A three-layer dielectric passivation film PERC solar cell and its manufacturing process
By adopting a three-layer dielectric passivation film structure in PERC solar cells, including SiO2, Al2O3 and SixNy:H, the problem of poor passivation effect is solved, the short-circuit current, open-circuit voltage and anti-PID performance of the battery are improved, and the battery is realized. Higher stability and reliability.
Patent Information
- Application Number
- CN201910364848.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-04-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2039-04-30
AI Technical Summary
The passivation effect of existing PERC solar cells is poor, resulting in degradation of electrical performance and PID failure, affecting the stability and reliability of the battery.
Using a three-layer dielectric passivation film structure, including thin silicon oxide (SiO2), aluminum oxide (Al2O3) and silicon nitride (SixNy:H), a brand new film stacking structure is formed through deposition and laser groove technology to enhance the blunt and optical utilization, improve the battery's anti-optical fading and anti-PID performance.
Effectively reduce the back surface recombination rate, improve short-circuit current and open-circuit voltage, enhance the battery's anti-optical fading and anti-PID stability and reliability performance, and reduce process costs and equipment requirements.
Smart Images

Figure CN109994553B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar photovoltaic power generation, and in particular relates to a three-layer dielectric passivation film PERC solar cell and a manufacturing process thereof. Background Art
[0002] With the continuous development and maturity of the solar photovoltaic power generation industry, its advantages continue to emerge in the new round of clean energy competition, such as wide application areas, abundant raw material sources, safety and reliability, not affected by energy crises and capital fuel markets, gradual improvement in industrialization and intelligence, and short construction cycle and less waste of power generation systems. Clean and sustainable photovoltaic power generation products have become an important part of the future development of new energy. Traditional BSF solar cells, preparation process such as Figure 1 As shown, after more than 10 years of industrialization, the photoelectric conversion efficiency of solar cells has been greatly improved through continuous improvement of the front emission junction process formula, upgrading of the gold semiconductor contact lead-out electrode process, optimization and transformation of the velvet preparation method and equipment, and development of the front anti-reflection passivation process equipment. Improving the conversion efficiency of solar cells is of great significance for promoting photovoltaic grid parity, reducing the cost per kilowatt-hour, and promoting the sustainable development of photovoltaic power generation.
[0003] For the back surface of traditional BSF solar cells, the back surface of commercial P-type solar cells is doped with concentrated aluminum to form an aluminum back field, and a P+ concentrated diffusion layer is formed on the back, forming a P+P- structure. A built-in electric field pointing from the P- region to the P+ is generated at the P+P- interface. This built-in electric field has a back-repelling "reflection" effect on the minority carrier electrons in the P-type base region, reducing their diffusion speed to the back surface, and also reducing the effective recombination rate on the back. This is actually a so-called field passivation effect. The back surface recombination rate can be reduced to about 1000cm / s, which improves the open circuit voltage and short circuit current to a certain extent. However, the area where the back metal and semiconductor contact is still an effective recombination center, and the recombination loss on the back surface is still large. In order to solve this structural design problem, the high-efficiency batteries launched by major research institutions at home and abroad have all done a certain passivation treatment on the back surface of the silicon wafer. For example, the main design principle of the current PERC battery is to reduce the back surface recombination and improve the long-wavelength photoelectric conversion quantum efficiency of the battery.
[0004] The concept of PERC cells was first reported by Martin Green's research group at UNSW in 1989. The PERC device structure was formed by growing a thick layer of silicon oxide at high temperature (>900 degrees) to passivate the surface of the silicon wafer, and then using semiconductor lithography, metal sputtering evaporation and electroplating. 2It is not suitable for industrial solar cell production. The main reason is that the high temperature process has a re-diffusion effect on the diffused PN junction, which is inconvenient for process control. In addition, the minority carrier lifetime of solar-grade silicon wafers is sensitive to high temperatures, especially when the temperature is about 900°C, the minority carrier lifetime of multicrystalline silicon wafers will be greatly reduced. Therefore, the passivation film suitable for industrial high-efficiency silicon solar cells should be prepared at low temperature and combined with thermally oxidized SiO 2 It has comparable passivation performance. In recent years, through previous accumulated attempts, it has been found that the negatively charged aluminum oxide dielectric film can passivate the silicon P-type silicon surface well, has good insulation and is not easy to cause inversion layer conduction and leakage, and the aluminum oxide film can be deposited at a lower temperature. With the introduction of industrialized aluminum oxide deposition equipment, industrialized PERC solar cells have gradually become the mainstream battery technology in the industry.
[0005] The advantages of PERC technology also lie in its good compatibility with other high-efficiency battery and component technologies, and its potential to continuously improve battery efficiency and power generation capacity, and reduce costs based on the original industrial production line. By combining technologies such as multi-busbar, selective emitter (SE) and TOPCon, the efficiency of PERC cells can be further improved; combining diamond wire cutting and black silicon technology can improve the cost performance of multicrystalline cells. The bifacial PERC+ cell achieves bifacial power generation with almost no increase in cost, and directly achieves a 10%-25% power generation gain on the system side, greatly enhancing the competitiveness and future development potential of PERC technology.
