A thermal radiation suppression laminate structure, preparation method and application thereof
By using a stacked structure consisting of a low infrared emissivity upper layer, a phase change energy storage middle layer, and a thermal radiation reflection lower layer, the shortcomings of existing materials in suppressing thermal radiation on high-temperature target objects for extended periods are overcome, achieving efficient thermal insulation and flexibility, making it suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202210883214.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-07-26
AI Technical Summary
Existing heat radiation suppression materials cannot effectively suppress high-temperature target objects for a long time, and they also have problems such as insufficient heat insulation performance or heavy and poor flexibility.
A stacked structure with a low infrared emissivity upper layer, a phase change energy storage middle layer, and a thermal radiation reflection lower layer is adopted. By depositing a metal coating and a phase change material on an aerogel film and combining it with a patterned aerogel film, a stacked structure with high reflectivity and low infrared emissivity is formed.
It achieves long-term suppression of thermal radiation from high-temperature targets, has high solar reflectivity, low infrared emissivity and high phase transition enthalpy, and good flexibility, and can be applied to fields such as heat insulation, energy storage and countering infrared detection.
Smart Images

Figure CN115257096B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated structure, in particular to a novel thermal radiation inhibiting laminated structure based on an aerogel film and composed of a low infrared emissivity upper layer, a phase change energy storage middle layer and a thermal radiation reflecting lower layer, a preparation method and application thereof, and belongs to the technical field of new nano materials. Background Art
[0002] Controlling the thermal radiation of an object is very important in the fields of energy conversion, infrared sensing, thermal imaging, and lighting. For example, enhancing thermal radiation is a common method for radiative cooling (Sci. Adv. 2019, 5, eaat9480), regulating the bandwidth of thermal radiation is crucial for infrared sensing (ACS Photonics 2017, 4, 1371-1380), and suppressing thermal radiation is an effective way to manipulate thermal imaging (Adv. Opt. Mater. 2018, 6, 1801006). According to the Steven-Boltzmann law, the thermal radiation energy is proportional to the emissivity and the fourth power of the thermodynamic temperature. Therefore, the thermal radiation of an object can be suppressed by lowering the thermodynamic temperature or emissivity.
[0003] As one of the methods to suppress the thermal radiation of an object, lowering the surface temperature can be simply achieved by covering it with an insulation layer (Adv. Mater. 2018, 30, 1706807). Aerogel, which is known for its ultra-low thermal conductivity, is the most promising insulation layer and can effectively suppress thermal radiation. However, the insulation layer will cause heat accumulation, which will cause the performance of the target object to deteriorate if the target object is a device or device. Another way to suppress thermal radiation is to reduce infrared emissivity (Adv. Mater. 2021, 33, 2004754), and infrared emissivity is closely related to the complex dielectric constant and conductivity of the material. According to Fresnel's law, electromagnetic wave transmission theory, and the Drude-Lorentz model, it can be deduced that infrared emissivity is essentially related to polarizability, which is closely related to the number of intrinsic dipole moments, ionic radius, and lattice constant. The number of polarization dipole moments is affected by the surface morphology of the material, and the solid surface morphology is one of the key factors affecting thermal emissivity. At the same time, according to the Hagen-Rubens relationship and Kirchhoff's radiation law, it can be deduced that high conductivity will lead to low infrared emissivity. However, the low infrared emissivity brought about by high conductivity will cause the thermodynamic temperature to rise sharply, thereby weakening the thermal radiation suppression performance. It can be seen that long-term thermal radiation suppression cannot be achieved by reducing the thermodynamic temperature or infrared emissivity alone, and a single uniform material is difficult to reduce the surface thermodynamic temperature and infrared emissivity at the same time. The laminated structure has become a new design idea.
[0004] The laminated structures currently prepared are usually used for stealth, such as a sandwich structure infrared stealth material with announcement number CN112937029A, which fixes the silica aerogel coating as a heat insulation layer between the upper and lower layers of low infrared emissivity fabric. However, the weight ratio of silica aerogel powder in the silica aerogel coating is 1 to 4 parts, the film-forming agent is 25 to 35 parts, and the curing agent is 5 to 7 parts, which cannot fully reflect the thermal insulation performance of the aerogel, and the surface flatness of the fabric is low, and a low infrared emissivity cannot be obtained, making the product unsuitable for stealth when the target temperature is higher than 50°C. In addition, the announcement number CN114179466A provides a stealth patch, including an infrared stealth layer, a visible light camouflage layer and a radar absorption layer, wherein the infrared stealth layer is composed of a transparent conductive film deposited on a polyester resin, and the infrared emissivity is less than 0.3, however, the radar absorption layer includes a first foam medium layer with a thickness of 1 to 2.5 mm, a second foam medium layer with a thickness of 6 to 10 mm, and a third foam medium layer with a thickness of 3 to 5 mm, and the thickness of the obtained stealth patch is relatively thick, and good flexibility cannot be obtained. Although the announcement number CN114193850A reports a lightweight, flexible, and bend-resistant target feature control composite material, this laminated structure includes a carbon fiber layer and a quartz fiber layer with a rubber matrix, and an absorbing layer and a low emissivity layer with a polyurethane resin or silicone rubber as a matrix, although the total thickness of this target feature control composite material is 2 mm to 6 mm, the density is relatively high, and the insulation requirements are not considered. Announcement No. CN113403566A reports a thermal barrier / low infrared emissivity integrated coating based on a fluorescent sublayer and its preparation method. Although it takes into account both the thermal insulation requirements and the low infrared requirements, the substrate needs to be placed in a box-type sandblasting machine for sandblasting roughening treatment in advance. The scope of application is limited and it is only applicable to metal substrates.
[0005] In terms of controlling thermal radiation, although the announcement number CN113276510B provides a Janus flexible composite film for intelligent radiation thermal control, the radiation heating layer fiber membrane on one side of the base film has high solar radiation absorption and low infrared emissivity, and the radiation cooling layer fiber membrane on the other side has high solar reflection and high infrared emissivity, but this Janus flexible composite film can reduce its own temperature through radiation cooling when the radiation cooling fiber membrane is outward, but it cannot suppress the thermal radiation of high-temperature target objects for a long time.
[0006] Therefore, there is an urgent need to develop a laminated structure that can suppress the thermal radiation of high-temperature target objects for a long time, and has low infrared emissivity, excellent thermal insulation performance and heat storage function. Summary of the invention
[0007] The main purpose of the present invention is to provide a laminated structure for long-term thermal radiation suppression and a preparation method thereof, so as to overcome the deficiency that the existing thermal radiation suppression materials cannot suppress the target object for a long time.
[0008] Another object of the present invention is to provide uses of the aforementioned laminated structure.
[0009] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0010] An embodiment of the present invention provides a thermal radiation suppression laminate structure, which is composed of a low infrared emissivity upper layer, a phase change energy storage middle layer and a thermal radiation reflecting lower layer, wherein the low infrared emissivity upper layer includes an aerogel film and a low infrared emissivity metal coating arranged on the surface of the aerogel film; the phase change energy storage middle layer includes a composite structure formed by an aerogel film and a phase change material; the thermal radiation reflecting lower layer includes a patterned aerogel film and a thermal radiation reflecting metal coating arranged on the patterned side of the patterned aerogel film.
[0011] The embodiment of the present invention also provides a method for preparing a thermal radiation suppression laminate structure, which comprises:
[0012] Depositing a low infrared emissivity metal coating on the surface of the aerogel film to obtain a low infrared emissivity upper layer;
[0013] Filling the phase change material into the aerogel film by melt filling or solution filling to obtain a phase change energy storage middle layer;
[0014] preparing a single-sided patterned aerogel film, and depositing a thermal radiation reflecting metal coating on the patterned side of the single-sided patterned aerogel film to obtain a thermal radiation reflecting lower layer;
[0015] The low infrared emissivity upper layer, the phase change energy storage middle layer, and the thermal radiation reflecting lower layer are assembled to obtain a thermal radiation inhibiting laminated structure.
