A steel slag counterweight and preparation method thereof

Through liquid slag processing technology synchronized with steelmaking, the problems of resource waste and pollution in the use of steel slag are solved, the preparation of high-density weight blocks is realized, the utilization efficiency and added value of steel slag are improved, and the development of the steel industry is promoted. sustainable development.

CN115959885BActive Publication Date: 2024-10-11姚胜南
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211447566.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-10-11
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

The existing steel slag utilization method leads to resource waste and environmental pollution, and has low added value, making it impossible to achieve large-scale and high-value utilization of bulk solid waste.

Method used

Using a method that is synchronized with steelmaking, liquid slag is used to melt other waste slag materials to make counterweights. Through preheating and casting technology, high-density and dense steel slag counterweights are formed, avoiding high-energy-consuming processes such as water quenching and crushing. , directly utilizing steel slag and other waste slag in the steelmaking process.

Benefits of technology

It effectively reduces the amount of solid waste, reduces energy consumption and environmental pollution, improves the utilization rate and added value of steel slag, and achieves the sustainable development of the steel industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115959885B_ABST
    Figure CN115959885B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of counterweight manufacturing, and discloses a slag counterweight and a preparation method thereof. A hollow counterweight structure is made of molten iron, and a layer of solid slag slurry is coated on the side wall while hot. The slurry on the inner wall is dried and solidified on the inner surface by the heat of the hollow counterweight structure itself to form a slurry layer of a certain thickness. In order to improve the bonding strength of the slag core block and reduce the possibility of cracking, an appropriate gelling agent is added to the liquid slag molten in the ladle and mixed evenly, and the evenly mixed liquid slag is poured into the hollow counterweight structure. By applying compressive stress, the compactness of the casting body is improved. The present invention can not only fully utilize the liquid slag produced by steelmaking, but also add the existing waste slag and other waste slag in the steel plant to the production of the counterweight, which not only avoids the emergence of new solid waste slag, but also reduces the waste slag inventory, reduces environmental pollution, and saves a lot of processing costs, energy and land occupation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel slag utilization, and in particular relates to a steel slag counterweight and a preparation method thereof. Background Art

[0002] Steel is the backbone of the national industry and an important part of the national economy. As a major energy and water consumer, steel companies have always been the eternal theme of development, reducing costs, increasing efficiency, and achieving sustainable development. Therefore, in a sense, the competition among steel companies is not only a competition in technology, but also a competition to improve the efficiency of resource and energy utilization.

[0003] Steel slag is solid waste discharged from converters, electric furnaces and other equipment during the steel smelting process. The emission volume is about 10% to 15% of crude steel. The main chemical components are oxides such as calcium, magnesium, silicon, iron, aluminum, and manganese. The main mineral phases are dicalcium silicate, tricalcium silicate, calcium magnesium olivine, and RO (metal oxide) phases, as well as a small amount of free metallic iron, calcium oxide, etc. With the development of my country's steel industry, the continuous increase in steel production, and the output of steel slag is also increasing. According to data, China's steel slag production has reached 160 million tons in 2020, an increase of 7.38% year-on-year. If it is not effectively processed and utilized, it will cause a large amount of dumping, occupy farmland, waste resources, and pollute the environment. At present, the cumulative stockpile of steel slag is nearly 2 billion tons, covering an area of ​​about 200,000 mu, resulting in a large waste of land resources and serious environmental risks.

[0004] At present, the commonly used steel slag treatment processes include hot stuffing method, water quenching method, hot pouring method, air quenching method and drum method.

[0005] 1. Hot stuffy method: using the sensible heat of high-temperature molten slag, the temperature stress generated when it meets water and the hydrolysis of free calcium oxide to crack the slag;

[0006] Advantages: The process is simple to operate, can process high-basicity steel slag, has good slag-iron separation effect, has high steel slag activity, good stability, and can process solid slag;

[0007] Disadvantages: The particle size is not uniform enough, the processing cycle is long, and the subsequent crushing processing volume is large.

[0008] 2. Water quenching method: The high-temperature molten slag flows out slowly, and is cut and crushed by high-pressure water when falling. The slag is quenched and contracted to form stress concentration and break. At the same time, heat exchange is carried out to granulate the slag in the water curtain.

[0009] Advantages: fast slag discharge, simple process, small footprint, low investment cost, small particle size of treated slag and stable performance;

[0010] Disadvantages: Improper operation during slag water quenching can easily cause explosion, the particle size uniformity of the steel slag is relatively poor, and only liquid slag can be processed.

