mol'1, 2.85 mL, 40.8 mmol) were introduced, in this order, in a flame-dried Schlenk tube. The Schlenk tube was sealed with a PTFE plug and removed from the glovebox. The solution was stirred at 80CC for 48 h (typically until the PPM precipitates in the bottom of the Schlenk and the supernatant looked clear). The resultant copolymer was recovered by precipitation in diethyl ether and then dried under vacuum to afford a highly viscous oil (Yield: 78 %). The influence of the total monomer concentration (1 M, 2 M, 4 M, 8 M and 14 M) on the monomer conversion was investigated by performing syntheses of star PPM with mes’o-erythritol as an initiator and total target DPs of 20, 40, 80, 120 and 200. Moreover, the influence of the total monomer concentration on the copolymerization process was investigatedby performing kinetic studies at 2 M, 4 M and 8 M, with meso-erythritol as an initiator and total target DP 40. The initial mixture was split in several vials, immersed in a preheated bath at 80 °C (corresponding to the time zero of the reaction), copolymerizations were conducted under stirring and stopped by quenching to ambient temperature and adding an excess of chloroform. The monomer conversions were determined by 'H NMR in CDCk on crude samples from reaction volumes. For comparison, the kinetics of copolymerization using propargyl alcohol as monofunctional initiator were investigated for monomer concentrations of 8 M and target total DPs of 10 and 40.Example 20Isomerization of PPM.

[0261] The PPM copolymer of Example 19 was dissolved in chloroform at a concentration of 0.5 mol'L'1of MAn residues and diethylamine (DEA) was added to reach 0.15 eq / MAn residue. As an example, four-arm star PPM with target total DP40 were isomerized in the corresponding four-arm star PPF as follows: star-shaped PPM (4.8 g. 7.62 x IQ'1mmol, 30.5 mmol of olefin) was dissolved into chloroform (61 mL, 0.5 mol-L’1of olefin), DEA (0.47 mL, 0.15 mol. eq. olefin) was added and the solution was heated under reflux for 24 h under a nitrogen atmosphere. After cooling to ambient temperature, the organic solution was washed with I M sodium phosphate solution (250 mL, pH = 6) and the copolymer was recovered after evaporation of the chloroform. Yield: 95 %.Example 21Representative synthesis of four-arm fumarate-based copolyester star polymer.

[0262] Four-arm star polypropylene maleate) (PPM) copolymers were synthesized by a ringopening copolymerization reported previously. See, e.g., Fer, G. L.; Luo, Y.; Becker, M. L. Poly(Propylene Fumarate) Stars, Using Architecture to Reduce the Viscosity of 3D Printable Resins. Polymer Chemistry 2019, 10 (34), 4655-4664. https: / / doi.org / 10.1039 / C9PY00738E; Kirillova, A.; Yeazel, T. R.; Gall, K.; Becker, M. L, Thiol-Based Three-Dimensional Printing of Fully Degradable Poly(Propylene Fumarate) Star Polymers. ACS AppL Mater. Interfaces 2022, 14 (34), 38436-38447. https: / / doi.org / 10.l021 / acsami.2c06553; and U. S. Patent No. 11,661,477, the disclosures of which are incorporated herein by reference in their entirety. Under an inert nitrogen atmosphere in a 1 -liter round bottom equipped with a stir bar, maleic anhydride (100.0 g, 1.0 mol, 150 eq.) and propylene oxide (71.0 mL, 1.0 mol, 150 eq.) were added to a solution containingmeso-erythritol initiator (0.83 g, 0.007 mol, 1.0 eq.) and catalyst Mg(BHT)2(THF)2 (1.650 g, 2.6 x 10'-’ mol, 0.4 cq.) dissolved in anhydrous toluene (300 mL) to achieve a target degree of polymerization (DPn) of 120. The solution was stirred at 80 °C for 10 days, at which point 80% conversion was achieved as determined by[H NMR spectroscopy of the crude solution. The polymerization was cooled to ambient temperature and quenched with chloroform. Four-arm star PPM was recovered by precipitation twice into hexanes and dried by rotary evaporation.