[0016] The embodiment of the present invention also provides the application of the thermal radiation suppression laminate structure in the fields of heat insulation, energy storage, infrared penetration prevention or infrared detection resistance.
[0017] Compared with existing thermal radiation suppression materials, the thermal radiation suppression laminated structure provided by the present invention is composed of a low infrared emissivity upper layer, a phase change energy storage middle layer and a thermal radiation reflection lower layer. It has the advantages of high sunlight reflectivity, low average infrared emissivity in the 3-15μm band, and high phase change enthalpy value. It can reflect most of the thermal radiation of high-temperature target objects and can be used for long-term thermal radiation suppression of high-temperature target objects under light. In addition, it has good flexibility and can be made into different shapes as needed. It is convenient for use in fields such as heat insulation, energy storage, and countering infrared detection, and has very broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 Schematic diagram of the thermal radiation suppression stack structure in a typical embodiment of the present invention.
[0020] Figure 2 It is an emissivity curve diagram of the infrared low emissivity upper layer obtained in Example 2 of the present invention in the mid-infrared band.
[0021] Figure 3a and Figure 3b This is a scanning electron microscope image of the phase change energy storage middle layer obtained in Example 4 of the present invention.
[0022] Figure 4 It is a DSC curve diagram of the phase change energy storage middle layer obtained in Example 5 of the present invention.
[0023] Figure 5 It is a reflectivity curve diagram of the thermal radiation reflecting lower layer obtained in Example 6 of the present invention.
[0024] Figure 6 This is an infrared photograph of the heat radiation reflecting lower layer obtained in Example 6 of the present invention after covering the heating plate.
[0025] Figure 7 This is an infrared photograph of the laminated structure obtained in Example 7 of the present invention covering a high-temperature target object under light.
[0026] Figure 8 This is an infrared photograph of the laminated structure obtained in Example 10 of the present invention suppressing the thermal radiation of a high-temperature target object under light for a long time. DETAILED DESCRIPTION
[0027] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.
[0028] One aspect of an embodiment of the present invention provides a thermal radiation suppression stack structure, the structure of which can be referred to as Figure 1 As shown, it includes an upper layer 1 with low infrared emissivity, a middle layer 2 for phase change energy storage, and a lower layer 3 for thermal radiation reflection.
[0029] In some embodiments, the total thickness of the thermal radiation inhibiting laminated structure is 150-3000 μm.
[0030] In some embodiments, the low infrared emissivity upper layer 1 comprises an aerogel film 11 and a low infrared emissivity metal coating 12 disposed on the surface of the aerogel film 11. The low infrared emissivity upper layer 1 is obtained by applying the low infrared emissivity metal coating 12 on the upper surface of the aerogel film 11.
[0031] In some embodiments, the phase-change energy storage middle layer 2 includes a composite structure formed by an aerogel film and a phase-change material, and the phase-change energy storage middle layer 2 is obtained by introducing the phase-change material into the aerogel film.
[0032] In some embodiments, the thermal radiation reflecting lower layer 3 includes a patterned aerogel film 31 and a thermal radiation reflecting metal coating 32 disposed on the patterned side of the patterned aerogel film 31. The thermal radiation reflecting lower layer 3 is obtained by applying the thermal radiation reflecting metal coating 32 on the patterned side of the single-sided patterned aerogel film.
[0033] In some embodiments, the material of the aerogel film in the low infrared emissivity upper layer includes but is not limited to any one or a combination of two or more of polyimide, cellulose, aramid, chitosan, silicon oxide, etc.
[0034] In some more specific embodiments, the aerogel film is prepared by spin coating, blade coating, roll-to-roll or mold film forming, and then undergoing sol-gel transition, aging treatment, solvent replacement and drying treatment.
[0035] In some embodiments, the thermal conductivity of the aerogel film 11 is 0.02 to 0.2 W·m -1 ·K -1 , density is 10~200mg·cm -3 , thickness is 50~1000μm, and tensile strength is 0.1~30MPa.
[0036] In some embodiments, the material of the low infrared emissivity metal plating layer in the low infrared emissivity upper layer includes but is not limited to any one or a combination of two or more of gold, silver, aluminum, germanium, zinc, etc.
[0037] In some more specific embodiments, the low infrared emissivity metal coating is obtained by physical vapor deposition, preferably any one of thermal evaporation, magnetron sputtering, vacuum ion plating, electron beam evaporation, etc., deposited on the surface of the aerogel film.
[0038] In some embodiments, the low infrared emissivity metal coating layer 12 has a thickness of 10-1000 nm.
[0039] In some embodiments, the low infrared emissivity upper layer 1 is obtained by applying a low infrared emissivity metal coating 12 on the upper surface of the aerogel film 11, and its solar reflectivity is 0.5-0.95, the average infrared emissivity in the 3-15 μm band is 0.05-0.5, and the thickness is 50-1000 μm.
[0040] In some embodiments, the phase-change energy storage middle layer 2 is obtained by compounding the phase-change material with the aerogel film by solution filling or melt filling.
[0041] Furthermore, the phase change material in the phase change energy storage middle layer 2 includes, but is not limited to, any one or more combinations of paraffins, polyols, fatty amines, higher fatty alcohols, higher fatty acids, and the like.
[0042] In some more specific embodiments, the content of phase change material in the phase change energy storage middle layer is adjustable, and the filling amount is below 99wt%, for example, it can be 10wt% to 99wt%, and preferably 50wt% to 98wt%; the phase change enthalpy value of the phase change energy storage middle layer is below 250J / g, for example, it can be 10 to 250J / g, and preferably 50 to 200J / g.
[0043] Furthermore, the thickness of the phase change energy storage middle layer is 50 to 1000 μm, and the tensile strength is 0.2 to 100 MPa.
[0044] In some embodiments, the material of the patterned aerogel film 31 includes, but is not limited to, any one or a combination of two or more of polyimide, cellulose, aramid, chitosan, silicon oxide, etc.
[0045] In some embodiments, the patterned aerogel film is a single-sided patterned film obtained by 3D printing or using a mold, and then prepared by sol-gel transformation, aging treatment, solvent replacement and drying processes.
[0046] Furthermore, the thermal conductivity of the patterned aerogel film is 0.02 to 0.2 W·m -1 ·K -1 , thickness is 50~1000μm, and tensile strength is 0.1~30MPa.
[0047] Furthermore, the patterns contained in the patterned aerogel film include but are not limited to honeycomb structures, lattice structures, curved arrangement structures, etc., and can be controlled and prepared by a preset program of a 3D printing device or by a customized patterned mold.
[0048] In some embodiments, the material of the heat radiation reflecting metal coating 32 includes, but is not limited to, any one or a combination of two or more of gold, silver, aluminum, germanium, zinc, etc.
[0049] In some embodiments, the thermal radiation reflective metal coating is deposited on the patterned side of the patterned aerogel film by physical vapor deposition, preferably any one of thermal evaporation, magnetron sputtering, vacuum ion plating or electron beam evaporation.
[0050] In some embodiments, the thermal radiation reflecting metal coating has a thickness of 10 to 1000 nm.
[0051] In some embodiments, the thermal radiation reflecting lower layer is obtained by applying a thermal radiation reflecting metal coating on the patterned side of the single-sided patterned aerogel film, and its thermal radiation reflectivity in the 3-16 μm band is 0.5-0.95 and its thickness is 50-1000 μm.
[0052] The thermal radiation suppression laminated structure provided by the present invention is composed of a low infrared emissivity upper layer, a phase change energy storage middle layer and a thermal radiation reflection lower layer. It has high sunlight reflectivity, low average infrared emissivity in the 3-15μm band, high phase change enthalpy value, and can reflect most of the thermal radiation of high-temperature target objects. It can be used for long-term thermal radiation suppression of high-temperature target objects under light.