[0011] 3. Hot pouring method: When the slag exceeds the quenchable temperature, a large amount of water is sprayed on the slag. The temperature stress formed will break the slag, and the hydration of free calcium oxide will further break the slag.

[0012] Advantages: fast slag discharge speed, short cooling time, conducive to mechanized production, large processing capacity; high slag activity; high production efficiency;

[0013] Disadvantages: large equipment loss, large floor space, large amount of dust and steam during crushing, which is not good for the environment and energy saving. Large amount of slag processing, poor stability of steel slag.

[0014] 4. Wind quenching method: The slag pot is tilted, and the molten slag is blown away by the ejected air and broken into particles. The heat emitted by the high-temperature air and the particle slag is recovered in the hood boiler and the slag particles are captured.

[0015] Advantages: safe and reliable, simple process, low investment, large processing capacity, complete one-time granulation, low water consumption, etc.

[0016] Disadvantages: There are great requirements for the fluidity of steel slag. Due to the high basicity and viscosity of steel slag, the steel slag that can be treated with wind quenching generally does not exceed 50% of the total steel slag, and the rest of the steel slag must be treated using other methods.

[0017] 5. Drum method: The slag enters the drum at a suitable flow rate. Under the action of centrifugal force and spray water, the slag is dispersed by water and condensed into small pieces to be collected. Condensation, crushing and separation of slag and steel are completed in the drum at the same time;

[0018] Advantages: (1) The slag has a fine particle size, with about 90% of the particles being less than 10 mm. The scrap steel and slag are completely separated, which is very beneficial for scrap steel recycling; (2) The free calcium oxide is low; (3) The production process is short, the land occupation is small, and the production efficiency is high; (4) There is little dust, and the steam is discharged through the chimney, which has good environmental protection performance; (5) The degree of automation is high and the labor intensity is low.

[0019] Disadvantages: (1) The equipment is complex and difficult to maintain; (2) The slag must have good fluidity; solid slag and slag with poor fluidity cannot be processed; (3) The operating cost is relatively high.

[0020] It can be seen from the above treatment methods that the existing steel slag treatment requires cooling and crushing the steel slag with a large amount of water or wind, but the crushed particle size is uneven, and it is easy to cause dust, wastewater pollution, etc., and the preheating of the steel slag is completely useless.

[0021] In the United States, 2 / 3 of the slag is used as a flux for ironmaking each year, which is directly added to the blast furnace or added to sintered ore and recycled within the steel plant. Among the components of steel slag, except for useless silicon and harmful phosphorus, calcium, iron, magnesium and manganese (accounting for 80% of the total amount of steel slag) are all utilized. However, steel slag with high sulfur and phosphorus content as a flux will reduce the utilization coefficient of blast furnace ironmaking and increase the coke ratio. France, Germany, Canada and other countries use this type of steel slag as railway ballast and road materials. The method is to store the processed steel slag for 3 to 6 months and use it after the volume stabilizes. This type of steel slag is widely used in the cushion layer and structural layer of road subgrade, and is especially suitable for use as aggregate of asphalt mixture to pave the road surface layer. Road construction with steel slag has the advantages of high strength, good abrasiveness and anti-skid properties, good durability and low maintenance costs.

[0022] Western European countries have a long history of using high-phosphorus steel slag as fertilizer. The calcium, silicon, manganese and trace elements in steel slag are all effective as fertilizers and can be applied to acidic soils as slag fertilizer.

[0023] All kinds of steel slag can be used as materials for filling pits and reclamation. China currently produces a small amount of steel slag cement. Converter steel slag is mixed with about 50% blast furnace granulated slag and about 10% gypsum to grind clinker-free steel slag cement, and about 15% cement clinker is used to replace steel slag to grind low-clinker cement. Some places in China use electric furnace steel slag to produce white steel slag cement. Japan and Germany use steel slag as cement raw material to roast ferrite cement, which can save energy. In addition, steel slag can also be used to make bricks, tiles, carbonized building materials, etc.