[0006] The current industrialized PERC cells are based on a dielectric passivation film structure of aluminum oxide on the back, silicon nitride on the back, and silicon nitride on the front. There are many ways to deposit aluminum oxide films, such as PECVD, ALD, APCVD, PE-ALD, and magnetron sputtering. Among them, the ALD deposition method often requires an additional annealing process, which will increase the industrial process cost. In addition, due to the possible presence of -OH and -CH in the aluminum oxide dielectric film layer, 3If the annealing process is not strictly matched, the group may react with the H in the SixNy:H stack from the capping stack during sintering, thereby destroying the passivation effect of the stack passivation film under the high temperature conditions of the back-end sintering (>860℃), resulting in a decrease in electrical performance and the production of EL test defective pieces; at the same time, after being placed for a period of time, a certain combination of light and temperature conditions may accumulate and escape residual secondary reactants, causing LID / LeTID phenomenon in PERC cells. The cause of the LeTID phenomenon is complex, and many research institutions such as SCHOTT, UNSW, Konstan University, ISFH, and Aalto University are conducting further research. The current mainstream view is that hydrogen is the main factor, and the attenuation caused by metal ions such as BO / FeB and Cu in the raw materials is also relatively serious. Therefore, the current industrialized PERC solar cells generally have problems such as easy damage to the passivation film layer, severe back-end attenuation, and EL abnormalities; on the other hand, there is a large room for improvement in the bifacial PID phenomenon of bifacial PERC+ cells. The PID attenuation of bifacial PERC modules encapsulated in EVA can be reduced to a certain extent by matching the dielectric passivation film structure design with the module packaging materials such as POE. However, since the bifacial cell combined with PID is a new product failure phenomenon that has appeared in recent years, and there are ambiguities and multi-factor constraints in the generation mechanism, inducing conditions, and influencing factors of the original PID phenomenon, matching the module packaging materials will inevitably increase the back-end manufacturing cost to a certain extent. Therefore, solar cell manufacturers are more inclined to reduce the PID failure phenomenon of industrialized PERC series solar cells through the design of the front-end dielectric film layer structure of the cell and the optimization of the process formula. As the modules and system ends require solar cells to have better CTM, light decay and thermally assisted light decay performance, and anti-PID performance, it is becoming increasingly important to improve the above stability and reliability of PERC cells. Summary of the invention
[0007] The purpose of the present invention is to solve the problem of poor passivation effect of PERC cells in the prior art, and to provide a three-layer dielectric passivation film PERC solar cell and a manufacturing process. The PERC cell structure adopts a three-layer dielectric passivation film deposition, which can effectively enhance the passivation and incident light comprehensive utilization rate, increase the short-circuit current and open-circuit voltage of the cell, and at the same time improve the light decay resistance and anti-PID stability and reliability performance of the cell of the structure.
[0008] The technical solution adopted by the present invention is as follows:
[0009] A three-layer dielectric passivation film PERC solar cell, comprising a P-type silicon substrate, an emitter junction region arranged on the upper side of the P-type silicon substrate, an N++SE heavily doped region arranged between the emitter junction region and the P-type silicon substrate, and a SiO 2 Passivation film, the SiO 2An aluminum oxide passivation film is attached to the outside of the passivation film, a silicon nitride anti-reflection capping layer is attached to the outside of the aluminum oxide passivation film, a Local-BSF P++ region is disposed on the other side of the P-type silicon substrate where the emitter junction region is disposed, a back Al back field electrode is disposed at the bottom of the silicon nitride anti-reflection capping layer, and an electrode column is disposed on the back Al back field electrode, and the electrode column passes through the silicon nitride anti-reflection capping layer, the aluminum oxide passivation film, and the SiO 2 Passivation film, the top of the electrode column is connected to the Local-BSF P++ area.
[0010] Furthermore, a front Ag electrode is provided on one side of the P-type silicon substrate provided with the N++SE heavily doped region, and the front Ag electrode passes through the silicon nitride anti-reflection capping layer, the aluminum oxide passivation film, the SiO 2 Passivation film, the front Ag electrode is connected to the emitter junction area at one end close to the P-type silicon substrate.
[0011] Furthermore, the back Al back field electrode is provided with a back Ag-Al or Ag electrode.
[0012] Furthermore, the Local-BSF P++ region is composed of a plurality of irregular hemispherical regions.
[0013] A three-layer dielectric passivation film PERC solar cell manufacturing process according to any one of claims 1 to 4, wherein the manufacturing process comprises the following steps:
[0014] (1) Pre-clean and texturize the silicon wafer to remove the 3-5um damaged layer on the surface of the silicon wafer.
