Array substrate and manufacturing method thereof, liquid crystal display panel and display device
By adjusting the etching steps in the production method of the array substrate, reducing the tailing of the active region and the ohmic contact region, the problems of large parasitic capacitance and leakage current in traditional processes are solved, and the production capacity and cost-effectiveness of the liquid crystal display are improved.
Patent Information
- Application Number
- CN202110582280.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-05-27
AI Technical Summary
In the traditional 2W2D process, the active area of the TFT is too large, resulting in too large parasitic capacitors and device sizes. The channel is contaminated during the process and leads to large leakage current, limiting the production capacity and cost-effectiveness of the LCD display.
In the production method of the array substrate, the ashing process is performed after the first dry etching, and the second dry etching is performed, and the photoresist is peeled off after the second wet etching, and then the first Secondary dry etching reduces tailings of active and ohmic contact areas, and reduces parasitic capacitance and leakage current.
Effectively reduce parasitic capacitance, improve water ripple and white spot poor, reduce thin film transistor size, reduce leakage current, promote the switching of 5 mask processes to 4 mask processes, improve production capacity and reduce product costs .
Smart Images

Figure CN113889434B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and more specifically, to an array substrate and a manufacturing method thereof, a liquid crystal display panel and a display device. Background Art
[0002] At present, liquid crystal display (LCD) is widely used in the field of liquid crystal display of various sizes due to its advantages of low power consumption, thin volume, wide viewing angle, high definition, etc. In order to increase production capacity and reduce production costs, the core process of making liquid crystal display, the production of thin film transistor (TFT) liquid crystal array, has also developed from the original 5-mask system to the currently commonly used 4-mask system, wherein the process involved in the 4-mask system includes conventional two wet etchings and two dry etchings (2wet 2Dry, 2W2D). However, the active area tail of the TFT formed by the traditional 2W2D process is too large, resulting in excessive parasitic capacitance and device size, and the channel is polluted in the process, resulting in large leakage current. Summary of the invention
[0003] An object of the present invention is to provide an array substrate and a manufacturing method thereof, a liquid crystal display panel and a display device, so as to solve at least one of the problems existing in the prior art.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] A first aspect of the present invention provides a method for manufacturing an array substrate, comprising:
[0006] An active layer film and a source-drain electrode layer film are formed on a substrate having a gate electrode and a gate insulating layer, wherein the active layer film includes a semiconductor layer film and an ohmic contact layer film which are sequentially formed in a direction away from the substrate;
[0007] forming a patterned photoresist on the source-drain electrode layer film, including a completely reserved area and a partially reserved area;
[0008] Performing a first wet etching on the exposed source-drain electrode layer film to obtain a first source-drain electrode layer film, wherein the orthographic projection of the first source-drain electrode layer film on the substrate is within the range of the orthographic projection of the completely reserved area on the substrate;
[0009] Performing an ashing process on the photoresist to remove a portion of the reserved area, and making the orthographic projection of the completely reserved area on the substrate coincide with the edge of the orthographic projection of the first source-drain electrode layer thin film on the substrate;
[0010] Performing a first dry etching on the exposed active layer film to expose the gate insulating layer;
[0011] Performing a second wet etching on the exposed first source-drain electrode layer film to form source-drain electrodes;
[0012] Removal of fully reserved areas; and
[0013] The exposed active layer film is subjected to a second dry etching to remove the exposed ohmic contact layer film and part of the semiconductor layer film, the remaining ohmic contact layer film forms an ohmic contact region, and the remaining semiconductor layer film forms a channel region, wherein the ohmic contact region is substantially aligned with the orthographic projection of the corresponding source and drain electrodes on the substrate.
[0014] In some optional embodiments, the etching gas of the first dry etching and / or the second dry etching is selected from one or more combinations of NF3 / He, CH4 / He, CHF3 / He and SF6 / He.
[0015] In some optional embodiments, ashing the photoresist to remove a portion of the reserved area, and making the orthographic projection of the completely reserved area on the substrate coincide with the edge of the orthographic projection of the first source-drain electrode layer thin film on the substrate further comprises:
[0016] The photoresist layer is ashed to shrink the completely reserved area toward the partially reserved area, so that the orthographic projection of the completely reserved area on the substrate coincides with the orthographic projection edge of the first source-drain electrode layer thin film on the substrate.