[0053] As another aspect of the technical solution of the present invention, it also relates to a method for preparing a thermal radiation suppression laminate structure, which comprises:
[0054] Depositing a low infrared emissivity metal coating on the surface of the aerogel film to obtain a low infrared emissivity upper layer;
[0055] Filling the phase change material into the aerogel film by melt filling or solution filling to obtain a phase change energy storage middle layer;
[0056] preparing a single-sided patterned aerogel film, and depositing a thermal radiation reflecting metal coating on the patterned side of the single-sided patterned aerogel film to obtain a thermal radiation reflecting lower layer;
[0057] The low infrared emissivity upper layer, the phase change energy storage middle layer, and the thermal radiation reflecting lower layer are assembled to obtain a thermal radiation inhibiting laminated structure.
[0058] In some embodiments, the low infrared emissivity upper layer is obtained by applying a low infrared emissivity metal coating on the upper surface of the aerogel film. The method for preparing the low infrared emissivity upper layer comprises: first preparing an aerogel film, and then depositing a low infrared emissivity metal coating on its upper surface to obtain a low infrared emissivity upper layer.
[0059] Specifically, the method for preparing the aerogel film includes: preparing the aerogel film by spin coating, blade coating, roll-to-roll or mold film forming on the nanostructured unit dispersion or precursor, and then subjecting the nanostructured unit dispersion or precursor to sol-gel transformation, aging treatment, solvent replacement and drying treatment. The material of the nanostructured unit dispersion or precursor includes but is not limited to any one or a combination of two or more of polyimide, cellulose, aramid, chitosan, silicon oxide, etc.
[0060] In some more specific implementation cases, the preparation method specifically includes: obtaining a nanostructured unit dispersion having a content of 0.1 wt% to 10 wt% of the nanostructured unit by chemical stripping or small molecule polymerization; forming the nanostructured unit dispersion into a film by spin coating, blade coating, roll-to-roll or by means of a mold, transferring the nanostructured unit dispersion to a coagulation bath for sol-gel transformation to obtain a gel film, wherein the coagulation bath components used in the sol-gel transformation include but are not limited to any one or a combination of two or more of water, ethanol, methanol, acetone, and hydrochloric acid aqueous solution, etc., performing an aging treatment after the gel is completed, and the aging treatment time is preferably 12 to 48 hours, transferring the nanostructured unit dispersion to a specific solvent for solvent replacement, wherein the solvent components used include but are not limited to any one or a combination of two or more of acetone, water, and tert-butyl alcohol aqueous solution, etc., and then obtaining an aerogel film by a special drying process (such as any one or a combination of two or more of atmospheric pressure drying, vacuum drying, freeze drying, supercritical drying, etc.), wherein the thermal conductivity of the aerogel film is 0.02 to 0.2 W·m -1 ·K -1 , density is 10~200mg·cm -3 , thickness is 50~1000μm, and tensile strength is 0.1~30MPa.
[0061] In some embodiments, the preparation method includes: using physical vapor deposition, preferably any one of methods such as thermal evaporation, magnetron sputtering, vacuum ion plating or electron beam evaporation, to deposit a metal material on the upper surface of the aerogel film to form a low infrared emissivity metal coating to obtain a low infrared emissivity upper layer; wherein the metal material includes but is not limited to any one of gold, silver, aluminum, germanium, zinc, etc., or a combination of two or more thereof.
[0062] Furthermore, the thickness of the low infrared emissivity metal coating is 10 to 1000 nm.
[0063] In some embodiments, the preparation method of the phase change energy storage middle layer is: fill the phase change material into the aerogel film prepared above by melt filling or solution filling, remove the excess phase change material on the surface, and obtain the phase change energy storage middle layer. The phase change material includes but is not limited to any one or more combinations of paraffins, polyols, fatty amines, higher fatty alcohols, and higher fatty acids.
[0064] In some more specific implementation cases, the preparation method of the phase change energy storage middle layer specifically includes: preparing the phase change material into a solution or heating it in a vacuum oven until it is completely melted, and then immersing the aerogel film in the phase change material solution or the molten phase change material for 1 to 24 hours, preferably 4 to 12 hours, taking out and removing excess phase change material on the surface to obtain a phase change energy storage middle layer.
[0065] Specifically, the melt filling method includes: placing the phase change material in a vacuum oven, heating until the phase change material is completely melted, immersing the aerogel film in the molten phase change material, immersing for 1 to 24 hours (within 24 hours), preferably 4 to 12 hours, taking it out and placing it on filter paper, and removing excess phase change material on the surface while the phase change material is molten to obtain a phase change energy storage middle layer.
[0066] Specifically, the solution filling method includes: preparing the phase change material into a solution, immersing the aerogel film in the phase change material solution, immersing for 1 to 24 hours (within 24 hours), preferably 4 to 12 hours, taking it out and placing it on filter paper, removing excess phase change material solution on the surface, and removing the solvent to obtain a phase change energy storage middle layer.
[0067] In some embodiments, the method for preparing the thermal radiation reflecting lower layer includes: first preparing a single-sided patterned aerogel film, and then depositing a thermal radiation reflecting metal coating on the patterned side to obtain the thermal radiation reflecting lower layer.
[0068] In some more specific implementation cases, the preparation method of the single-sided patterned aerogel film includes: first designing the pattern, including but not limited to honeycomb structure, lattice structure, curved arrangement structure, etc. The material of the single-sided patterned aerogel film includes but is not limited to polyimide, cellulose, aramid, chitosan, silicon oxide, etc. The preparation method is to obtain a single-sided patterned film by 3D printing or with the help of a mold, transfer it to a coagulation bath for sol-gel transformation to obtain a gel film, the coagulation bath components include but are not limited to water, ethanol, methanol, acetone, hydrochloric acid aqueous solution, etc., after the gel is completed, an aging treatment is performed, and the aging treatment time is preferably 12 to 48 hours, and the film is transferred to a specific solvent for solvent replacement, and the solvent components include but are not limited to acetone, water, tert-butanol aqueous solution, etc., and then a special drying process (such as atmospheric pressure drying, vacuum drying, freeze drying, supercritical drying, etc.) is performed to obtain a single-sided patterned aerogel film.
[0069] Furthermore, when using the 3D printing method, the pattern is preset into the printing program, and the prepared nano-building unit dispersion is processed through freezing 3D printing or light-curing 3D printing to obtain a single-sided patterned aerogel film; it is then transferred to a coagulation bath, and undergoes sol-gel transition, solvent replacement, aging treatment and drying treatment to prepare a single-sided patterned aerogel film.
[0070] Furthermore, when using the mold molding method, the prepared nano-building unit dispersion or precursor is injected into a special mold with a pattern, and then transferred to a coagulation bath together. After sol-gel transition, solvent replacement, aging treatment, drying treatment and demolding, a single-sided patterned aerogel film is obtained.
[0071] Furthermore, the pattern includes but is not limited to a honeycomb structure, a lattice structure, a curved arrangement structure, etc., which can be performed through a preset program of a 3D printing device or controlled through a customized patterned mold.
[0072] In some embodiments, the preparation method includes: using physical vapor deposition, preferably any one of thermal evaporation, magnetron sputtering, vacuum ion plating or electron beam evaporation, to deposit a metal material on the patterned side of the single-sided patterned aerogel film to form a thermal radiation reflective metal coating with a thickness of 10-1000nm, and obtain a thermal radiation reflective lower layer. Wherein, the metal material includes but is not limited to any one or a combination of two or more of gold, silver, aluminum, germanium, zinc, etc.
[0073] In some embodiments, the preparation method includes: assembling a low infrared emissivity upper layer, a phase change energy storage middle layer, and a thermal radiation reflecting lower layer, utilizing the thermal insulation properties of the aerogel film in the low infrared emissivity upper layer, the low infrared emissivity of the low infrared emissivity metal coating, the excellent thermal management function of the phase change energy storage middle layer, and the thermal insulation properties of the patterned aerogel film in the thermal radiation reflecting lower layer, and the high reflectivity of the thermal radiation reflecting metal coating to thermal radiation in the 3-16μm band, to achieve long-term thermal radiation suppression of high-temperature target objects under illumination.
