Anodized antibacterial metal material, method for making the material and reactivation method thereof

Through controlled anodization and antibacterial solution treatment, a metal surface with a controlled pore structure is formed, which solves the problem of insufficient antibacterial properties of anodized metal surfaces in the prior art, and realizes effective killing and antibacterial properties of broad-spectrum microorganisms. Extended, suitable for a variety of metal materials.

CN114745955BActive Publication Date: 2024-11-05A3 SURFACES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080082939.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-25
Filing Date
2020-12-09
Publication Date
2024-11-05
Estimated Expiration
2040-12-09

AI Technical Summary

Technical Problem

The prior art is difficult to effectively handle anodized metal surfaces, especially aluminum and their alloys, and cannot effectively kill broad-spectrum microorganisms, and known antibacterial metal products have short service life and cannot extend their service life.

Method used

通过受控电流密度对金属表面进行阳极化,形成具有受控空间密度和深度的孔,并使其与抗菌溶液接触,密封孔,随后可能再次接触抗菌溶液,并用酸性溶液冲洗以形成裂纹,提高抗菌特性。

Benefits of technology

It realizes effective killing of broad-spectrum microorganisms, extends the service life of antibacterial metal products, and is simple, fast and economical. It is suitable for a variety of anodized metals, including aluminum and its alloys, improving the high humidity environment. Antibacterial properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003668577540000131
    Figure BDA0003668577540000131
  • Figure BDA0003668577540000151
    Figure BDA0003668577540000151
  • Figure BDA0003668577540000161
    Figure BDA0003668577540000161
Patent Text Reader

Abstract

A method for preparing a metal product having antimicrobial properties is disclosed, first comprising anodizing a product having at least one metal surface (e.g., aluminum, steel) using a controlled current density to form pores on the surface having a controlled spatial density and depth. The method also comprises contacting the anodized metal surface with a first antimicrobial solution before sealing the pores. Preferably, the metal surface can be contacted with the first antimicrobial solution again after the sealing step. A method for reactivating the antimicrobial properties of a metal product is also disclosed, comprising contacting the antimicrobial product with a second antimicrobial solution again. Preferably, for safety reasons, the concentration of the second solution is lower than the first solution. The present invention provides a simpler, faster, cheaper and improved method for treating or reactivating metal surfaces to obtain metal products with excellent and lasting antimicrobial properties.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This patent application claims the benefit of priority to U.S. Provisional Patent Application No. 62 / 946,272, filed with the U.S. Patent and Trademark Office on December 10, 2019, entitled “Method for Making Antimicrobial Metal Materials,” and U.S. Provisional Patent Application No. 63 / 044,164, filed with the U.S. Patent and Trademark Office on June 25, 2020, entitled “Method for Preparing Antimicrobial Metal Materials and Method for Reloading Them,” the contents of which are incorporated herein by reference. Technical Field

[0003] The present invention generally relates to a method for preparing a metal material or product, and more particularly to a metal product having an anodized surface with antimicrobial properties. The present invention also generally relates to an antimicrobial metal product made by the process and method. The present invention further relates to a method for reactivating an antimicrobial metal product after a certain period of time to maintain its antimicrobial properties. Background Art

[0004] Pathogenic microorganisms are ubiquitous and their spread in public places plays an important role in triggering infectious outbreaks. Nosocomial (hospital-acquired) infections are the sixth leading cause of death in Western countries, with higher rates in developing countries. Another major culprit for the spread of infectious diseases is public transportation, such as buses, trams and subways. Antimicrobial materials for high-touch areas such as hospitals and public transportation have been developed to reduce the risks associated with bacteria that can survive for months on regular metal surfaces.

[0005] Aluminum and aluminum alloy materials are lightweight, have strength, flexibility and provide some corrosion resistance durability after anodizing. Aluminum alloy products have many applications, including kitchen utensils, household furniture, appliances, door handles, medical devices, etc. However, aluminum itself does not have antimicrobial properties, and microorganisms can easily survive on its surface. Various methods have been developed for treating the surface of aluminum or aluminum alloy products to improve their antimicrobial properties. However, these methods and the products obtained therefrom are not optimal because the antimicrobial activity is weak or limited to a few bacterial species and / or because the antimicrobial treatment is incompatible with the dyeing of aluminum products. In addition, these methods may not be suitable for the antimicrobial treatment of other anodizable metals such as magnesium, zinc, niobium, tantalum and titanium.

[0006] Steel and stainless steel are mainly used to manufacture products such as kitchen counters, door handles or sliding door panels, to name just a few. However, surface treatment of steel products usually means pre-coating the steel sheet before being able to render the surface of the steel product biocidal. As disclosed in US 2018 / 0133370 (Turner et al.), the steel sheet must be pre-plated or coated with a metal, such as titanium.

[0007] WO 2013 / 155618 A1 (Arsenault et al.) discloses a metal product having an anodized surface with antimicrobial properties, and a method for producing such a metal product. The antimicrobial metal product comprises a porous surface layer formed by anodization, the porous surface layer comprising an electrodeposit of at least one metal and at least one antimicrobial compound. The electrodeposited metal may be selected from silver, gold, copper, nickel, zinc, tin, palladium, cadmium and platinum. Arsenault et al. specify that silver (Ag) is electrodeposited to the porous surface layer because this metal has both aesthetic and antimicrobial properties. However, the electrodeposition step of the method disclosed by Arsenault et al. implies significant additional costs for the manufacture of the product.

