Forming method of additional aluminum ribs for prestressed composite reinforcement based on Fe-SMA sleeve

By installing Fe-SMA casing on the composite ribs and using its shape memory effect, the problem of insufficient anchoring performance of composite ribs is solved, and the anchoring performance improvement and interface shear strength control is achieved, which simplifies operation and is suitable for pre-pre-pre- Stressed components.

CN114925467BActive Publication Date: 2024-11-08SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210482765.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-05
Publication Date
2024-11-08
Estimated Expiration
2042-05-05

AI Technical Summary

Technical Problem

The anchoring performance of existing composite ribs in concrete is weak, and the lateral shear strength and compressive strength are low. The existing molding process has high manual and mechanical requirements, which can easily lead to microcracks inside the composite ribs and the positioning of prestressed ribs. It is easy to damage when extruded with additional aluminum ribs.

Method used

The prestressed composite ribs with an aluminum rib molding method based on Fe-SMA sleeve is adopted. By placing an aluminum alloy tube and a pre-deformed Fe-SMA sleeve on the composite ribs, the shape memory effect of the Fe-SMA sleeve is used. The aluminum alloy tube is shrinked and extruded during heating to form additional ribs to improve anchoring performance.

Benefits of technology

The anchoring performance of composite ribs is improved, the interface shear strength and anchoring force of additional aluminum ribs are controlled, the on-site operation is simplified, and it is suitable for prestressed components of pre-tensioning method, which reduces the extrusion space requirement of aluminum alloy pipes, and Improves construction controllability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114925467B_ABST
    Figure CN114925467B_ABST
Patent Text Reader

Abstract

The method for forming additional aluminum ribs of prestressed composite reinforcement based on Fe‑SMA sleeves comprises the following steps: pre-deformation of the Fe‑SMA long tube, wherein the inner diameter of the Fe‑SMA long tube is smaller than the outer diameter of the aluminum alloy tube before pre-deformation, and the inner diameter of the Fe‑SMA long tube is larger than the outer diameter of the aluminum alloy tube after pre-deformation. The aluminum alloy tube and the Fe‑SMA sleeve are sleeved on the composite reinforcement, and after the composite reinforcement is tensioned, the aluminum alloy tube and the Fe‑SMA sleeve are temporarily fixed to the designed position on the composite reinforcement. The Fe‑SMA sleeve is heated and the temperature is monitored. After the Fe‑SMA sleeve undergoes a reverse martensitic phase transformation, it shrinks, and radial synchronous extrusion is formed on the aluminum alloy tube, so that the aluminum alloy tube is attached to the reinforcement surface to form additional ribs, and there is a stable normal internal stress at the interface between the additional ribs and the composite reinforcement. The present invention stimulates the "shape memory" effect of the Fe‑SMA sleeve, shrinks and extrudes the aluminum alloy tube to form additional ribs to improve the anchoring performance of the composite reinforcement, and realizes controllable reinforcement slippage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of improving the anchoring performance of prestressed composite reinforcement, and in particular to a method for forming additional aluminum ribs of prestressed composite reinforcement based on a Fe-SMA sleeve. Background Art

[0002] Fiber reinforced polymer (FRP) is a polymer formed by winding, molding or pultrusion of reinforcing fiber materials and matrix materials. It has excellent properties such as light weight, high strength, non-magnetic, corrosion resistance, and fatigue resistance. The reinforcement made of this material, referred to as composite reinforcement, can be used in corrosive environments to give full play to its material performance advantages.

[0003] Although composite reinforcement has the above advantages, its anchoring performance in concrete is weak, and its transverse shear strength and compressive strength are low. When the method of radially extruding aluminum alloy tubes to form additional ribs for composite reinforcement is adopted to improve its anchoring performance, the slippage of composite reinforcement is controllable, the anchoring efficiency is high, and the damage to the reinforcement is small. However, the current forming process has the following shortcomings:

[0004] 1. The extrusion of aluminum alloy tubes has high requirements on labor and machinery. For example, when using electric hydraulic pliers, the aluminum alloy tubes need to be extruded in sections. During each section, the tubes are gradually extruded by rotating the angle, and the tubes are extruded from one end to the other several times in a cycle to make them evenly extruded.

[0005] 2. The extrusion pressure tends to flatten one side of the composite reinforcement, which is very likely to cause microcracks inside the composite reinforcement and reduce its mechanical properties.

[0006] 3. When prestressing is required for the composite reinforcement, it is difficult to extrude the prestressed reinforcement after positioning due to construction conditions. It is often necessary to first extrude additional aluminum ribs on the composite reinforcement and then tension the composite reinforcement. However, when tensioning the composite reinforcement, the interface between the composite reinforcement and the additional aluminum rib will produce relative slippage, causing damage to the composite reinforcement and the interface between the composite reinforcement and the additional aluminum rib. Summary of the invention

[0007] The technical problem to be solved by the present invention is to address the deficiencies of the above-mentioned prior art and to provide a method for forming additional aluminum ribs for prestressed composite reinforcement based on Fe-SMA sleeves. The method comprises: sleeveing ​​an aluminum alloy tube and a pre-deformed Fe-SMA sleeve on the composite reinforcement, heating the Fe-SMA sleeve to stimulate its "shape memory" effect, and causing the Fe-SMA sleeve to shrink to form radial synchronous extrusion of the aluminum alloy tube. The extruded aluminum alloy tube is attached to the surface of the composite reinforcement to form additional ribs to improve the reinforcement anchoring performance.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0009] A method for forming an additional aluminum rib of a prestressed composite reinforcement based on a Fe-SMA sleeve comprises the following steps.

