A plasmon-enhanced Raman spectroscopy method for characterizing SEI formation and evolution
By applying the plasmon-enhanced Raman spectroscopy method in lithium batteries, using PERS substrate combined with in-situ electrochemical Raman technology, the problem of difficult tracking of SEI formation and evolution process is solved, and accurate real-time monitoring and in-depth monitoring of SEI is achieved analyze.
Patent Information
- Application Number
- CN202211421483.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-14
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-11-14
AI Technical Summary
The prior art is difficult to comprehensively track and detect the formation and evolution process of SEI in lithium batteries, especially when operating in non-aqueous electrolytes, where there are problems of signal detection difficulties and information limitations.
Using the plasmon-enhanced Raman spectroscopy method, the nanostructured metal substrate with SERS activity is prepared and core-shell nanoparticles are formed to form a PERS substrate. Combined with in situ electrochemical Raman technology, high spatial and temporal resolution of SEI is achieved. and non-destructive testing.
It realizes accurate real-time monitoring of SEI, can have an in-depth understanding of the formation and evolution mechanism of SEI, has high Raman enhancement factor and sub-nanometer spatial resolution, and is suitable for in-situ characterization of different electrolyte systems.
Smart Images

Figure CN115656140B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of surface interface characterization and spectral characterization of lithium battery systems, and in particular to a plasmon enhanced Raman spectroscopy method for characterizing SEI formation and evolution processes. Background Art
[0002] In lithium battery systems, the negative electrode / electrolyte interface reaction has an important influence on the electrochemical performance of the battery. In particular, the formation of the solid electrolyte interface (SEI) at the interface can directly affect the electrochemical behavior of lithium metal deposition-dissolution, thereby determining the cycle efficiency and stability of the battery (D.Lin, Y.Liu and Y.Cui, Nat Energy, 2017, 12, 194-206; H.Wu, H.Jia, C.Wang, JGZhang and W.Xu, Adv Energy Mater, 2020, 11, 2003092). Therefore, the study of the formation of SEI and its chemical composition and structural evolution during charging and discharging has always been the core issue and hot direction of lithium battery system research. For decades, people have used various surface and interface characterization methods combined with theoretical simulations to conduct extensive research on the composition and structure of SEI, and have formed a preliminary understanding (E.Peled and S.Menkin, JElectrochem Soc, 2017, 164, A1703-A1719). However, SEI has diverse components, complex structures and dynamic changes, and a comprehensive and accurate understanding of SEI is still lacking. Therefore, it is urgent to develop in-situ characterization methods with high temporal and spatial resolution and non-destructiveness to conduct in-depth analysis of the formation and dynamic evolution mechanism of SEI.
[0003] Compared with other characterization techniques, electrochemical Raman spectroscopy has a very powerful and unique advantage in in-situ analysis of conventional electrode / electrolyte interface processes. However, SEI thickness is generally only a few nanometers to a few hundred nanometers, and conventional Raman signals are weak and relatively difficult to detect, so surface enhanced Raman spectroscopy (SERS) is needed to analyze it. There are currently a few reports on the use of SERS technology to study the composition and structure of SEI (MJPiernas- A.Tornheim, S.Trask, Z.Zhang and I.Bloom, Chem Commun, 2021, 57, 2253-2256). However, according to the electromagnetic effect mechanism, the electromagnetic field in SERS technology is limited to a few nanometers in the hot spot area. Therefore, this technology can only provide limited SEI composition and structure information near the corresponding hot spot, and cannot fully track and detect the formation and evolution of SEI. In 2010, the applicant's research group invented shell-isolated nanoparticle enhanced Raman spectroscopy, abbreviated as SHINERS (JFLi, YFHuang, Y.Ding, ZL Yang, SBLi, XSZhou, FRFan, W.Zhang, ZYZhou, DYWu, B.Ren, ZLWang, ZQTian, Nature 2010, 464, 392-395). The principle of SHINERS is to coat the surface of metal nanoparticles with SERS activity with an inert ultra-thin shell layer to form a core-shell structure, which not only retains the SERS activity of the core particles, but also avoids direct contact with the species to be measured. This core-shell structure particle can be spread on the surface of any substrate for interface process tracking, ensuring that the collected Raman signal comes entirely from the reaction of the substrate. However, due to the complexity of operation in non-aqueous electrolytes, there are few reports on the use of SHINERS to study the negative electrode SEI of lithium battery systems. In short, there is a lot of room for development in the use of SERS and SHINERS to study the negative electrode / electrolyte interface process, which deserves in-depth exploration and improvement. Summary of the invention