[0008] Furthermore, known solutions do not allow to extend the service life of antimicrobial metal products once they have been permanently installed on site, such as urban furniture, support poles in public transport (e.g. buses, subway cars), door handles, kitchen counters, etc.

[0009] Therefore, there is a need for an improved method for treating anodizable metal surfaces to obtain metal products with antimicrobial properties that can effectively kill a broad spectrum of microorganisms, including Gram-positive microbial pathogens, Gram-negative microbial pathogens, viruses such as coronaviruses (e.g., SARS-CoV-2), and yeasts.

[0010] There is also a need for a method for reactivating the metal surface of a metal antimicrobial product and thereby extending the useful life of the antimicrobial metal product.

[0011] The present invention addresses other needs, as will become apparent from a review of the following disclosure, drawings, and description of the features of the invention. Summary of the invention

[0012] The shortcomings of the prior art are generally alleviated by the methods described herein for preparing metal products having long-lasting antimicrobial properties.

[0013] According to a first aspect, the present invention relates to a method for preparing a metal product having antimicrobial properties, the method comprising:

[0014] anodizing a product having at least one metal surface using a controlled current density, the controlled anodizing allowing pores to be formed throughout the at least one metal surface with a controlled spatial density and depth; or

[0015] providing a product that is pre-anodized to have at least one anodized metal surface;

[0016] contacting the at least one metal surface with a first antimicrobial solution for a first period of time; and sealing the aperture.

[0017] According to a preferred embodiment, the method further comprises, after sealing the hole: bringing the at least one metal surface of the metal product into contact with the first antimicrobial solution again.

[0018] According to a preferred embodiment, the method further comprises, after anodizing: rinsing the metal product with an acidic solution. Preferably, the acidic solution may comprise 0.15 to 5% sulfuric acid.

[0019] According to a preferred embodiment, the method may further comprise rinsing the metal product again with a second acidic solution or water, wherein the temperature of the second acidic solution or water is lower than the temperature of the metal product, so as to form cracks on the at least one metal surface.

[0020] According to a preferred embodiment, the anodizing step comprises using about 1A / dm 2 Up to 5A / dm 2 , preferably 2 to 4 A / dm 2 The at least one metal surface is anodized with a current within a range.

[0021] According to a preferred embodiment, the first antimicrobial solution comprises at least one antibiotic, antimicrobial peptide, enzyme, cationic compound or a combination thereof at a first concentration. Preferably, the first antimicrobial solution comprises at least one cationic compound, such as at least one quaternary ammonium compound.

[0022] According to a preferred embodiment, the first antibacterial solution may further include at least one metal salt. Preferably, the at least one metal salt is Ni(NO3)2, AgNO3, Ti(NO3)3, Zn(NO3)2, Cu(NO3)2, NiCl2, AgCl, ZnCl2, CuCl2, Ni3(PO4)2, Ag3PO4, Zn3(PO4)2, Cu3(PO4)2 or a combination thereof.

[0023] According to a preferred embodiment, the at least one metal salt is AgNO 3 , whereby in use, AgNO 3 forms AgCl in situ with the at least one quaternary ammonium compound.

[0024] According to a preferred embodiment, the contacting step comprises: immersing the at least one metal surface in the first antimicrobial solution for a first period of time, preferably from about 15 seconds to about 60 minutes, preferably from about 5 to 45 minutes, more preferably from about 15 to 30 minutes.

[0025] According to a preferred embodiment, the step of sealing the holes comprises heating the at least one metal surface in a water bath or a nickel acetate solution bath at a temperature of about 70-90° C. for a second period of time, preferably about 1 to 15 minutes.

[0026] According to a preferred embodiment, the at least one metal surface comprises steel, aluminum, titanium, zinc, magnesium, niobium, tantalum or an anodizable alloy thereof. Preferably, the metal product comprises aluminum or an anodizable alloy thereof. Alternatively, the metal product may comprise steel or an anodizable alloy thereof.

[0027] According to a second aspect, the present invention relates to an antimicrobial metal product obtained by the process claimed herein, wherein said metal product has at least one treated anodized surface with sealed pores having a pore depth of 5 to 150 μm, preferably 50 to 100 μm. In addition to the pores formed during the anodizing step, the anodized surface of said antimicrobial metal product may also include a plurality of cracks or fissures, which are usually formed during the preferred step of washing the product with an acidic solution and low temperature water.

[0028] According to a preferred embodiment, the antimicrobial metal product comprises steel, aluminum, titanium, zinc, magnesium, niobium, tantalum or an anodizable alloy thereof. Preferably, the metal product comprises aluminum or an anodizable alloy thereof. In addition, the antimicrobial metal product may comprise steel or an anodizable alloy thereof.

[0029] According to a preferred embodiment, the metal product has a treated anodized surface with sealed pores over the entire surface, the pores having a diameter of 5 to about 100 nm.

[0030] The antimicrobial metal products of the present invention are particularly useful in making articles used in homes, medical facilities and public transportation, such as kitchenware, kitchen countertops, hospital countertops, furniture, fixtures, appliances, office equipment, door handles, door push plates, medical equipment, wall panels, flooring, machine keyboards and handrails.

[0031] The products obtained by the method disclosed herein show controlled color and longer lasting antimicrobial properties. In addition, the antimicrobial metal surface obtained by the method has improved antimicrobial properties in high humidity and water environments.

[0032] The methods disclosed herein are simpler, faster, and less expensive than before for treating anodizable metal surfaces, for example by eliminating steps associated with electrodepositing the metal onto the anodized surface.