[0024] Since the iron content in steel slag is about 20%, its density is about 3.2-3.6g / cm3. There are also application cases of using steel slag as counterweight in the prior art. At present, there are many concrete blocks for counterweight on the market, which are mainly used in elevators, engineering machinery, electrical appliances and other fields. Its role is to balance and save energy. Taking the counterweight required for elevators as an example, most of them are made of cast iron, but the cost of cast iron is relatively high; Chinese invention patent application CN101417763A discloses a counterweight brick for elevators, which is filled with barite (or metal ores such as hematite and pyrite) and cement, mainly because the price of the filled counterweight is much lower than that of cast iron. However, barite has a disadvantage that its concrete workability is very poor, and it is difficult to obtain uniform quality and compact concrete, which will affect the performance of the machine. The elevator counterweight has a slightly uneven quality, which will cause its center of gravity to shift. In the specific use process, especially for ultra-high-speed elevators, it will affect its service life; and due to the shift in the center of gravity, the counterweight may wear the elevator counterweight track. In addition, this type of counterweight uses solid steel slag from the yard. When using it, the solid steel slag needs to be crushed to a certain degree, and then mixed with cement, sand, and water to solidify into high-density concrete for use as counterweight. It is easy to form loose shapes, which may cause the counterweight block to fail to reach the weight required by the design, affecting the use effect, and even posing a safety hazard due to the weight not meeting the standard.

[0025] From the application of steel slag at home and abroad, we can see that the resource utilization of steel slag is showing a diversified trend. Various countries have developed unique steel slag products based on the actual composition and performance of steel slag. Japan mainly uses steel slag in composite roadbed materials, marine fields, purification materials and industrial fertilizers, while Europe uses steel slag in industries such as building materials, wastewater treatment and filler treatment.

[0026] Under the current steel slag utilization model, the development and application of domestic steel slag resource technology has achieved certain results, and the effective utilization of steel slag has been achieved on a certain scale. However, in general, the utilization rate of steel slag in my country is still not high, and there are still constraints on the stable and reliable application of steel slag. For example, when steel slag is used as a metallurgical raw material, the large fluctuation of steel slag composition brings certain difficulties to production control; when steel slag is used as a building material, it cannot completely replace cement due to its expansibility; steel slag phosphate fertilizer is difficult to promote due to its high application cost and high alkalinity; steel slag as a wastewater treatment adsorbent is still difficult to put into actual industrial application; steel slag preparation of microcrystalline glass is still in the research stage. Moreover, all applications of steel slag require a large amount of water to cool, crush and pulverize the steel slag produced by steelmaking, and then apply it in the fields of construction, counterweights, fertilizers, etc. The preparation process wastes a lot of cooling water and electricity, causing environmental pollution and energy waste, and the added value generated is very low.

[0027] Through the above analysis, the problems and defects of the prior art are as follows:

[0028] The added value generated by the existing methods of utilizing steel slag is very low, and it is impossible to achieve large-scale and high-value utilization of bulk solid waste.

[0029] Compared with iron ore smelting, melting and recycling of scrap steel is a green resource that is more energy-saving and environmentally friendly. However, the current scrap steelmaking ratio is only about 11%. Strengthening the large-scale and high-value utilization of bulk solid waste has become a key common problem that the industry urgently needs to solve. Therefore, further research on the comprehensive utilization of steel slag and scrap steel, especially expanding its large-scale consumption and high-value-added utilization in the non-building materials field, is of great significance and application prospects for achieving sustainable development of the steel industry. Summary of the invention

[0030] In view of the problems existing in the prior art, the present invention provides a steel slag counterweight and a preparation method thereof.

[0031] The present invention is achieved in that a method for preparing a slag counterweight comprises:

[0032] Step 1: Design the proportion of cast iron and steel slag, the hollow structure of cast iron counterweight and the corresponding drawings of steel slag core block according to the density of counterweight.

[0033] Step 2, pouring molten iron to cast a hollow counterweight cavity 1;

[0034] Step 3: spray a certain amount of crushed steel slag slurry mixed with a gelling agent into the counterweight cavity to form a slurry layer 2 of a certain thickness on the inner wall;

[0035] Step 4, drying the counterweight cavity and the slurry layer and preheating them to a certain temperature;

[0036] Step 5, pouring the molten slag produced by steelmaking into a certain amount of preheated stock slag or other waste slag, and completely melting it to form a molten mixed melt of new and old slag;

[0037] Step 6, pouring the molten mixed solution of new and old steel slag from the opening end of the preheated hollow counterweight cavity into the formed counterweight cavity, so that the interior is filled with steel slag core blocks 3;

[0038] Step seven, after the casting is completed, the upper end is sealed with a steel plate 4 and a certain pressure is applied and maintained for a certain period of time, so that the cover plate is fully in contact with the molten slag and thus fused together. The application of compressive stress also improves the density of the slag core block 3.