[0015] (2) depositing a doping source on the surface of the silicon substrate processed in step (1) and performing thermal diffusion to prepare a PN junction; the doping source is phosphorus oxychloride and oxygen, and the heating time is 30 to 60 minutes under high temperature diffusion conditions to form a PN junction; during the diffusion process, POCl 3 Using N 2 Carry, flow carrying N 2 Flow rate: 1000-2000sccm, time: 20-35 minutes, carrying amount: POCl 3 15–25 g; O 2 Flow rate: 1000-3000sccm, time: 40-55 minutes, temperature: 830-870°C;
[0016] (3) Irradiate the silicon wafer after diffusion in step (2) with a laser having a wavelength of 532 nm, and perform doping diffusion on the phosphorus atoms in the surface phosphosilicate glass after diffusion in a local designed area through laser local heating ablation technology. The area ratio of this area is 4.5% - 8.5%, so as to form a low sheet resistance doped emitter (SE) on the silicon wafer surface. The sheet resistance after laser doping is 50 - 90 Ω / sq;
[0017] (4) Etching. Clean and polish the back surface of the silicon wafer after laser doping in step (3). Use a mixed solution of HF, HNO 3 and H 2 SO 4 to etch and remove the n-type layer on the back surface of the silicon wafer, and remove the phosphosilicate glass on the front surface, removing the back PN junction, the peripheral PN junction, and the phosphosilicate glass layer; and perform a polishing treatment of 3 - 8 μm on the back surface of the silicon wafer to form a mirror structure;
[0018] (5) Perform thin oxidation SiO 2 on the front, back, and periphery of the silicon wafer. During the annealing process, introduce oxygen and form a dense 1.5 - 6.5 nm oxide layer (SiO 2 containing H) on the silicon wafer surface, and its refractive index is controlled to be 1.45 - 1.85;
[0019] (6) Deposit a passivating alumina film on the outer layer of the thin oxidation SiO 2 in step (5). That is, the second high-density passivation film is formed by using an aluminum-containing precursor (aluminum precursors include aluminum trichloride, trimethylaluminum, triethylaluminum, dimethylaluminum chloride, aluminum ethoxide, aluminum isopropoxide), and can be deposited by atomic layer deposition (ALD), PECVD, CVD. Its passivation temperature is 230 - 280 °C. Use the ALD method of vapor phase chemical deposition to grow an alumina layer with a film thickness of 3 - 8 nm on the outer layer of the thin oxidation SiO 2 , with a refractive index of 1.58 - 1.73 and a reaction time of 25 - 35 min;
[0020] (7) Evaporate and deposit a third anti-reflection protective film layer on the front and back of the battery after depositing the passivating alumina film on the outer layer in step (6). The processing temperature for depositing silicon nitride films by PECVD on the front and back is 380 - 480 °C. The refractive index of the silicon nitride film on the front is controlled to be 1.86 - 2.33, and the film thickness is 65 - 95 nm; the refractive index of the silicon nitride film on the back is 1.9 - 2.4, and the film thickness is 95 - 180 nm;
[0021] (8) Laser grooving: using a 532-1064 nm ps or ns laser to locally groove the silicon wafer after the silicon nitride film is coated in step (7), the grooved area accounts for 0.5% to 6% of the silicon wafer area, and the local laminated film is removed to form an aluminum back surface field in the local area and lead out the current to form the positive electrode of the battery;
[0022] (9) screen printing an Ag or Ag-Al back electrode on the back of the solar cell prepared in step (8) and drying the back electrode;
[0023] (10) matching the laser slotting pattern in process step (8), screen printing thick film aluminum paste on the non-back electrode area on the back side and drying it, with a thickness of 10 to 30 μm and a distance from the edge of 0.8 to 1.6 mm;
[0024] (11) screen printing a front electrode of Ag paste on the front of the solar cell obtained in step (10) and drying it;
[0025] (12) The printed battery in step (11) is rapidly sintered at high temperature (IR heating 300-800° C.) so that the silver paste on the front side penetrates the laminated film and forms an ohmic contact with the emitter region, and the aluminum paste on the back side is melted and in contact with the p-type substrate to form a P+ back electric field;
[0026] (13) Reduce the light-induced degradation (LID) of the battery through a light decay furnace or an electric injection furnace: Under strong light conditions, the furnace tube heating temperature is >180°C;
[0027] (14) Performing IV testing and battery sorting on the battery obtained in step (13).
[0028] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0029] 1. In the present invention, compared with the conventional BSF solar cell production process, the PERC solar cell production process of the present invention adds a three-layer dielectric structure passivation film as the front and back passivation layers and the optical receiving layer, which can greatly reduce the recombination rate of the back surface and improve the collection rate of photogenerated carriers. On the silicon substrate, a three-layer structure of thin silicon oxide (SiO2), aluminum oxide (Al2O3) and silicon nitride (SixNy:H) is deposited on both sides from the inside to the outside as a dielectric passivation film layer to form a new three-layer film stacking structure on the surface of the silicon wafer. By adopting the three-layer dielectric passivation film deposition on the PERC structure, the comprehensive utilization rate of passivation and incident light can be effectively enhanced, the short-circuit current and open-circuit voltage of the battery can be increased, and the anti-light decay and anti-PID stability and reliability performance of the battery of the structure can be improved.
[0030] 2. In the present invention, the passivation of the dangling bonds on the silicon surface is achieved by a thermal oxide film on the front, back and surrounding surfaces, which is different from the related patents that use Al2O3 directly contacting the silicon surface. 2 O 3 The process of passivating the dangling bonds by subsequent heat treatment with oxygen ions rich in the film is essentially different. This process uses three layers of dielectric passivation film to passivate the silicon wafer surface, so the thickness of the oxide film required by this process is only 1.5-6.5nm, so the process time is greatly shortened, which is beneficial to energy saving and environmental protection requirements. The first layer of high refractive index dense oxide layer SiO 2 It contains a large amount of hydrogen and has good density, which can passivate the dangling bonds on the surface of the silicon wafer and increase the open circuit voltage (Voc) of the battery.
[0031] 3. In the present invention, SiO 2 On the basis of thin film passivation, the auxiliary dense aluminum oxide film layer can not only enhance the passivation effect, but also prevent the mobile ions in the passivation layer from moving and migrating under the external electric field, temperature and humidity, enhance the anti-PID effect, and avoid power attenuation caused by leakage of battery components. It has good anti-PID performance and anti-light decay LID performance.
[0032] 4. In the present invention, the back silicon nitride film layer can protect the adjacent aluminum oxide film to prevent slurry corrosion, and release hydrogen in the silicon nitride during high-temperature sintering in the later stage to produce hydrogen passivation, thereby enhancing the passivation effect on the silicon wafer. The H+ positive charge in the silicon nitride film can neutralize the electric field effect generated by the negative charge of the aluminum oxide film, while taking into account the passivation of the N-type and P-type silicon surfaces, and improving the open circuit voltage of the battery.