[0033] The present invention also relates to a method for reactivating the antimicrobial properties of an antimicrobial metal product obtained by the method claimed herein, the method comprising:

[0034] At least one surface of the antimicrobial metal product is contacted with a second antimicrobial solution to extend the useful life of the product.

[0035] According to a preferred embodiment, the step of contacting at least one surface of the antibacterial metal product with a second antibacterial solution comprises: spraying the second solution on the at least one surface; and allowing the spread second solution to remain on the at least one surface for a third period of time. The third period of time is preferably 5 seconds to 30 minutes. Preferably, the method may further comprise: removing excess portions of the second antibacterial solution from the at least one surface.

[0036] According to another preferred embodiment, the step of contacting at least one surface of the antibacterial metal product with a second antibacterial solution comprises: applying the second antibacterial solution to the at least one surface with a cloth pre-soaked in the second antibacterial solution. Preferably, applying the second solution to the at least one surface with a cloth pre-soaked in the solution comprises: wiping the at least one surface at least once with the soaked cloth. Preferably, wiping the at least one surface several times with the soaked cloth.

[0037] According to another preferred embodiment, the step of contacting at least one surface of the antibacterial metal product with a second antibacterial solution comprises:

[0038] soaking the antimicrobial metal product in the second solution for a given period of time; and removing the antimicrobial metal product from the second solution.

[0039] According to a preferred embodiment, the method further comprises removing excess portions of the second solution from the at least one surface.

[0040] According to a preferred embodiment, the second antimicrobial solution comprises at least one of antibiotics, antimicrobial peptides, enzymes, cationic compounds or a combination thereof at a second concentration.

[0041] According to a preferred embodiment, the second solution comprises at least one cationic compound. Preferably, the cationic compound comprises at least one quaternary ammonium compound.

[0042] According to a preferred embodiment, the antibacterial solution may further include at least one metal salt, such as Ni(NO3)2, AgNO3, Ti(NO3)3, Zn(NO3)2, Cu(NO3)2, NiCl2, AgCl, ZnCl2, CuCl2, Ni3(PO4)2, Ag3PO4, Zn3(PO4)2, Cu3(PO4)2 and combinations thereof. More preferably, the salt is AgNO3 which reacts with a quaternary ammonium chloride to form silver chloride AgCl in situ.

[0043] According to a preferred embodiment, the second concentration of the second solution is lower than the first concentration of the first solution claimed herein. Preferably, the second concentration is lower than the first concentration by a factor of ten.

[0044] Advantageously, the antimicrobial metal product according to the present invention can be further treated by the method claimed herein for a period of time to reactivate the antimicrobial properties of the metal surface and thus extend the service life of the antimicrobial metal product. This is particularly convenient when the metal product to be reactivated is fixed, such as a door handle, a railing in a transport vehicle (such as a car, bus, train and subway) or a kitchen counter.

[0045] Other and further aspects and advantages of the invention will be better understood after reading the illustrative embodiments to be described or indicated in the appended claims, and various advantages not mentioned herein will occur to those skilled in the art after using the invention in practice. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The above and other aspects, features and advantages of the present invention will become more apparent from the following description with reference to the accompanying drawings, in which:

[0047] Figure 1 A method for preparing a metal product having long-lasting antimicrobial properties according to a preferred embodiment is shown; and

[0048] Figure 2 A method of reactivating the antimicrobial properties of an antimicrobial metal product according to a preferred embodiment is shown. DETAILED DESCRIPTION

[0049] A novel method for preparing an antimicrobial metal product and a novel method for reactivating an antimicrobial metal product are described below. Although the present invention is described in terms of specific illustrative embodiments, it should be understood that the embodiments described herein are merely examples and the scope of the present invention is not intended to be limited thereby.

[0050] The terms used herein are subject to the definitions set forth below.

[0051] As used herein, unless otherwise indicated, % or wt.% refers to weight %. As used herein, % refers to weight % compared to the total weight percentage of the phase or composition in question.

[0052] "About" means that the value of weight % (wt.%), time, pH, volume or temperature can vary within a certain range, depending on the error margin of the method or device used to evaluate such weight %, time, pH, volume or temperature. A 10% error margin is generally accepted.

[0053] "Room temperature" refers to the temperature of the immediate environment, for example a temperature of 20°C ± 10°C.

[0054] The following description and the embodiments described therein are provided by way of examples of specific embodiments illustrating the principles and aspects of the present invention. These embodiments are provided to explain, but not to limit, those principles of the present invention. In the following description, throughout the specification and the accompanying drawings, identical parts and / or steps are marked with the same corresponding reference numerals.

[0055] According to a first aspect, the present invention relates to a method for producing an antimicrobial metal product having at least one antimicrobial surface.

[0056] Figure 1 A preferred embodiment of a method (1000) for preparing a metal product having antimicrobial properties is shown, the method comprising:

[0057] anodizing (1100a) a product having at least one metal surface using a controlled current density, the controlled anodizing allowing pores having a controlled spatial density and depth to be formed throughout the at least one metal surface; or

[0058] Providing a product (1100b) that is previously anodized to have at least one anodized metal surface;

[0059] contacting the at least one metal surface with a first antimicrobial solution for a first period of time (1200); and

[0060] The hole is sealed (1300).

[0061] According to a preferred embodiment, Figure 1 In the illustrated embodiment, the method (1000) may further include another step (1400) of contacting the at least one metal surface of the metal product with the first antimicrobial solution again after the sealing step (1300). It has been found that a second contact with the antimicrobial solution can increase the useful life of the antimicrobial metal product even after the aperture is sealed.

