A high pressure resistant deoxidized copper tube and preparation method thereof

Boron oxide is generated through ultrasonic cleaning and high-frequency induction furnace smelting, and a directional crystal structure is formed through hot rolling process, which solves the problem of insufficient performance of existing deoxygenated copper tubes in high-pressure environments, and achieves high yield strength and compressive strength The improvement meets the high performance requirements of air conditioning and refrigeration equipment.

CN116200621BActive Publication Date: 2024-11-15SHANGYU SHUANGMAO COPPER IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310438422.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-23
Publication Date
2024-11-15
Estimated Expiration
2043-04-23

AI Technical Summary

Technical Problem

Existing deoxygenated copper tubes cannot meet service requirements under high pressure and corrosive environments, and when using boron as a deoxidizing agent, an increase in boron content will reduce the tensile strength and toughness of the material, limiting its widespread application.

Method used

Using ultrasonic cleaning and high-frequency induction furnace melting, boron is added under the protection of inert gas to deoxygenate to generate boron oxide, and the boron oxide forms a directional crystal structure through hot extrusion or hot rolling process to avoid annealing process and reduce the Stress concentration.

Benefits of technology

It significantly improves the yield strength and compressive strength of copper alloys, meets the requirements of high-pressure environment, reduces processing difficulty, and meets the requirements of oxygen content index in oxygen-free copper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of deoxidized copper tubes, and in particular to a high-pressure resistant deoxidized copper tube and a preparation method thereof. The present invention provides a high-pressure resistant deoxidized copper tube and a preparation method thereof, and the technical scheme is: a high-pressure resistant deoxidized copper tube and a preparation method thereof, comprising the following steps: S1) raw material pretreatment: weigh a certain amount of electrolytic copper raw material according to the total mass percentage, and use ultrasonic cleaning, etc.; after cleaning, dry and preheat treatment; the temperature polarity of boron oxide can adapt to the structural strengthening characteristics of the grains in the casting and rolling process, so that it undergoes plastic deformation, and this deformation will cause dislocation slip inside the grains and rotation of the grains, so that the boron oxide grain structure has a certain stability and approaches a consistent directionality; in this state, the yield strength of the copper alloy can be effectively improved, and the high-pressure resistance of the copper alloy can be strengthened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of deoxidized copper tubes, and in particular to a high-pressure resistant deoxidized copper tube and a preparation method thereof. Background Art

[0002] Deoxidized copper tubes are widely used in transportation pipelines for high-pressure fluids such as gasoline and oil, or as condensers for air-conditioning and refrigeration equipment. The preparation process of deoxidized copper tubes mainly includes the selection of copper raw materials, smelting deoxidation, casting, and then rolling, extrusion or drawing, and subsequent annealing to remove internal stress and other processing and forming steps. Among them, the selection of copper raw materials and the forming process are the key factors that determine the performance of copper tubes. The oxygen content in the copper raw materials will affect the strength, toughness and corrosion resistance of the copper tubes; different forming processes also affect the strengthening characteristics of the internal structure of the material.

[0003] The deoxidizers used in the preparation methods of common deoxidized copper include boron, phosphorus (CU-P alloy), rare earth, hydrogen or methane. Hydrogen is a widely used deoxidizer. During smelting, hydrogen reacts with cuprous oxide to generate water vapor. Since H2O cannot dissolve in the Cu lattice, it gathers into holes in the form of water vapor; it is easy to cause microcracks in the finished product, leading to cracking and leakage. At present, the materials used for condenser tubes are mostly oxygen-free copper tubes or phosphorus-deoxidized copper tubes, but when serving in special environments, such as high pressure and corrosive environments, ordinary TP2 or oxygen-free copper tubes cannot meet the service environment requirements.