[0263] The four-arm star PPM was isomerized to the trans fumarate -based copolyester star polymer by refluxing with diethylamine (15.00 mL, 0.145 mol, 0.15 eq. relative to alkene) in chloroform at 60 °C overnight. Following complete isomerization, the polymer was washed three times w ith a 1.0 M solution of sodium phosphate. The organic layer was collected and dried with sodium sulfate. The polymer was dried by rotary evaporation, followed by high vacuum to yield four-arm fumarate-based copolyester star polymer.Example 22Animal Model

[0264] Thirty-two adult New Zealand White rabbits were purchased from Charles River (Wilmington, Massachusetts). Rabbits underwent rib fracture surgery of the 4thand 6thribs with immediate fixation using a plate. Rabbits were sacrificed at four weeks post-operatively, and hemithoraces were removed for evaluation with x-ray imaging. Of the eight rabbits in each biomaterial group, four underwent mechanical testing of their explanted ribs and four underwent micro CT followed by staining. Ribs who received titanium rib plates did not undergo mechanical testing. The study was approved by the Institutional Animal Care and Use Committee at our institution (A122-20-06), and all investigators complied with the National Research Council’s Guide for the Care and Use of Laboratory Animals. Using the Enhancing the Quality and Transparency Of Health Research (EQUATOR) Network guidelines it was determined that “none of the most popular checklists are appropriate for your study design, but you may still useful guidelines by searching the full EQUATOR library’, which covers 250+ study designs.” Further search for reporting guidelines using “Animal pre-clinical studies” as “Study type” and “Surgery” as “Clinical Area” did not yield any reporting guidelines.Materials

[0265] All reagents used in Examples 23 -35 were purchased from Sigma-Aldrich and used as received unless otherwise specified. Solvents were purchased from either Fisher Scientific or Sigma-Aldrich and dried using a Pure Solv MD-3 solvent purification system (Inert Corporation, Amesbury, MA). Propylene oxide was dried over calcium hydride prior to distillation. Meso- erythritol was dried overnight under vacuum prior to polymerization.100266] Titanium midface plates were obtained from DePuy Synthes (Matrix IDFACE Plates, part #04.503.346) and cut to 4 screw holes. PLA midface plates were 3D printed on an Dremel DigiLab 3D45 (Mount Prospect, IL) printer with 1.75 mm PLA filament.Example 23CLIP photochemical 3D printing.

[0267] All samples were fabricated using a Carbon (Redwood, CA) M2 printer ( λ = 385 nm).Four-arm fumarate-based copolyester star polymer was dissolved in ethyl acetate (7:3 w / w), to which 0.6 wt% phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO) and 0.4 wt.% of oxybenzone (OB) relative to polymer mass were added and shaken overnight to form a resin. Immediately prior to printing, trimethylolpropane tris(3-mercaptopropionate) was added to the resin to achieve the desired crosslinking ratio of 20:1 of polymer backbone alkene to thiol crosslinker (mol / mol). In resins containing hydroxyapatite (HAp), 10 wt% of HAp was added immediately before printing, with respect to the total mass of polymer, BAPO, OB, and thiol crosslinker. Cure tests were performed to determine optimal photocuring conditions.

[0268] The STL files were obtained from open-source locations or created using AutoCAD. For the tensile measurements, ASTM D638 Type V tensile bars were printed. (See, e.g., FIG. 10B). The printed parts were washed with ethyl acetate and isopropyl alcohol (IPA), placed in a deionized water bath, then post-cured in a B9 Model Cure UV oven (B9Creations, 70W, 55 Hz, λ = 390-420 nm) for 15 minutes. Post-cured parts were dried under vacuum at 60 °C for 5 days prior to further analysis.Example 24Mechanical characterization of 3D printed fumarate-basedcopolyester star polymers and orthopedic plates.

[0269] Uniaxial tensile tests of 3D printed tensile bars were conducted using an Instron 5800 Series Universal Testing System (Instron, Norwood, MA). The force was measured with a 100 Nload cell at room temperature with a crosshead speed of 10 mm min-1. The elastic modulus was determined from the slope of the stress-strain curve at the initial linear region (0-3% strain) for both fumarate-based copolyester and HAp composite samples at room temperature and 37 °C (n = 5). Three-point bend flexural tests of 3D printed orthopedic plates were conducted using a Discovery DMA 850 (TA Instruments, New Castle, DE) at a strain rate of 5 mm min-1. The flexural modulus was determined from the slope of the of the stress-strain curve at the initial linear region (0-3% strain) for PLA, fumarate-based copolyester, and fumarate-based copolyester-HAp composite plates at ambient temperature and 37 °C (n = 3). (See, e.g., FIG. 7C)Example 25Live / dead assays.