[0074] Another aspect of the embodiments of the present invention further provides a thermal radiation suppression laminate structure prepared by the aforementioned method.
[0075] Another aspect of the embodiments of the present invention further provides applications of the thermal radiation suppression stacked structure.
[0076] Furthermore, the thermal radiation suppression laminated structure of the present invention can achieve long-term thermal radiation suppression of high-temperature target objects under light. In addition, it has good flexibility and can be made into different shapes according to needs. It is convenient for use in heat insulation, energy storage, thermal management, reflection of sunlight, anti-infrared transmission, and countering infrared detection. The application prospects are very broad.
[0077] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention, and do not have any limiting effect on it. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are usually carried out under conventional conditions or under the conditions recommended by the manufacturer.
[0078] Example 1
[0079] A 2% cellulose nanofiber dispersion was coated on a glass substrate using a doctor blade, transferred to water (coagulation bath), and a cellulose hydrogel was obtained through sol-gel transformation. After aging treatment and solvent replacement, a cellulose aerogel film was obtained through freeze drying, and its thermal conductivity was 0.04 W·m -1 ·K -1 , density is 30mg·cm -3 , thickness of 1000μm, and tensile strength of 1MPa. Subsequently, a 10nm thick aluminum coating was deposited on the upper surface of the cellulose aerogel by magnetron sputtering to obtain a low-emissivity upper layer with a solar reflectivity of 0.5 and an average infrared emissivity of 0.5 in the 3-15μm band.
[0080] Paraffin is placed in a vacuum oven and heated until the paraffin is completely melted. The cellulose aerogel film is immersed in the molten paraffin and allowed to stand for 12 hours. The film is taken out and placed on filter paper, and excess paraffin on the surface is removed while the paraffin is molten to obtain a phase change energy storage middle layer. The phase change material filling amount is 98wt%, the phase change enthalpy value is 200J / g, the thickness is 1000μm, and the tensile strength is 3MPa.
[0081] Using 3D printing technology, the lattice pattern was preset into the printing program, and the prepared 2% cellulose nanofiber dispersion was printed on a cold stage to obtain a single-sided lattice pattern film gel, which was then transferred to low-temperature water (coagulation bath) to undergo sol-gel transformation of cellulose hydrogel, aging treatment, solvent replacement, and freeze-drying to obtain a single-sided lattice pattern cellulose aerogel film with a thermal conductivity of 0.03 W·m -1 ·K -1 , thickness of 1000μm, tensile strength of 0.5MPa. Subsequently, a 10nm thick aluminum coating was deposited on one side of the cellulose aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.5.
[0082] The three layers of film are assembled in the order of top, middle and bottom to obtain a thermal radiation suppression laminate structure, such as Figure 1 shown.
[0083] Example 2
[0084] A 4% cellulose nanofiber dispersion was coated on a glass substrate using a doctor blade, transferred to water (coagulation bath), and a cellulose hydrogel was obtained through sol-gel transition. After aging treatment and solvent replacement, a cellulose aerogel film was obtained through freeze drying, and its thermal conductivity was 0.05 W·m -1 ·K -1 , density is 45mg·cm- 3 , thickness of 300μm, and tensile strength of 2MPa. Subsequently, a 500nm thick silver coating was deposited on the upper surface of the cellulose aerogel by magnetron sputtering to obtain a low emissivity upper layer, whose solar reflectivity was 0.9 and the average infrared emissivity in the 3-15μm band was 0.1, such as Figure 2 shown.
[0085] Polyethylene glycol 2000 was placed in a vacuum oven and heated until the polyethylene glycol 2000 was completely melted. The cellulose aerogel film was immersed in the molten polyethylene glycol 2000 and allowed to stand for 12 hours. The film was taken out and placed on filter paper. The excess polyethylene glycol 2000 on the surface was removed while the polyethylene glycol 2000 was molten to obtain a phase change energy storage middle layer. The phase change material filling amount was 80wt%, the phase change enthalpy value was 150J / g, the thickness was 300μm, and the tensile strength was 6MPa.
[0086] Using 3D printing technology, the lattice pattern was preset into the printing program, and the prepared 2% cellulose nanofiber dispersion was printed on a cold stage to obtain a single-sided lattice pattern film gel, which was then transferred to low-temperature water (coagulation bath) and transformed into a cellulose hydrogel through sol-gel, aging treatment, solvent replacement, and freeze-drying to obtain a single-sided lattice pattern cellulose aerogel film with a thermal conductivity of 0.04 W·m -1 ·K -1 , thickness of 300μm, and tensile strength of 2MPa. Subsequently, a 500nm thick silver coating was deposited on one side of the cellulose aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0087] The three layers of film are assembled in the order of upper, middle and lower to obtain a thermal radiation inhibiting laminated structure.
[0088] Example 3
[0089] A 6% cellulose nanofiber dispersion was coated on a glass substrate using a doctor blade, transferred to water (coagulation bath), and a cellulose hydrogel was obtained through sol-gel transformation. After aging treatment and solvent replacement, a cellulose aerogel film was obtained through freeze drying, and its thermal conductivity was 0.06 W·m -1 ·K -1, density is 50mg·cm -3 , thickness of 300μm, and tensile strength of 3MPa. Subsequently, a 1000nm thick silver coating was deposited on the upper surface of the cellulose aerogel by magnetron sputtering to obtain a low-emissivity upper layer with a solar reflectivity of 0.95 and an average infrared emissivity of 0.05 in the 3-15μm band.
[0090] Stearic acid is placed in a vacuum oven and heated until the stearic acid is completely melted. The cellulose aerogel film is immersed in the molten stearic acid and allowed to stand for 4 hours. The film is taken out and placed on filter paper, and the excess stearic acid on the surface is removed while the stearic acid is molten to obtain a phase change energy storage middle layer, whose phase change material filling amount is 50wt%, the phase change enthalpy value is 50J / g, the thickness is 300μm, and the tensile strength is 9MPa.
[0091] Using 3D printing technology, the lattice pattern was preset into the printing program, and the prepared 2% cellulose nanofiber dispersion was printed on a cold stage to obtain a single-sided lattice pattern film gel, which was then transferred to low-temperature water (coagulation bath) and transformed into a cellulose hydrogel through sol-gel treatment, aging treatment, solvent replacement, and freeze drying to obtain a single-sided lattice pattern cellulose aerogel film with a thermal conductivity of 0.05 W·m -1 ·K -1 , thickness of 300μm, and tensile strength of 3MPa. Subsequently, a silver coating with a thickness of 1000nm was deposited on one side of the cellulose aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.95.
[0092] The three layers of film are assembled in the order of upper, middle and lower to obtain a thermal radiation inhibiting laminated structure.
[0093] Example 4
[0094] A 1% aramid nanofiber dispersion was coated on an aluminum foil substrate by spin coating, transferred to water (coagulation bath), and aramid hydrogel was obtained by sol-gel transformation. After aging treatment and solvent replacement, aramid aerogel film was obtained by supercritical drying, and its thermal conductivity was 0.03 W·m -1 ·K -1 , density is 20mg·cm -3 , thickness of 50μm, and tensile strength of 1MPa. Subsequently, a 200nm thick gold coating was deposited on the upper surface of the aramid aerogel by magnetron sputtering to obtain a low-emissivity upper layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0095] Place paraffin in a vacuum oven and heat until the paraffin is completely melted. Immerse the aramid aerogel film in the molten paraffin and let it stand for 12 hours. Take it out and place it on filter paper. Remove the excess paraffin on the surface while the paraffin acid is molten to obtain a phase change energy storage middle layer. The microscopic morphology is as follows: Figure 3a and Figure 3b As shown, the phase change material filling amount is 80wt%, the phase change enthalpy value is 150J / g, the thickness is 50μm, and the tensile strength is 3MPa.
