A reprocessing method for high-nickel catalytic cracking balance agent

By forming a modified metal coating on the surface of the catalytic cracking balancer, combined with demetallization treatment, the problems of catalyst activity stability and product distribution optimization in high nickel environments are solved, and the effect of reducing dehydrogenation activity and hydrogen to methane ratio is achieved.

CN116020526BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111242844.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-25
Publication Date
2024-10-11
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

Existing catalytic cracking balancing agents are difficult to effectively reduce dehydrogenation activity and hydrogen-to-methane ratio in high-nickel environments, and conventional demetallization methods have problems of low efficiency and high safety.

Method used

The macromolecular complex metal loading method is used to form a modified metal coating on the surface of the catalyst. Through contact treatment with modified metal compounds such as Ti, Mn, Ba, etc., combined with demetallization and activation treatments, a catalyst containing a modified metal coating is formed. .

Benefits of technology

It significantly reduces the dehydrogenation coking activity of nickel, improves the activity stability and service life of the catalyst, and optimizes the distribution of catalytic cracking products, especially reducing the hydrogen yield and hydrogen to methane ratio.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000006106950000111
    Figure GHA0000006106950000111
Patent Text Reader

Abstract

A reprocessing method for a high-nickel catalytic cracking balance agent, comprising: (a) providing an FCC balance agent, optionally subjecting the FCC balance agent to a demetallization treatment and / or activation treatment; referred to as a first balance agent; (b) contacting the first balance agent obtained in step (a) with a compound containing a modified metal to form a coating on the surface of the first balance agent, thereby obtaining an FCC balance agent containing a modified metal coating; the modified metal is one or more of Ti, Mn, and Ba; and the contact treatment method is a macromolecular complex metal loading method. The revived catalyst obtained by the method of the present invention has good activity stability and can effectively reduce the hydrogen-methane ratio of heavy oil conversion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a reprocessing method for a catalytic cracking balance agent suitable for high nickel, and in particular to a balance agent processing method for improving nickel tolerance of heavy oil catalytic cracking. Background Art

[0002] Fluid catalytic cracking (FCC) technology has become an important means of secondary processing of heavy oil in the world today because of its low investment, strong adaptability to raw materials and simple operation, and catalytic cracking catalyst plays a key role in this process. With the increasing depletion of high-quality light crude oil resources worldwide and the increase in delayed coking capacity, refineries have been blending a large proportion of low-quality crude oil such as residual oil, coking wax oil and deasphalted oil in catalytic cracking units in order to increase efficiency, which has a serious impact on the stable operation of catalytic cracking units and the distribution of cracking products, and has put forward higher requirements on the performance of catalytic cracking catalysts.

[0003] Since residual oil feed usually contains pollutant metals such as Ni, V, Fe, Na, and Ca, heavy metals such as nickel and vanadium in the feed oil are continuously deposited on the catalyst surface during the use of catalytic cracking catalysts, causing certain poisoning effects on the catalysts. For example, Ni can induce dehydrogenation and significantly increase the yield of H2 and coke.

[0004] Conventional catalytic cracking balance agents contain about 1-4% rare earth oxide, 1000-6000 ppm V, 1000-8000 ppm Ni, 1000-8000 ppm Fe, Ca, Cu, etc. They were originally landfilled, but are also used to be mixed with building materials as fillers, or to pave asphalt or cement roads.

[0005] If the nickel content is too high, resulting in high hydrogen and coke yields, the balance agent needs to be revived to reduce the hydrogen-methane ratio. The revivification and reuse of FCC balance catalysts has been reported at home and abroad, mainly including acid washing, high-intensity magnetic separation, oxidation-chlorination-sulfurization, etc. Magnetic separation mainly uses magnetic force to distinguish the high-nickel iron and low-nickel iron particles in the balance agent, which consumes a lot of energy and has low separation efficiency; acid washing and alkaline washing are effective for removing vanadium, but inorganic acids and alkalis have basically no effective removal of nickel, and organic acids can remove up to 30% of nickel; oxidation-chlorination-sulfurization, such as the Demet method in the United States, uses gases such as H2S and HCl, and the demetallization effect can reach more than 70%, but it is dangerous and has high technical requirements;. The core of this resurrection method is that it can be directly used for post-treatment without demetallization to reduce the pollution of active nickel, and also achieve the effect of fixing vanadium, which is simple and convenient.

[0006] The existing acid washing and alkali elution metal removal processes often have limited nickel removal effects and are prone to destroying the crystallinity of the molecular sieve, which is not conducive to stabilizing the activity. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for resurrecting a catalytic cracking balancer (also called FCC balancer, or balancer for short) with a high nickel content, which can reduce the dehydrogenation activity of the resurrected catalyst.

[0008] The present invention provides a method for treating a high-nickel catalytic cracking balance agent, comprising:

[0009] (a) providing an FCC balance agent, and optionally subjecting the FCC balance agent to a demetallization treatment and / or an activation treatment; referred to as a first balance agent;

[0010] (b) contacting the first balance agent obtained in step (a) with a compound containing a modified metal to form a coating on the surface of the first balance agent, thereby obtaining an FCC balance agent containing a modified metal coating; the modified metal is one or more of Ti, Mn, and Ba; and the contact treatment method is a macromolecular complex metal loading method.