[0270] Bone marrow derived human mesenchymal stem cells (BM-hMSCs) from LifeLine Cell Technology (Frederick, MD) were cultured and expanded in DMEM (ThermoFisher, Waltham, MA) supplemented with 10% fetal bovine serum (FBS) (Sigma Aldrich, St. Louis, MO) and 1% penicillin streptomycin, and Amphotericin B (ThermoFisher, Waltham, MA). BM-hMSCs were seeded at P6-P7 on 22 mm x 22mm fumarate-based copolyester and fumarate-based copolyester-composite spin coated coverslips. The cells were seeded at a density of 5,000 cells / cm2. Cell number and viability were obtained at 24 and 72 hours using LIVE / DEAD Viability / Cytotoxicity kit (Invitrogen, Waltham, MA). Cell counts and viability were completed with Cell Profiler (Cambridge, MA) and statistical analysis was performed using GraphPad Prism (Boston, MA). See, e.g., FIGS. 16A-C).Example 26In vivo rabbit rib fracture model.

[0271] Animal protocols were approved by the Institutional Animal Care and Use Committee at Duke University (A122-20-06), and all investigators complied with the National Research Council’s Guide for the Care and Use of Laboratory Animals. Pre-operative analgesic in the form of Buprenorphine (0.05 mg kg’1) and Carprofen (5 mg kg-1) was administered prior to anesthesia. Thirty-two adult New Zealand white rabbits (Charles River Laboratories, Wilmington. MA) underwent rib fracture surgery of the 4thand 6thribs with immediate fixation. At the 4thand 6thribs, the rib plate was first partially fixated with one 4- or 5-mm titanium self-tapping screw (MatrixMIDFACE Screw, part #04.503.223.01). The position of the second screw was determinedusing the plate, and the hole for the second screw was made. The rib was then sharply divided with wire clippers at the midpoint of the plate, and the rib plate was fully fixated with the second screw.

[0272] Rabbits were sacrificed at two or four weeks post-operatively, and hemi-thoraces were removed for evaluation with x-ray imaging. Of the eight rabbits in each group, four underwent mechanical testing of their explanted ribs and four underwent radiological evaluation and micro-CT, followed by histological characterization. (See, e.g., FIGS. 22A-D, 23, 24, 25A-F, and 26A-B).Example 27Biomechanical characterization of explanted rabbit ribs.

[0273] Three-point bending tests were conducted using an Instron 5800 Series Universal Testing System (Instron, Norwood, MA). Rib plates were removed prior to testing. Ribs were placed concave on the stage with the midpoint of the attachment at the site of fracture, stabilized by rubber bands on both ends. The specimen was stressed at a rate of 5 mm min-1until failure. The flexural modulus of the sample was obtained from the slope of the stress-strain curve at the initial linear region (0-5% strain). Flexural strength values were obtained from the point of the inflexion on the stress-strain curves. Toughness was calculated from the area under the curve up to this point of inflexion.Example 28Micro-computed tomography (µCT) of explanted rabbit ribs.

[0274] Explanted rabbit ribs were fixed in 10% formalin for 48 h at room temperature (25 °C) and then transferred to 70% ethanol. Titanium implants and screws were removed from the ribs prior to scanning. The quality of fracture repair was assessed using the Faxitron MX20 X-ray system (Faxitron, Tucson, AZ, USA). Quantitative three-dimensional evaluation of the fracture callus and healing was then undertaken by µCT using a Viva CT 80 (Scanco, Brüttisellen, Switzerland) at 55kVp and 145 pA with a resolution of 15.6 µm voxel size. A hydroxyapatite calibration phantom was used to scale values of linear attenuation for the calcified tissues to bone density values (mg cm-3). Morphometric parameters were quantified from the plate screw hole to screw hole with site of fracture situated in the middle, or the length of the healing callus, whichever was larger. The original grayscale image datasets of the selected region of interest were then imported into the manufacturer software and the calcified tissues were segmented from soft tissues using a global threshold of 480 mg HA / cm3, representing 45% of the attenuation of mature corticalbone. Morphometric parameters such as bone volume / total volume (BV / TV) were analyzed using ASBMR guidelines.Example 29Histology and ISO scoring of explanted rabbit ribs.