[0096] Using 3D printing technology, the grid pattern was preset into the printing program, and the prepared 1% aramid nanofiber dispersion was printed on a cold stage to obtain a single-sided grid pattern film gel, which was then transferred to low-temperature water (coagulation bath) to obtain aramid hydrogel through sol-gel transformation. After aging treatment and solvent replacement, a single-sided grid pattern aramid aerogel film was obtained through supercritical drying, and its thermal conductivity was 0.028 W·m -1 ·K -1 , thickness of 50μm, and tensile strength of 0.5MPa. Subsequently, a 200nm thick gold coating was deposited on one side of the aramid aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0097] The three layers of film are assembled in the order of upper, middle and lower to obtain a thermal radiation inhibiting laminated structure.
[0098] Example 5
[0099] A 2% aramid nanofiber dispersion was coated on an aluminum foil substrate using a doctor blade, transferred to water (coagulation bath), and aramid hydrogel was obtained through sol-gel transformation. After aging treatment and solvent replacement, aramid aerogel film was obtained through supercritical drying, and its thermal conductivity was 0.035 W·m -1 ·K -1 , density is 30mg·cm -3 , thickness of 300μm, and tensile strength of 2MPa. Subsequently, a 200nm thick gold coating was deposited on the upper surface of the aramid aerogel by magnetron sputtering to obtain a low-emissivity upper layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0100] The paraffin was placed in a vacuum oven and heated until the paraffin was completely melted. The aramid aerogel film was immersed in the molten paraffin and allowed to stand for 12 hours. The film was taken out and placed on filter paper. The excess paraffin on the surface was removed in the molten state of the paraffin acid to obtain a phase change energy storage middle layer. The phase change material filling amount was 80wt% and the phase change enthalpy value was 150J / g (such as Figure 4 As shown), the thickness is 300μm and the tensile strength is 6MPa.
[0101] Using 3D printing technology, the grid pattern was preset into the printing program, and the prepared 2% aramid nanofiber dispersion was printed on a cold stage to obtain a single-sided grid pattern film gel, which was then transferred to low-temperature water (coagulation bath) to obtain aramid hydrogel through sol-gel transformation. After aging treatment and solvent replacement, a single-sided grid pattern aramid aerogel film was obtained through supercritical drying, and its thermal conductivity was 0.03 W·m -1 ·K -1 , thickness of 300μm, and tensile strength of 1.5MPa. Subsequently, a 200nm thick gold coating was deposited on one side of the aramid aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0102] The three layers of film are assembled in the order of upper, middle and lower to obtain a thermal radiation inhibiting laminated structure.
[0103] Example 6
[0104] 4% aramid nanofibers were dispersed and extruded using a roll-to-roll device and transferred into water (coagulation bath). Aramid hydrogel was obtained through sol-gel transformation. After aging treatment and solvent replacement, aramid aerogel film was obtained through supercritical drying. The thermal conductivity of the film was 0.06 W·m -1 ·K -1 , density is 50mg·cm -3 , thickness of 300μm, and tensile strength of 5MPa. Subsequently, a 200nm thick gold coating was deposited on the upper surface of the aramid aerogel by magnetron sputtering to obtain a low-emissivity upper layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0105] Paraffin is placed in a vacuum oven and heated until the paraffin is completely melted. The aramid aerogel film is immersed in the molten paraffin and allowed to stand for 12 hours. The film is taken out and placed on filter paper, and excess paraffin on the surface is removed while the paraffin acid is molten to obtain a phase change energy storage middle layer, wherein the phase change material filling amount is 80wt%, the phase change enthalpy value is 150J / g, the thickness is 300μm, and the tensile strength is 15MPa.
[0106] Using 3D printing technology, the grid pattern was preset into the printing program, and the prepared 2% aramid nanofiber dispersion was printed on a cold stage to obtain a single-sided grid pattern film gel, which was then transferred to low-temperature water (coagulation bath) to obtain aramid hydrogel through sol-gel transformation. After aging treatment and solvent replacement, a single-sided grid pattern aramid aerogel film was obtained through supercritical drying, and its thermal conductivity was 0.03 W·m -1 ·K -1, thickness of 300μm, tensile strength of 1.5MPa. Then, a 200nm thick gold coating was deposited on one side of the aramid aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9, such as Figure 5 As shown, covered on a high-temperature target object, the infrared photo is as follows Figure 6 shown.
[0107] The three layers of film are assembled in the order of upper, middle and lower to obtain a thermal radiation inhibiting laminated structure.
[0108] Example 7
[0109] A 6% aramid nanofiber dispersion was injected into a custom-made polytetrafluoroethylene mold with an internal size of 50cm*50cm*1cm, and then transferred to water (coagulation bath) for aging treatment and solvent replacement. Aramid hydrogel was obtained through sol-gel transformation. After demoulding, aramid aerogel film was obtained through supercritical drying. Its thermal conductivity is 0.1W·m -1 ·K -1 , density is 60mg·cm -3 , thickness of 300μm, and tensile strength of 10MPa. Subsequently, a 600nm thick aluminum coating was deposited on the upper surface of the aramid aerogel by evaporation to obtain a low-emissivity upper layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0110] Polyethylene glycol 2000 was prepared into a 60wt% aqueous solution, and the aramid aerogel film was immersed in the polyethylene glycol 2000 aqueous solution and allowed to stand for 12 hours. The film was taken out and placed on filter paper to remove excess polyethylene glycol 2000 on the surface. After vacuum drying, a phase change energy storage middle layer was obtained, in which the phase change material filling amount was 50wt%, the phase change enthalpy value was 50J / g, the thickness was 300μm, and the tensile strength was 30MPa.
[0111] A 6% aramid nanofiber dispersion was injected into a custom-made polytetrafluoroethylene mold with a honeycomb pattern on the bottom, and then transferred to water (coagulation bath) to obtain aramid hydrogel through sol-gel transformation. After demoulding, aging treatment, solvent replacement, and supercritical drying, a single-sided honeycomb pattern aramid aerogel film was obtained, with a thermal conductivity of 0.2 W·m -1 ·K -1 , thickness of 300μm, and tensile strength of 10MPa. Subsequently, a 600nm thick aluminum coating was deposited on one side of the aramid aerogel honeycomb pattern by evaporation to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0112] The three layers of film are assembled in the order of top, middle and bottom to obtain a thermal radiation suppression laminate structure, which is covered on a high-temperature target object under light. The infrared photo shows Figure 7 shown.
[0113] Example 8
[0114] A custom polytetrafluoroethylene mold with an internal size of 50cm*50cm*1cm was injected with 8% aramid nanofiber dispersion, and then transferred to a 1% hydrochloric acid aqueous solution (coagulation bath). Aramid hydrogel was obtained through sol-gel transformation. After demoulding, aging treatment, solvent replacement, and supercritical drying, an aramid aerogel film was obtained, and its thermal conductivity was 0.15W·m -1 ·K -1 , density is 80mg·cm -3 , thickness of 300μm, tensile strength of 20MPa, and then by evaporation, a 500nm thick germanium coating was deposited on the upper surface of the aramid aerogel to obtain a low emissivity upper layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0115] Polyethylene glycol 2000 was prepared into a 60wt% aqueous solution, and the aramid aerogel film was immersed in the polyethylene glycol 2000 aqueous solution and allowed to stand for 12 hours. The film was taken out and placed on filter paper to remove excess polyethylene glycol 2000 on the surface. After vacuum drying, a phase change energy storage middle layer was obtained, in which the phase change material filling amount was 80wt%, the phase change enthalpy value was 150J / g, the thickness was 300μm, and the tensile strength was 60MPa.