[0017] In some optional embodiments, removing the completely reserved area further comprises:
[0018] In the same operating space as the second wet etch, the completely retained area is stripped by wet etching; or
[0019] In the same operation space as the second dry etching, the completely retained area is stripped by dry etching.
[0020] In some optional embodiments,
[0021] The gas flow rate of the ashing treatment is 2000-15000sccm, 200-2000 / 2000-15000sccm; the power is 5-15 / 5-15kw, the gas pressure is 20-70mT, and the ashing time is 40-80s.
[0022] In some optional embodiments,
[0023] The gas flow rate of the first dry etching and / or the second dry etching is 2000-6000sccm / 2000-6000sccm, the power is 5-15 / 5-15kw, and the gas pressure is 20-70mT.
[0024] In some optional embodiments, the source-drain electrode layer film is a multi-layer metal structure, and the film layer combination is selected from one of Mo / AL / Mo, Mo / Cu, MoNb / Cu, MoNb / Cu / MoTi or a stack thereof.
[0025] In some optional embodiments, the material of the semiconductor layer film is polysilicon, and the material of the ohmic contact layer film is doped polysilicon.
[0026] In some optional embodiments, a patterned photoresist is formed on the source-drain electrode layer film, including a completely reserved area and a partially reserved area, and further comprising:
[0027] forming a photoresist layer on the source-drain electrode layer film;
[0028] The photoresist layer is exposed by photolithography using a dual-tone mask to form a completely reserved area and a partially reserved area.
[0029] In some optional embodiments, it also includes:
[0030] forming a passivation layer and a via in the passivation layer;
[0031] A pixel electrode is formed.
[0032] A second aspect of the present invention provides an array substrate, characterized in that it comprises:
[0033] substrate;
[0034] An array of thin film transistors is formed on a substrate, wherein the thin film transistor comprises a gate electrode, a gate insulating layer, an active region, an ohmic contact region and a source-drain electrode, wherein the ohmic contact region is substantially aligned with the orthographic projection of the corresponding source-drain electrode on the substrate.
[0035] A third aspect of the present invention provides a liquid crystal display panel, comprising:
[0036] Color film substrate;
[0037] The array substrate as described above; and
[0038] The liquid crystal layer is encapsulated between the color filter substrate and the array substrate.
[0039] A fourth aspect of the present invention provides a display device, comprising the liquid crystal display panel described above.
[0040] The beneficial effects of the present invention are as follows:
[0041] In view of the existing problems, the present invention develops an array substrate and a manufacturing method thereof, a liquid crystal display panel and a display device, and reduces the tailing of the active area and the ohmic contact area generated in the first dry etching, the second wet etching and the second dry etching by first ashing the photoresist after the first dry etching and then performing the first dry etching, thereby reducing the parasitic capacitance, improving the water ripple and white spot defects, reducing the size of the thin film transistor, and facilitating the reduction of the frame; in addition, the above method can effectively reduce the leakage current and improve the reliability defects related to the leakage current; and the improved method further promotes the switching from the 5-mask process to the 4-mask process, improves the production capacity, reduces the product cost, and has a wide application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0043] Figure 1 A schematic cross-sectional view showing a 2W2D process flow according to the prior art.
[0044] Figure 2 A flow chart of a method for manufacturing an array substrate according to an embodiment of the present invention is shown.
[0045] Figure 3-10 A schematic cross-sectional view showing a method for manufacturing an array substrate according to an embodiment of the present invention.
[0046] Fig.11 A schematic top view of a TFT according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0047] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same or similar reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0048] In the drawings, the size of each component, the thickness of a layer, or a region may be exaggerated for clarity.