[0275] Following µCT. explanted rabbit ribs were decalcified in 14% EDTA (pH 7.4) for 14 days at 4 degrees. Samples were subsequently dehydrated in a graded ethanol series and embedded into melted paraffin wax. Samples were sectioned at 5 µm thickness and collected on microscope slides. After drying overnight, mounted sections were stained with either Hematoxylin and Eosin (H& E) or Alcian Blue / Picrosirius Red. Images were collected on a KEYENCE BZ-X710 Analyzer (KEYENCE Corporation, Osaka, Japan). ISO (10993-6:2016) scoring of H& E-stained slides was performed on 2-3 sites per animal at different areas of the device and then scores averaged for final analysis, following ISO recommendations.Example 30Statistical analyses

[0276] Statistical analyses were performed using GraphPad Prism 10. Data are expressed as mean ± standard deviation (SD). Rib mechanical data were analyzed using one-way ANOVA, followed by post-hoc Tukey multiple comparisons test. pCT quantifications and live / dead data were analyzed by two-way ANOVA with Tukey multiple comparisons test. P-value thresholds of *p < 0.05, **p < 0.01, ***p < 0.001, ****p < 0.0001 were used to define statistical significance.Example 31Representative synthesis of Mg(BHT)2(THF)2 catalyst.

[0277] Mg(BHT)2(THF)2 was synthesized by a method reported previously. See, Wilson, J. A.; Luong, D.; Kleinfehn, A. P.; Sallam, S.; Wesdemiotis, C.; Becker, M. L. Magnesium Catalyzed Polymerization of End Functionalized Poly(Propylene Maleate) and PolyfPropylene Fumarate) for 3D Printing of Bioactive Scaffolds. J. Am. Chem. Sac. 2018, 140 (1), 277-284. https: / / doi.org / 10.1021 / jacs.7b09978, the disclosure of which is incorporated by reference in its entirety. A 2-neck 500-mL, round bottom was equipped with an addition funnel, flow control adapter, and a stir bar and placed under an inert nitrogen atmosphere. Butylhydroxytoluene (BHT) (26.9 g, 0.122 mol, 2.0 eq.) was added to the flask and dissolved in anhydrous tetrahydrofuran (THF) (60.0 mL, 0.733 mol, 12.0 eq.). n-butyl-sec-butylmagnesium (85.8 mL, 0.061 mol, 1.0 eq.,0.7 M in hexane) was added dropwise to the stirring solution via the addition funnel, and the reaction was stirred overnight at room temperature, Solvent was removed under reduced pressure to yield the catalyst as a white solid (33.0 g, 86% yield). The catalyst was dried under high vacuum for 4 days then transferred to a nitrogen-filled glovebox.Example 32Nuclear magnetic resonance (NMR) spectroscopy.

[0278] Proton (1H) (500 MHz) and carbon (13C) (125 MHz) NMR spectra were acquired on a Bruker AVANCE NEO 500 MHz spectrometer at room temperature. Chemical shifts were recorded in parts per million (ppm) relative to the chloroform (CDCh) reference resonance at d = 7.26 ppm for T1 NMR and 6 = 77.16 ppm forl’C NMR. (See, e.g., FIGS. 12A-B, 13).Example 33Size exclusion chromatography (SEC).

[0279] Weight average (M̄w) and number average (M̄n) molecular mass were determined by size exclusion chromatography (SEC) using an EcoSEC HLC-8320GPC (Tosoh Bioscience LLC, King of Prussia, PA) with a TSKgel G HHR- mixed bed column, refractive index (RI) detector and NIST-certified poly(styrene) standards. Samples were prepared at -3 mg / mL using HPLC grade tetrahydrofuran (THF) for injection with a 0.4 mL min’1flow rate at 40 °C.Example 34Thermal gravimetric analysis (TGA).

[0280] Degradation temperatures (Td) were determined by TGA using a TA Instruments Discovery TGA550 (TA Instruments - Waters L. L. C, New Castle, DE). Approximately 10 mg of sample was heated from 25-600 °C at a ramp rate of 20 °C / min. Degradation temperature was evaluated at the inflection point in the thermogram. (See, e.g. FIG. 18A).Example 35Differential scanning calorimetry (DSC).