[0033] 5. In the present invention, matching silicon oxide (SiO 2 ), aluminum oxide (Al 2 O 3 ) and silicon nitride (SixNy:H) three-layer stacked structure can reduce the front light reflection ratio while enhancing the back light reflection ratio, ensuring the balanced utilization of short-wave and long-wave light, thereby enhancing the comprehensive utilization rate of incident light and increasing the short-circuit current of the battery.
[0034] 6. In the present invention, the equipment used in the present invention is more than 80% compatible with traditional solar cell equipment, does not require too much new equipment investment, has low process transformation costs, large production capacity, significant performance improvement advantages, and has very good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic diagram of the structure of a three-layer dielectric passivation film PERC solar cell of the present invention.
[0036] Figure 2 The present invention is a schematic diagram of the preparation process of a three-layer dielectric passivation film PERC solar cell.
[0037] Figure 3 This is the back laser groove pattern of the present invention.
[0038] Markings in the figure: 1-silicon nitride anti-reflection capping layer, 2-aluminum oxide passivation film, 3-SiO 2 Passivation film, 4-P-type silicon substrate, 5-back Ag-Al electrode, 6-front Ag electrode, 7-back Al back field electrode, 8-Local-BSF P++ region, 9-emitter junction region, 10-N++SE heavily doped region, 11-electrode column. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] A three-layer dielectric passivation film PERC solar cell, comprising a P-type silicon substrate 4, an emitter junction region 9 arranged on the upper side of the P-type silicon substrate 4, an N++SE heavily doped region 10 arranged between the emitter junction region 9 and the P-type silicon substrate 4, and a SiO2-doped region 10 arranged on the P-type silicon substrate 4. 2 Passivation film 3, the SiO 2 An aluminum oxide passivation film 2 is attached to the outside of the passivation film 3, and a silicon nitride anti-reflection capping layer 1 is attached to the outside of the aluminum oxide passivation film 2. The P-type silicon substrate 4 is provided with an emitter junction region 9 and the other side thereof is provided with a Local-BSF P++ region 8. A back Al back field electrode 7 is provided at the bottom of the silicon nitride anti-reflection capping layer 1, and an electrode column 11 is provided on the back Al back field electrode 7. The electrode column 11 passes through the silicon nitride anti-reflection capping layer 1, the aluminum oxide passivation film 2, and the SiO 2 The passivation film 3, the top of the electrode column 11 is connected to the Local-BSF P++ area 8; the back surface passivation layer of aluminum oxide, silicon dioxide, silicon nitride and their stacked structure greatly reduces the back surface recombination rate, improves the back reflectivity, and at the same time reduces the component CTM, improves the battery light decay and thermal assisted light decay performance, and anti-PID performance.
[0041] Preferably, a front Ag electrode 6 is arranged on one side of the P-type silicon substrate 4 where the N++SE heavily doped region 10 is arranged, and the front Ag electrode 6 passes through the silicon nitride anti-reflection capping layer 1, the aluminum oxide passivation film 2, the SiO 2 The passivation film 3 , the front Ag electrode 6 is connected to the emitter junction region 9 at one end close to the P-type silicon substrate 4 .
[0042] Preferably, the back Al back field electrode 7 is provided with a back Ag—Al electrode 5 .
[0043] Preferably, the Local-BSF P++ region 8 is composed of a plurality of irregular hemispherical regions 12.
[0044] A manufacturing process of a three-layer dielectric passivation film PERC solar cell as described in any one of claims 1-4, the manufacturing process comprising the following steps:
[0045] (1) Perform pre-cleaning and texturing on the silicon wafer to remove the damaged layer of 3-5 μm on the surface of the silicon wafer, reduce the recombination rate of photo-generated carriers, and at the same time form a textured surface on the front surface of the cell to reduce the reflectivity. For polycrystalline silicon wafers, acid texturing is used, and the solution used is a mixed solution of nitric acid, hydrofluoric acid and water, nitric acid: hydrofluoric acid: water = 2:1:2 or 5:1:2; for single-crystalline silicon wafers, alkali texturing is used, and the ratio of solvents is NaOH or KOH, isopropyl alcohol, single-crystalline silicon texturing additive and water. The p-type silicon substrate sequentially passes through surface cleaning and micro-etching, alkali texturing, water washing tank 1, acid tank, water washing tank 2, alkali washing tank, water washing tank 3, acid tank, water washing tank 4, three chemical reaction tanks and three water washing tanks, and then the silicon wafer is dried.
[0046] (2) Deposit a doping source on the surface of the above silicon substrate and perform thermal diffusion to prepare a P-N junction; the doping source is phosphorus oxychloride and oxygen. Under high-temperature diffusion conditions, the heating time is 30-60 minutes. Phosphorus oxychloride will decompose, and free phosphorus and oxygen will enter the surface of the silicon wafer to form a P-N junction; the free chlorine will form chlorine gas and be discharged together with the excess oxygen in the form of chlorine gas. During the diffusion process, POCl 3 is carried by N 2 with a flow rate of N 2 in the range of 1000-2000 sccm, and the time is 25-35 minutes. A total of about 15-25 g of POCl can be carried. 3 The flow rate of O 2 is controlled in the range of 1000-3000 sccm, the time is 40-55 minutes, and the temperature is 830-870 °C.