[0049] It should be noted that the terms “having”, “including”, “comprising”, etc. described in the present invention are all open-ended meanings, that is, when describing that a module “has”, “including” or “comprising” the first element, the second element and / or the third element, it means that the module includes other elements in addition to the first element, the second element and / or the third element. In addition, the ordinal numbers such as “first”, “second” and “third” in the present invention are not intended to limit the specific order, but only to distinguish the various parts. In the present invention, when describing that layer A and layer B are “set in the same layer”, it means that layer A and layer B are made of the same material and the same process.
[0050] The terms “on”, “formed on” and “disposed on” in the present invention may mean that one layer is directly formed or disposed on another layer, or may mean that one layer is indirectly formed or disposed on another layer, i.e., there are other layers between the two layers.
[0051] In the present invention, unless otherwise specified, the expression "patterning process" generally includes the steps of photoresist coating, exposure, development, etching, photoresist stripping, etc. The expression "one-time patterning process" means a process of forming a patterned layer, component, member, etc. using one mask.
[0052] The term “substantially” in the present disclosure means that the limit is not strictly defined and a value within a range of process and measurement errors is allowed.
[0053] In the prior art, in the commonly used 4-mask process, the first mask patterning process forms the gate electrode, the second mask patterning process forms the source and drain electrodes and the active layer with the channel, the third patterning process forms the via hole, and the fourth mask patterning process forms the pixel electrode. The typical process of the second patterning process is 2W2D.
[0054] Reference Figure 1As shown, the specific process of 2W2D is as follows: the first wet etching (a), firstly, an active layer film and a source-drain electrode layer film are arranged on the gate insulating layer GI, the active layer film includes an a-Si film and an n+a-Si film, a patterned photoresist (PR) is formed on the source-drain electrode layer film, and the source-drain electrode layer film is first wet-etched based on the photoresist; the first dry etching (b), the active layer film is etched based on the PR, and the PR is ashed to obtain the remaining PR. It can be seen that a large tail is generated in this etching process①; The second wet etching (b), based on the remaining PR, the source-drain electrode layer film is further wet-etched to form source-drain electrodes. As the source-drain electrode layer film is further etched, a larger tail ② will further appear in the active layer film; the second dry etching (d), based on the remaining PR, the active layer film is etched to form an active area. Due to the existence of the remaining PR, the formed active area almost retains the tail ②; (e), the remaining PR is wet-stripped, and the formed TFT will include tail ① and tail ②, which also includes the ohmic contact area tail. It can be seen that the active area tail of the TFT formed by the 2W2D process in the prior art is too large, and the parasitic capacitance of the transistor will increase accordingly, affecting the switching characteristics of the transistor; at the same time, the characteristics of the active area are different under light and without light, and the excessive tail causes pixel charging differences, resulting in water ripples (Waterfall) and white spot defects; and because the tail is too large, the size of the thin film transistor is also large in design, which will limit the narrow frame design of the array substrate; in addition, the PR glass liquid or stripping liquid remaining in the wet glass and the surface reaction products of the source and drain metal also remain in the back channel of the final TFT, and the back channel is polluted, which increases the leakage current of the TFT. In this field, in order to minimize the tail, the 5-mask process is often used as a second choice, which undoubtedly increases the process cost of the product and reduces the production capacity.
[0055] Based on one of the above questions, refer to Figure 2 As shown, an embodiment of the present invention provides a method for manufacturing an array substrate, comprising:
[0056] S1. forming an active layer film and a source-drain electrode layer film on a substrate having a gate electrode and a gate insulating layer formed thereon, wherein the active layer film comprises a semiconductor layer film and an ohmic contact layer film sequentially formed in a direction away from the substrate;
[0057] S2, forming a patterned photoresist on the source-drain electrode layer film, including a completely reserved area and a partially reserved area;
[0058] S3, performing a first wet etching on the exposed source-drain electrode layer thin film to obtain a first source-drain electrode layer thin film, wherein the orthographic projection of the first source-drain electrode layer thin film on the substrate is within the range of the orthographic projection of the completely reserved area on the substrate;
[0059] S4, performing an ashing process on the photoresist to remove a portion of the reserved area, and making the orthographic projection of the completely reserved area on the substrate coincide with the edge of the orthographic projection of the first source-drain electrode layer thin film on the substrate;
[0060] S5, performing a first dry etching on the exposed active layer film to expose the gate insulating layer;
[0061] S6, performing a second wet etching on the exposed source-drain electrode layer film to form source-drain electrodes;
[0062] S7, removing the completely reserved area; and
[0063] S8. Perform a second dry etching on the exposed active layer film to remove the exposed ohmic contact layer film and part of the semiconductor layer film, the remaining ohmic contact layer film forms an ohmic contact region, and the remaining semiconductor layer film forms a channel region, wherein the ohmic contact region is substantially aligned with the orthographic projection of the corresponding source and drain electrodes on the substrate.