[0010] Step 1, pre-deformation construction of Fe-SMA long tube: pre-deform the Fe-SMA long tube whose inner diameter is smaller than the outer diameter of the aluminum alloy tube, so that the inner diameter of the Fe-SMA long tube after construction is larger than the outer diameter of the aluminum alloy tube; and cut the pre-deformed Fe-SMA long tube into N Fe-SMA sleeves.

[0011] Step 2: Installing aluminum alloy tubes and Fe-SMA sleeves: Install several Fe-SMA sleeves on the outer circumferences of M aluminum alloy tubes according to the additional rib forming requirements, and then install the M aluminum alloy tubes with Fe-SMA sleeves on Z composite bars in sequence, where N≥M≥Z≥1.

[0012] Step 3: tensioning the composite reinforcement to form a prestressed composite reinforcement with a set prestress.

[0013] Step 4: Axial positioning of the aluminum alloy tube and the Fe-SMA sleeve: Move the aluminum alloy tube to the designed position of the prestressed composite reinforcement, adjust the relative position of the Fe-SMA sleeve on the aluminum alloy tube, and position and restrict the axial positions of the aluminum alloy tube and the Fe-SMA sleeve.

[0014] Step 5, heating the Fe-SMA sleeve: the Fe-SMA sleeve is heated and its temperature is monitored. The Fe-SMA sleeve shrinks after undergoing reverse martensitic transformation, so that its inner diameter is smaller than the initial outer diameter of the aluminum alloy tube.

[0015] Step 6: Additional aluminum rib forming: During the shrinkage process of the Fe-SMA sleeve due to the reverse martensitic transformation, the aluminum alloy tube is extruded so that the aluminum alloy tube is attached to the surface of the prestressed composite reinforcement to form additional aluminum ribs.

[0016] By controlling the heating temperature T of the Fe-SMA sleeve, the recovery stress of the pre-deformed Fe-SMA sleeve can be changed, thereby achieving the control of the shear strength of the composite reinforcement-additional aluminum rib interface and the anchoring force of the additional aluminum rib composite reinforcement in step 6.

[0017] In step 5, the method for determining the heating temperature T of the Fe-SMA sleeve includes the following steps.

[0018] Step 5A1. Establish an aluminum alloy tube extrusion model: for a Fe-SMA casing with a set inner diameter and a set wall thickness, an aluminum alloy tube extrusion model is established by using an experimental or simulation method; the aluminum alloy tube extrusion model includes a prestressed composite reinforcement, an aluminum alloy tube, a Fe-SMA casing and a Fe-SMA casing temperature monitoring device; the Fe-SMA casing and the aluminum alloy tube are coaxially sleeved on the outer periphery of the composite reinforcement in sequence; the Fe-SMA casing temperature monitoring device is used to monitor the heating temperature of the Fe-SMA casing.

[0019] Step 5A2, establishing a T-τ curve: T is the heating temperature of the Fe-SMA sleeve, and τ is the shear strength of the composite reinforcement-additional aluminum rib interface; the T-τ curve establishing method includes the following steps.

[0020] Step 5A21, prestressed additional aluminum rib composite reinforcement tensile strength test, includes the following steps.

[0021] Step 5A211, tensioning the composite reinforcement to a set prestress: an aluminum alloy tube with a Fe-SMA sleeve is sleeved on the composite reinforcement, and both ends of the composite reinforcement are anchored with glue using seamless steel pipes, one of the anchored seamless steel pipes is clamped on the lower clamp of the universal testing machine, and the other anchored seamless steel pipe is clamped on the upper clamp of the universal testing machine, and the composite reinforcement is lifted and tensioned to the set prestress through the upper clamp.

[0022] Step 5A212, forming additional aluminum ribs: fix the aluminum alloy tube to the designed position, and form the Fe-SMA sleeve in the austenite phase transition temperature range A s ~A f The interior is heated from low temperature to high temperature according to the set temperature interval to the set temperature; wherein, A s is the austenite transformation starting temperature, A f It is the end temperature of austenite phase transformation; after heating, the aluminum alloy tube is attached to the surface of the prestressed composite reinforcement to form additional aluminum ribs.

[0023] Step 5A213, perform a tensile strength test on the prestressed composite reinforcement with additional aluminum ribs, and record the tensile strength F1 when the prestressed composite reinforcement is destroyed.

[0024] Step 5A214, calculate the strength damage rate, and record the specification A and heating temperature T1 of the Fe-SMA sleeve in the prestressed composite reinforcement whose strength damage rate is within the set range; wherein the calculation formula of the strength damage rate is:

[0025]

[0026] Where F0 is the tensile strength of the composite reinforcement without additional aluminum ribs.