[0004] The purpose of the present invention is to solve the above problems in the prior art and to provide a plasmon enhanced Raman spectroscopy method with high temporal and spatial resolution and in-situ non-destructiveness for characterizing the formation and evolution process of SEI, which can reveal the formation and evolution mechanism of SEI at the molecular level.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] A plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution process of SEI comprises the following steps:
[0007] (1) Preparation of nanostructured metal substrates with SERS activity and shell-isolated core-shell nanoparticles;
[0008] (2) assembling the shell-isolated core-shell nanoparticles prepared in step (1) onto a nanostructured metal substrate having SERS activity to form a coupled substrate having plasmon enhanced activity, referred to as a PERS substrate;
[0009] (3) Assembling the PERS substrate obtained in step (2) into an airtight Raman electrolytic cell, injecting an electrolyte therein, using the PERS substrate as a working electrode, and subjecting it to electrochemical control so that the electrolyte reacts on the PERS substrate to form SEI, while using in situ electrochemical Raman for tracking detection, that is, implementing a plasmon enhanced Raman spectroscopy method based on the PERS substrate to characterize the SEI formation and evolution process.
[0010] Preferably, the material of the nanostructured metal substrate with SERS activity in step (1) is copper, lithium, gold, silver or nickel.
[0011] Preferably, the configuration of the nanostructured metal substrate with SERS activity in step (1) is a flat foil, a three-dimensional mesh, a three-dimensional foam or a three-dimensional cylinder.
[0012] Preferably, the shell-isolated core-shell nanoparticles in step (1) are at least one of Au@SiO2, Au@Al2O3, Ag@SiO2, and Ag@Al2O3.
[0013] Preferably, the particle size of the shell-isolated core-shell nanoparticles in step (1) is 50 to 200 nm.
[0014] Preferably, the configuration of the airtight Raman electrolytic cell in step (3) can be a two-electrode system, namely, comprising a working electrode and a counter electrode; or a three-electrode system, namely, comprising a working electrode, a counter electrode and a reference electrode.
[0015] Preferably, the electrolyte in step (3) can be an aqueous electrolyte, and generally, aqueous lithium-ion batteries, aqueous zinc-ion batteries, aqueous zinc-air batteries and the like suitable electrolytes can be used; it can also be a non-aqueous electrolyte, and generally, non-aqueous lithium-ion batteries, lithium-sulfur batteries, lithium-air batteries, lithium-mediated nitrogen reduction reactions and the like suitable electrolytes can be used.
[0016] Preferably, the electrochemical control in step (3) is at least one of constant potential polarization, constant current polarization, variable potential polarization, and variable current polarization.
[0017] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0018] (1) The Raman enhancement factor of the PERS substrate in the present invention is as high as 10 10 , the spatial resolution is sub-nanometer, which can effectively enhance the Raman signal of SEI;
[0019] (2) The PERS substrate in the present invention has the characteristic of depth sensitivity, and can accurately detect the components and structures of SEIs of different thicknesses and at different depths of SEI. That is, the nanostructured metal substrate with SERS activity can detect the composition and structural information of the inner side of SEI at the initial stage of formation, and the nanostructured metal substrate with SERS activity coupled with the shell-isolated core-shell nanoparticles can detect the composition of the outer side of SEI and the changes in the composition and structure of SEI at a later stage. In short, the PERS substrate can be used to track the film formation process of SEI from the inside out and from the bottom up, and fully understand the formation and evolution mechanism of SEI.