[0047] (3) Use a laser with a wavelength of 532 nm to irradiate the silicon wafer after diffusion in step (2), and perform local doping diffusion of phosphorus atoms in the surface phosphosilicate glass after diffusion through laser local heating ablation technology. The area of this region accounts for 4.5%-8.5% of the overall area of the silicon wafer, so as to form a selective low sheet resistance doped emitter (SE) on the surface of the silicon wafer. The sheet resistance after laser doping is 50-90 Ω / sq.
[0048] (4) Etching. The silicon wafer after laser doping in step (3) is cleaned and polished on the back. Since n-type layers are formed on both the front and back surfaces of the silicon wafer during the diffusion process, and the surface has phosphosilicate glass; this process is mainly through HF, HNO 3 and H 2 SO 4The mixed solution and the KOH / NaOH solution in the subsequent alkaline tank corrode and remove the n-type layer on the back side, and remove the phosphosilicate glass on the front side. In this process, the silicon wafer enters three chemical reaction tanks, namely the acid etching tank, the alkaline tank, and the pickling tank, in sequence and undergoes chemical reactions. The silicon wafer is then dried to remove the back PN junction, the peripheral PN junction, and the phosphosilicate glass layer. The back surface of the silicon wafer is polished by 3 to 8 um to form a mirror structure to increase the back reflectivity.
[0049] (5) Thin SiO2 oxide is applied on the front, back and periphery of the silicon wafer. 2 , the following methods can be used, such as thermal oxidation, ozone oxidation, N2O oxidation, and nitric acid oxidation; the thin oxidation annealing process is preferred: after the above process, the phosphorus content on the surface of the p-type silicon wafer is certain, and the surface concentration of phosphorus is high; high phosphorus will aggravate the recombination of minority carriers and have an adverse effect on the conversion efficiency of the battery. The unactivated phosphorus can be further activated through the annealing process, reducing the surface concentration of phosphorus, thereby reducing the surface recombination of minority carriers and improving the conversion efficiency of the battery. In addition, during the annealing process, an appropriate amount of oxygen is introduced to form a dense 1.5-6.5nm oxide layer (SiO 2 Containing H), its refractive index is controlled at 1.45-1.85, which can passivate the dangling bonds on the surface of the silicon wafer very well: 2 Better matching with Si, which can effectively reduce the interface state density on the Si surface, thereby increasing the chemical passivation effect; SiO 2 The Si in the quartz crystal is tetrahedral, while the Al 2 O 3 The source of the negative charge on the surface is the tetrahedral AlO 4 -,SiO 2 The presence of is conducive to the formation of an aluminum oxide layer with high negative charge density, thereby increasing the Al 2 O 3 In addition, it can effectively block the sodium ions, -OH and -CH 3 The subsequent products of the radical migrate into the interior of the battery, avoiding leakage of battery components and power attenuation, and have good anti-PID performance and light decay performance.
[0050] (6) The thin oxide SiO 2The outer layer is plated with a passivated aluminum oxide film, that is, the second layer of high-density passivation film uses aluminum-containing precursors (typical aluminum precursors are aluminum chloride, trimethyl aluminum, triethyl aluminum, dimethyl aluminum chloride, aluminum ethoxide, aluminum isopropoxide) to form by atomic layer deposition (ALD), PECVD, CVD, or solid target material is formed by PVD formation. Its function is to contain a large amount of fixed negative charge. In addition to chemically passivating the dangling bonds on the surface of the silicon wafer, it can also have a field passivation effect. At the same time, it prevents the mobile ions in the passivation layer from moving and migrating under the external electric field and temperature and humidity to a certain extent, and enhances the anti-PID effect. It is preferred to grow a 3-8nm thick aluminum oxide layer at 230-280℃ by atmospheric chemical deposition ALD, with a refractive index of 1.58-1.73 and a reaction time of 25-35min. It grows atomically one level at a time on the front and back surfaces of the silicon wafer, so that it has good step coverage for different surface undulations.
[0051] (7) The third anti-reflection protective film layer is deposited on the front and back sides of the battery. It is recommended to use PECVD silicon nitride film as the capping layer and the optical anti-reflection and anti-reflection functional layer (both CVD and PVD can be produced). Other materials with large refractive index, compatible with silicon processing technology, and good interface properties with silicon can also be used, including but not limited to TiO 2 , SiNxCy or SiNxOy as alternatives. The front and back PECVD silicon nitride film is coated in a low-pressure environment of 380-480℃, and a radio frequency electric field is applied to the injected ammonia and silane gas to ionize the gas and generate plasma; the high-energy particle flow hits the reaction gas adsorbed on the surface of the silicon wafer, breaking the reaction gas bonding bonds and becoming active substances. These active substances react to form SiNx:H thin films on the surface of the silicon wafer, thereby achieving the expected capping protection and optical effects. The refractive index of the front silicon nitride film is controlled at 1.86-2.33, and the film thickness is controlled at 65-95nm; the refractive index of the back silicon nitride film is controlled at 1.9-2.4, and the film thickness is controlled at 95-180nm; tubular PECVD is preferred, and the front and back are coated in stages, and the coating order of the front and back can be changed.
[0052] (8) Laser grooving: using a 532-1064 nm ps or ns laser to locally groove the silicon wafer after the silicon nitride film is coated in step (7). Since the laminated film formed by the above process is a dense insulating dielectric film layer, currently the front silver paste that matches the right one can penetrate it, but the back aluminum paste cannot be directly burned through, so it is impossible to form a back P+ contact area and lead the current out from the back of the silicon wafer; the grooving area accounts for 0.5% to 6%, and the grooving patterns include but are not limited to dot, line, dotted line, rectangle and hexagonal patterns, such as Figure 1 As shown, a local portion of the stacked film is removed to form an aluminum back surface field in the local region and to lead out the current, thereby forming the positive electrode of the battery.