[0064] In this embodiment, after the first dry etching, the photoresist is ashed and then the first dry etching is performed, and after the second wet etching, the photoresist is stripped before the second dry etching is performed, so that the tailing of the active area and the ohmic contact area generated in the first dry etching, the second wet etching and the second dry etching is reduced, the parasitic capacitance is reduced, the water ripples and white spots are improved, and the size of the thin film transistor is reduced, which is conducive to reducing the frame; in addition, the above method can effectively reduce the leakage current and improve the reliability related to the leakage current; and the improved method further promotes the switching from the 5-mask process to the 4-mask process, improves the production capacity, reduces the product cost, and has a broad application prospect.
[0065] Refer to the following Figures 3 to 10 As shown, a method for manufacturing an array substrate according to an embodiment of the present invention is described in detail.
[0066] like Figure 3 As shown, a gate electrode 315 and a gate insulating layer (Gate Insulator, GI) 303 are formed on the provided substrate 301. For example, a gate metal layer can be formed on the substrate 301 by magnetron sputtering or thermal evaporation process, and a gate electrode 315 can be formed by patterning process, and a gate insulating layer 303 can be deposited on the gate electrode 315. The material of the substrate 301 can be quartz glass; the gate metal layer can be a multilayer metal structure, and the film layer combination can be selected from one of molybdenum / aluminum / molybdenum (Mo / AL / Mo), molybdenum / copper (Mo / Cu), molybdenum-niobium alloy / copper (MoNb / Cu), molybdenum-niobium alloy / copper / molybdenum-titanium alloy (MoNb / Cu / MoTi) or a stack thereof; the material of the gate insulating layer (GI) 303 can be an inorganic insulating material such as silicon oxide, silicon nitride or silicon oxynitride.
[0067] Specifically, in step S1, an active layer film and a source-drain electrode layer film 309 are formed on the substrate 301 formed with the gate electrode 315 and the gate insulating layer 303. The active layer film can be formed by a deposition process such as plasma enhanced chemical vapor deposition (PECVD), and the source-drain electrode layer film 309 is formed on the active layer film by magnetron sputtering or thermal evaporation. The active layer film includes a semiconductor layer film 305 and an ohmic contact layer film 307 formed in sequence in a direction away from the substrate 301.
[0068] The material of the semiconductor layer film 305 can be polysilicon (a-Si), and the material of the ohmic contact layer film 307 can be doped polysilicon, for example, polysilicon heavily doped with n-type doping materials (n+a-Si), and of course, polysilicon heavily doped with p-type doping materials (p+a-Si). The n-type doping material can be arsenic (As), phosphorus (P), etc., and the p-type doping material can be aluminum (Al), indium (In), etc. The source-drain electrode layer film 309 can be a multilayer metal structure, and the film layer combination can be selected from one of Mo / AL / Mo, Mo / Cu, MoNb / Cu, MoNb / Cu / MoTi or a stack thereof.
[0069] Reference Figure 4 As shown, in step S2, a patterned photoresist 310 is formed on the source-drain electrode layer film 309, and the photoresist 310 includes a completely reserved area B and a partially reserved area A. Specifically, a photoresist layer can be coated on the source-drain electrode layer film 309, and a two-tone mask is used to perform photolithography exposure on the photoresist layer to complete patterning to form the photoresist 310, and the photoresist 310 includes a completely reserved area B and a partially reserved area A, and of course also includes a completely removed area (blank area outside A and B). The two-tone mask can specifically be a gray tone mask or a halftone mask.