[0116] A 4% aramid nanofiber dispersion was injected into a custom-made polytetrafluoroethylene mold with a honeycomb pattern on the bottom, and then transferred to a 1% hydrochloric acid aqueous solution (coagulation bath) to obtain an aramid hydrogel through a sol-gel transition. After demoulding, aging treatment, solvent replacement, and supercritical drying, a single-sided honeycomb pattern aramid aerogel film was obtained, and its thermal conductivity was 0.1 W·m -1 ·K -1 , thickness of 300μm, tensile strength of 20MPa. Then, by evaporation, a 500nm thick silver coating was deposited on one side of the aramid aerogel honeycomb pattern to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0117] The three layers of film are assembled in the order of upper, middle and lower to obtain a thermal radiation inhibiting laminated structure.
[0118] Example 9
[0119] A 10% aramid nanofiber dispersion was injected into a custom-made polytetrafluoroethylene mold with an internal size of 50cm*50cm*1cm, and then transferred to a 1% hydrochloric acid aqueous solution (coagulation bath). Aramid hydrogel was obtained through sol-gel transformation. After demoulding, an aramid aerogel film was obtained through supercritical drying. Its thermal conductivity is 0.2W·m -1 ·K-1 、Density is 200mg·em -3 , thickness of 300μm, and tensile strength of 30MPa. Then, a 500nm thick gold coating was deposited on the upper surface of the aramid aerogel by evaporation to obtain a low-emissivity upper layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0120] Polyethylene glycol 2000 was prepared into a 60wt% aqueous solution, and the aramid aerogel film was immersed in the polyethylene glycol 2000 aqueous solution and allowed to stand for 12 hours. The film was taken out and placed on filter paper to remove excess polyethylene glycol 2000 on the surface. After vacuum drying, a phase change energy storage middle layer was obtained, in which the phase change material filling amount was 80wt%, the phase change enthalpy value was 150J / g, the thickness was 300μm, and the tensile strength was 100MPa.
[0121] A 10% aramid nanofiber dispersion was injected into a custom-made polytetrafluoroethylene mold with a honeycomb pattern on the bottom, and then transferred to a 1% hydrochloric acid aqueous solution (coagulation bath) to obtain an aramid hydrogel through a sol-gel transition. After demoulding, aging treatment, solvent replacement, and supercritical drying, a single-sided honeycomb pattern aramid aerogel film was obtained, and its thermal conductivity was 0.1 W·m -1 ·K -1 , thickness of 300μm, tensile strength of 30MPa, and then by evaporation, a 500nm thick gold coating was deposited on one side of the aramid aerogel honeycomb pattern to obtain a thermal radiation reflecting lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.95.
[0122] The three layers of film are assembled in the order of upper, middle and lower to obtain a thermal radiation inhibiting laminated structure.
[0123] Example 10
[0124] A polytetrafluoroethylene mold with an internal size of 50cm*50cm*1cm was customized, and a condensation-polymerized silicon (CS, commonly known as silicone oil) solution was injected and transferred to an ammonia-ethanol solution (coagulation bath). After sol-gel transformation, aging, solvent replacement, and supercritical drying, a silica aerogel film was obtained, and its thermal conductivity was 0.02W·m -1 ·K -1 , density is 10mg·cm -3 , thickness of 300μm, tensile strength of 0.1MPa. Then, by evaporation, a zinc coating with a thickness of 500nm was deposited on the upper surface of the silica aerogel to obtain a low-emissivity upper layer with a solar reflectivity of 0.90 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0125] Paraffin is placed in a vacuum oven and heated until the paraffin is completely melted. The silica aerogel film is immersed in the molten paraffin and allowed to stand for 12 hours. The film is taken out and placed on filter paper, and excess paraffin on the surface is removed while the paraffin acid is molten to obtain a phase change energy storage middle layer with a phase change material filling amount of 98wt%, a phase change enthalpy of 200J / g, a thickness of 300μm, and a tensile strength of 0.2MPa.
[0126] A polytetrafluoroethylene mold with a honeycomb pattern on the bottom was customized, and the polycondensed silicon solution was injected and transferred to an ammonia ethanol solution (coagulation bath). After sol-gel transition, aging, solvent replacement, and supercritical drying, a patterned silicon oxide aerogel film was obtained, with a thermal conductivity of 0.02 W·m -1 ·K -1 , thickness of 300μm, tensile strength of 0.1MPa. Then, by evaporation, a 500nm thick silver coating was deposited on one side of the silicon oxide aerogel honeycomb pattern to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0127] The three layers of film are assembled in the order of top, middle and bottom to obtain a thermal radiation suppression laminate structure, which is used to suppress the thermal radiation of a high-temperature target object under light. After 12 hours, the infrared photo shows that it is still integrated with the background environment, such as Figure 8 shown.
[0128] Comparative Example 1
[0129] Paraffin is placed in a vacuum oven and heated until the paraffin is completely melted. The aramid aerogel film is immersed in the molten paraffin and allowed to stand for 12 hours. The film is taken out and placed on filter paper, and excess paraffin on the surface is removed while the paraffin acid is molten to obtain a phase change energy storage layer having a phase change material filling amount of 80wt%, a phase change enthalpy of 150J / g, a thickness of 300μm, and a tensile strength of 15MPa.
[0130] Using 3D printing technology, the grid pattern was preset into the printing program, and the prepared 2% aramid nanofiber dispersion was printed on a cold stage to obtain a single-sided grid pattern film gel, which was then transferred to low-temperature water (coagulation bath) to obtain aramid hydrogel through sol-gel transformation. After aging treatment and solvent replacement, a single-sided grid pattern aramid aerogel film was obtained through supercritical drying, and its thermal conductivity was 0.03 W·m -1 ·K -1 , thickness of 300μm, and tensile strength of 1.5MPa. Subsequently, a 200nm thick gold coating was deposited on one side of the aramid aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0131] The above-mentioned phase change energy storage layer is assembled as the upper layer and the thermal radiation reflection layer is assembled as the lower layer. Due to the lack of a low-emissivity upper layer, it is impossible to suppress the thermal radiation of a high-temperature target object under illumination.
[0132] Comparative Example 2
[0133] 4% aramid nanofibers were dispersed and extruded using a roll-to-roll device and transferred into water (coagulation bath). Aramid hydrogel was obtained through sol-gel transformation, aging treatment, solvent replacement, and supercritical drying to obtain an aramid aerogel film as the upper layer, with a thermal conductivity of 0.06 W·m -1 ·K -1 , density is 50mg·cm -3 , thickness is 300μm, tensile strength is 5MPa. The solar reflectivity is about 0.2, and the average infrared emissivity in the 3-15μm band is about 0.8.
[0134] Paraffin is placed in a vacuum oven and heated until the paraffin is completely melted. The aramid aerogel film is immersed in the molten paraffin and allowed to stand for 12 hours. The film is taken out and placed on filter paper, and excess paraffin on the surface is removed while the paraffin acid is molten to obtain a phase change energy storage middle layer, wherein the phase change material filling amount is 80wt%, the phase change enthalpy value is 150J / g, the thickness is 300μm, and the tensile strength is 15MPa.
[0135] Using 3D printing technology, the grid pattern was preset into the printing program, and the prepared 2% aramid nanofiber dispersion was printed on a cold stage to obtain a single-sided grid pattern film gel, which was then transferred to low-temperature water (coagulation bath) to obtain aramid hydrogel through sol-gel transformation. After aging treatment and solvent replacement, a single-sided grid pattern aramid aerogel film was obtained through supercritical drying, and its thermal conductivity was 0.03 W·m -1 ·K -1 , thickness of 300μm, and tensile strength of 1.5MPa. Subsequently, a 200nm thick gold coating was deposited on one side of the aramid aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0136] The three layers of film are assembled into a stacked structure in the order of top, middle and bottom. Since the infrared emissivity of the upper layer is as high as 0.8, it is impossible to suppress the thermal radiation of the high-temperature target object under light.