[0053] (9) Screen printing Ag or Ag-Al back electrode on the back of the solar cell prepared by the above process and drying it, which is consistent with the conventional BSF process;
[0054] (10) matching the laser slotting pattern in process step (8), screen printing thick film aluminum paste on the non-back electrode area on the back side and drying it, with a thickness of 10 to 30 μm and a distance from the edge of 0.8 to 1.6 mm;
[0055] (11) Screen printing a Ag paste front electrode on the front side of the solar cell prepared by the above process and drying it, using a conventional screen printing process;
[0056] (12) The printed battery in step (11) is rapidly sintered at high temperature (IR heating 300-800°C), organic matter is removed, and annealing and sintering are performed to form a good ohmic contact: the silver paste on the front side penetrates the above-mentioned laminated film to form an ohmic contact with the emission region, and the aluminum paste on the back side is melted and contacted with the p-type substrate to form a P+ back electric field. The back electric field can prevent minority carriers from diffusing to the back surface to participate in recombination, thereby reducing the recombination loss on the back surface and further increasing the opening voltage and current density of the battery.
[0057] (13) Reduce the light-induced degradation (LID) of the cell by using a light decay furnace or an electric injection furnace: Under strong light conditions, the furnace tube is heated to above 180 degrees, which will cause the boron and oxygen atoms to combine into a stable state and no longer produce defects to capture minority carriers. The LID loss of PERC cells is about 3-6% when they are not treated. After being treated by the LID furnace process, the LID loss will drop to less than 2%.
[0058] (14) Performing IV testing and battery sorting on the batteries obtained in step (13): Designing a test grading procedure based on the optimal operating voltage, optimal operating current, maximum power, conversion efficiency, open circuit voltage, short circuit current, fill factor, etc. of the PERC battery. The performance parameters of the batteries after the process is completed must be measured and graded using precise testing instruments.
[0059] Example 1
[0060] The present invention comprises the following specific steps:
[0061] (1) Using a 40 g / L NaOH solution to remove a 4 μm mechanical damage layer on the surface of a single crystal p-type silicon wafer, the surface of the silicon wafer was cleaned, and at the same time, a 18 g / L NaOH liquid was used to anisotropically etch the surface of the silicon wafer to form a 2-3 μm inverted pyramid velvet texture;
[0062] (2) Using POCl 3The silicon wafer cleaned in step (1) is diffused in a diffusion furnace tube by a liquid source negative pressure to form a PN junction. The diffusion temperature is 830° C., the process time is 55 min, and the diffusion block resistance is controlled at 130-150Ω / □;
[0063] (3) Laser SE doping: On the silicon wafer diffused in step (2), the phosphorus atoms on the surface phosphorus silicon glass diffused are laser doped in the main grid and fine grid electrode area that are subsequently screen-printed. The area of this area accounts for 5% to 6% of the silicon wafer area, forming a local heavily doped area with a sheet resistance of 70-80Ω / □ in the concentrated diffusion area;
[0064] (4) Using HF:HNO 3 =35g / L:350g / L, the volumes of the components are HF: 55.26L, HNO3: 214.78L, DI water: 173.80L, H2SO4: 80L, the liquid flow rate in the reaction tank is 30L / min, the reaction temperature is 6-8°C, the mixed solution is used to clean the back junction, and the back of the silicon wafer is polished to 6um to present a mirror structure and remove the peripheral PN junction, the alkaline tank (KOH concentration is 5%) neutralizes the acid and removes the porous silicon; the mixed solution of HCl, HF (concentration is 5%) and DI-water is used to clean the phosphorus silicon glass;
[0065] (5) Dry oxygen is introduced into the annealing oxidation furnace to form a thin layer of silicon oxide on the front and back sides and around the edges of the silicon wafer processed in step (4). The thickness of the silicon oxide is 3 nm and the refractive index is 1.58;
[0066] (6) Trimethylaluminum is introduced into an ALD deposition furnace at 250°C to adsorb and react with OH groups on the surface of the silicon wafer to generate an aluminum oxide film with a thickness of 5±1 nm;
[0067] (7) PECVD deposition of back silicon nitride film: Silane (SiH 4 ) and NH 3 (Ammonia) is deposited by ionization reaction on the back of the silicon wafer, and the silicon nitride prepared by PECVD has a thickness of 135nm and a refractive index of 2.18;
[0068] (8) PECVD deposition of front silicon nitride film: silane (SiH 4 ) and NH 3 (Ammonia) is deposited by ionization reaction on the front side of the silicon wafer. The thickness of silicon nitride prepared by PECVD is 85nm and the refractive index is 2.15.
[0069] (9) using a 532 nm ns laser to locally groove the back side of the laminated silicon wafer, the groove area accounts for 3.2%, and the groove pattern is a dotted line pattern with a real-dummy ratio of 85%;
[0070] (10) Screen-print the Ag electrode on the back and dry it at 200°C; then screen-print the Al paste on the back and dry it at 210°C, with a film thickness of 23 μm and a distance of 1.0 mm from the edge;
[0071] (11) Turn the cell over, screen print the Ag electrode main grid and auxiliary grid on the front side, and dry at 220°C;
[0072] (12) After the silicon wafer is transferred to the sintering furnace, the organic matter in the slurry is volatilized and discharged, and the wafer is rapidly sintered and annealed in a sintering furnace with a peak setting of 890°C. The front and back electrodes are both sintered once to form good ohmic contacts, and the IV characteristics are tested;
[0073] (13) The silicon wafer passes through a light decay furnace and is illuminated by a strong halogen lamp (0.8 Sun) at a temperature of 230°C to reduce the light induced degradation (LID) of the battery.