[0011] The contacting treatment of the first balance agent with the compound containing the modified metal is, for example, contacting the first balance agent with a complex solution containing the modified metal. The first balance agent is an FCC balance agent or a treated balance agent obtained by demetallization and / or activation of the FCC balance agent.

[0012] According to the treatment method of the high-nickel catalytic cracking balance agent provided by the present invention, the nickel weight content of the FCC balance agent is higher than 2000ppm, for example, the nickel weight content of the FCC balance agent is 2000ppm to 9000ppm, for example, 3500 to 8000ppm. The method provided by the present invention also has a significant effect on inhibiting the toxicity of vanadium, so the FCC balance agent can contain vanadium, and the vanadium content is not limited, preferably not more than 6000ppm, for example, it can be 500 to 6000 ppm by weight.

[0013] According to the treatment method of the high nickel catalytic cracking balance agent provided by the present invention, the FCC balance agent (also called catalytic cracking balance agent) can be first subjected to demetallization treatment. The demetallization treatment, such as magnetic separation, wet and pyrometallization treatment, further includes but is not limited to: pyrometallization such as chlorination-sulfidation, organic acid demetallization, inorganic acid demetallization, alkaline demetallization, etc., and these methods can adopt existing methods. Preferably, the metal content in the FCC balance agent after the demetallization treatment is each Ni content not exceeding 9000ppm by weight, for example, 4000-9000ppm, and V content not exceeding 8000ppm by weight 3000-8000ppm.

[0014] In one embodiment, the weight content of nickel in the first balancing agent is, for example, less than 9000 ppm, for example, 2000-9000 ppm or 3500-8000 ppm, and the resurrection effect after treatment is better; the weight content of vanadium in the first balancing agent does not exceed 6000 ppm, for example, 500-6000 ppm.

[0015] According to the method for treating a high nickel catalytic cracking balance agent provided by the present invention, the FCC balance agent is a balance agent obtained after using a fully synthetic catalyst and a semi-synthetic catalyst, and is not limited to a catalytic cracking or catalytic cracking catalyst. Generally, the FCC balance agent contains a molecular sieve, and the molecular sieve is, for example, one or more of a Y-type molecular sieve, an MFI structure molecular sieve, and a β molecular sieve.

[0016] According to the method for treating the high-nickel catalytic cracking balance agent provided by the present invention, the product of step (b) can be directly used as a resurrection catalyst. Optionally, the method may further include step (c), activating, drying and calcining the product of step (b). The product of step (c) is used as a resurrection catalyst.

[0017] The present invention may or may not be subjected to activation treatment, and the activation treatment may be conducted before or after the contact treatment, without any special provisions. Generally, if the activation treatment is conducted, only one of step a and step c may be used.

[0018] According to the method for treating a high-nickel catalytic cracking balance agent provided by the present invention, the activation treatment in step (a) or step (c) may include weak acid washing and / or ammonium washing and / or phosphorus treatment and / or rare earth treatment.

[0019] The weak acid washing method is as follows: the balance agent is placed in an acid solution with a pH of 2 to 6, stirred at 60 to 90° C. for 0.1 to 3 hours, and the weak acid washing treatment can be performed once or multiple times, for example, once to twice. The acidic substance used is selected from one or more of hydrochloric acid, nitric acid, phosphoric acid, sulfuric acid, oxalic acid, and citric acid, but is not limited thereto.

[0020] The ammonium washing method is as follows: placing the balance agent in a solution containing ammonia water or an ammonium salt with a pH value of 2 to 7, such as 3 to 5, at 40 to 90°C, stirring for 0.1h to 3h, once or twice; the ammonium salt is, for example, one or more of ammonium sulfate, ammonium chloride, ammonium phosphate and ammonium hydrogen phosphate, but is not limited thereto.

[0021] The phosphorus treatment method is as follows: placing the balance agent in a solution containing a phosphorus compound at a pH of 2 to 5, wherein the phosphorus compound can be selected from one or more of phosphoric acid, pyrophosphoric acid, phosphorous acid, ammonium phosphate, and alkali metal phosphate. The treatment makes the phosphorus content in the revived catalyst 0 to 2 weight %, for example, 0.01 to 0.5 weight %, calculated as P2O5.

[0022] The rare earth treatment method is as follows: placing a balance agent in a solution containing a rare earth compound, wherein the rare earth compound can be selected from one or more of chlorides, nitrates, sulfates, hydroxides, and oxides of lanthanum and / or cerium. The rare earth treatment is performed so that the rare earth content in the resurrected catalyst is 0-2.5 wt %, for example, 0.1-1 wt %, calculated as RE2O3.

[0023] According to the method for treating a high-nickel catalytic cracking balance agent provided by the present invention, in the contact treatment of step (b), the modified metal in the obtained FCC balance agent containing the modified metal coating is calculated as an element and accounts for 0.05% to 5%, for example, 0.05% to 1.0% or 0.05% to 3% of the total dry weight of the FCC balance agent containing the modified metal coating.