[0070] Reference Figure 5 As shown, in step S3, the exposed source-drain electrode layer film 309 is first wet-etched to obtain a first source-drain electrode layer film 309-1, wherein the orthographic projection of the first source-drain electrode layer film 309-1 on the substrate 301 is within the range of the orthographic projection of the completely reserved area B on the substrate 301.
[0071] Reference Figure 6As shown, in step S4, the photoresist 310 is ashed to remove the partially reserved area A and make the orthographic projection of the completely reserved area B on the substrate 301 coincide with the orthographic projection edge of the first source-drain electrode layer film 309-1 on the substrate 301. Specifically, the photoresist is ashed to make the completely reserved area B shrink inward toward the partially reserved area A, so that the orthographic projection of the completely reserved area B on the substrate 301 coincides with the orthographic projection edge of the first source-drain electrode layer film 309-1 on the substrate 301. Optional ashing parameters are: the ashing gas combination is selected from one of O2, NF3 / O2 or a combination of the two, the gas flow rate is 2000-15000sccm, 200-2000 / 2000-15000sccm; the power is 5-15 / 5-15kw, the gas pressure is 20-70mT, and the ashing time is 40-80s, wherein the range of two gases in the above combination gas is separated by " / ".
[0072] Reference Figure 7b As shown, in step S5 , based on the ashing photoresist 310 , the exposed active layer film is subjected to a first dry etching to expose the gate insulating layer 303 .
[0073] Through the above steps S4 and S5, the ashing process of the photoresist 310 is set before the first dry etching, such as Figure 6 As shown, the lower bottom edge of the photoresist 310 is retracted by ashing treatment until its orthographic projection on the substrate 301 is flush with the lower bottom edge of the first source-drain electrode layer film 309-1, so that after dry etching of the photoresist 310 in which area B is completely retained after the ashing treatment, there is no tailing of the active layer film.
[0074] In addition, refer to Figure 7b As shown, if the photoresist 310 is ashed and retracted to be flush with the upper edge of the first source-drain electrode layer film 309-1 or retracted into the first source-drain electrode layer film 309-1, that is, retracted to the edge of the positive projection on the substrate 301 within the range of the positive projection of the first source-drain electrode layer film 309-1 on the substrate 301, although the active layer tail length can still be achieved to be zero, the remaining film layer of the gate insulation layer near the bottom edge of the first source-drain electrode layer film 309-1 after the first dry etching will be thin, which may easily cause a short circuit between the gate electrode and the source-drain electrode of the produced TFT during use. Under the same conditions, the thicker the source-drain electrode layer film, the thinner the actual gate insulation layer of the device after the first dry etching, and the higher the device defect rate.
[0075] In an embodiment of the present invention, the photoresist 310 is shrunk during the ashing process so that the orthographic projection of the completely retained area on the substrate 301 coincides with the orthographic projection edge of the first source-drain electrode layer film 309-1 on the substrate 301, thereby ensuring the thickness of the gate insulation layer while achieving zero tailing of the active layer, thereby ensuring the device yield.
[0076] It is worth noting that during the ashing process in step S4, the partially reserved area is completely removed due to the shrinkage of the photoresist, thereby exposing the source-drain electrode layer film corresponding to the partially reserved area, that is, the source-drain electrode layer film corresponding to the channel of the TFT.
[0077] The process of shrinking the photoresist by ashing makes the source and drain metal layer film corresponding to the TFT channel not protected by the photoresist in the first dry etching. The etching gas in the conventional process contains chlorine (Cl2), which is a highly corrosive gas that reacts with metals to generate chloride byproducts. The byproducts are difficult to remove. In the subsequent channel etching process, for example, further reaction with amines (Amine) usually contained in wet etching aggravates the contamination of the back channel, affects the etching quality, makes it difficult to form the expected channel length, increases leakage current, and reduces device performance.