[0281] Glass transition temperatures (Tg) were determined by DSC using a TA Instruments Discovery DSC250 (TA Instruments - Waters L. L. C., New’ Castle, DE). Approximately 10 mg of sample was heated / cooled at a ramp rate of 10 °C / min for 2 heating and cooling cycles. Glass transition temperature was evaluated at the inflection point in the curve. (See, e.g., FIG. 18B).

[0282] One skilled in the art will readily appreciate that the present disclosure is well adapted to carry out the objects and obtain the ends and advantages mentioned, as well as those inherent therein. The present disclosure described herein are presently representative of preferred embodiments, are exemplary, and are not intended as limitations on the scope of the present disclosure. Changes therein and other uses will occur to those skilled in the art which are encompassed within the spirit of the present disclosure as defined by the scope of the claims.

[0283] No admission is made that any reference, including any non-patent or patent document cited in this specification, constitutes prior art. In particular, it will be understood that, unless otherwise stated, reference to any document herein does not constitute an admission that any of these documents forms part of the common general knowledge in the art in the United States or in any other country. Any discussion of the references states what their authors assert, and the applicant reserves the right to challenge the accuracy and pertinence of any of the documents cited herein. All references cited herein are fully incorporated by reference, unless explicitly indicated otherwise. The present disclosure shall control in the event there are any disparities between any definitions and / or description found in the cited references.

[0284] In light of the foregoing, it should be appreciated that the present invention significantly advances the art by providing a resorbable composite plate that is structurally and functionally improved in a number of ways, While particular embodiments of the invention have been disclosed in detail herein, it should be appreciated that the invention is not limited thereto or thereby inasmuch as variations on the invention herein will be readily appreciated by those of ordinary' skill in the art. The scope of the invention shall be appreciated from the claims that follow.

Claims

CLAIMSWhat is claimed is:

1. A resin for use in a resorbable 3D printed osteosynthetic apparatus for rib fracture repair comprising:a linear or star-shaped polypropylene fumarate)-based copolymer comprising at least one of an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block and a star-shaped polypropylene fumarate) copolymer;a thiol-based crosslinker; anda plurality of filler nanoparticles,2. The resin of claim 1 further comprising a diluent and a photoinitiator.

3. The resin of claim 2 further comprising a photoinhibitor.

4. The resin of claim 1 wherein said linear or star-shaped polypropylene fumarate)-based copolymer is an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block comprising the residue of a difunctional alcohol initiator.

5. The resin of claim 1 comprising an ABA block copolymer having a formula selected from:where each n is an integer from about 1 to about 20, each m is an integer from about 2 to about 70, and I is the residue of an initiator having at least two reactive hydroxyl, thiol or carboxylic acid groups.

6. The resin of claim 1 wherein said linear or star-shaped polypropylene fumarate)-based copolymer is a star-shaped polypropylene fumarate) copolymer comprising 3 or 4 polypropylene fumarate) aims extending from a multi-functional alcohol initiator.

7. The resin of claim 1 comprising a star-shaped polypropylene fumarate) copolymer having the formula:where each m is an integer from about 10 to about 50.

8. The resin of claim 1 wherein said ABA block copolymer has a degree of polymerization of from about 10 to about 100.

9. The resin of claim 1 wherein said star-shaped polypropylene fumarate) copolymer has a degree of polymerization of from about 40 to about 200.

10. The resin of claim 6 wherein each arm of said 3 or 4 polypropylene fumarate) arms extending from a multi-functional alcohol initiator copolymer has a degree of polymerization of from about 10 to about 50.

11. The resin of claims 2 or 3 wherein said linear or star-shaped polypropylene fumarate)-based copolymer comprises from about 50 wt.% to about 90 wt.% of said resin.

12. The resin of claims 2 or 3 wherein said linear or star-shaped polypropylene fumarate)-based copolymer comprises about 70 wt.% of said resin.

13. The resin of claim 1 wherein said thiol-based crosslinker is a molecule having 3 available thiol functional groups.

14. The resin of claim 1 wherein the thiol-based crosslinker comprises trimethylolpropane tris(3- mercaptopropionate), trimethylolpropanetris(3-mercaptopropionate), Thiocure 332 and Thiocure 333, ETTMP-700, ETTMP-1300, and combinations thereof.i 5. The resin of claim 1 wherein the thiol-based crosslinker has a formula selected from:

16. The resin of claim 1 wherein the thiol-based crosslinker comprises from about 0.5 to about 10 mole percent of said resin.