[0024] According to the method for treating a high-nickel catalytic cracking balance agent provided by the present invention, the method of contacting the catalytic cracking balance agent obtained in step (a), i.e., the first balance agent, with a compound containing a modified metal to form a coating on the surface of the first balance agent in step (b) is as follows:

[0025] (B1) contacting the catalytic cracking balance agent obtained in step (a), i.e., the first balance agent, with a complex solution containing a modified metal, optionally with an aluminum compound solution or an aluminum-containing colloid; obtaining a balance agent having a surface layer containing a modified element, referred to as a second balance agent, wherein the complex solution containing the modified metal is a macromolecular complex solution of the modified metal;

[0026] Aluminum introduced through complex solution or aluminum introduced through contact with aluminum compound solution or aluminum-containing colloid is called post-loaded aluminum, which can improve the bonding ability between the modified metal and the substrate, and the modified metal is not easy to fall off;

[0027] (B2) The second balancing agent is subjected to a first calcination, optionally treated in a reducing environment such as a reducing gas, and optionally subjected to a second calcination treatment to obtain a revived catalyst.

[0028] According to the method for treating a high-nickel catalytic cracking balance agent as described in any of the above technical solutions, the contact between the complex solution and the first balance agent can be carried out by impregnation (for example, equal volume impregnation method, slurry impregnation method (a method in which the complex is adsorbed on the catalyst surface)), immersion, spraying (spray impregnation method is referred to as spraying method) or deposition method. Preferably, spray impregnation and equal volume impregnation methods are adopted; the modified metal complex is loaded on the surface of the first balance agent (forming a covering coating, referred to as coating or surface layer) through contact. In a preferred embodiment, the complex solution is sprayed at high temperature to evaporate the water in the solution sprayed on the first balance agent in time, reduce the migration of macromolecular complexes to macropores and even to mesopores, which is beneficial to reduce the adverse effects of modified metals on the resurrection catalyst and improve the anti-metal pollution effect; in an embodiment, while spraying the complex solution on the first balance agent, the first balance agent is stirred to promote uniform spraying.

[0029] The spray impregnation method allows the complex solution to be evenly dispersed and sprayed onto the first balancing agent, and the spraying amount and spraying temperature are adjusted so that the water in the solution evaporates in time while spraying onto the surface; at the same time, the microspheres are turned over until the amount of complex sprayed makes the amount of metal in the first balancing agent meet the requirements. Preferably, the first balancing agent is contacted with the complex solution at a higher temperature so that the solvent in the complex solution sprayed onto its surface evaporates as quickly as possible.

[0030] The slurry impregnation method is to mix the first balancing agent with the complex solution and then precipitate with an alkaline precipitant. The complex can be adsorbed on the surface of the first balancing agent, and the addition of the alkaline precipitant can deposit the remaining modified metal complex on the catalyst surface during stirring.

[0031] According to the method for treating a high-nickel catalytic cracking balance agent described in any of the above technical solutions, in one embodiment, the first balance agent is alternately contacted with the complex solution and the aluminum compound dispersion to obtain a first balance agent containing a modified metal element surface layer; wherein the molar ratio of aluminum to the modified metal is: 10:1-1:50, for example, 10:50-2:50; the alternate contact means that the complex solution and the aluminum compound dispersion are alternately contacted with the first balance agent to deposit the modified metal and the aluminum compound on the surface of the first balance agent, the number of alternations is, for example, 1-10 times, the amount of the complex solution contacted with the complex solution each time can be 10-100% by weight of the total amount of the complex solution, and the amount of the aluminum compound dispersion contacted with the aluminum compound dispersion each time can be 10-100% by weight of the total amount of the aluminum compound solution; preferably, after contacting with all the modified metal complex solutions, at least one contact with the aluminum compound dispersion is carried out to improve the wear resistance of the surface layer; preferably, during spraying, the temperature of the first balance agent is preferably 60-200°C, preferably 90-150°C.

[0032] According to the method for treating a high-nickel catalytic cracking balance agent as described in any of the above technical solutions, in step (B1), the first balance agent is further contacted with an aluminum compound dispersion to deposit aluminum on the surface of the first balance agent, and the aluminum compound dispersion is an aluminum compound solution and / or an aluminum-containing colloid. For example, the aluminum compound dispersion can be a solution containing Al ions such as an aluminum salt solution, or a solution containing an aluminum complex, or an aluminum-containing colloid such as an aluminum sol.

[0033] According to the method for treating a high-nickel catalytic cracking balance agent as described in any of the above technical solutions, the temperature at which the complex solution is contacted with the first balance agent in step (B1) (the temperature of the first balance agent) is 0 to 200°C, for example, 90 to 200°C, for example, 120 to 150°C, and the temperature of the sprayed complex solution is usually not more than 100°C, for example, 60-95°C.

[0034] According to the method for treating a high-nickel catalytic cracking balance agent described in any of the above technical solutions, the first calcination in step (B2) is carried out at a temperature of 200-700°C, for example, a calcination temperature of 300-600°C, and a time of 0.1-3h, for example, a calcination time of 0.5-2.5h.

[0035] According to the method for treating a high-nickel catalytic cracking balance agent described in any of the above technical solutions, wherein the second calcination in step (B2) is carried out at a temperature of 300 to 750°C, for example, 350 to 700°C, and for a time of 0.5 to 4 hours, for example, 1 to 3 hours, the modified metal can be better combined with the catalyst surface matrix.