[0020] (3) The plasmon-enhanced Raman spectroscopy method based on the PERS substrate in the present invention can perform accurate real-time and non-destructive detection of SEI;
[0021] (4) The plasmon enhanced Raman spectroscopy method based on PERS substrate in the present invention can meet the in-situ characterization of SEI film formation process in different electrolyte systems and has wide applicability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Flowchart for characterizing SEI using plasmon-enhanced Raman spectroscopy based on PERS substrate.
[0023] Figure 2 This is a scanning electron microscope image of the nano copper foil substrate.
[0024] Figure 3 This is the Raman spectrum of pyridine adsorbed on the nano copper foil substrate and the flat copper foil substrate.
[0025] Figure 4 Transmission electron microscopy image of shell-isolated core-shell Au@SiO2 nanoparticles.
[0026] Figure 5 This is a scanning electron micrograph of the PERS substrate.
[0027] Figure 6 Raman spectra of the formation and evolution of SEI in LiTFSI / DME-DOL electrolyte characterized by plasmon-enhanced Raman spectroscopy based on PERS substrate. DETAILED DESCRIPTION
[0028] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer and more understandable, the present invention is further described in detail in combination with the embodiments and drawings. The following specific embodiments are only preferred embodiments of the present invention, so the scope of the implementation of the present invention cannot be limited thereto, that is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope covered by the present invention.
[0029] Example 1
[0030] The present invention provides a plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution process of SEI. The method flow chart is shown in Figure 1 , including the following steps:
[0031] (1) Preparation of nanostructured metal substrates with SERS activity and shell-isolated core-shell nanoparticles;
[0032] This example takes the preparation of nano copper foil with SERS activity as an example:
[0033] A copper foil with a diameter of 2 mm was immersed in a 0.1M KCl aqueous solution, and the copper foil was used as a working electrode, the foil was used as a counter electrode, and a saturated calomel electrode was used as a reference electrode. The copper foil working electrode was treated by an electrochemical oxidation-reduction cycle method: the oxidation potential was controlled at 0.4 V, and the duration was 10 to 30 s; the reduction potential was controlled at -0.4 V, and the duration was 10 to 30 s; the number of cycles was 2 to 20 times; after the electrochemical oxidation-reduction cycle, the copper foil working electrode was rinsed with deionized water to remove the residual solution, and then dried with high-purity nitrogen and dried in a vacuum drying oven to obtain a nano copper foil substrate with SERS activity; Figure 2 This is a scanning electron microscope image of the copper foil surface after electrochemical oxidation-reduction cycle treatment. It can be seen that spherical nanostructures are formed on the copper foil surface after treatment. In order to investigate the SERS activity of the nano copper foil substrate, pyridine was used as a probe molecule for SERS detection. The results are shown in Figure 2. Figure 3 As shown, it can be seen that compared with the flat copper foil that has not been treated by electrochemical oxidation-reduction cycling, a strong pyridine analysis signal is detected on the copper foil substrate with spherical nanostructures on the surface, indicating that the nano copper foil substrate has strong SERS activity.