[0137] Comparative Example 3
[0138] 4% aramid nanofibers were dispersed and extruded using a roll-to-roll device and transferred into water (coagulation bath). Aramid hydrogel was obtained through sol-gel transformation. After aging treatment and solvent replacement, aramid aerogel film was obtained through supercritical drying. The thermal conductivity of the film was 0.06 W·m -1 ·K -1, density is 50mg·cm -3 , thickness of 300μm, and tensile strength of 5MPa. Subsequently, a 200nm thick gold coating was deposited on the upper surface of the aramid aerogel by magnetron sputtering to obtain a low-emissivity upper layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0139] Using 3D printing technology, the grid pattern was preset into the printing program, and the prepared 2% aramid nanofiber dispersion was printed on a cold stage to obtain a single-sided grid pattern film gel, which was then transferred to low-temperature water (coagulation bath) to obtain aramid hydrogel through sol-gel transformation. After aging treatment and solvent replacement, a single-sided grid pattern aramid aerogel film was obtained through supercritical drying, and its thermal conductivity was 0.03 W·m -1 ·K -1 , thickness of 300μm, and tensile strength of 1.5MPa. Subsequently, a 200nm thick gold coating was deposited on one side of the aramid aerogel lattice pattern by magnetron sputtering to obtain a thermal radiation reflective lower layer, whose thermal radiation reflectivity in the 3-16μm band is 0.9.
[0140] The above-mentioned low-emissivity upper layer and the thermal radiation reflecting lower layer are assembled, but due to the lack of a phase change energy storage layer, long-term thermal radiation suppression cannot be achieved.
[0141] Comparative Example 4
[0142] 4% aramid nanofibers were dispersed and extruded using a roll-to-roll device and transferred into water (coagulation bath). Aramid hydrogel was obtained through sol-gel transformation. After aging treatment and solvent replacement, aramid aerogel film was obtained through supercritical drying. The thermal conductivity of the film was 0.06 W·m -1 ·K -1 , density is 50mg·cm -3 , thickness of 300μm, and tensile strength of 5MPa. Subsequently, a 200nm thick gold coating was deposited on the upper surface of the aramid aerogel by magnetron sputtering to obtain a low emissivity layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0143] Paraffin is placed in a vacuum oven and heated until the paraffin is completely melted. The aramid aerogel film is immersed in the molten paraffin and allowed to stand for 12 hours. The film is taken out and placed on filter paper, and excess paraffin on the surface is removed while the paraffin acid is molten to obtain a phase change energy storage layer having a phase change material filling amount of 80wt%, a phase change enthalpy of 150J / g, a thickness of 300μm, and a tensile strength of 15MPa.
[0144] The above-mentioned low emissivity layer is assembled as the upper layer and the phase change energy storage layer is assembled as the lower layer. Due to the lack of a heat-insulating thermal radiation reflection layer, it is impossible to suppress the thermal radiation of a high-temperature target object.
[0145] Comparative Example 5
[0146] 4% aramid nanofibers were dispersed and extruded using a roll-to-roll device and transferred into water (coagulation bath). Aramid hydrogel was obtained through sol-gel transformation. After aging treatment and solvent replacement, aramid aerogel film was obtained through supercritical drying. The thermal conductivity of the film was 0.06 W·m -1 ·K -1 , density is 50mg·cm -3 , thickness of 300μm, and tensile strength of 5MPa. Subsequently, a 200nm thick gold coating was deposited on the upper surface of the aramid aerogel by magnetron sputtering to obtain a low-emissivity upper layer with a solar reflectivity of 0.9 and an average infrared emissivity of 0.1 in the 3-15μm band.
[0147] Paraffin is placed in a vacuum oven and heated until the paraffin is completely melted. The aramid aerogel film is immersed in the molten paraffin and allowed to stand for 12 hours. The film is taken out and placed on filter paper, and excess paraffin on the surface is removed while the paraffin acid is molten to obtain a phase change energy storage middle layer, wherein the phase change material filling amount is 80wt%, the phase change enthalpy value is 150J / g, the thickness is 300μm, and the tensile strength is 15MPa.
[0148] Using 3D printing technology, the grid pattern was preset into the printing program, and the prepared 2% aramid nanofiber dispersion was printed on a cold stage to obtain a single-sided grid pattern film gel, which was then transferred to low-temperature water (coagulation bath) to obtain aramid hydrogel through sol-gel transformation. After aging treatment and solvent replacement, a single-sided grid pattern aramid aerogel film was obtained through supercritical drying as the thermal insulation lower layer, with a thermal conductivity of 0.03 W·m -1 ·K -1 , thickness is 300μm, tensile strength is 1.5MPa. Its thermal radiation reflectivity in the 3-16μm band is 0.1.
[0149] The three layers of film are assembled in the order of upper, middle and lower to obtain a laminated structure. Since the lower insulating layer lacks the function of reflecting heat radiation, it is unable to suppress heat radiation for a long time.
[0150] Through Examples 1-10, it can be found that the thermal radiation suppression laminated structure obtained by the above technical solution of the present invention can suppress the thermal radiation of a high-temperature target object under light for a long time. In addition, it has good flexibility and can be made into different shapes as needed, which is convenient for application in fields such as heat insulation, energy storage, and countering infrared detection.
[0151] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0152] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.
Claims
1. A thermal radiation suppression laminate structure, characterized in that: The thermal radiation suppression laminated structure is composed of a low infrared emissivity upper layer, a phase change energy storage middle layer and a thermal radiation reflection lower layer, wherein the low infrared emissivity upper layer comprises an aerogel film and a low infrared emissivity metal coating arranged on the surface of the aerogel film, wherein the material of the aerogel film is selected from any one or a combination of two or more of polyimide, cellulose, aramid, chitosan and silicon oxide, and the material of the low infrared emissivity metal coating is selected from any one or a combination of two or more of gold, silver, aluminum, germanium and zinc, wherein the solar reflectivity of the low infrared emissivity upper layer is 0.5-0.95, the average infrared emissivity in the 3-15 μm band is 0.05-0.5, and the thickness is 50-1000 μm; the phase change energy storage middle layer comprises a composite structure formed by an aerogel film and a phase change material, and the filling amount of the phase change material in the phase change energy storage middle layer is 99 wt% or less, the phase change enthalpy of the phase change energy storage middle layer is below 250 J / g, the thickness of the phase change energy storage middle layer is 50-1000 μm, and the tensile strength is 0.2-100 MPa; the thermal radiation reflecting lower layer comprises a patterned aerogel film and a thermal radiation reflecting metal coating arranged on the patterned side of the patterned aerogel film, the material of the patterned aerogel film is selected from any one or a combination of two or more of polyimide, cellulose, aramid, chitosan, and silicon oxide, the material of the thermal radiation reflecting metal coating is selected from any one or a combination of two or more of gold, silver, aluminum, germanium, and zinc, the thermal radiation reflectivity of the thermal radiation reflecting lower layer in the 3-16 μm band is 0.5-0.95, and the thickness is 50-1000 μm.
2. The heat radiation suppression laminate structure according to claim 1, characterized in that: The aerogel film is prepared by spin coating, blade coating, roll-to-roll or mold film forming, and then undergoes sol-gel transformation, aging treatment, solvent replacement and drying treatment. The thermal conductivity of the aerogel film is 0.02-0.2 W·m -1 ·K -1 , density is 10~200mg·cm -3 , thickness is 50~1000 μm, and tensile strength is 0.1~30 MPa.
3. The heat radiation suppression laminate structure according to claim 1, characterized in that: The low infrared emissivity metal coating is deposited on the surface of the aerogel film by physical vapor deposition.
4. The heat radiation suppression laminate structure according to claim 3, characterized in that: The low infrared emissivity metal coating is deposited on the surface of the aerogel film by any one of thermal evaporation, magnetron sputtering, vacuum ion plating and electron beam evaporation.