[0062] According to a preferred embodiment, the metal surface is anodized (1100) using about 1A / dm 2 To about 5A / dm 2 , preferably 2 to 4 A / dm 2 As described in detail below, it has been found that low current density will provide smaller pore sizes and slower diffusion of the antimicrobial solution from the pores, thereby providing longer-lasting antimicrobial properties to the metal product.

[0063] According to a preferred embodiment, the first antibacterial solution comprises at least one of an antibiotic, an antimicrobial peptide, an enzyme, a cationic compound or a combination thereof. More particularly, the first antibacterial solution comprises at least one cationic compound, such as a quaternary ammonium compound (QAC). In fact, among the antibacterial candidates studied, QAC is effective against a broad spectrum of Gram-positive and Gram-negative bacteria. The advantages of QAC include amphiphilic solubility, effectiveness over a wide pH range, low toxicity to human cells, low vapor pressure and odorlessness, etc. More specifically, QAC is very effective against Staphylococcus aureus, which is the most common source of hospital infection and infection from public transportation environments.

[0064] The applicant has particularly developed a first antimicrobial solution, hereinafter named A3S solution, which generally comprises a quaternary ammonium, such as alkyl dimethyl benzyl ammonium chloride (ADBAC). More preferably, the porous surface layer comprises at least two quaternary ammonium compounds, namely alkyl dimethyl benzyl ammonium chloride (ADBAC) and didecyl dimethyl ammonium chloride (DDAC). The solution may also comprise Ni(NO3)2, AgNO3, Ti(NO3)3, Zn(NO3)2, Cu(NO3)2, NiCl2, AgCl, ZnCl2, CuCl2, Ni3(PO4)2, Ag3PO4, Zn3(PO4)2, Cu3(PO4)2 or a mixture thereof.

[0065] According to a preferred embodiment, the first solution comprises a quaternary ammonium chloride as disclosed herein and silver nitrate (AgNO3), resulting in the in-situ formation of silver chloride (AgCl). It has been found that the in-situ presence of AgCl in the first treatment solution increases or promotes the antimicrobial properties of the antimicrobial metal product.

[0066] According to a preferred embodiment, impregnating the pores with the first antimicrobial solution comprises immersing the anodized metal in the antimicrobial solution for a first period of time. Typically, the first period of time is about 15 seconds to 1 hour, preferably 5 minutes to 45 minutes, and more preferably about 15-30 minutes.

[0067] According to a preferred embodiment, the sealing of the pores comprises heating the treated anodized metal product in a water bath or more preferably in a solution bath of nickel acetate, magnesium acetate, etc., at a temperature of about 70-90° C. for a given period of about 1-15 minutes, preferably 2-5 minutes, more preferably about 2 minutes. Other sealing methods may be used without departing from the scope of the present invention.

[0068] According to a preferred embodiment, the metal surface of the product to be treated may comprise steel, aluminum, titanium, zinc, magnesium, niobium, tantalum or an anodizable alloy thereof. More preferably, the metal is aluminum or an anodizable alloy thereof. In addition, the antimicrobial metal product may comprise steel or an anodizable alloy, such as preferably stainless steel, such as but not limited to 304 or 316 stainless steel.

[0069] According to a preferred embodiment, Figure 1 In the illustrated embodiment, the method (1000) may further include, after anodizing, rinsing the metal product with an acidic solution, such as a 0.1 to 5% sulfuric acid solution (1500). It has been found that this step of rinsing with an acidic solution can produce a plurality of small cracks on the surface of the metal product. The size of the cracks is generally larger than the pores produced by anodizing, thereby increasing the storage capacity of the metal product for the antimicrobial solution, especially when the antimicrobial solution contains metal salts that provide Ag, Cu, Ni, Ti and / or Zn particles (such as those disclosed herein), increasing the storage capacity for metal particles.

[0070] The methods disclosed herein are simpler, faster, and less expensive than previous methods for treating anodizable metal surfaces, for example by eliminating steps associated with electrodepositing metal on anodized surfaces.

[0071] Antimicrobial Metal Products:

[0072] As mentioned above, the present invention also relates to an antimicrobial metal product obtained by the method claimed herein. The metal product may be characterized by an anodized surface with sealed pores, the depth of the pores being 5 to 150 μm, preferably 50 to 100 μm, and the diameter of the pores being 5 to about 100 nm.

[0073] Furthermore, it has been found that, according to a preferred embodiment, the method can result in an anodized surface having, in addition to the pores formed during the anodizing step, a plurality of cracks or fissures formed on the surface, usually due to thermal plugging during a preferred step of rinsing the product with a cold weak acid solution and cold water. In practice, the rinsing step can consist in immersing the metal product, whose temperature can be about 60-100° C., in a bath containing a cold weak acid solution or cold water. The presence of cracks or fissures can allow a better impregnation of the antimicrobial solution on the anodized surface, thus providing a longer service life of the antimicrobial metal product.

[0074] Of course, the antimicrobial metal product also comprises steel, aluminum, titanium, zinc, magnesium, niobium, tantalum or an anodizable alloy thereof. Preferably, the metal product comprises aluminum or an anodizable alloy thereof. In addition, the antimicrobial metal product may comprise steel or an anodizable alloy thereof.

[0075] The products obtained by the methods disclosed herein show controlled color and longer antimicrobial properties. In addition, the antimicrobial metal surfaces obtained by these methods have improved antimicrobial properties in high humidity and water environments.