[0036] According to the method for treating a high-nickel catalytic cracking balance agent described in any of the above technical schemes, wherein the treatment in step (B2) under a reducing environment, such as a reducing atmosphere, has a treatment temperature of 350-700°C, such as 500-680°C or 580°C, 600°C or 650°C, and a treatment time of 0.5-6h, such as 0.5-4h. The reducing environment is in contact with a reducing agent, for example, it can be a reducing atmosphere, such as an atmosphere containing one or more of hydrogen, CO, and H2S, or it can be an environment in which one or more reducing agents among S and C are present. When the modified metal includes Ba, the temperature of the treatment in the reducing environment, preferably the reducing atmosphere, is 550-700°C, such as 600-650°C, such as 600°C, 610°C, 620°C, 630°C or 640°C. When the modified metal includes Ti or Mn, the temperature of the treatment in the reducing environment, preferably the reducing atmosphere, is 600-700°C, such as 600°C, 610°C, 630°C, 650°C or 670°C, which can promote the combination with the surrounding matrix elements. Preferably, the treatment and the second calcination treatment are carried out in a reducing environment, preferably a reducing gas. Treatment in a reducing environment, preferably a reducing atmosphere, can promote the redistribution of the modified metal, can make the modified metal distribution better, the bonding is stronger, and the surface layer metal is less prone to wear.

[0037] According to the method for treating a high-nickel catalytic cracking equalizer as described in any of the above technical schemes, the concentration of the complex in the complex solution is 0.01 to 20 weight %, such as 0.5 to 15 weight %; the content of aluminum compounds in the aluminum compound solution calculated as alumina is 0.1 to 30 weight %, such as 1 to 25 weight % or 2 to 20 weight %.

[0038] According to the treatment method of high-nickel catalytic cracking equalizer provided by the present invention, the complex solution containing modified metal is prepared by the following method: a modified metal compound, a macromolecular complexing agent and water are mixed and reacted; in the mixture, the concentration of the metal compound is preferably 0.001-0.15 g / ml, such as 0.01-0.1 g / ml, and the reaction is carried out at 0-150°C, such as 70-90°C, for 0.5-24h, such as 2-14h.

[0039] In a preferred embodiment, the complex solution containing the modified metal is prepared by the following method:

[0040] (1) mixing a modified metal compound, a macromolecular complexing agent and water, wherein the concentration of the metal compound in the mixture is preferably 0.001 to 0.15 g / ml, such as 0.01 to 0.1 g / ml, and reacting, for example, at 0 to 150° C., such as 70 to 90° C., for 0.5 to 24 h, such as 2 to 14 h;

[0041] (2) adding a small molecule alcohol such as ethanol or one or more of methanol, propanol, and ethylene glycol to the product of step (1); the weight ratio of water to alcohol in the resulting mixture is preferably 1:10 to 20:1;

[0042] (3) separation such as filtration and drying;

[0043] (4) The product of step (3) is dissolved, for example, in water to obtain a complex solution containing the modified metal.

[0044] This preferred embodiment can have better treatment effects, for example, the activity of the revived catalyst is more stable after aging (after a long period of aging, the activity is higher) and the hydrogen yield is lower.

[0045] According to the method for treating a high-nickel catalytic cracking balance agent provided by the present invention, the molar ratio of the macromolecular complexing agent to the modified metal ion in the complex containing the modified metal is preferably 0.5:1 to 10:1, for example 0.5 to 6:1, preferably 1 to 4:1.

[0046] In the preferred embodiment, the concentration of the complex solution containing the modified metal obtained in step (4) is, for example, 0.01 to 20 wt %, preferably 0.5 to 15 wt %.

[0047] According to the treatment method of the high-nickel catalytic cracking balance agent provided by the present invention, the modified metal compound is, for example, an oxide of a modified metal element and / or a salt of a modified metal element, and the modified metal element salt is, for example, one or more of a nitrate of a modified metal element, a chloride of a modified metal element, and a sulfate of a modified metal element; for example, the modified metal compound is one or more of titanium oxide, titanium salt, manganese oxide, manganese salt, barium oxide, and barium salt;

[0048] The macromolecular complexing agent is a complexing agent that can effectively complex with a modified metal selected from Ti, Ba, and Mn to form a macromolecular complex or a macromolecular complex cluster, and the formed macromolecular complex and the formed macromolecular complex cluster are difficult to enter the micropore channels of the catalyst, and are also not easy to enter the mesopore channels. The macromolecular complexing agent is, for example, EDTA, EDTA derivatives, polypyridines, macromolecular organic acids, NTA (nitrilotriacetic acid), macromolecular organic acid salts, EDDS (ethylenediamine disuccinic acid), PEI (polyetherimide), pyrophosphate, o-phenanthroline, and polyphosphates. The macromolecular complexing agent is preferably selected from one or more of ethylenediaminetetraacetic acid, ethylenediamine disuccinic acid, polyphosphoric acid, and salts of the above acids, diethanolamine, triethanolamine, polypyridines, and EDTA derivatives.

[0049] The modified metal compound, macromolecular complexing agent and water are mixed. There is no special requirement for the order of the mixture. For example, the metal compound can be added to water under stirring, and then the complexing agent is added.