[0039] Furthermore, the counterweight cavity 1 made by the molten iron in step 2 is used to adjust the density of the counterweight block.

[0040] Furthermore, the slurry layer 2 of step three is formed by crushing the existing solid steel slag and stirring it with a gelling agent; the thickness of slurry layer 2 should be such that the cast liquid steel slag can only melt a small amount of the inner wall of the cast iron cavity, so that the steel slag core block 3 in the inner cavity becomes one with the cast iron cavity.

[0041] Furthermore, the gelling agent in step three is one or a mixture of one or more of basic magnesium sulfate cement powder, clay, kaolin, waste porcelain powder, porcelain clay, titanium dioxide, water glass, fly ash and alumina.

[0042] Furthermore, the preheating temperature of step 4 is 400-1200 degrees.

[0043] Furthermore, the amount of stock slag or other waste slag added in step five is between 20% and 50% of the weight of the slag core block, and the preheating temperature should be able to completely melt the stock slag or other waste slag into molten steel after pouring into the molten slag produced by steelmaking.

[0044] Furthermore, other waste residues in step five include red mud, copper slag, ceramic waste residue, etc.

[0045] Furthermore, at the end of the casting in step seven, the pressure applied by the steel plate 4 at the upper end thereof can adopt an alternating load, thereby further improving the compactness of the molten steel slag and the quality of its bonding with the molten steel slag.

[0046] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of this technical solution are as follows:

[0047] The implementation of the present invention is carried out simultaneously with steelmaking, and liquid molten slag is used to melt other waste slag materials to make counterweights, which can not only avoid the emergence of solid waste such as new steel slag after steelmaking, but also add the existing waste steel slag and other waste slag to the production of counterweights, which can effectively reduce the inventory of waste steel slag, red mud, copper slag, ceramic slag, etc.

[0048] In the production of this counterweight block, the waste heat of molten steel slag is fully utilized to preheat and melt the existing steel slag, and the treatment of waste steel slag no longer requires water quenching, crushing with a crusher, grinding with a ball mill, and other energy-consuming and wastewater-producing processes as in the past, which reduces environmental pollution and saves a lot of processing costs and land occupation. By adding tempering and modifying components, the density of the steel slag counterweight block can be increased, and its bonding strength can also be improved, reducing the possibility of cracking.

[0049] Second, considering the technical solution as a whole or from the perspective of the product, the technical effects and advantages of the technical solution to be protected by the present invention are described in detail as follows:

[0050] Directly using liquid slag for preparation avoids the energy loss and environmental pollution caused by the need to use a large amount of water for cooling, crushing and stacking the molten slag;

[0051] The heat of liquid steel slag is used to directly melt the existing waste slag together and cast it into the required shape, avoiding the crushing, mixing, stirring, drying and sintering steps required in the existing preparation process and directly forming the required product.

[0052] The steel slag produced in the steelmaking process is directly utilized, completely avoiding the generation of new waste steel slag.

[0053] This solution can also make full use of solid waste components such as red mud, solid steel slag, solid copper slag, etc., thereby realizing the comprehensive utilization of multiple solid wastes.

[0054] The value of the counterweight block prepared by the present invention is far higher than that in the fields of construction applications, and it is a way to consume steel slag on a large scale and utilize it with high added value, which is of great significance and application prospects for achieving sustainable development of the steel industry.

[0055] Third, as auxiliary evidence of the inventiveness of the present invention, it is also reflected in the following important aspects:

[0056] (1) The expected benefits and commercial value of the technical solution of the present invention after transformation are as follows: Through the use of the present invention, not only can the generation of new steel slag be avoided, but also existing solid wastes such as steel slag, red mud, solid copper slag, and waste ceramics can be utilized, reducing the stock of steel slag and other solid wastes, and avoiding the large-scale land occupation and environmental pollution caused by steel slag. At present, the market price of counterweights is about 3,000-7,000 yuan / ton. Even if the average price of steel slag counterweights is 3,000 yuan / ton, my country can generate an output value of more than 30 billion yuan if it uses 10 million tons of steel slag every year.