[0027] Step 5A22, prestressed composite reinforcement-additional aluminum rib interface shear performance test, specifically includes the following steps:

[0028] Step 5A221, specimen clamping: a Fe-SMA sleeve of specification A is sleeved on the outer periphery of the aluminum alloy tube, and an aluminum alloy tube with a Fe-SMA sleeve of specification A, a steel backing plate, a force sensor, a through-type jack and a steel frame are sequentially sleeved on the composite reinforcement.

[0029] Both ends of the composite reinforcement are anchored with glue using seamless steel pipes, the seamless steel pipe adjacent to the steel frame is clamped on the lower clamp of the universal testing machine, and the other seamless steel pipe is clamped on the upper clamp of the universal testing machine.

[0030] Step 5A222, applying prestress to the composite reinforcement: lifting the upper clamp to tension the composite reinforcement to a set prestress.

[0031] Step 5A223, forming additional aluminum ribs: fix the aluminum alloy tube to the designed position, heat the Fe-SMA sleeve with the outer periphery specification of the aluminum alloy tube A to the temperature T1; the aluminum alloy tube is attached to the surface of the prestressed composite reinforcement to form additional aluminum ribs.

[0032] Step 5A224, adjust the through-type jack so that the lower surface of the additional aluminum rib fits the steel pad.

[0033] Step 5A225: Install a displacement sensor on the additional aluminum rib to measure the relative slip between the additional aluminum rib and the composite reinforcement.

[0034] Step 5A226, lift with a through-type jack to achieve the interface shear test between the composite reinforcement and the additional aluminum rib; during the lifting process, stop lifting when the relative slip between the composite reinforcement and the additional aluminum rib is not less than 25 mm: at this time, record the lifting loading strength F of the through-type jack max , and the shear strength is calculated using the following formula:

[0035]

[0036] Where: d represents the diameter of the composite reinforcement, l d It is the actual contact length between the aluminum alloy tube and the composite reinforcement.

[0037] Step 5A23, change the set temperature when heating the Fe-SMA sleeve in step 5A21, repeat 5A21 to 5A22, and draw a T-τ curve.

[0038] Step 5A24, change the set inner diameter or set wall thickness of the Fe-SMA sleeve in step 5A1, repeat steps 5A1 and 5A2, and draw T-τ curves for Fe-SMA sleeves with different set inner diameters or different set wall thicknesses.

[0039] Step 5A3, determine the heating temperature T of the Fe-SMA sleeve: According to the required anchoring strength of the composite reinforcement, the specifications of the Fe-SMA sleeve and the T-τ curve established in step 5A24, determine the heating temperature T of the Fe-SMA sleeve, so as to achieve the anchoring force F of the composite reinforcement. max controllable.

[0040] In step 5, a non-contact temperature meter is used to monitor the heating temperature of the Fe-SMA sleeve.

[0041] In step 5, the Fe-SMA sleeve is heated by an electric excitation device or a ceramic heating ring. The specific heating method is:

[0042] B1. Heating with ceramic heating ring: When the resistivity of the Fe-SMA sleeve is less than the set resistivity threshold, the Fe-SMA sleeve is indirectly heated by a ceramic heating ring.

[0043] B2. Heating by electric excitation device, specifically including the following two types:

[0044] (1) Series heating: When the maximum difference in heating rates of N Fe-SMA sleeves is less than the set heating rate threshold, the N Fe-SMA sleeves are connected in series with the electric excitation device and heated by the electric excitation device.

[0045] (2) Parallel heating: When the maximum difference of the heating rates of N Fe-SMA sleeves is not less than the set heating rate threshold, the N Fe-SMA sleeves are respectively connected in parallel with the electric excitation device and heated by the electric excitation device.

[0046] In step 1, the method of pre-deforming the Fe-SMA long tube is: using stress to induce martensitic phase transformation in the Fe-SMA long tube, at the martensitic phase transformation starting temperature M s and the martensitic transformation end temperature M f The Fe-SMA long tube is uniformly expanded in the radial direction to be larger than the outer diameter of the aluminum alloy tube, and the Fe-SMA long tube remains unchanged in the axial length direction.

[0047] The Fe-SMA long tube is pre-deformed by using a diameter expanding machine.

[0048] In step 1, the length of each Fe-SMA sleeve cut from the Fe-SMA long tube is consistent with the length of a single extruded section of the aluminum alloy tube; in step 2, after the Fe-SMA sleeve is installed on the outer periphery of the corresponding aluminum alloy tube, the interval between adjacent Fe-SMA sleeves is 1-2 mm, and the two ends of the outermost Fe-SMA sleeve are 1-2 mm shorter than the corresponding ends of the aluminum alloy tube.

[0049] The present invention has the following beneficial effects:

[0050] Compared with the prior art, the present invention has the following characteristics and advantages:

[0051] 1. The Fe-SMA sleeve will undergo reverse martensitic transformation at high temperature, which makes it tend to recover to the shape before pre-deformation, that is, the inner diameter larger than the outer diameter of the aluminum alloy tube after expansion is restored to the smaller inner diameter before expansion, thereby uniformly extruding the aluminum alloy tube radially.

[0052] 2. By controlling the heating temperature T of the Fe-SMA sleeve, the recovery stress of the pre-deformed Fe-SMA sleeve can be changed, thereby achieving control of the anchoring force of the additional aluminum rib composite reinforcement and the shear strength of the composite reinforcement-additional aluminum rib interface.