[0076] The antimicrobial metal products of the present invention are particularly useful in making articles for use in homes, medical facilities and public transportation, such as for preparing kitchenware, kitchen countertops, hospital countertops, furniture, fixtures, electrical appliances, office equipment, door handles, medical equipment, wall panels, flooring, machine keyboards and handrails.

[0077] Reactivation method:

[0078] Although the preparation method according to the present invention allows the manufacture of antimicrobial metal products with a longer service life than products known in the art, said metal products cannot be easily removed or replaced with new products once installed on site. Therefore, a new method for extending the service life and antimicrobial properties of antimicrobial metal products (obtained by the method disclosed herein or any anodized metal surface) has been developed.

[0079] According to a preferred embodiment, Figure 2 In the illustrated embodiment, the method involves contacting (2100) the anodized surface of the pre-treated antimicrobial metal product with a second antimicrobial solution to reactivate the pores with the second solution.

[0080] According to a preferred embodiment, the second solution may contain the same ingredients as the first solution used in the manufacturing method (1000). However, the second solution may have a lower concentration of its active ingredients (a diluted solution). Advantageously, the method provides a simple way to reactivate or reload the product without having to move the product from the site. In addition, the second "reactivation" solution has a lower concentration of QAC, providing a safer method for people responsible for maintaining or cleaning metal parts to regularly treat the surface. For example, a subway or bus fixed pole can be reactivated by spraying the second solution on the surface.

[0081] Different ways of reactivating the surface with a second antimicrobial solution have been tested and are effective.

[0082] First, as described above, the second solution can be sprayed on the surface; and the spread second solution is allowed to remain on the surface for a third period of time, typically 5 seconds to 30 minutes. It must be understood that the contact time and solution volume of the surface to be treated vary with the thickness of the anodized surface (number and size of pores, presence of cracks, etc.). Preferably, the method may also include removing excess portions of the second solution that have not been absorbed into the pores after the third period of time. This first option is particularly suitable for reactivating vertical surfaces, such as transport handlebars, for example during the cleaning of transport vehicles.

[0083] Alternatively, the surface of the antimicrobial metal product may be contacted with the second antimicrobial solution by applying the second solution to the surface with a cloth previously soaked or impregnated with the second solution. Preferably, the solution is wiped with the soaked cloth at least once, preferably several times, until the pores are refilled with the second solution. This second option is particularly useful for reactivating horizontal surfaces, such as kitchen counters.

[0084] Third, reloading the surface of the antimicrobial metal product with a second antimicrobial solution can involve soaking or immersing the antimicrobial metal product in the second solution for a second period of time; removing the antimicrobial metal product from the second solution, and optionally removing excess portions of the second solution that are not absorbed into the pores. Such solutions are particularly useful for mobile and small products that can be removed from the field, such as metal tools.

[0085] According to a preferred embodiment, the second antimicrobial solution comprises at least one of antibiotics, antimicrobial peptides, enzymes, cationic compounds or a combination thereof at a second concentration.

[0086] According to a preferred embodiment, the second solution comprises at least one cationic compound. Preferably, the cationic compound comprises at least one quaternary ammonium compound (QAC), such as a diluted solution of D-germ-5. For the A3S solution used in the preparation of the antimicrobial product, the second "reload" solution may further comprise at least one metal salt, such as Ni(NO3)2, AgNO3, Ti(NO3)3, Zn(NO3)2, Cu(NO3)2, NiCl2, AgCl, ZnCl2, CuCl2, Ni3(PO4)2, Ag3PO4, Zn3(PO4)2, Cu3(PO4)2 and combinations thereof. More preferably, the salt is AgNO3 which reacts with the QAC in situ to form silver chloride AgCl, which is particularly effective as a bactericide.

[0087] Preferably, the second concentration of the second solution is lower than the first concentration of the first solution claimed herein, for example a 10-fold diluted solution. Advantageously, the lower concentration second solution is safer to use for personnel responsible for reactivating metal surfaces.

[0088] Example:

[0089] The purpose of the following examples is to demonstrate or establish the effect of control of the anodization step on the resulting density, location and size of pores produced on the metal surface, the correlation between density and size, and the correlation between pore architecture and microbiological properties of the final product.

[0090] Antimicrobial solutions (manufacturing and reactivation solutions)

[0091] Table 1: Examples of a first solution for making an antimicrobial metal product and a second solution for reloading:

[0092]

[0093] (*10.85% fifth generation quaternary ammonium salt, such as D-Germ 5 solution)

[0094] Manufacturing method

[0095] Example 1: Sealing / impregnation sequence for antimicrobial and sealing treatment

[0096] Four pieces of 3" x 3" aluminum are hard anodized (3-5A / dm 2 ) until the pore depth was 22 ± 2 μm, followed by post-anodization. Each piece was cleaned in a 53°C industrial aluminum soap solution for 8 minutes, rinsed in water, etched in a 56°C sodium hydroxide solution for one minute, rinsed in water again, cleaned in a deoxygenated solution mixture for 5 minutes, and then rinsed a final time with water. The piece that was not treated with antimicrobial agents but was sealed was used as a negative control that should not have any antimicrobial activity. The second piece was treated in an antimicrobial A3S solution before sealing. The third piece was treated with an A3S solution both before and after sealing. The fourth and final piece was treated with A3S after the sealing procedure. The antimicrobial treatment was carried out for 15 minutes at room temperature while sealing was performed in a nickel acetate bath at 80°C. In the test against Staphylococcus aureus ( 6538), the sheets were rinsed and dried before antimicrobial testing.