[0050] According to the treatment method of the high nickel catalytic cracking balance agent provided by the present invention, the complex solution containing the modified metal also contains an additive, and the additive is one or more of Al and / or B and / or P and / or rare earth compounds, or, it also includes contacting with a compound dispersion containing additives, such as a dispersion containing B and / or P and / or Al and / or RE (such as La and / or Ce) compounds, preferably a dispersion of complexes of the above elements, to deposit the above element compounds on the FCC balance agent so that the coating contains B and / or P and / or rare earth and / or Al. In terms of elements, the weight ratio of the additive to the modified metal element is 0 to 2:1. Optionally, the complex solution contains one or more of aluminum, phosphorus, boron, and rare earth compounds. The phosphorus compound can be selected from one or more of phosphoric acid, pyrophosphoric acid, phosphorous acid, ammonium phosphate, and alkali metal phosphate; the rare earth compound can be selected from one or more of chlorides, nitrates, sulfates, hydroxides, and oxides of lanthanum and / or cerium; the boron compound can be selected from one or more of boric acid, boric oxide, tri-n-butyl borate, boron powder, and ammonium fluoroborate; the aluminum compound can be one or more of aluminum salts (such as chlorides, sulfates, nitrates), aluminum sol, phosphate aluminum colloid, and aluminum hydroxide.

[0051] In one embodiment, the method comprises the following steps:

[0052] (a) treating an FCC balance agent with or without demetallization and with or without acidification activation to obtain a first balance agent;

[0053] (b) modifying the first balancing agent obtained in step (a) with a Ti, Ba, Mn macromolecular complex to form an oxide surface coating containing one or more metal ions, thereby obtaining balancing agent microspheres containing one or more coatings of Ti, Ba, Mn elements;

[0054] (3) After drying, the obtained balance agent microspheres are optionally calcined; optionally, after drying, they can also be activated by rare earth or phosphoric acid, ammonium salt, and the activation treatment can be performed before, after or during calcination.

[0055] The invention provides a revived FCC balance agent, comprising a coating containing a modified element compound and an FCC balance agent matrix, wherein the modified element compound is one or more of a Ti metal ion compound, a Ba metal ion compound and a Mn metal ion compound.

[0056] According to the revived FCC balance agent described in the above technical solution, the thickness of the coating is 0.1nm to 1000nm, and the weight concentration of the modified metal in the coating is more than 30 times the weight concentration inside the catalyst.

[0057] Preferably, in the revived FCC balance agent, the thickness of the modified metal coating layer is 0.1 nm to 800 nm, and the weight concentration of the modified metal in the modified metal surface layer is more than 50 times the weight concentration inside the catalyst.

[0058] According to any of the above technical solutions, the FCC balance agent matrix is ​​the first balance agent.

[0059] According to any of the above technical schemes, in one embodiment, the content of modified metal elements in the resurrection catalyst, calculated as elements, accounts for 0.01% to 1% of the total dry weight of the resurrection catalyst. Preferably, the content of modified metal elements, calculated as elements, accounts for 0.03% to 1.0%, for example 0.05% to 0.5%, of the total dry weight of the resurrection catalyst.

[0060] The present invention treats the FCC balance agent in a simple manner, can reduce the dehydrogenation coke activity of nickel, improve the activity stability, and extend the service life of the balance agent. Furthermore, by adjusting the acidity of the catalyst with rare earth compounds and / or phosphorus compounds, the performance of the catalytic cracking balance agent or the spent catalyst can be restored.

[0061] The resurrected catalyst obtained by treating the balance agent with the method disclosed in the present invention can effectively reduce the hydrogen yield of hydrocarbon oil conversion and reduce the hydrogen-methane ratio. The resurrected catalyst has good activity stability and the dry gas yield of heavy oil conversion can be low. Preferably, it can have a higher gasoline yield and a higher liquefied gas yield.

[0062] The method provided by the present invention can be used for resurrecting waste catalysts or balance agents produced in FCC, RFCC or DCC catalytic cracking processes. DETAILED DESCRIPTION

[0063] The resurrection method of the FCC balance agent provided by the present invention is suitable for the reprocessing of the catalytic cracking balance agent with a high nickel content.

[0064] The present invention will be further described in the following examples, but the present invention is not limited thereto.

[0065] The balance agent used in the embodiment is from Sinopec Shijiazhuang Refinery, denoted as ECat-A, containing Y-type molecular sieve, and its basic chemical composition is shown in Table 1. The chemical composition is determined by X-ray fluorescence (XRF), and the specific steps refer to ASTM D7085-04 (2010) Standard Guide for Determination of Chemical Elements in Fluid Catalytic Cracking Catalysts - Guide for Determination by X-ray Fluorescence Spectrometry.

[0066] Micro-reaction activity index: The standard method of RIPP92-90 (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990) was used to evaluate the light oil micro-reaction activity of the sample. The catalyst loading was 5.0 g, the reaction temperature was 460°C, the feed oil was straight-run light diesel with a distillation range of 235-337°C, and the product composition was analyzed by gas chromatography. The light oil micro-reaction activity MA was calculated based on the product composition.

[0067] The surface layer thickness range measurement method of the embodiment: randomly measure the cross-section of 10 particles of the sample, and randomly measure three surface layer thicknesses of each particle cross-section to obtain the distribution range of the particle modified metal coating thickness.