[0053] 3. Carry out experiments and numerical simulations to establish the corresponding relationship between the shrinkage extrusion pressure of the Fe-SMA sleeve, the extrusion degree of the aluminum alloy tube and the heating temperature. The heating temperature of the Fe-SMA sleeve can be used to obtain the anchoring performance of the composite reinforcement after the pre-deformed Fe-SMA sleeve applies extrusion pressure to the aluminum alloy tube, and the construction is controllable.

[0054] 4. Fe-SMA casing austenite phase transformation end temperature A f It shows an upward trend with the increase of pre-deformation. During the service life of the structure, it can be heated and shrunk as needed to enhance the anchorage of the reinforcement.

[0055] 5. The slippage of the composite reinforcement with additional aluminum ribs is controllable, and the prestress loss of the composite reinforcement after tensioning is small.

[0056] 6. The on-site operation is simple and suitable for improving the anchoring performance of composite reinforcement in prestressed components.

[0057] 7. Aluminum alloy extrusion requires little space and is suitable for prestressed composite reinforcement anchors.

[0058] 8. The non-contact thermometer directly measures the temperature of the Fe-SMA sleeve to ensure the accuracy of the anchoring force generated by the heating and shrinkage of the Fe-SMA sleeve; and the detection range is wide, which is convenient for installation and transfer. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 This is an axonometric view of the composite reinforcement sleeved with an aluminum alloy tube and a Fe-SMA sleeve in the present invention.

[0060] Figure 2 This is an axonometric view of the composite reinforcement after the additional aluminum rib is formed in the present invention.

[0061] Figure 3 It is a front view of the composite reinforcement strength loss test specimen in the present invention.

[0062] Figure 4 It is a front view of the shear performance test of the composite reinforcement-additional aluminum rib interface in the present invention.

[0063] Figure 5 It is a schematic diagram of the Fe-SMA sleeves in series powered excitation in the present invention.

[0064] Figure 6 Schematic diagram of the construction of prefabricated components using the prestressing method in the present invention: (a) is a schematic diagram of the installation of Fe-SMA sleeves and aluminum alloy tubes; (b) is a schematic diagram of tensioning composite reinforcement; (c) is a schematic diagram of forming additional aluminum ribs; (d) is a schematic diagram of pouring concrete; (e) is a schematic diagram of tensioning prestressed reinforcement.

[0065] The accompanying drawings are marked as follows: 1. composite reinforcement; 2. aluminum alloy tube; 3. additional aluminum rib; 4. Fe-SMA casing; 5. seamless steel tube; 6. lower chuck; 7. upper chuck; 8. steel pad; 9. force sensor; 10. through-type jack; 11. steel frame; 12. displacement sensor; 13. pointer top plate; 14. non-contact thermometer; 15. wire; 16. electric excitation device. DETAILED DESCRIPTION

[0066] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific preferred embodiments.

[0067] In the description of the present invention, it should be understood that the terms "left side", "right side", "upper part", "lower part" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as limiting the present invention. The specific dimensions used in this embodiment are only for illustrating the technical solution and do not limit the scope of protection of the present invention.

[0068] like Figure 6 As shown, the method for forming prestressed composite reinforcement with additional aluminum ribs based on Fe-SMA sleeve includes the following steps.

[0069] Step 1: Fe-SMA long tube pre-deformation construction

[0070] The Fe-SMA long tube with an inner diameter smaller than the outer diameter of the aluminum alloy tube is pre-deformed, and the inner diameter of the Fe-SMA long tube after the construction is larger than the outer diameter of the aluminum alloy tube; and the pre-deformed Fe-SMA long tube is cut into N Fe-SMA sleeves 4.

[0071] Shape memory alloys (SMA) are materials composed of two or more metal elements that have shape memory effect (SME) through thermoelasticity and martensitic phase transformation and its inversion. Fe-SMA refers to an iron-based alloy that exhibits shape memory effect when heated and reversed to austenite with fcc structure and martensite with bct or hcp crystal structure. When on-site construction conditions are insufficient, Fe-SMA components can be used to achieve specific functions by utilizing its "shape memory" effect.

[0072] The above-mentioned Fe-SMA long tube pre-deformation construction method is: using stress to induce martensitic phase transformation in the Fe-SMA long tube, at the martensitic phase transformation starting temperature M s and the martensitic transformation end temperature M f The Fe-SMA long tube is uniformly expanded in the radial direction to be larger than the outer diameter of the aluminum alloy tube, and the Fe-SMA long tube remains unchanged in the axial length direction.

[0073] In the present invention, a diameter expander is preferably used to pre-deform the Fe-SMA long tube, so that the Fe-SMA long tube undergoes radial deformation, while axial deformation should be avoided.

[0074] The number of extrusion sections is determined according to the length of the aluminum alloy tube, and the length of a single extrusion section is consistent with the diameter of the composite bar. An aluminum alloy tube includes no less than one extrusion section, and the distance between adjacent extrusion sections is 1-2 mm. The length of each Fe-SMA sleeve cut from the Fe-SMA long tube is preferably consistent with the length of a single extrusion section of the aluminum alloy tube. The pre-deformed Fe-SMA long tube is cut according to the length of a single extrusion section of the aluminum alloy tube. The temperature should be controlled during cutting to prevent the Fe-SMA sleeve from shrinking and deforming.