[0034] This example takes the preparation of Au@SiO2 nanoparticles as an example:
[0035] 200 mL of 0.01% chloroauric acid aqueous solution was stirred and heated to boiling, and 1.4 mL of 1% sodium citrate aqueous solution was quickly added, and the mixture was heated to reflux for 0.5 to 1 h, and then the heating was stopped and the mixture was cooled in air to obtain an Au nanoparticle sol having an average particle size of about 60 nm; 30 mL of the aforementioned Au nanoparticle sol was placed in a round-bottom flask, and 0.4 mL of 1 mM 3-aminopropyltrimethoxysilane aqueous solution was added, and after stirring for 10 to 15 min, 3.2 mL of 0.54% sodium silicate aqueous solution was added and continued to stir for 5 to 10 min, and then the round-bottom flask was transferred to a boiling water bath and heated and stirred for 15 to 60 min, and after cooling, Au@SiO2 nanoparticles having a SiO2 shell thickness of about 2 nm were obtained; the transmission electron microscope image of the prepared shell-isolated core-shell Au@SiO2 nanoparticles is shown in FIG. Figure 4 As shown;
[0036] (2) assembling the shell-isolated core-shell nanoparticles prepared in step (1) onto a nanostructured metal substrate having SERS activity to form a coupled substrate having plasmon enhanced activity, referred to as a PERS substrate;
[0037] Take 0.05-0.2 mL of the aforementioned shell-isolated core-shell Au@SiO2 nanoparticles and drop them on a nano copper foil substrate with SERS activity. After fully removing water and drying in a vacuum drying oven, a coupling substrate with plasmon enhancement activity, namely a PERS substrate, can be obtained. The scanning electron microscope image of the PERS substrate is shown in FIG. Figure 5 As shown in the figure, the enhancement ability of the PERS substrate was calculated using the finite element method, and the results showed that the Raman enhancement factor of the PERS substrate was as high as 10 10 , the spatial resolution is sub-nanometer, which can effectively enhance the Raman signal of SEI.
[0038] (3) Assembling the PERS substrate obtained in step (2) into an airtight Raman electrolytic cell, injecting an electrolyte therein, using the PERS substrate as a working electrode, and subjecting it to electrochemical control so that the electrolyte reacts on the PERS substrate to form SEI, while using in situ electrochemical Raman for tracking detection, that is, implementing a plasmon enhanced Raman spectroscopy method based on the PERS substrate to characterize the SEI formation and evolution process.
[0039] Specifically, this embodiment uses a plasmon enhanced Raman spectroscopy method based on a PERS substrate to characterize the formation and evolution of SEI in the LiTFSI / DME-DOL electrolyte:
[0040] The aforementioned PERS substrate was assembled into an airtight Raman electrolytic cell in an argon atmosphere glove box, with the PERS substrate as the working electrode, the lithium sheet as the counter electrode, and the lithium wire as the reference electrode; the ether electrolyte LiTFSI / DME-DOL was injected into the aforementioned Raman electrolytic cell; variable potential polarization control was applied to the aforementioned PERS working electrode to reduce the electrolyte on the PERS working electrode, and in-situ Raman spectroscopy was used for tracking detection: the laser wavelength was 785 nm, the laser power was 0.3 mW, and the acquisition time was 60 s; the aforementioned process was used to characterize the formation and evolution process of SEI.
[0041] Figure 6 The Raman spectrum of the formation and evolution of SEI in LiTFSI / DME-DOL electrolyte is characterized by the plasmon enhanced Raman spectroscopy method based on PERS substrate. The thickness of SEI in this system is about 10-15nm. It can be seen that as the potential changes, the characteristic peaks of each SEI component appear in the spectrum ( Figure 6This indicates that the PERS-based plasmon-enhanced Raman spectroscopy method can monitor the formation of the SEI and the composition and structural characteristics at different depths in real time and non-destructively.
[0042] Example 2
[0043] A PERS substrate is prepared according to the method shown in steps (1) to (2) in Example 1; the aforementioned PERS substrate is assembled into an airtight Raman electrolytic cell in an argon atmosphere glove box, with the PERS substrate as a working electrode, a lithium sheet as a counter electrode, and a lithium wire as a reference electrode; a carbonate electrolyte LiDFOB-LiBF4 / DEC-FEC is injected into the aforementioned Raman electrolytic cell; a constant current polarization control is applied to the aforementioned PERS working electrode to reduce the electrolyte on the PERS working electrode, and at the same time, in-situ Raman spectroscopy is used for tracking detection: the laser wavelength is 785nm, the laser power is 0.3mW, and the acquisition time is 60s; the aforementioned process is used to characterize the formation and evolution of SEI. The thickness of SEI formed by the carbonate electrolyte LiDFOB-LiBF4 / DEC-FEC system is about 30-40nm. The plasmon enhanced Raman spectroscopy method based on the PERS substrate can monitor the formation and evolution of SEI of different electrolyte systems and different thicknesses in real time and non-destructively.