[0068] Table 1

[0069] ECat-A Composition <![CDATA[Na2O. % (by weight)]]> 0.226 MgO.% (weight) 0.118 <![CDATA[Al2O3. % (by weight)]]> 49.7 <![CDATA[SiO2. % (by weight)]]> 42.1 <![CDATA[P2O5. %(by weight)]]> 0.481 <![CDATA[SO3. % (by weight)]]> 0.149 <![CDATA[K2O. %(by weight)]]> 0.317 CaO.% (weight) 0.674 <![CDATA[TiO2. %(by weight)]]> 0.230 <![CDATA[V2O5. %(by weight)]]> 0.686 <![CDATA[Fe2O3. % (by weight)]]> 0.618 <![CDATA[Co2O3. % (by weight)]]> 0.0633 NiO.% (weight) 0.79 ZnO.% (weight) 0.0549 <![CDATA[Y2O3. % (by weight)]]> 0.225 <![CDATA[Sb2O3. % (by weight)]]> 0.289 <![CDATA[La2O3. %(by weight)]]> 1.45 <![CDATA[CeO2. % (by weight)]]> 1.70

[0070] Example 1

[0071] Preparation of EDTA-Mn: In a 500 ml round bottom flask reactor, 19.79 g of manganese chloride tetrahydrate and 32.43 g of EDTA-2NH4 + Add to 100 ml of water, heat in a water bath at 80°C under magnetic stirring, adopt condensation reflux, and react for 3 hours to obtain a complex solution SOL1. After the reaction is completed, cool, add anhydrous ethanol to prepare a cold ethanol aqueous solution (the volume ratio of water to ethanol is 1:9) for precipitation, filter to obtain a precipitate, and then vacuum dry the product in a drying oven at 80°C for 12 hours to obtain 35.1 g of EDTA-Mn complexing agent.

[0072] Preparation of AlCl3 solution: Take 2.68g AlCl3.6H2O and add it to 30g distilled water to make aluminum chloride solution.

[0073] 3.6g of EDTA-Mn complexing agent was dissolved in 40g of distilled water to prepare complexing agent solution SOL2, which was fully mixed with the aluminum chloride solution prepared above, and then 100g of Ecat-A (on a dry basis, the temperature was 95°C) was sprayed with the mixed solution of EDTA-Mn complex and aluminum chloride (referred to as SOL3, the temperature of which was 80°C) by ultrasonic atomization method, and fully stirred while spraying, and then dried at 120°C for 2h to obtain Ecat-A loaded with Mn. Then, Ecat-A loaded with Mn was fully mixed with the aluminum chloride solution prepared above, and then dried at 120°C for 2h, calcined at 500°C in air atmosphere for 2h, reduced in hydrogen at 500°C for 0.5h, and then calcined at 500°C in air atmosphere for 1h to obtain catalyst Ecat-C1. The Mn weight fraction of Ecat-C1 was 0.5%. The Mn-containing coating is 200-350 nm, and the Mn concentration in the modified coating is 150 times that of the internal Mn concentration.

[0074] The EPMA electron microscope analysis of the catalyst microsphere cross section and the analysis method for detecting the internal Mn content are as follows: after cutting the catalyst particles, take any particle, take a diameter line on the cross section, and perform Mn element line scanning analysis. The thickness of the modified metal coating in the cross section and the modified metal concentration in the coating and the interior (the area more than 100 microns away from the non-coated edge of the particle) can be measured.

[0075] Example 2

[0076] Using bis(pentamethylcyclopentadienyl)barium dimethoxyethane adduct (C 20 H 30 B4H 10 2.5 g of 2-nitrogen O2 was dissolved in 40 g of kerosene, and then impregnated into 100 g of dry basis ECAT-A with equal volume, dried at 120°C for 2 h, calcined in air at 500°C for 4 h, reduced in 20% hydrogen by volume at 600°C for 1 h, calcined at 500°C for 1 h, treated in 300 ml of hydrochloric acid solution at 70°C with a pH of 3.5 for 40 min, and dried to obtain catalyst Ecat-C2. The Ba weight fraction of Ecat-C2 is 0.65%. The Ba coating thickness is about 100 to 200 nm, and the Ba concentration in the modified coating is 142 times the Ba content in the interior.

[0077] Example 3

[0078] The method of Example 1 was used for preparation, except that the prepared EDTA-Mn complex solution SOL2 was replaced by the complex solution SOL1 to obtain Ecat-C3, in which the weight fraction of Mn was about 0.5%. The thickness of the Mn coating was about 300-450 nm, and the Mn concentration in the modified coating was 57 times the Mn content in the interior.

[0079] Example 4

[0080] Prepared by the method of Reference Example 1, 100 g of the prepared Ecat-C1 was added to 500 mL of a rare earth chloride solution having a concentration of about 0.3% as rare earth oxide at 80°C, and the pH was adjusted to 3.5 with hydrochloric acid. The mixture was stirred for 30 minutes, and the catalyst was filtered and dried to obtain the resurrected catalyst Ecat-C4. The Mn concentration in the modified coating was 57 times the Mn content in the interior.

[0081] Comparative Example 1

[0082] MnCl2·H2O 4g, dilute to 80g with distilled water, stir for a while, add 96g hydrochloric acid and stir thoroughly, spray into 95g FCC balance agent Ecat-A by homogenizing spray equipment. After further thorough stirring, dry at 120.4℃ for 2h, roast at 500℃ / 2h, treat in 300ml hydrochloric acid solution with pH 3.5 and temperature of 70℃ for 40min and dry, Ecat-D1. The Mn weight fraction of Ecat-D1 is about 1%.