[0075] Step 2: Installing aluminum alloy tubes and Fe-SMA sleeves: Install several pre-deformed Fe-SMA sleeves on the outer circumferences of the M aluminum alloy tubes according to the additional rib forming requirements. After installation, the two ends of the outermost Fe-SMA sleeves are preferably 1-2 mm shorter than the corresponding ends of the aluminum alloy tubes. Figure 1 As shown, M aluminum alloy tubes 2 sleeved with Fe-SMA sleeves are sequentially sleeved on Z composite bars 1, wherein N≥M≥Z≥1, preferably N=2M / 4M / 6M.

[0076] Commonly used reinforcing fiber materials include carbon fiber, glass fiber, aramid fiber and basalt fiber, among which carbon fiber, as an inert inorganic fiber, has better mechanical performance index. The composite reinforcement in the present invention is preferably carbon fiber reinforced polymer (CFRP) reinforcement, referred to as CFRP reinforcement.

[0077] Step 3: tensioning the composite reinforcement to form a prestressed composite reinforcement with a set prestress.

[0078] Step 4: Axial positioning of the aluminum alloy tube and the Fe-SMA sleeve: Move the aluminum alloy tube to the designed position of the prestressed composite reinforcement, adjust the relative position of the Fe-SMA sleeve on the aluminum alloy tube, and position and restrict the axial positions of the aluminum alloy tube and the Fe-SMA sleeve.

[0079] Step 5, heating the Fe-SMA sleeve: the Fe-SMA sleeve is heated and its temperature is monitored. The Fe-SMA sleeve shrinks after undergoing reverse martensitic transformation, so that its inner diameter is smaller than the initial outer diameter of the aluminum alloy tube.

[0080] The method for determining the heating temperature T of the Fe-SMA sleeve comprises the following steps.

[0081] Step 5A1. Establish an aluminum alloy tube extrusion model: for a Fe-SMA casing with a set inner diameter and a set wall thickness, an aluminum alloy tube extrusion model is established by using an experimental or simulation method; the aluminum alloy tube extrusion model includes a prestressed composite reinforcement, an aluminum alloy tube, a Fe-SMA casing and a Fe-SMA casing temperature monitoring device; the Fe-SMA casing and the aluminum alloy tube are coaxially sleeved on the outer periphery of the composite reinforcement in sequence; the Fe-SMA casing temperature monitoring device is used to monitor the heating temperature of the Fe-SMA casing.

[0082] Step 5A2, establish a T-τ curve: T is the heating temperature of the Fe-SMA sleeve, and τ is the shear strength of the composite reinforcement-additional aluminum rib interface. The T-τ curve establishment method includes the following steps.

[0083] Step 5A21, prestressed additional aluminum rib composite reinforcement tensile strength test, includes the following steps.

[0084] Step 5A211: Tension the composite reinforcement to the set prestress

[0085] An aluminum alloy tube with a Fe-SMA sleeve is set on the composite reinforcement, and seamless steel pipes are used at both ends of the composite reinforcement. Figure 3 In the glue-injected anchoring shown, one seamless steel pipe 5 is clamped on the lower clamp 6 of the universal testing machine, and the other seamless steel pipe is clamped on the upper clamp 7, and the composite reinforcement is lifted and tensioned by the upper clamp to a set prestress.

[0086] Step 5A212, forming additional aluminum ribs: fix the Fe-SMA sleeve and the aluminum alloy tube to the designed position, and form the Fe-SMA sleeve in the austenite phase transition temperature range A. s ~A f The interior is heated from low temperature to high temperature according to the set temperature interval to the set temperature; wherein, As is the austenite transformation starting temperature, A f It is the end temperature of austenite phase transformation; after heating, the aluminum alloy tube is attached to the surface of the prestressed composite reinforcement to form additional aluminum ribs.

[0087] Step 5A213, perform a tensile strength test on the prestressed composite reinforcement with additional aluminum ribs, and record the tensile strength F1 when the prestressed composite reinforcement is destroyed.

[0088] Step 5A214, calculate the strength damage rate, and record the specification A and heating temperature T1 of the Fe-SMA sleeve in the prestressed composite reinforcement whose strength damage rate is within the set range; wherein the calculation formula of the strength damage rate is:

[0089]

[0090] Where F0 is the tensile strength of the composite reinforcement without additional aluminum ribs.

[0091] Step 5A22, prestressed composite reinforcement-additional aluminum rib interface shear performance test, specifically includes the following steps.

[0092] Step 5A221, specimen clamping: Figure 4 As shown, a Fe-SMA sleeve with specification A is sleeved on the outer periphery of the aluminum alloy tube, and an aluminum alloy tube with a Fe-SMA sleeve with specification A, a steel pad 8, a force sensor 9, a through-type jack 10 and a steel frame 11 are sleeved on the composite reinforcement in sequence. Among them, the steel pad is preferably a U-shaped plate, and after being installed on the composite reinforcement, a filling block is installed so that the center of the steel pad is a hole that can only allow the composite reinforcement to pass through.