[0097] Use 7,5.10 5 The bacteria were inoculated into the disc and incubated at 22°C for 10 minutes. The bacteria were then harvested and plated overnight at 37°C. Water depletion tests were performed, with each depletion being performed for one hour. Inoculation, harvesting, and plating were performed after each depletion. A total of four depletions were performed per aluminum disc.

[0098] Table 2: Experiment #1 results.

[0099] Exhaustion Negative control Sealing pretreatment Double processing Sealing post-processing 0 +++ - - - 1 +++ + - - 2 +++ + ± ± 3 +++ + ± + 4 +++ +++ + +++

[0100] In Table 2, the symbol "-" indicates no bacterial growth, "±" indicates a few colonies were visible, "+" indicates weak bacterial growth, "++" indicates average bacterial growth, and "+++" indicates strong bacterial growth or a bacterial lawn.

[0101] Results showed similar efficiencies between A3S-treated sheets before or after sealing before depletion testing. The dual and post-seal treatments showed sustained antimicrobial activity after one depletion test, while the pre-seal did not kill all bacteria within the 10-minute time frame. The dual treatment showed better efficiency than the post-seal treatment after 3 depletions and was the only sheet that still had any antimicrobial efficiency after 4 depletions. The negative control never showed any antimicrobial properties.

[0102] According to the preferred embodiment, the dual treatment approach appears to be more durable and effective than the single treatment approach.

[0103] Example 2: Effect of anodizing current on antibacterial efficiency after water consumption.

[0104] Two pieces of 3” x 3” aluminum were hard anodized to a hole depth of 22 ± 2μm. Both pieces were washed in a 53°C industrial aluminum soap solution for 8 minutes, rinsed in water, etched in a 56°C sodium hydroxide solution for 1 minute, rinsed again in water, cleaned in a deoxidized solution mixture for 5 minutes, and then rinsed a final time in water. The two pieces were anodized using different currents, 2A / dm 2 and 4A / dm 2 The post-anodization treatment was identical, with both sheets immersed in A3S antimicrobial solution for 15 minutes, then sealed in nickel acetate solution at 80°C for 2 minutes, and then immersed again in antimicrobial solution. The sheets were rinsed and dried prior to antimicrobial testing against Staphylococcus aureus (ATCC 6538).

[0105] Use 1.5.10 6 The bacteria were inoculated into the disc and incubated at 22°C for 5 minutes. The bacteria were then harvested and plated overnight at 37°C. Water depletion tests were performed, with each depletion being performed for 10 minutes. Inoculation, harvesting, and plating were performed after each depletion. A total of nine depletions were performed per aluminum disc.

[0106] Table 3: Experiment #2 results. CFU (colony forming units) were measured for each plate. TNC = too many to measure.

[0107]

[0108]

[0109] The results in Table 3 show that the use of a lower current (2 A / dm 2 ) had a longer lasting antimicrobial activity. The slower anodization had lower CFU counts at each depletion until the 7th time, with numerous bacterial lawns on both plates at the 7th time. Low current anodization appeared to be more resistant to water depletion.

[0110] Example 3: Effect of anodizing current on antibacterial efficiency of agar plate depletion

[0111] Four circular pieces of aluminum with a diameter of 1.1 cm were hard anodized to a pore depth of 60 ± 2 μm. Each piece was washed in an industrial aluminum soap solution at 53°C for 8 minutes, rinsed in water, etched in a sodium hydroxide solution at 56°C for one minute, rinsed again in water, cleaned in a deoxidized solution mixture for 5 minutes, and then rinsed a final time in water. The four pieces were anodized using different currents, one piece at 2 A / dm 2 , two pieces at 3A / dm 2 And the last piece is at 4A / dm 2 . Anodizing post-treatment is the same, 2 and 4A / dm 2 The sheets were immersed in A3S antimicrobial solution for 15 minutes, sealed in nickel acetate solution at 80°C for 2 minutes, and then immersed in the antimicrobial solution again for 15 minutes. 3A / dm 2 One was simply sealed for 15 minutes and used as a control, while the last piece was treated in the A3S solution for 15 minutes and then sealed for 5 minutes. The pieces were rinsed and dried before antimicrobial testing against Staphylococcus aureus (ATCC 6538).

[0112] Inoculate the agar plate using a cotton swab dipped in a 0.1-DO600 solution of Staphylococcus aureus. Streak the plate 3 times, rotating it 60 degrees each time to ensure even distribution of the inoculum. Let it dry for 3 minutes, then place the aluminum sheet for 5 minutes, then place it in another position for a second deposition, and so on for 24 depositions. Perform 6 depositions on each agar plate to prevent over-drying. The other three sheets are treated in the same way. The agar plate is then placed at 37°C overnight and the radius of the inhibition zone is measured the next day.

[0113] Table 4: Results of Experiment 3. The measured inhibition zone is the diameter obtained by multiplying the shortest radius by 2.

[0114]

[0115]

[0116] After 24 depositions in Table 4, the sheet with the lower current during anodization was the sheet with the largest inhibition zone. 2 Initially with a ratio of 3A / dm 2 Larger area, but less effective after 24 cycles. Despite longer sealing time and no re-impregnation, 3A / dm 2 Ultimately, it is more efficient. Controlling the amperage used in the anodizing step allows control of the zone of inhibition of the treated material. For example, as can be seen from these data, a 2A / dm 2 The inhibition zone ratio is 4A / dm 2 Big.