[0083] Comparative Example 2

[0084] This comparative example revives the waste agent according to the method described in Example 1 of CN101219396A, and the specific steps are as follows:

[0085] 30 g of FCC waste catalyst was added to a three-necked flask, and 240 g of hydrochloric acid solution with a pH value of 1 was added under stirring, and heated to 80°C; then 150 g of 0.05 mol of oxalic acid solution was added, and the reaction was maintained at 80°C for 8 hours; after the reaction was completed and naturally cooled to room temperature, the product was filtered and washed until the pH value of the filtrate was about 7; the washed product was dried at 100°C for 24 hours to obtain the revived catalyst Ecat-D2.

[0086] Example 5

[0087] This example illustrates the reaction performance of the resurrected catalyst provided by the present invention.

[0088] Ecat-C1, Ecat-C2, Ecat-C3 and Ecat-C4 were subjected to micro-reactive MA test, see Table 3. Ecat-C1, Ecat-C2, Ecat-C3 and Ecat-C4 were aged in a fixed bed with 100% steam by volume and 780°C / 4h, and then evaluated in an ACE fluidized bed device. The ACE-evaluated crude oil properties are shown in Table 2, and the evaluation conditions and results are shown in Table 3.

[0089] Comparative Example 3

[0090] After the treated balance agent was aged in a fixed bed with 100 volume % steam at 780°C / 4h, Ecat-A, Ecat-D1 and Ecat-D2 were evaluated in an ACE fluidized bed device, respectively. The ACE evaluated crude oil properties are shown in Table 2, and the evaluation conditions and results are shown in Table 3.

[0091] Table 2

[0092]

[0093] Table 3

[0094] Catalyst name Ecat-C1 Ecat-C2 Ecat-C3 Ecat-C4 ECat-A Ecat-D1 Ecat-D2 MA, % 64 67 61 69 62 68 72 MA (780℃ / 4h), % 61 60 58 63 55 53 52 ACE Experiment Reaction temperature,℃ 500.0 500.0 500.0 500.0 500.0 500.0 500.0 Agent-oil ratio, wt / wt 4.02 4.02 4.02 4.02 4.02 4.02 4.02 Oil inlet response time, s 112 112 112 112 112 112 112 Yield, wt%: Dry gas 2.63 2.63 2.69 2.58 2.97 2.80 2.78 LPG 15.77 15.55 15.47 15.32 14.81 14.58 13.82 Coke 7.63 8.06 8.10 8.03 8.65 6.84 7.84 gasoline 38.43 38.24 37.61 39.11 35.22 32.86 31.97 LCO 19.95 19.38 20.02 19.57 19.94 22.97 23.97 heavy oil 15.59 16.14 16.11 15.39 18.41 19.95 19.62 hydrogen 0.52 0.56 0.57 0.46 0.94 0.68 0.87 Ethane 1.25 1.17 1.28 1.28 1.11 1.29 1.08 Ethylene 0.54 0.56 0.52 0.56 0.56 0.52 0.54 Propane 0.32 0.34 0.32 0.28 0.36 0.31 0.29 Propylene 0.91 0.88 0.82 0.95 0.84 0.86 0.79 n-Butane 6.28 6.43 6.19 6.00 6.09 6.11 5.95 Isobutane 0.83 0.82 0.79 0.84 0.71 0.65 0.57 C4 olefins 2.38 2.26 2.32 2.41 2.16 1.82 1.62 Conversion rate.,wt% 64.46 64.48 63.87 65.04 61.65 57.08 56.41 Hydrogen to methane ratio (mol ratio) 3.33 3.83 3.56 2.88 6.77 4.22 6.44

[0095] As can be seen from Table 3, the resurrected catalyst obtained by the high nickel catalytic cracking balance agent treatment method provided by the present invention has a higher conversion rate after hydrothermal aging relative to the unresurrected ECat-A catalyst, indicating that it has a more stable activity, and has a significantly lower hydrogen yield, which can greatly reduce the hydrogen-methane ratio, and can have a lower coke yield when the heavy oil conversion rate is high. The existing acidic resurrection method, although the apparent activity is high, the activity stability (activity after hydrothermal aging) is relatively poor. The catalytic cracking balance agent treatment method of the present invention is more advantageous, and the resurrected catalyst obtained has higher activity stability. In the preferred case, for example, when the modified metal element is Mn, the resurrected catalyst obtained by the method provided by the present invention can have a higher light olefin yield, a higher conversion rate and a higher gasoline yield.