[0093] Both ends of the composite reinforcement are anchored with glue using seamless steel pipes, the seamless steel pipe adjacent to the steel frame is clamped on the lower clamp of the universal testing machine, and the other seamless steel pipe is clamped on the upper clamp of the universal testing machine.

[0094] Step 5A222, applying prestress to the composite reinforcement: pull up the upper clamp to tension the composite reinforcement to a set prestress.

[0095] Step 5A223, forming additional aluminum ribs: fix the aluminum alloy tube to the designed position, heat the Fe-SMA sleeve with the outer periphery specification of the aluminum alloy tube A to the temperature T1; the aluminum alloy tube is attached to the surface of the prestressed composite reinforcement to form additional aluminum ribs.

[0096] Step 5A224, adjust the through-type jack so that the lower surface of the additional aluminum rib fits the steel pad.

[0097] Step 5A225, install a displacement sensor 12 on the additional aluminum rib to measure the relative slip between the additional aluminum rib and the composite reinforcement. The preferred installation method of the displacement sensor is: install the displacement sensor on the composite reinforcement 30 mm above the additional aluminum rib, the shear force at the composite reinforcement-additional aluminum rib interface is the load size, and the load is directly measured by the force sensor; install a pointer top plate 13 on the upper surface of the additional aluminum rib, the displacement sensor pointer is connected to the pointer top plate, and the data measured by the displacement sensor is the relative slip between the composite reinforcement and the additional aluminum rib.

[0098] Step 5A226, the through-type jack is preferably lifted at a lifting rate of 0.75 mm / min to achieve shear resistance test of the composite reinforcement-additional aluminum rib interface. During the lifting process, the lifting is stopped when the relative slip between the composite reinforcement and the additional aluminum rib is not less than 25 mm. At this time, the lifting loading strength F of the through-type jack is recorded. max , and the shear strength is calculated using the following formula:

[0099]

[0100] Where: d represents the diameter of the composite reinforcement, l d It is the actual contact length between the aluminum alloy tube and the composite reinforcement.

[0101] Step 5A23, change the set temperature when heating the Fe-SMA sleeve in step 5A21, repeat 5A21 to 5A22, and draw a T-τ curve.

[0102] Step 5A24, change the set inner diameter or set wall thickness of the Fe-SMA sleeve in step 5A1, repeat steps 5A1 and 5A2, and draw T-τ curves for Fe-SMA sleeves with different set inner diameters or different set wall thicknesses.

[0103] Step 5A3, determine the heating temperature T of the Fe-SMA sleeve: According to the required anchoring strength of the composite reinforcement, the specifications of the Fe-SMA sleeve and the T-τ curve established in step 5A24, determine the heating temperature T of the Fe-SMA sleeve, so as to achieve the anchoring force F of the composite reinforcement. max controllable.

[0104] Furthermore, the present invention preferably uses a non-contact temperature measuring instrument 14 to monitor the heating temperature of the Fe-SMA sleeve.

[0105] Furthermore, the present invention preferably uses an electric excitation device or a ceramic heating ring to heat the Fe-SMA sleeve, and the specific heating method is:

[0106] B1. Heating with ceramic heating coil: According to Joule's law, Q = I 2Rt, R = ρL / S (Q is heat, I is current, R is resistance, t is time, ρ is resistivity, L is resistance length, S is the resistance cross-sectional area perpendicular to the current). It can be seen that when the cross-sectional area of ​​the Fe-SMA sleeve is large and the resistivity is small, the excitation current is often large and the heating time is long when the Fe-SMA sleeve is heated to a high temperature by its own resistance. Other heat sources can be used to indirectly heat the Fe-SMA sleeve. Therefore, when the resistivity of the Fe-SMA sleeve is less than the set resistivity threshold, the ceramic heating ring is used to indirectly heat the Fe-SMA sleeve.

[0107] B2. Heating by electric excitation device, specifically including the following two types:

[0108] (1) Series heating: Figure 5 As shown, when the maximum difference in heating rates of the N Fe-SMA sleeves is less than the set heating rate threshold, the N Fe-SMA sleeves are connected in series with the electric excitation device 16 through the wires 15 and heated by the electric excitation device.

[0109] (2) Parallel heating: When the maximum difference of the heating rates of N Fe-SMA sleeves is not less than the set heating rate threshold, the N Fe-SMA sleeves are respectively connected in parallel with the electric excitation device and heated by the electric excitation device.

[0110] Step 6: Additional aluminum rib forming: During the process of the Fe-SMA sleeve undergoing reverse martensitic transformation and shrinkage, the aluminum alloy tube is extruded to fit the aluminum alloy tube on the surface of the prestressed composite reinforcement to form a Figure 2 Additional aluminum ribs 3 are shown.

[0111] By controlling the heating temperature T of the Fe-SMA sleeve, the recovery stress of the pre-deformed Fe-SMA sleeve can be changed, thereby achieving the control of the shear strength τ of the prestressed composite reinforcement-additional aluminum rib interface and the anchoring force F of the additional aluminum rib composite reinforcement in step 6.