[0074] (14) Solar cell IV testing and sorting.
[0075] Example 2
[0076] The present invention comprises the following specific steps:
[0077] (1) Using a 30 g / L NaOH solution to remove a 3.5 μm mechanical damage layer on the surface of a single crystal p-type silicon wafer, the surface of the silicon wafer is cleaned, and at the same time, a 20 g / L NaOH liquid is used to anisotropically etch the surface of the silicon wafer to form a 3-4 μm inverted pyramid velvet texture;
[0078] (2) Using POCl 3 The silicon wafer cleaned in step (1) is diffused in the diffusion furnace tube by liquid source negative pressure to form a PN junction. The diffusion temperature is 850°C, the process time is 45 minutes, and the diffusion square resistance is controlled at 140-170Ω / □.
[0079] (3) Laser SE doping: On the silicon wafer diffused in step (2), the phosphorus atoms on the diffused surface phosphorus silicon glass are laser doped in the main gate and fine gate electrode area that are subsequently screen-printed. The area of this area accounts for 5.2% of the silicon wafer area, forming a local heavily doped area with a sheet resistance of 60-70Ω / □ in the concentrated diffusion area;
[0080] (4) Using HF:HNO 3 =30g / L:330g / L, the volumes of each component are HF:45.58L, HNO 3 : 184.16L, DI water: 183.50L, H 2 SO 4:70L, the liquid flow rate in the reaction tank is 32L / min, the reaction temperature is 6-8℃, the mixed solution is used to clean the back junction, and the back of the silicon wafer is polished to 4.5um to form a mirror structure and remove the peripheral PN junction. The alkaline tank (NaOH concentration is 6%) neutralizes the acid and removes porous silicon. The phosphorus silicon glass is cleaned with a mixed solution of HCl, HF (concentration 5%) and DI-water and then hot-air dried;
[0081] (5) Dry oxygen is introduced into the annealing oxidation furnace to form a 1.5 nm thick SiO layer on the back of the silicon wafer processed in step (4) using an ozone generator. 2 Then, it enters the annealing oxidation furnace and introduces dry oxygen to form a thin layer of silicon oxide on the front, back and edge of the silicon wafer. The thickness of silicon oxide is 3.5nm, and the refractive index is 1.52. At this time, the thickness of silicon oxide on the front and surrounding areas is 3.5nm, but the total thickness of silicon oxide on the back is 5.0nm.
[0082] (6) Trimethylaluminum is introduced into an ALD deposition furnace at 230°C to adsorb and react with OH groups on the surface of the silicon wafer to generate an aluminum oxide film with a thickness of 3 to 5 nm;
[0083] (7) PECVD deposition of front silicon nitride film: silane (SiH 4 ) and NH 3 (Ammonia) is deposited by ionization reaction on the front side of the silicon wafer. The thickness of silicon nitride prepared by PECVD is 80nm and the refractive index is: 2.13;
[0084] (8) PECVD deposition of back silicon nitride film: Silane (SiH 4 ) and NH 3 (Ammonia) is deposited by ionization reaction on the back of the silicon wafer, and the silicon nitride prepared by PECVD has a thickness of 150nm and a refractive index of 2.16;
[0085] (9) using a 1064 nm ps laser to locally groove the back side of the laminated silicon wafer, the groove area accounts for 2.8%, and the groove pattern is a continuous straight line pattern;
[0086] (10) Screen-print the Ag electrode on the back and dry it at 210°C; then screen-print the Al paste on the back and dry it at 210°C, with a film thickness of 20 μm and a distance of 1.5 mm from the edge;
[0087] (11) Turn the cell over, screen print the Ag electrode main grid and auxiliary grid on the front side, and dry at 220°C;
[0088] (12) After the silicon wafer is transferred to the sintering furnace, the organic matter in the slurry is volatilized and discharged, and the wafer is rapidly sintered and annealed in a sintering furnace with a peak setting of 900°C. The front and back electrodes are both sintered once to form good ohmic contacts, and the IV characteristics are tested;
[0089] (13) The silicon wafer is treated with auxiliary lighting for 1800 to 2400 seconds at a temperature of 170 to 200°C and an injection current of 3.5 to 4A to reduce the light-induced degradation (LID) of the battery.
[0090] (14) Solar cell IV testing and sorting.
[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A three-layer dielectric passivation film PERC solar cell, Features: The invention comprises a P-type silicon substrate (4), an emitter junction region (9) arranged on the upper side of the P-type silicon substrate (4), an N++SE heavily doped region (10) arranged between the emitter junction region (9) and the P-type silicon substrate (4), and a SiO 2 The passivation film (3), the SiO 2 An aluminum oxide passivation film (2) is attached to the outside of the passivation film (3), a silicon nitride anti-reflection capping layer (1) is attached to the outside of the aluminum oxide passivation film (2), a Local-BSF P++ region (8) is provided on the other side of the P-type silicon substrate (4) on which an emitter junction region (9) is provided, a back Al back field electrode (7) is provided at the bottom of the silicon nitride anti-reflection capping layer (1), and an electrode column (11) is provided on the back Al back field electrode (7), and the electrode column (11) passes through the silicon nitride anti-reflection capping layer (1), the aluminum oxide passivation film (2), the SiO 2 A passivation film (3), the top of the electrode column (11) is connected to the Local-BSF P++ region (8); SiO 2 The thickness of the passivation film (3) is 1.5~6.5nm, SiO 2 The thickness and refractive index of the passivation film (3) are controlled within a range of 1.45 to 1.