17. The resin of claim 1 wherein the ratio of available alkene groups in said linear or star-shaped polypropylene fumarate)-based copolymer to available thiol groups in said thiol-based crosslinker in said resin is from about 3:1 to about 40:1.

18. The resin of claim 1 wherein the ratio of available alkene groups in said linear or star-shaped polypropylene fumarate)-based copolymer to available thiol groups in said thiol-based crosslinker in said resin is about 20:1.

19. The resin of claim 1 wherein said plurality of filler nanoparticles comprises are selected from hydroxyapatite (HAp), strontium carbonate, tricalcium phosphate, barium phosphate and combinations thereof.

20. The resin of claims 2 or 3 wherein said plurality of filler nanoparticles comprises from about 1 to about 20 weight percent of said resin.

21. The resin of claims 2 or 3 wherein said plurality of filler nanoparticles comprise about 10 weight percent of said resin.

22. The resin of claim 1 wherein said plurality of filler nanoparticles have a mean particle size of from about 100 nm to about 1000 nm.

23. The resin of claim 1 wherein said plurality of filler nanoparticles are hydroxyapatite (HAp) nanoparticles having a mean particle size of from about 100 nm to about 500 nm.

24. The resin of claims 2 or 3 having a complex viscosity of less than 50 Pa -sec.

25. The resin of claims 2 or 3 having a complex viscosity of from about 5 to about 15 Pa-sec.

26. The resin of claims 2 or 3 having a complex viscosity suitable for 3D printing by Continuous Liquid Interface Production (CLIP) photochemical printing.

27. The resin of claim 2 or 3 wherein said diluent comprises from about 10 wt.% to about 50 wt.% of said resin.

28. The resin of claims 2 or 3 wherein said diluent comprises from about 30 wt.% of said resin.

29. The resin of claims 2 or 3 wherein said diluent is selected from the group ethyl acetate, acetone, dioxane, and combinations thereof.

30. The resin of claims 2 or 3 wherein said photoinitiator is selected from the group consisting of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO).

31. The resin of claim 3 wherein said photoinhibitor is selected from the group consisting of oxybenzone (HMB).

32. A 3D printed osteosynthetic composite material comprising the resin of any one of claims 1- 31.

33. The 3D printed osteosynthetic composite material of claim 32 comprising:a linear or star-shaped poly(propylene fumarate)-based copolymer comprising at least one of an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block and a star-shaped polypropylene fumarate) copolymer;a thiol -based crosslinker; anda plurality of filler nanoparticles.DUK. P W0001234. A 3D printed osteosynthetic apparatus for rib fracture repair comprising the 3D printed osteosynthetic composite material of claim 33.

35. The 3D printed osteosynthetic apparatus for rib fracture repair of claim 34 wherein said linear or star-shaped polypropylene fumarate)-based copolymer comprises a resorbable ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block, wherein said first and second polypropylene fumarate) A blocks are each bonded covalently to an end of said polypropylene succinate) B polymer block to form an ABA block copolymer.

36. The 3D printed osteosynthetic apparatus for rib fracture repair of claim 34 wherein said linear or star-shaped polypropylene fumarate)-based copolymer comprises a resorbable starshaped polypropylene fumarate) copolymer comprising 3 or 4 polypropylene fumarate) arms extending from a multi-functional alcohol initiator.

37. The resorbable 3D printed osteosynthetic apparatus for rib fracture repair of claim 34, further comprising a filler material to promote bone repair and / or regrowth.

38. The resorbable 3D printed osteosynthetic apparatus for rib fracture repair of claim 34, wherein said filler material is hydroxyapatite.

39. The resorbable 3D printed osteosynthetic apparatus for rib fracture repair of claim 34, comprising from 1 wt.% to 20 wt.% hydroxyapatite.

40. The resorbable 3D printed osteosynthetic apparatus for rib fracture repair of claim 34, wherein said apparatus is a plate.

41. The resorbable 3D printed osteosynthetic apparatus for rib fracture repair of claim 40, further comprising a plurality of openings sized to receive surgical screws.