[0112] The present invention stimulates the "shape memory" effect of the pre-deformed Fe-SMA sleeve, shrinks and extrudes the aluminum alloy tube to form additional ribs of the composite reinforcement to improve the anchoring performance of the composite reinforcement, and can achieve controllable reinforcement slip. In addition, according to the service conditions of the structure, the Fe-SMA sleeve can be appropriately heated to shrink it to improve the reinforcement anchoring force; when the structure is subjected to excessive load, the composite reinforcement-aluminum rib interface can slip, and the surface of the outer reinforcement can be peeled off to achieve the effect of improving the ductility of the component.

[0113] The preferred embodiments of the present invention are described in detail above; however, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, various equivalent transformations can be made to the technical solutions of the present invention, and these equivalent transformations all belong to the protection scope of the present invention.

Claims

1. A method for forming an additional aluminum rib of a prestressed composite reinforcement based on a Fe-SMA sleeve, characterized in that: The following steps are involved: Step 1, pre-deformation construction of Fe-SMA long tube: pre-deform the Fe-SMA long tube whose inner diameter is smaller than the outer diameter of the aluminum alloy tube, so that the inner diameter of the Fe-SMA long tube after construction is larger than the outer diameter of the aluminum alloy tube; and cut the pre-deformed Fe-SMA long tube into N Fe-SMA sleeves; Step 2, sleeve aluminum alloy tubes and Fe-SMA sleeves: sleeve a plurality of Fe-SMA sleeves on the outer circumferences of M aluminum alloy tubes according to the additional rib forming requirements, and then sleeve the M aluminum alloy tubes sleeved with Fe-SMA sleeves on Z composite bars in sequence, where N≥M≥Z≥1; Step 3, tensioning the composite reinforcement to form a prestressed composite reinforcement with a set prestress; Step 4: Axial positioning of the aluminum alloy tube and the Fe-SMA sleeve: Move the aluminum alloy tube to the designed position of the prestressed composite reinforcement, adjust the relative position of the Fe-SMA sleeve on the aluminum alloy tube, and position and restrict the axial positions of the aluminum alloy tube and the Fe-SMA sleeve; Step 5, heating the Fe-SMA sleeve: heating the Fe-SMA sleeve and monitoring its temperature, the Fe-SMA sleeve shrinks after undergoing reverse martensitic transformation, so that its inner diameter is smaller than the initial outer diameter of the aluminum alloy tube; The method for determining the heating temperature T of the Fe-SMA sleeve comprises the following steps: Step 5A1, establishing an aluminum alloy tube extrusion model: for a Fe-SMA casing with a set inner diameter and a set wall thickness, an aluminum alloy tube extrusion model is established respectively by using an experimental or simulation method; the aluminum alloy tube extrusion model includes a prestressed composite reinforcement, an aluminum alloy tube, a Fe-SMA casing and a Fe-SMA casing temperature monitoring device; the Fe-SMA casing and the aluminum alloy tube are coaxially sleeved on the outer periphery of the composite reinforcement in sequence; the Fe-SMA casing temperature monitoring device is used to monitor the heating temperature of the Fe-SMA casing; Step 5A2, establishing a T-τ curve: T is the heating temperature of the Fe-SMA sleeve, and τ is the shear strength of the composite reinforcement-additional aluminum rib interface; the T-τ curve establishing method includes the following steps: Step 5A21, prestressed additional aluminum rib composite reinforcement tensile strength test, including the following steps: Step 5A211, tensioning the composite reinforcement to a set prestress: an aluminum alloy tube with a Fe-SMA sleeve is sleeved on the composite reinforcement, and both ends of the composite reinforcement are anchored with glue using seamless steel pipes, one of the anchored seamless steel pipes is clamped on the lower clamp of the universal testing machine, and the other anchored seamless steel pipe is clamped on the upper clamp of the universal testing machine, and the composite reinforcement is lifted and tensioned to the set prestress through the upper clamp; Step 5A212, forming additional aluminum ribs: fix the aluminum alloy tube to the designed position, and form the Fe-SMA sleeve in the austenite phase transition temperature range A s ~A f The interior is heated from low temperature to high temperature according to the set temperature interval to the set temperature; wherein, A s is the austenite transformation starting temperature, A f is the end temperature of austenite phase transformation; after heating, the aluminum alloy tube is attached to the surface of the prestressed composite reinforcement to form additional aluminum ribs; Step 5A213, performing a tensile strength test on the prestressed composite reinforcement with additional aluminum ribs, and recording the tensile strength F1 when the prestressed composite reinforcement is destroyed; Step 5A214, calculate the strength damage rate, and record the specification A and heating temperature T1 of the Fe-SMA sleeve in the prestressed composite reinforcement whose strength damage rate is within the set range; wherein the calculation formula of the strength damage rate is: Where F0 is the tensile strength of the composite reinforcement without additional aluminum ribs; Step 5A22, prestressed composite reinforcement-additional aluminum rib interface shear performance test, specifically includes the following steps: Step 5A221, specimen clamping: sleeve an Fe-SMA sleeve of specification A on the outer periphery of the aluminum alloy tube, and sequentially sleeve an aluminum alloy tube with an Fe-SMA sleeve of specification A, a steel backing plate, a force sensor, a through-type jack and a steel frame on the composite reinforcement; The two ends of the composite reinforcement are anchored with glue using seamless steel pipes. The seamless steel pipe adjacent to the steel frame is clamped on the lower clamp of the universal testing machine, and the other seamless steel pipe is clamped on the upper clamp of the universal testing machine. Step 5A222, applying prestress to the composite reinforcement: lifting the upper clamp to tension the composite reinforcement to a set prestress; Step 5A223, forming additional aluminum ribs: fix the aluminum alloy tube to the designed position, heat the Fe-SMA sleeve with the outer periphery specification of the aluminum alloy tube A to the temperature t1; the aluminum alloy tube is attached to the surface of the prestressed composite reinforcement to form additional aluminum ribs; Step 5A224, adjust the through-type jack so that the lower surface of the additional aluminum rib fits the steel pad; Step 5A225, install a displacement sensor on the additional aluminum rib to measure the relative slip between the additional aluminum rib and the composite reinforcement; Step 5A226, lift with a through-type jack to achieve an interface shear test between the composite reinforcement and the additional aluminum rib; stop lifting when the relative slip between the composite reinforcement and the additional aluminum rib is not less than 25 mm; at this time, record the lifting load force F of the through-type jack max , and the shear strength is calculated using the following formula: Where: d represents the diameter of the composite reinforcement, l d is the actual contact length between the aluminum alloy tube and the composite reinforcement; Step 5A23, changing the set temperature when heating the Fe-SMA sleeve in step 55A21, repeating 5A21 to 5A22, and drawing a T-τ curve; Step 5A24, changing the set inner diameter or set wall thickness of the Fe-SMA sleeve in step 5A1, repeating steps 5A1 and 5A2, and drawing T-τ curves of Fe-SMA sleeves with different set inner diameters or different set wall thicknesses; Step 5A3, determine the heating temperature T of the Fe-SMA sleeve: According to the required anchoring strength of the composite reinforcement, the specifications of the Fe-SMA sleeve and the T-τ curve established in step 5A24, determine the heating temperature T of the Fe-SMA sleeve, so as to achieve the anchoring force F of the composite reinforcement. max controllable; Step 6, additional aluminum rib forming: during the martensitic reverse phase transformation shrinkage process of the Fe-SMA sleeve, the aluminum alloy tube is extruded so that the aluminum alloy tube is attached to the surface of the prestressed composite reinforcement to form additional aluminum ribs; by controlling the heating temperature T of the Fe-SMA sleeve, the recovery stress of the pre-deformed Fe-SMA sleeve can be changed, thereby realizing the control of the shear strength of the prestressed composite reinforcement-additional aluminum rib interface and the anchoring force of the additional aluminum rib composite reinforcement in step 6.