[0078] More preferably, in an embodiment of the present invention, the etching gas in the first dry etching process does not contain Cl2, thereby avoiding the corrosion of the TFT channel by the photoresist that shrinks after the ashing treatment, and forming a good channel. Optionally, the etching gas for the first dry etching is selected from a combination of one or more of NF3 / He, CH4 / He, CHF3 / He and SF6 / He to avoid adverse reactions to the channels that may be exposed and improve the characteristics of the TFT transistor. In addition, removing Cl2 from the first dry etching gas can also reduce safety management risks and waste gas emissions. Optionally, the first dry etching gas flow rate is 2000~6000sccm / 2000~6000sccm, the power is 5~15 / 5~15kw, and the gas pressure is 20~70mT, where " / " separates the ranges of the two gases in the above combined gas.
[0079] Reference Figure 8 As shown, in step S6, the exposed first source-drain electrode layer thin film 309-1 is wet-etched for the second time to form source-drain electrodes 311. Specifically, after the second wet-etching, the orthographic projection of the formed source-drain electrode 311 on the substrate 301 is within the range of the orthographic projection of the completely reserved area B on the substrate 301, ensuring that there is no residue in the TFT channel. At this time, the critical dimension bias (CD bias) of the source-drain metal is the smallest, and the smaller the metal CD bias is, the smaller the tail of the active area formed next.
[0080] Reference Fig. 9 As shown, in step S7, the completely reserved area B is removed. Optionally, after the second wet etching, the completely reserved area B can be stripped by wet etching in the same operating space as the second wet etching. By directly wet-stripping the photoresist 310 of the completely reserved area B after the second wet etching, the transportation time can be saved, the production tact time can be saved, and the work efficiency can be improved. In addition, further optionally, the completely reserved area B can be stripped by dry etching by utilizing the same operating space as the subsequent second dry etching. Before etching the ohmic contact layer in the TFT channel, the completely reserved area of the photoresist 310 is first dry-etched in the same operating space, which can also save transportation time, save production tact time, and improve work efficiency.
[0081] Furthermore, because the step of stripping the photoresist is performed before the second dry etching, the stripping solution, impurities, and byproducts remaining in the TFT channel after stripping the photoresist will be completely removed in the subsequent dry etching process, thereby ensuring that the TFT channel is free from contamination, improving TFT characteristics, especially reducing leakage current, and improving the reliability problem related to leakage current. In addition, removing Cl2 from the second dry etching gas can also reduce safety management risks and waste gas emissions.
[0082] Reference Fig.10 As shown, in step S8, the exposed active layer film is dry-etched for the second time to remove the exposed ohmic contact layer film 307 and part of the semiconductor layer film 305, and the remaining ohmic contact layer film 307 forms an ohmic contact region 313, and the remaining semiconductor layer film 305 forms a channel region 312. Specifically, during the second dry etching, the already formed source-drain electrode 311 is used as an etching barrier layer, so that the ohmic contact region is substantially aligned with the orthographic projection of the corresponding source-drain electrode 311 on the substrate 301. Optionally, the etching gas for the second dry etching can also be selected from a combination of one or more of NF3 / He, CH4 / He, CHF3 / He and SF6 / He. Optionally, the gas flow rate of the second dry etching is 2000-6000sccm / 2000-6000sccm, the power is 5-15 / 5-15kw, and the gas pressure is 20-70mT, where the range of two gases in the above combination of gases is separated by " / ".
[0083] In the above manner, the second dry etching step is set after the step of removing the completely reserved area B of the photoresist 310, so that the finally formed source-drain electrode 311 can be used as an etching barrier layer. Compared with the method in the prior art of using the completely reserved area B with a projection area larger than the source-drain electrode 311 as a barrier layer for the second dry etching and then stripping the photoresist 310, according to the implementation principle of the etching process, this makes the positive projection of the source-drain electrode 311 corresponding to the ohmic contact area directly contacting the source-drain electrode 311 on the substrate 301 basically aligned, so that the tail of the ohmic contact area is almost zero, and because a part of the semiconductor layer film will also be etched away, the active area formed by the active layer film relatively far away from the source-drain electrode 311 has only a very small tail a. Therefore, the tail of the active area is further reduced by the above method.