[0057] (2) At present, the utilization of steel slag at home and abroad is to reuse it after the steel slag has formed a solid state, while the present invention utilizes the liquid slag in the steel smelting process, uses its high temperature to melt the existing solid waste to make them melt together, and then casts it into the cast iron cavity to form a weighted counterweight. The present invention fully utilizes various types of waste, such as steel slag, red mud, and copper slag, to achieve low energy consumption and large-scale application, filling the gap at home and abroad.

[0058] (3) The resource utilization of steel slag has always been a technical problem that both China and foreign countries have wanted to overcome. The present invention not only makes the resource utilization of steel slag possible, but also has a simple production process, fully utilizes the preheating of molten steel slag, has low energy consumption, and greatly reduces the pollution to the environment caused by the preparation process.

[0059] (4) The present invention will turn steel slag into a high value-added resource, thereby overcoming the technical prejudice that steel slag is a waste that is difficult to treat. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 is a flow chart of a method for preparing a steel slag counterweight provided by an embodiment of the present invention;

[0061] Figure 2 It is a rendering of the effects of different counterweights prepared by the method for preparing slag counterweights provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0062] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0063] In order to enable those skilled in the art to fully understand how to implement the present invention in detail, this section is an explanatory embodiment that expands and describes the technical solution.

[0064] like Figure 1 As shown, the method for preparing the steel slag counterweight provided in the embodiment of the present invention comprises:

[0065] Step 1, designing the proportion of cast iron and steel slag, the hollow structure of the cast iron counterweight and the corresponding drawings of the steel slag core block according to the density of the counterweight;

[0066] Step 2, pouring molten iron to cast a hollow counterweight cavity 1;

[0067] Step 3: spray a certain amount of crushed steel slag slurry mixed with a gelling agent into the counterweight cavity to form a slurry layer 2 of a certain thickness on the inner wall;

[0068] Step 4, drying the counterweight cavity and the slurry layer and preheating them to a certain temperature;

[0069] Step 5, pouring the molten slag produced by steelmaking into a certain amount of preheated stock slag or other waste slag, and completely melting it to form a molten mixed melt of new and old slag;

[0070] Step 6, pouring the molten mixed solution of new and old steel slag from the opening end of the preheated hollow counterweight cavity into the formed counterweight cavity, so that the interior is filled with steel slag core blocks 3;

[0071] Step seven, after the casting is completed, the upper end is sealed with a steel plate 4 and a certain pressure is applied and maintained for a certain period of time, so that the cover plate is fully in contact with the molten slag and thus fused together. The application of compressive stress also improves the density of the slag core block 3.

[0072] There are also application cases of using steel slag as counterweight in the prior art, but they all use cold steel slag, which needs to be crushed to a certain degree and then added to water, cement, sand and gravel for mixing and solidification.

[0073] The implementation of the present invention is carried out simultaneously with steelmaking, so that not only can steel slag be used to make counterweights to avoid the appearance of solid waste such as new steel slag after steelmaking, but also the existing waste steel slag in the steel plant can be added to the production of counterweights, which can reduce the stock of waste steel slag in the steel plant. In the production of this counterweight, the waste heat of molten steel slag is fully utilized to melt the steel slag and other solid substances, and the waste heat of steelmaking in the steel plant is used to preheat molten iron and steel slag, so that the treatment of waste steel slag no longer needs to be carried out by water quenching, crushing with a crusher, grinding with a ball mill, etc., which are both energy-consuming and wastewater-producing processes as in the past, reducing environmental pollution, saving a large amount of processing costs and land occupation, and adding a tempering modifier can improve the bonding strength of the steel slag counterweight and reduce the possibility of cracking. Due to the method of first casting molten iron or making the molten iron and the steel slag molten liquid fully uniform, the molten steel can be evenly distributed on one side of the entire counterweight, avoiding the uneven weight of the counterweight caused by uneven mixing of molten steel and steel slag. At the same time, the value of counterweight blocks is far higher than that in fields such as construction applications. It is a way to consume steel slag on a large scale and utilize it with high added value. It is of great significance and application prospects for achieving sustainable development of the steel industry.

[0074] In order to prove the creativity and technical value of the technical solution of the present invention, this section provides application examples of the technical solution on specific products or related technologies.

[0075] The method for preparing the steel slag counterweight provided in the embodiment of the present invention can be used to make various counterweights such as elevator counterweights, ship hull counterweights, and household appliance counterweights. Different counterweights have different requirements for density.