[0044] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI, characterized in that The following steps are involved: (1) Preparation of nanostructured metal substrates with SERS activity and shell-isolated core-shell nanoparticles; (2) assembling the shell-isolated core-shell nanoparticles prepared in step (1) onto a nanostructured metal substrate having SERS activity to form a coupled substrate having plasmon enhanced activity, referred to as a PERS substrate; (3) Assembling the PERS substrate obtained in step (2) into an airtight Raman electrolytic cell, injecting an electrolyte therein, using the PERS substrate as a working electrode, and subjecting it to electrochemical control so that the electrolyte reacts on the PERS substrate to form SEI, while using in-situ electrochemical Raman for tracking detection, that is, implementing a plasmon enhanced Raman spectroscopy method based on the PERS substrate to characterize the SEI formation and evolution process; The method for preparing a nanostructured metal substrate with SERS activity comprises the following steps: immersing the substrate in a KCl aqueous solution, using the substrate as a working electrode, a foil as a counter electrode, and a saturated calomel electrode as a reference electrode, and treating the substrate working electrode by an electrochemical oxidation-reduction cycle method: the oxidation potential is controlled at 0.4 V, and the duration is 10-30 s; the reduction potential is controlled at -0.4 V, and the duration is 10-30 s; the number of cycles is 2-20 times; after the electrochemical oxidation-reduction cycle, the substrate working electrode is rinsed with deionized water to remove residual solution, and then dried with high-purity nitrogen and dried in a vacuum drying oven to obtain a nanostructured metal substrate with SERS activity.
2. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 1, characterized in that: The material of the nanostructured metal substrate with SERS activity in step (1) is copper, lithium, gold, silver or nickel.
3. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 1, characterized in that: The configuration of the nanostructured metal substrate with SERS activity in step (1) is a flat foil, a three-dimensional mesh, a three-dimensional foam or a three-dimensional cylinder.
4. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 1, characterized in that: The shell-isolated core-shell nanoparticles in step (1) are at least one of Au@SiO2, Au@Al2O3, Ag@SiO2, and Ag@Al2O3.
5. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 1, characterized in that The particle size of the shell-isolated core-shell nanoparticles in step (1) is 50-200 nm.
6. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 1, characterized in that: The configuration of the airtight Raman electrolytic cell in step (3) is a two-electrode system, namely, comprising a working electrode and a counter electrode; or a three-electrode system, namely, comprising a working electrode, a counter electrode and a reference electrode.
7. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 1, characterized in that: The electrolyte in step (3) is an aqueous electrolyte or a non-aqueous electrolyte.
8. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 7, characterized in that: The aqueous electrolyte is an electrolyte suitable for aqueous lithium ion batteries, aqueous zinc ion batteries, and aqueous zinc-air batteries.
9. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 7, characterized in that: The non-aqueous electrolyte is an electrolyte suitable for non-aqueous lithium-ion batteries, lithium-sulfur batteries, lithium-air batteries, and lithium-mediated nitrogen reduction reactions.
10. The plasmon enhanced Raman spectroscopy method for characterizing the formation and evolution of SEI according to claim 1, characterized in that: The electrochemical control in step (3) is at least one of constant potential polarization, constant current polarization, variable potential polarization, and variable current polarization.
Citation Information
Patent Citations
Silver nanodendrite surface enhanced Raman scattering (SERS) substrate, and preparation method and application thereof
CN102181891A