Claims

1. A method for treating a high-nickel catalytic cracking balance agent, include: (a) providing an FCC balance agent, wherein the FCC balance agent is subjected to a demetallization treatment and / or an activation treatment; the first balance agent is referred to as a first balance agent; the first balance agent has a nickel weight content of 2000 to 9000 ppm; (b) contacting the first balance agent obtained in step (a) with a compound containing a modified metal to form a coating on the surface of the first balance agent, thereby obtaining an FCC balance agent containing a modified metal coating, wherein the modified metal in the obtained FCC balance agent containing a modified metal coating accounts for 0.05% to 5% of the total weight of the FCC balance agent containing a modified metal coating on a dry basis in terms of element; the modified metal is one or more of Ti, Mn, and Ba; the contact treatment method is a macromolecular complex metal loading method, and the method of contacting the first balance agent obtained in step (a) with a compound containing a modified metal to form a coating on the surface of the first balance agent in step (b) is as follows: (B1) contacting the first balancing agent obtained in step (a) with a complex solution containing a modified metal, and with an aluminum compound solution or an aluminum-containing colloid; obtaining a balancing agent having a surface layer containing a modified element, referred to as a second balancing agent, wherein the complex solution containing the modified metal is a macromolecular complex solution of the modified metal; the macromolecular complexing agent is selected from one or more of ethylenediaminetetraacetic acid, ethylenediamine disuccinic acid, polyphosphoric acid and salts of the above acids, diethanolamine, triethanolamine, polypyridine, and EDTA derivatives; (B2) The second balancing agent is subjected to a first calcination, optionally treated in a reducing environment, and optionally subjected to a second calcination to obtain a revived catalyst.

2. The method according to claim 1, It is characterized in that The nickel content of the FCC balance agent is higher than 2000 ppm by weight; the vanadium content of the first balance agent is 500-6000 ppm by weight.

3. The method according to claim 1, It is characterized in that The FCC balance agent contains molecular sieves, and the molecular sieves are one or more of Y-type molecular sieves, MFI structure molecular sieves and β molecular sieves.

4. The method according to claim 1, It is characterized in that The contact treatment in step (b) is performed so that the modified metal in the obtained FCC balance agent containing the modified metal coating accounts for 0.05% to 1.0% of the total dry weight of the FCC balance agent containing the modified metal coating as an element.

5. The method according to claim 1, It is characterized in that The modified metal-containing complex solution is prepared by the following method: a modified metal compound, a macromolecular complexing agent and water are mixed and reacted; in the mixture, the concentration of the metal compound is 0.001-0.15 g / mL, and the reaction is carried out at 0-150° C. for 0.5-24 hours.

6. The method according to claim 1, It is characterized in that The complex solution containing modified metal is prepared by the following method: (1) Mixing a modified metal compound, a macromolecular complexing agent and water, wherein the concentration of the metal compound in the mixture is 0.001-0.15 g / mL and reacting at 0-150° C. for 0.5-24 hours; the macromolecular complexing agent is one or more of EDTA, EDTA derivatives, polypyridine, macromolecular organic acid, NTA, macromolecular organic acid salt, ethylenediamine disuccinic acid, polyetherimide, pyrophosphate, o-phenanthroline, and polyphosphate; (2) adding a small molecule alcohol to the product of step (1), wherein the weight ratio of water to alcohol in the resulting mixture is 1:10 to 20:1; (3) Separation and drying; (4) The product of step (3) is dissolved to obtain a complex solution containing the modified metal.

7. The method according to claim 6, It is characterized in that In step (1), the concentration of the metal compound is 0.01-0.1 g / mL, and the reaction is carried out at 70-90° C. for 2-14 h; the small molecule alcohol is one or more of ethanol or methanol, propanol, and ethylene glycol.

8. The method according to claim 6, It is characterized in that The molar ratio of the macromolecular complexing agent to the modified metal ion in the modified metal-containing complex is 0.5:1 to 10:1; and the concentration of the modified metal-containing complex solution obtained in step (4) is 0.01 to 20% by weight.

9. The method according to claim 6, It is characterized in that The molar ratio of the macromolecular complexing agent to the modified metal ion in the modified metal-containing complex is 1-4:1; and the concentration of the modified metal-containing complex solution obtained in step (4) is 0.5-15% by weight.

10. The method according to claim 6, 7 or 8, It is characterized in that The modified metal compound is one or more of titanium oxide, titanium salt, manganese oxide, manganese salt, barium oxide and barium salt.

11. The method according to claim 1, It is characterized in that The complex solution containing modified metals also contains additives, and the additives are one or more of Al and / or B and / or P and / or rare earth compounds. Alternatively, the method further includes contacting with a compound dispersion containing additives to deposit the above element compounds on an FCC balance agent so that the coating contains B and / or P and / or rare earth and / or Al; the weight ratio of the additive to the modified metal element is 0 to 2:1 in terms of elements; and the compound dispersion containing additives is a dispersion containing B and / or P and / or Al and / or RE compounds or complexes of the above elements.

12. The method according to claim 11, It is characterized in that The compound in the compound dispersion containing additives is a complex of the above P, B, Al, and RE elements.

13. The method according to claim 1, It is characterized in that The first calcination is carried out at a temperature of 200-700°C for a time of 0.1-3h; the second calcination is carried out at a temperature of 300-750°C for a time of 0.5-4h; the treatment under a reducing environment is carried out under a reducing atmosphere at a temperature of 350-700°C for a treatment time of 0.5-6h; Optionally, the method further comprises (c), activating, drying and calcining the product of step (b); the activation treatment in step (a) or step (c) is weak acid washing and / or ammonium washing and / or phosphorus treatment and / or rare earth treatment.

14. A revived FCC balance agent, comprising a coating containing a modified element compound and an FCC balance agent matrix, wherein the modified element compound is one or more of a Ti metal ion compound, a Ba metal ion compound, and a Mn metal ion compound, and the revived FCC balance agent is obtained by the treatment method of the high-nickel catalytic cracking balance agent according to any one of claims 1 to 13.