[0076] Implementation case 1: The density of molten iron is about 7.8×10 3 kg / m 3 The density of large steel slag is about 3.8×10 3 kg / m 3 In order to prepare a density of 6.0×10 3 kg / m 3 The left and right counterweights can be achieved by mixing 55% of the weight of the counterweight with 45% of the waste slag;

[0077] Implementation case 2: The density of molten iron is about 7.8×10 3 kg / m 3 The density of large steel slag is about 3.8×10 3 kg / m 3 In order to prepare a density of 5.0×10 3 kg / m 3The left and right counterweights can be achieved by mixing 30% of the weight of the counterweight with 70% of the waste slag;

[0078] Implementation case 3: The density of molten iron is about 7.8×10 3 kg / m 3 The density of large steel slag is about 3.8×10 3 kg / m 3 In order to prepare a density of 4.0×10 3 kg / m 3 The left and right counterweights are realized by mixing 10% of the weight of the counterweight with 90% of the waste slag;

[0079] From the calculation, the counterweights can meet the expected design density requirements. Even the high-density counterweights in the implementation case 1 also use 45% of the steel slag, and for the low-density counterweights, the utilization rate of the steel slag can reach 90% or even higher, thus fundamentally utilizing the steel slag in a resource-efficient manner, avoiding the generation of new solid waste in the steelmaking process, and also using existing solid waste in the production process, which also reduces the stock of solid waste.

[0080] The method provided in the embodiment of the present invention solves the defects of the prior art in the resource utilization of steel slag and achieves good results, as shown in the following table:

[0081] Current status of steel slag resource utilization

[0082]

[0083]

[0084]

[0085] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modification, equivalent substitution and improvement made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a steel slag counterweight, characterized in that: The preparation method of the steel slag counterweight comprises: Step 1, designing the proportion of cast iron and steel slag, the hollow structure of the cast iron counterweight and the corresponding drawings of the steel slag core block according to the density of the counterweight; Step 2, casting molten iron to form a hollow counterweight cavity; Step 3: spray a certain amount of crushed steel slag slurry mixed with a gelling agent into the counterweight cavity to form a slurry layer of a certain thickness on the inner wall; Step 4, drying the counterweight cavity and the slurry layer and preheating them to a certain temperature; Step 5, pouring the molten slag produced by steelmaking into a certain amount of preheated stock slag or other waste slag, and completely melting it to form a molten mixed melt of new and old slag; Step 6: pouring the molten mixed solution of new and old steel slag from the open end of the preheated hollow counterweight cavity into the formed counterweight cavity to fill the cavity and form a steel slag core block; Step 7: After the casting is completed, a steel plate is used to cover the upper end and a certain pressure is applied and maintained for a certain period of time, so that the cover plate is fully in contact with the molten slag and thus fused together. The compactness of the slag core block is also improved by applying compressive stress; The counterweight cavity made by the molten iron in step 2 is used to adjust the density of the counterweight block; The slurry layer in step three is formed by crushing the original solid steel slag and stirring and mixing it with a gelling agent, and its thickness should be such that the cast liquid steel slag can only melt a small amount of the inner wall of the cast iron cavity.

2. The method for preparing a steel slag counterweight according to claim 1, characterized in that: The gelling agent in step three is one or a mixture of basic magnesium sulfate cement powder, clay, kaolin, waste porcelain powder, porcelain clay, titanium dioxide, water glass, fly ash and alumina.

3. The method for preparing a steel slag counterweight according to claim 1, characterized in that: Step 4: The preheating temperature of the machine is 400-1200 degrees.

4. The method for preparing a steel slag counterweight according to claim 1, characterized in that: The amount of stock slag or other waste slag added in step five is between 20% and 50% of the weight of the slag core block, and the preheating temperature should be such that the stock slag can be completely melted after being poured into the molten slag produced by steelmaking.

5. The method for preparing a steel slag counterweight according to claim 1, characterized in that: The other waste residues in step five include red mud, copper residue and ceramic waste residue.

6. The method for preparing a steel slag counterweight according to claim 1, characterized in that: In step 7, at the end of casting, the pressure applied by the steel plate at the upper end adopts an alternating load.

7. A counterweight for elevators, ships, household appliances, etc., characterized in that: The elevator counterweight is prepared by the method for preparing a steel slag counterweight according to any one of claims 1 to 6.

Citation Information

Cited By

  • 3D printing balancing weight and preparation method thereof