2. The method for forming an additional aluminum rib of a prestressed composite reinforcement based on a Fe-SMA sleeve according to claim 1 is characterized in that: In step 5, a non-contact temperature meter is used to monitor the heating temperature of the Fe-SMA sleeve.

3. The method for forming an additional aluminum rib of a prestressed composite reinforcement based on a Fe-SMA sleeve according to claim 1, characterized in that: In step 5, the Fe-SMA sleeve is heated by an electric excitation device or a ceramic heating ring. The specific heating method is: B1. Heating with ceramic heating ring: When the resistivity of the Fe-SMA sleeve is less than the set resistivity threshold, the Fe-SMA sleeve is indirectly heated with a ceramic heating ring; B2. Heating by electric excitation device, specifically including the following two types: (1) Series heating: When the maximum difference in heating rates of N Fe-SMA sleeves is less than the set heating rate threshold, the N Fe-SMA sleeves are connected in series with the electric excitation device and heated by the electric excitation device; (2) Parallel heating: When the maximum difference of the heating rates of N Fe-SMA sleeves is not less than the set heating rate threshold, the N Fe-SMA sleeves are respectively connected in parallel with the electric excitation device and heated by the electric excitation device.

4. The method for forming an additional aluminum rib of a prestressed composite reinforcement based on a Fe-SMA sleeve according to claim 1, characterized in that: In step 1, the method of pre-deforming the Fe-SMA long tube is: using stress to induce martensitic phase transformation in the Fe-SMA long tube, at the martensitic phase transformation starting temperature M s and the martensitic transformation end temperature M f The inner diameter of the Fe-SMA long tube is uniformly expanded in the radial direction to be larger than the outer diameter of the aluminum alloy tube, and the Fe-SMA long tube remains unchanged in the axial length direction.

5. The method for forming an additional aluminum rib of a prestressed composite reinforcement based on a Fe-SMA sleeve according to claim 4 is characterized in that: The Fe-SMA long tube is pre-deformed by using a diameter expanding machine.

6. The method for forming prestressed composite reinforcement with additional aluminum ribs based on Fe-SMA sleeve according to claim 1, characterized in that: In step 1, the length of each Fe-SMA sleeve cut from the Fe-SMA long tube is consistent with the length of a single extruded section of the aluminum alloy tube; in step 2, after the Fe-SMA sleeve is installed on the outer periphery of the corresponding aluminum alloy tube, the interval between adjacent Fe-SMA sleeves is 1-2 mm, and the two ends of the outermost Fe-SMA sleeve are 1-2 mm shorter than the corresponding ends of the aluminum alloy tube.