[0084] After step S8, those skilled in the art should understand that subsequent processes of the array substrate can be carried out, for example, a passivation layer is formed on the substrate 301, and a via is formed in the passivation layer, and then a pixel electrode is formed. The TFT transistor can be electrically connected to the pixel electrode through the via. The specific process will not be repeated here.
[0085] By using the method of the embodiment of the present invention, by changing the step sequence of the 2W2D reaction, the tailing of the active area and the ohmic contact area can be effectively reduced, the parasitic capacitance, for example, parasitic capacitances such as Cpd, Cgd and Cgs can be reduced, and water ripples and white spot defects can be improved; and after the tailing of the ohmic contact area is reduced, such as Fig.11 As shown, the effective channel n+ to n+ distance b increases, which can reduce the design value of the Metal to Metal distance c, thereby realizing the miniaturization of the TFT size. At the same time, the width of the non-display area GOA region can be reduced, thereby further reducing the border area of the narrow frame. The reduction of the tailing of the active area and the ohmic contact area makes it unnecessary to force the manufacturing process of the array substrate to select the 5-mask process, so that it can switch from the 5-mask process to the 4-mask process, thereby improving the exposure capacity and reducing the product cost.
[0086] Accordingly, if Fig.10 As shown, an embodiment of the present invention further provides an array substrate, comprising:
[0087] Substrate 301;
[0088] An array of TFTs is formed on a substrate 301 , wherein the TFTs include a gate electrode 315 , a gate insulating layer 303 , an active region 312 , an ohmic contact region 313 and a source-drain electrode 311 , wherein the ohmic contact region is substantially aligned with the corresponding source-drain electrode 311 in terms of their orthographic projection on the substrate.
[0089] In this embodiment, the tailing of the ohmic contact area of the TFT is almost zero, which reduces the parasitic capacitance, improves the water ripples and white spot defects, and reduces the size of the thin film transistor, which is conducive to reducing the frame; in addition, the above method can effectively reduce the leakage current and improve the reliability defects related to the leakage current; and the improved method further promotes the switching from the 5-mask process to the 4-mask process, improves the production capacity, reduces the product cost, and has broad application prospects.
[0090] The array substrate according to the embodiment of the present invention can be used in an OLED display panel or an LCD display device.
[0091] An embodiment of the present invention further provides a liquid crystal display panel, comprising:
[0092] Color film substrate;
[0093] The array substrate according to the above embodiment; and
[0094] The liquid crystal layer is encapsulated between the color filter substrate and the array substrate.
[0095] Since the array included in the display device provided in the embodiment of the present application corresponds to the array substrate provided in the above embodiment, the previous embodiment is also applicable to the use method provided in this embodiment and will not be described in detail in this embodiment.
[0096] An embodiment of the present invention further provides a display device, comprising:
[0097] The liquid crystal display panel described in the above embodiments.
[0098] In this embodiment, the display device may be any product or component with a display function, such as a mobile phone, a tablet computer, a television, a monitor, a notebook computer, a digital photo frame or a navigator.
[0099] In view of the existing problems, the present invention develops an array substrate and a manufacturing method thereof, a liquid crystal display panel and a display device, and after the first dry etching, the photoresist is first ashed and then the first dry etching is performed, and after the second wet etching, the photoresist is first stripped and then the second dry etching is performed, so that the tailing of the active area and the ohmic contact area generated in the first dry etching, the second wet etching and the second dry etching is reduced, the parasitic capacitance is reduced, the water ripple and the white spot defects are improved, and the size of the thin film transistor is reduced, which is conducive to reducing the frame; in addition, the above method can effectively reduce the leakage current and improve the reliability defects related to the leakage current; and the improved method further promotes the switching from the 5-mask process to the 4-mask process, improves the production capacity, reduces the product cost, and has a wide application prospect.