42. A method for making the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of claim 34 comprising:A) measuring and / or imaging a rib fracture on a subject having a rib fracture;B) generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in said subject, based upon the measurements and or images taken of the rib fracture;C) preparing a 3D printable resin according to anyone of claims 1-31 and loading the resin mixture into a suitable 3D printer;D) 3D printing the resorbable 3D printed osteosynthetic apparatus for rib fracture repair based upon said 3D printable file.

43. The method of claim 42 further comprising:E) post curing the resorbable 3D printed osteosynthetic apparatus for rib fracture repair of Step D with ultraviolet light44. The method of claim 42 wherein the step of preparing a 3D printable resin according to any one of claims 1-31 (step C) comprises:Al) dissolving a linear or star-shaped poly( propylene fumarate)-based copolymer comprising at least one of an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block and a starshaped poly( propylene fumarate) copolymer in a suitable diluent;A2) adding a plurality of filler nanoparticles to the solution of C 1;A3) adding said photoinitiator to said ABA block copolymer;A4) adding a thiol-based crosslinker and mixing to form said 3D printable resin.

45. The method of claim 42 wherein the step of adding a thiol-based crosslinker (Cl) does not take place until immediately before less than 30 minutes before the step of 3D printing the resorbable 3D printed osteosynthetic apparatus (step D).

46. The method of claim 42 wherein the step of preparing a 3D printable resin according to any one of claims 1-31 further comprises adding radical scavenger or photoinhibitor to the solution of Cl.

47. The method of claim 42 wherein said 3D printable resin of step A wherein said filler nanoparticles promote bone repair and / or regrowth.

48. The method of claim 47 wherein said filler nanoparticles to promote bone repair and / or regrowth are selected from the group consisting of hydroxyapatite, strontium carbonate, b- tricalcium phosphate, and combinations thereof.

49. The method of claim 42 wherein the molar ratio of said 3D printable resin to said thiol-based crosslinker in the crosslinker / resin mixture of step D is from about 3:1 to about 40:1.

50. The method of claim 42 wherein said thiol-based crosslinker comprises trimethylolpropane tris(3-mercaptopropionate), Thiocure 332, and Thiocure 333, respectively.

51. A method for treating a rib fracture in a subject comprising:A) preparing a 3D printed composite plate for rib fracture repair according to claim 40, wherein said 3D printable composite plate is sized for use in repairing a rib fracture at a rib fracture site in a subject; andB) surgically inserting said 3D printed composite plate into the subject and securing it across said rib fracture site such that said 3D printed composite plate is mechanically secured to the rib on either side of said rib fracture.

52. The method of claim 51 wherein the step of preparing a 3D printed composite plate for rib fracture repair (step A) comprises:Al) preparing a 3D printable resin comprising an ABA block copolymer having a first and second polypropylene fumarate) A blocks and a polypropylene succinate) B block, wherein said first and second polypropylene fumarate) A blocks are each bonded covalently to an end of said polypropylene succinate) B polymer block to form an ABA block copolymer: a filler material: and a photoinitiator;A2) measuring and / or imaging a rib fracture on a subject having a rib fracture;A3) generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in said subject, based upon the measurements and or images taken of the rib fracture;A4) adding a thiol-based crosslinker to 3D printable resin and loading the crosslinker / resin mixture into a suitable 3D printer; andA5) 3D printing the 3D printable resin composite based upon said 3D printable file to produce a 3D printed composite plate for rib fracture repair.

53. The method of claim 51 wherein the step of preparing a 3D printed composite plate for rib fracture repair (step A) comprises:Al) preparing a 3D printable resin comprising a star-shaped PPF copolymer having 3 or 4 arms, a filler material, and a photoinitiator;A2) measuring and / or imaging a rib fracture on a subject having a rib fracture;A3) generating a 3D printable file comprising a 3-dimentional image of a plate for rib fracture repair sized to repair the rib fracture in said subject, based upon the measurements and or images taken of the rib fracture;A4) adding a thiol-based crosslinker to 3D printable resin and loading the crosslinker / resin mixture into a suitable 3D printer; andA5) 3D printing the 3D printable resin composite based upon said 3D printable file to produce a 3D printed composite plate for rib fracture repair.

54. The method of claim 51 wherein said 3D printed composite plate comprises one or more openings sized to receive and retain a surgical screw.

55. The method of claim 51 wherein said the step of mechanically securing said 3D printed composite plate to the rib on either side of said rib fracture (step B) is performed using two or more screw's running through said 3D printed composite plate.