85.
2. A three-layer dielectric passivation film PERC solar cell as claimed in claim 1, Features: A front Ag electrode (6) is arranged on one side of the P-type silicon substrate (4) provided with an N++SE heavily doped region (10), and the front Ag electrode (6) passes through the silicon nitride anti-reflection capping layer (1), the aluminum oxide passivation film (2), the SiO 2 A passivation film (3), wherein one end of the front Ag electrode (6) close to the P-type silicon substrate (4) is connected to the emitter junction region (9).
3. A three-layer dielectric passivation film PERC solar cell as claimed in claim 1, Features: The back Al back field electrode (7) is provided with a back Ag-Al or Ag electrode (5).
4. A three-layer dielectric passivation film PERC solar cell as claimed in claim 1, Features: The Local-BSF P++ region (8) is composed of a plurality of irregular hemispherical regions (12).
5. A process for manufacturing a three-layer dielectric passivation film PERC solar cell according to any one of claims 1 to 4, It is characterized in that The manufacturing process includes the following steps: (1) Pre-clean and texturize the silicon wafer to remove the damaged layer of 3-5 μm on the surface of the silicon wafer and form a pyramid texture surface with uniform size; (2) depositing a doping source on the surface of the silicon substrate processed in step (1) and performing thermal diffusion to prepare a PN junction; the doping source is phosphorus oxychloride and oxygen, and the heating time is 30 to 60 minutes under high temperature diffusion conditions to form a PN junction; during the diffusion process, POCl 3 Using N 2 Carry, flow carrying N 2 Flow rate: 1000~2000sccm, time: 20~35 minutes, carrying amount: POCl 3 15-25 g, O 2 Flow rate: 1000~3000sccm, time: 40~55 minutes, temperature: 830~870℃; (3) irradiating the silicon wafer diffused in step (2) with a laser having a wavelength of 532 nm, and further doping and diffusing the phosphorus atoms in the diffused surface phosphorus-silicate glass in a local designed area by laser local heating ablation technology, wherein the area of the area accounts for 4.5% to 8.5% of the silicon wafer, thereby forming a low-resistance doped emitter SE on the surface of the silicon wafer, and the resistance after laser doping is 50 to 90 Ω / cm; (4) Etching: cleaning and back polishing of the silicon wafer after laser doping in step (3), and etching with HF, HNO 3 and H 2 SO 4 The mixed solution and the KOH / NaOH solution in the subsequent alkaline tank corrode and remove the n-type layer on the back of the silicon wafer, remove the phosphosilicate glass on the front, remove the back PN junction, the peripheral PN junction and the phosphosilicate glass layer; and perform a 3-8μm polishing treatment on the back surface of the silicon wafer to form a mirror structure; (5) Thin SiO2 is oxidized on the front, back and periphery of the silicon wafer processed in step (4). 2 During the annealing process, oxygen is introduced to form a dense 1.5~6.5nm oxide layer SiO on the surface of the silicon wafer. 2 Containing H, its refractive index is controlled at 1.45~1.85; (6) The thin oxide SiO 2 The outer layer of the passivation aluminum oxide film, that is, the second layer of high-density passivation film, uses aluminum-containing precursors and can be deposited by atomic layer deposition ALD, PECVD, and CVD. The passivation temperature is: 230~280℃. The atmospheric chemical deposition ALD method is used on the thin oxide SiO 2 The outer layer grows a 3~8nm thick aluminum oxide layer with a refractive index of 1.58~1.73 and a reaction time of 25~35min; (7) After the processing in step (6), a third anti-reflection protective film layer is evaporated on the front and back sides of the battery. The processing temperature of the front and back PECVD silicon nitride films is: 380~480℃, the refractive index of the front silicon nitride film is controlled to be 1.86~2.33, and the film thickness is: 65~95nm; the refractive index of the back silicon nitride film is: 1.9~2.4, and the film thickness is: 95~180nm; (8) Laser grooving: using a 532-1064 nm ps or ns laser to locally groove the silicon wafer after the silicon nitride film is coated in step (7), the grooved area accounts for 0.5%-6% of the silicon wafer area, and the local laminated film on the surface is removed; (9) screen printing an Ag or Ag-Al back electrode on the back of the solar cell prepared in step (8) and drying the back electrode; (10) matching the laser slotting pattern in process step (8), screen printing thick film aluminum paste on the non-back electrode area on the back side and drying it, with a thickness of 10-30 μm and a distance from the edge of 0.8-1.6 mm; (11) screen printing a front electrode of Ag paste on the front of the solar cell obtained in step (10) and drying it; (12) IR heating the printed battery in step (11) at a high temperature of 300-800° C. for rapid sintering, so that the silver paste on the front side penetrates the laminated film and forms an ohmic contact with the emitter region, and the aluminum paste on the back side melts and contacts with the p-type substrate to form a P+ back electric field; (13) Reduce the light-induced degradation (LID) of the battery through a light decay furnace or an electric injection furnace: Under strong light conditions, the furnace tube temperature is >180°C; (14) Performing IV testing and battery efficiency sorting on the battery obtained in step (13).