[0100] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the embodiments here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for manufacturing an array substrate, characterized in that: include: Forming an active layer film and a source-drain electrode layer film on a substrate having a gate electrode and a gate insulating layer, wherein the active layer film comprises a semiconductor layer film and an ohmic contact layer film sequentially formed in a direction away from the substrate; Forming a patterned photoresist on the source-drain electrode layer film, including a completely reserved area and a partially reserved area; Performing a first wet etching on the exposed source-drain electrode layer film to obtain a first source-drain electrode layer film, wherein the orthographic projection of the first source-drain electrode layer film on the substrate is within the range of the orthographic projection of the completely reserved area on the substrate; Performing an ashing process on the photoresist to remove the partially reserved area, and making the orthographic projection of the completely reserved area on the substrate coincide with the edge of the orthographic projection of the first source-drain electrode layer thin film on the substrate; Performing a first dry etching on the exposed active layer film to expose the gate insulating layer, wherein the etching gas of the first dry etching does not contain Cl2; Performing a second wet etching on the exposed first source-drain electrode layer film to form source-drain electrodes; removing the completely reserved area; as well as The exposed active layer film is subjected to a second dry etching to remove the exposed ohmic contact layer film and part of the semiconductor layer film, the remaining ohmic contact layer film forms an ohmic contact region, and the remaining semiconductor layer film forms a channel region, wherein the ohmic contact region is substantially aligned with the orthographic projection of the corresponding source and drain electrodes on the substrate.
2. The method according to claim 1, characterized in that: The etching gas for the first dry etching and / or the second dry etching is selected from one or more combinations of NF3 / He, CH4 / He, CHF3 / He and SF6 / He.
3. The production method according to claim 1 or 2, characterized in that: The step of ashing the photoresist to remove the partially reserved area and making the orthographic projection of the completely reserved area on the substrate coincide with the edge of the orthographic projection of the first source-drain electrode layer film on the substrate further comprises: The photoresist layer is ashed to shrink the completely reserved area toward the partially reserved area, so that the orthographic projection of the completely reserved area on the substrate coincides with the orthographic projection edge of the first source-drain electrode layer thin film on the substrate.
4. The method according to claim 1 or 2, characterized in that: The removing of the completely reserved area further comprises: In the same operation space as the second wet etching, stripping the completely reserved area by wet etching; or In the same operation space as the second dry etching, the completely reserved area is stripped by dry etching.
5. The manufacturing method according to claim 3, characterized in that: The gas flow rate of the ashing treatment is 2000-15000sccm, 200-2000 / 2000-15000sccm; the power is 5-15 / 5-15kw, the gas pressure is 20-70mT, and the ashing time is 40-80s.
6. The method according to claim 2, characterized in that: The gas flow rate of the first dry etching and / or the second dry etching is 2000-6000sccm / 2000-6000sccm, the power is 5-15 / 5-15kw, and the gas pressure is 20-70mT.
7. The manufacturing method according to claim 1, characterized in that: The source-drain electrode layer thin film is a multi-layer metal structure, and the film layer combination is selected from one of Mo / AL / Mo, Mo / Cu, MoNb / Cu, MoNb / Cu / MoTi or a stack thereof.
8. The manufacturing method according to claim 1, characterized in that: The material of the semiconductor layer film is polysilicon, and the material of the ohmic contact layer film is doped polysilicon.
9. The manufacturing method according to claim 1, characterized in that: The patterned photoresist formed on the source-drain electrode layer film includes a completely reserved area and a partially reserved area, and further includes: forming a photoresist layer on the source-drain electrode layer thin film; The photoresist layer is exposed by photolithography using a dual-tone mask to form the completely reserved area and the partially reserved area.
10. The manufacturing method according to claim 1, characterized in that: Also includes: forming a passivation layer and a via in the passivation layer; A pixel electrode is formed.
11. An array substrate manufactured by the manufacturing method according to any one of claims 1 to 10, characterized in that: include: substrate; An array of thin film transistors is formed on a substrate, wherein the thin film transistor comprises a gate electrode, a gate insulating layer, an active region, an ohmic contact region and a source-drain electrode, wherein the ohmic contact region is substantially aligned with the orthographic projection of the corresponding source-drain electrode on the substrate.
12. A liquid crystal display panel, comprising: Color film substrate; The array substrate according to claim 11; as well as The liquid crystal layer is packaged between the color filter substrate and the array substrate.
13. A display device comprising the liquid crystal display panel according to claim 12.