5. The heat radiation suppression laminate structure according to claim 1, characterized in that: The thickness of the low infrared emissivity metal coating is 10-1000 nm.
6. The heat radiation suppression laminate structure according to claim 1, characterized in that: The phase-change energy storage middle layer is obtained by compounding the phase-change material with the aerogel film in a solution filling or melt filling manner.
7. The heat radiation suppression laminate structure according to claim 1, characterized in that: The phase change material is selected from any one of paraffins, polyols, fatty amines, higher fatty alcohols, and higher fatty acids, or a combination of two or more thereof.
8. The heat radiation suppression laminate structure according to claim 1, characterized in that: The filling amount of the phase change material in the phase change energy storage middle layer is 50 wt% to 98 wt%.
9. The heat radiation suppression laminate structure according to claim 1, characterized in that: The phase change enthalpy value of the phase change energy storage middle layer is 50-200 J / g.
10. The heat radiation suppression laminate structure according to claim 1, characterized in that: The patterned aerogel film is a single-sided patterned film obtained by 3D printing or by using a mold, and then subjected to sol-gel transformation, aging treatment, solvent replacement and drying treatment to obtain a single-sided patterned aerogel film. The thermal conductivity of the patterned aerogel film is 0.02-0.2 W·m -1 ·K -1 , thickness is 50~1000 μm, and tensile strength is 0.1~30 MPa.
11. The heat radiation suppression laminate structure according to claim 1, characterized in that: The pattern contained in the patterned aerogel film is selected from any one of a honeycomb structure, a lattice structure, and a curved arrangement structure.
12. The heat radiation suppression laminate structure according to claim 1, characterized in that: The thermal radiation reflecting metal coating is obtained by depositing it on the patterned side of the patterned aerogel film by physical vapor deposition.
13. The heat radiation suppression laminate structure according to claim 12, characterized in that: The thermal radiation reflecting metal coating is obtained by depositing on the patterned side of the patterned aerogel film by any one of thermal evaporation, magnetron sputtering, vacuum ion plating or electron beam evaporation.
14. The heat radiation suppression laminate structure according to claim 1, characterized in that: The thickness of the heat radiation reflecting metal coating is 10-1000 nm.
15. The heat radiation suppression laminate structure according to claim 1, characterized in that: The total thickness of the thermal radiation suppression laminate structure is 150-3000 μm.
16. The method for preparing the thermal radiation suppression laminate structure according to any one of claims 1 to 15, characterized in that: include: Depositing a low infrared emissivity metal coating on the surface of the aerogel film to obtain a low infrared emissivity upper layer; Filling the phase change material into the aerogel film by melt filling or solution filling to obtain a phase change energy storage middle layer; preparing a single-sided patterned aerogel film, and depositing a thermal radiation reflecting metal coating on the patterned side of the single-sided patterned aerogel film to obtain a thermal radiation reflecting lower layer; The low infrared emissivity upper layer, the phase change energy storage middle layer, and the thermal radiation reflecting lower layer are assembled to obtain a thermal radiation inhibiting laminated structure.
17. The preparation method according to claim 16, characterized in that: The preparation method of the aerogel film comprises: preparing the aerogel film by subjecting the nanostructured unit dispersion or precursor to spin coating, blade coating, roll-to-roll or mold film formation, and then subjecting the nanostructured unit dispersion or precursor to sol-gel transformation, aging treatment, solvent replacement and drying treatment; wherein the material of the nanostructured unit dispersion or precursor is selected from any one or a combination of two or more of polyimide, cellulose, aramid, chitosan and silicon oxide.
18. The preparation method according to claim 17, characterized in that: The preparation method specifically comprises: obtaining a nanostructured unit dispersion having a nanostructured unit content of 0.1 wt% to 10 wt% by chemical stripping or small molecule polymerization.
19. The preparation method according to claim 17, characterized in that: The coagulation bath used in the sol-gel transition is selected from any one of water, ethanol, methanol, acetone, and hydrochloric acid aqueous solution, or a combination of two or more thereof.
20. The preparation method according to claim 17, characterized in that: The aging treatment time is 12 to 48 hours.
21. The preparation method according to claim 17, characterized in that: The solvent used in the solvent replacement is selected from any one of acetone, water, and tert-butyl alcohol aqueous solution or a combination of two or more thereof.
22. The preparation method according to claim 17, characterized in that: The drying treatment is selected from any one of atmospheric pressure drying, vacuum drying, freeze drying, and supercritical drying, or a combination of two or more thereof.
23. The preparation method according to claim 16, characterized in that: The preparation method comprises: depositing a metal material on the upper surface of the aerogel film by physical vapor deposition to form a metal coating with low infrared emissivity; wherein the metal material is selected from any one of gold, silver, aluminum, germanium, and zinc, or a combination of two or more thereof.
24. The preparation method according to claim 23, characterized in that: The preparation method comprises: utilizing any one of thermal evaporation, magnetron sputtering, vacuum ion plating or electron beam evaporation to deposit metal material on the upper surface of the aerogel film to form a metal coating layer with low infrared emissivity.
25. The preparation method according to claim 16, characterized in that: The melt filling method includes: heating the phase change material until it is completely melted, immersing the aerogel film into the molten phase change material, and immersing it for less than 24 hours to obtain a phase change energy storage middle layer.
26. The preparation method according to claim 25, characterized in that The immersion time is 1 to 24 hours.
27. The preparation method according to claim 26, characterized in that The immersion time is 4 to 12 hours.
28. The preparation method according to claim 16, characterized in that The solution filling method includes: immersing the aerogel film into the phase change material solution for less than 24 hours to obtain a phase change energy storage middle layer.
29. The preparation method according to claim 28, characterized in that The immersion time is 1 to 24 hours.
30. The preparation method according to claim 29, characterized in that The immersion time is 4 to 12 hours.
31. The preparation method according to claim 16, characterized in that: The method for preparing the single-sided patterned aerogel film comprises: designing a pattern, pre-setting the pattern into a printing program when using a 3D printing method, and obtaining a single-sided patterned aerogel film by freezing 3D printing or light-curing 3D printing technology on a nanostructured unit dispersion; then transferring the dispersion to a coagulation bath, and preparing a single-sided patterned aerogel film by sol-gel transformation, solvent replacement, aging treatment and drying treatment; Alternatively, when using the mold molding method, the nanostructured unit dispersion is injected into a mold with a pattern, and then transferred to a coagulation bath, and subjected to sol-gel transition, solvent replacement, aging treatment, drying treatment and demolding to obtain a single-sided patterned aerogel film.
32. The preparation method according to claim 31, characterized in that: The pattern is selected from any one of a honeycomb structure, a lattice structure, and a curved arrangement structure.
33. The preparation method according to claim 16, characterized in that: The preparation method comprises: depositing a metal material on the patterned side of the single-sided patterned aerogel film by physical vapor deposition to form a thermal radiation reflective metal coating; wherein the metal material is selected from any one of gold, silver, aluminum, germanium, and zinc, or a combination of two or more thereof.
34. The preparation method according to claim 33, characterized in that: The preparation method comprises: using any one of thermal evaporation, magnetron sputtering, vacuum ion plating or electron beam evaporation to deposit a metal material on the patterned side of the single-sided patterned aerogel film to form a thermal radiation reflective metal coating.
35. Application of the thermal radiation suppression laminate structure according to any one of claims 1 to 15 in the fields of heat insulation, energy storage, infrared penetration prevention or infrared detection resistance.
Citation Information
Patent Citations
Infrared stealth composite material with sandwich structure
CN112937029A
A Janus flexible composite film for intelligent radiative thermal control and its preparation method
CN113276510B
Thermal barrier / infrared low-emissivity integrated coating based on fluorescent sublayer and preparation method thereof
CN113403566A
Invisible patch
CN114179466A
Lightweight flexible bending-resistant target characteristic control composite material and preparation method thereof
CN114193850A