[0117] Thus, an antimicrobial metal product is obtained by the process claimed herein. The treated metal product will have an anodized surface with sealed pores over the entire surface, the depth of the pores being between 5 and 150 μm, preferably 50-100 μm. It has been found that the smaller the pores, the longer the time it takes for the antimicrobial solution to diffuse out of the sealed pores. According to the results presented herein, there is a clear correlation between the size and distribution of the pores on the surface and the antimicrobial properties of the final product.

[0118] Advantageously, anodization of the pores and a simple immersion-sealing treatment, optionally followed by an additional immersion in a microbiological solution, firstly shows excellent results with a higher microbiological activity, which lasts longer than previous methods.

[0119] The newly treated product will be useful in manufacturing a variety of equipment or furniture for housing, medical facilities and public transportation. For users of public transportation, it will be safer and less stressful to use fixing rods and support elements made of the antimicrobial product obtained by the present method. The antimicrobial metal product made by the present method can be used to prepare kitchenware, kitchen countertops, hospital countertops, furniture, electrical appliances, office equipment, door handles, door push panels, medical equipment, wall panels, flooring, machine keyboards and handrails.

[0120] Example 5: Steel Treatment

[0121] Four 2” x 6” pieces of stainless steel 304 were hard anodized at 55-60V in ethylene glycol solution containing 10% perchloric acid at 5°C and then post-anodized. Each piece was washed in industrial aluminum soap solution at 53°C for 8 minutes and rinsed in water. Stainless steel without antimicrobial treatment was used as a negative control that should not have any antimicrobial activity. Antimicrobial treatment was performed at room temperature for 5 or 15 minutes. Prior to antimicrobial testing, the sheets were rinsed and dried.

[0122] At room temperature, 2.45 x 10 7 The bacterial inoculum was incubated for 5 minutes. The bacteria were then harvested and plated overnight at 37°C. The count of viable microorganisms was achieved. The mean value of colony forming units (in mL) for each sample, the log mean value, and the antimicrobial activity for each test were calculated using the formula provided in Section 8.1 of the ISO 22196 method.

[0123] Table 5: Experiment #5 results.

[0124]

[0125] In Table 5, the results show the mean counts of negative control and treated samples after 5 days. The negative control never showed any antimicrobial properties.

[0126] By comparing untreated and treated samples with the same contact time, the treatment was able to achieve a 4 log10 reduction in E. coli at a 5 minute contact time.

[0127] According to a preferred embodiment, the antimicrobial steel sheet can be prepared by anodizing the steel sheet before contacting it with the antimicrobial solution. It has been demonstrated that the antimicrobial properties of the anodized steel sheet remain active over time, although as shown in this example, the step of sealing the pores may be optional.

[0128] Example 6: Reactivation Method

[0129] Two door handles made of the antimicrobial metal product obtained by the method were installed in the applicant's laboratory. The results are listed in Table 6 below.

[0130] Table 6: Experiment #6 results.

[0131]

[0132]

[0133] The handles were first tested on April 29, 2020, after approximately 10 months of use. Table 6 above shows low or almost non-existent bacterial contamination. On May 1, 2020, the handles were reactivated using an A3S solution during the handle cleaning process. A 2% quaternary ammonium chloride solution was sprayed on the surface and allowed to dry. The next five controls show the efficiency of the reactivation method.

[0134] While illustrative and presently preferred embodiments of the invention have been described above in detail, it should be understood that the inventive concept may be embodied and employed in other different forms and that the appended claims are intended to be interpreted to include such variations unless limited by prior art.

Claims

1. A method for preparing a metal product having antibacterial properties, the method comprising: Anodizing a product having at least one metallic surface using a controlled current density, the controlled anodizing allowing the formation of pores having a controlled spatial density and depth in the metallic surface to be treated, or Alternatively providing a pre-anodized product having at least one anodized metal surface with pores; rinsing the anodized metal product with a first acidic solution, wherein the first acidic solution is 0.1 to 5% sulfuric acid; rinsing the anodized metal product again with a second acidic solution or water, wherein the second temperature of the second acidic solution or water is lower than the first temperature of the anodized metal product so as to form cracks or fissures on the at least one metal surface; contacting the at least one anodized metal surface with a first antimicrobial solution for a first period of time; and sealing the hole; The method is free of steps associated with electrodepositing metal onto the at least one anodized surface.

2. The method of claim 1 , further comprising, after sealing the hole: The at least one metal surface of the metal product is contacted with the first antimicrobial solution again.

3. The method according to claim 1, wherein: The first acidic solution is 0.15 to 5% sulfuric acid.

4. The method according to any one of claims 1 to 3, wherein: Anodizing includes: Use 1A / dm 2 Up to 5A / dm 2 Anodize each of the metal surfaces with an electric current.

5. The method according to claim 4, wherein: The current is 2 to 4A / dm 2 .

6. The method according to any one of claims 1 to 3, wherein: The first antimicrobial solution comprises a first concentration of at least one of an antibiotic, an antimicrobial peptide, an enzyme, or a cationic compound.

7. The method according to claim 6, wherein: The first antimicrobial solution comprises at least one cationic compound.

8. The method according to claim 7, wherein: The cationic compound includes at least one quaternary ammonium compound.

9. The method according to claim 7, wherein: The cationic compound comprises at least one metal salt.

10. The method according to claim 9, wherein: The at least one metal salt is Ni(NO3)2, AgNO3, Ti(NO3)3, Zn(NO3)2, Cu(NO3)2, NiCl2, AgCl, ZnCl2, CuCl2, Ni3(PO4)2, Ag3PO4, Zn3(PO4)2, Cu3(PO4)2 or a combination thereof.

11. The method according to claim 10, wherein: The at least one metal salt is AgNO3, whereby in use, AgNO3 forms AgCl in situ with the at least one quaternary ammonium compound.

12. The method according to any one of claims 1 to 3, wherein: Contacting the at least one anodized metal surface with the first antimicrobial solution comprises: The at least one anodized metal surface is immersed in the first antimicrobial solution for a first period of time.

13. The method according to claim 12, wherein: The first time period is from 15 seconds to 60 minutes.

14. The method according to claim 12, wherein: The first time period is from 5 minutes to 45 minutes.

15. The method according to claim 12, wherein: The first time period is 15 minutes to 30 minutes.

16. The method according to any one of claims 1 to 3, wherein: Sealing the hole includes heating the at least one metal surface in a water bath or a nickel acetate solution bath for a second period of time, the bath having a temperature of 70-90°C.

17. The method according to claim 16, wherein: The second time period is from 1 minute to 15 minutes.

18. The method according to any one of claims 1 to 3, wherein: The metal product comprises steel, aluminum, titanium, zinc, magnesium, niobium, tantalum or anodizable alloys thereof.

19. The method according to claim 18, wherein: The metal product comprises aluminum or an anodizable alloy thereof.

20. The method of claim 18, wherein the metal product comprises steel or an anodizable alloy thereof.

21. An antimicrobial metal product obtained by the method according to any one of claims 1 to 20, wherein: The metal product comprises at least one anodized metal surface treated to have sealed pores having a depth of 5 to 150 μm over the entire surface; wherein, in addition to the pores formed during the anodizing step, the at least one anodized surface treated comprises a plurality of cracks or fissures formed during the rinsing step, and The antimicrobial metal product is free of electrodeposited metal on the anodized surface.

22. The antimicrobial metal product according to claim 21, wherein: The at least one metal surface comprises steel, aluminum, titanium, zinc, magnesium, niobium, tantalum or anodizable alloys thereof.

23. The antimicrobial metal product according to claim 21 or 22, wherein: The metal product comprises aluminum or an anodizable alloy thereof.

24. The antimicrobial metal product according to claim 21 or 22, wherein: The metal product comprises steel or an anodizable alloy thereof.

25. The antimicrobial metal product of claim 21 or 22 is used to manufacture articles for use in homes, medical facilities, public areas or vehicles.

26. The antimicrobial metal product of claim 21 or 22 is used to prepare kitchen countertops, hospital countertops, fixtures, furniture, appliances, support rods or handles in public transportation, office equipment, door handles, door push panels, medical equipment, wall panels, flooring, machine keyboards or handrails.

27. A method for reactivating the antimicrobial properties of an antimicrobial metal product obtained by the method of any one of claims 1 to 20 or claimed in any one of claims 21 to 24, the method comprising: contacting the at least one metal surface of the antimicrobial metal product with a second antimicrobial solution; wherein the second antimicrobial solution comprises a second concentration of at least one of the following: an antibiotic, an antimicrobial peptide, an enzyme, or a cationic compound; and wherein the second concentration of the second antibacterial solution is lower than the first concentration of the first antibacterial solution used to prepare the antibacterial metal compound; The first antimicrobial solution contains at least one of the following in a first concentration: an antibiotic, an antimicrobial peptide, an enzyme or a cationic compound.

28. The method according to claim 27, wherein: The step of contacting at least one surface of the antimicrobial metal product with a second antimicrobial solution comprises: The second antimicrobial solution is sprayed on the at least one surface, and the spread second antimicrobial solution is allowed to remain on the at least one surface for a third period of time.

29. The method of claim 28, comprising, after the third period of time: Excess portions of the second antimicrobial solution are removed from the at least one surface.

30. The method according to claim 28 or 29, wherein: The third time period is from 5 seconds to 30 minutes.

31. The method of claim 27, wherein: The step of contacting at least one surface of the antimicrobial metal product with a second antimicrobial solution comprises: The second antimicrobial solution is applied to the at least one surface using a cloth pre-soaked in the second antimicrobial solution.

32. The method according to claim 31, wherein: Applying the second antimicrobial solution to the at least one surface using a cloth pre-soaked in the solution comprises: Wipe the at least one surface at least once with the moistened cloth.

33. The method according to claim 32, wherein: Wipe the at least one surface several times with the dampened cloth.

34. The method of claim 27, wherein: The step of contacting at least one surface of the antimicrobial metal product with a second antimicrobial solution comprises: soaking the antimicrobial metal product in the second antimicrobial solution for a fourth period of time; and The antimicrobial metal product is removed from the second antimicrobial solution.

35. The method of claim 34, further comprising removing excess portions of the second antimicrobial solution from the at least one surface.

36. The method of claim 27, wherein: The second antimicrobial solution comprises at least one cationic compound.

37. The method of claim 36, wherein: The cationic compound includes at least one quaternary ammonium compound.

38. The method of claim 36, wherein: The cationic compound comprises at least one metal salt.

39. The method of claim 38, wherein: The at least one metal salt is Ni(NO3)2, AgNO3, Ti(NO3)3, Zn(NO3)2, Cu(NO3)2, NiCl2, AgCl, ZnCl2, CuCl2, Ni3(PO4)2, Ag3PO4, Zn3(PO4)2, Cu3(PO4)2 or a combination thereof.

40. The method of claim 27, wherein: The second concentration is ten times lower than the first concentration.