[0004] Boron is used as a deoxidizer during smelting, which can reduce the oxygen content to below 0.005%, meeting the requirements of T2 and C10200 for oxygen-free copper. The boron oxide generated in this process is an excellent covering agent during copper alloy smelting, but the increase in boron oxide content reduces the tensile strength and toughness of the material, and it is not easy to remove in subsequent processing, which limits its widespread use as a deoxidizer. There are also few related studies and applications on the preparation of deoxidized copper using boron as a deoxidizer at home and abroad. Summary of the invention

[0005] In order to overcome the disadvantages, the technical problem to be solved is: to provide a high-pressure resistant deoxidized copper tube and a preparation method thereof.

[0006] The technical solution is: a high-pressure resistant deoxidized copper tube and a preparation method thereof, comprising the following steps:

[0007] S1) Raw material pretreatment: weigh a certain amount of electrolytic copper raw material according to the total mass percentage, clean it with ultrasound, dry it after cleaning and perform preheating treatment;

[0008] S2) Smelting and deoxidation: the treated electrolytic copper raw material is put into a high-frequency induction furnace, and smelted under the protection of inert gas or nitrogen. After the electrolytic copper raw material in the furnace is completely melted, the smelting temperature is controlled at 1100° C. to 1200° C., 0.1 to 0.4% boron is added to the melt, and the melt is stirred for 10 to 20 minutes by an electromagnetic stirring device at the bottom of the furnace and then kept warm for 2 to 3 hours, so that the molten electrolytic copper raw material undergoes a reduction reaction to deoxidize and generate boron oxide; then it is cast into a tubular mold and cooled and solidified to obtain a deoxidized copper tube;

[0009] S3) Processing and forming: The cast deoxidized copper tube is processed and formed by hot extrusion or hot rolling to obtain a finished deoxidized copper tube of a desired size and shape.

[0010] As a further preferred embodiment, the process steps of step S3 are: heating the deoxidized copper tube to 450-500° C. to change the structure of the boron oxide and generate a directional crystalline structure, thereby laying a foundation for the subsequent hot rolling process; sending the heated deoxidized copper tube into a rolling mill for rolling, and controlling the hot rolling temperature between 350 and 400° C. to obtain a finished deoxidized copper tube.

[0011] As a further preferred solution, in step S1, the ultrasonic frequency is controlled at 2.5-5 MHz, and after cleaning, the surface is dried at 100-200° C. and kept warm for 1-2 hours for preheating.

[0012] As a further preferred solution, the power of the high-frequency induction furnace is controlled at 15-20KW.

[0013] Control of smelting temperature is an important factor affecting the deoxidation effect and the quality of copper tubes. Too high a temperature will lead to the volatilization of boron and excessive deoxidation, while too low a temperature will affect the dissolution and dispersion of boron. The amount of boron added should be determined according to the oxygen content in the electrolytic copper raw material and the required degree of deoxidation. Too much or too little boron will affect the mechanical properties and corrosion resistance of the copper tube.

[0014] As a further preferred solution, the measured value of the oxygen content in the selected electrolytic copper raw material is 85-90 ppm; and the required boron addition amount is 0.25-0.3%.

[0015] Boron is added to the molten metal, and it reacts with oxygen to form boron oxide; 3Cu 2O + 2B = B2O 3 + 6Cu

[0016] The present invention has the following advantages: 1. The temperature polarity of boron oxide can adapt to the structural strengthening characteristics of grains in the casting and rolling process, causing them to undergo plastic deformation. This deformation will cause dislocation slip inside the grains and rotation of the grains, so that the boron oxide grain structure has a certain stability and tends to be consistent in directionality; in this state, the yield strength of the copper alloy can be effectively improved and the high pressure resistance of the copper alloy can be enhanced.

[0017] 2. In the casting and rolling process, since the interfacial force between the boron oxide grains and the copper grains can be completely converted into the plastic deformation of the boron oxide grains, this can greatly reduce the stress concentration during the rolling process, avoid internal stress, and no annealing process is required after rolling. This also avoids the surface oxidation phenomenon caused by the annealing process and reduces the processing difficulty of tubular copper materials. DETAILED DESCRIPTION

[0018] The present invention will be further described below in conjunction with specific embodiments.

[0019] A high-pressure resistant deoxidized copper tube and a preparation method thereof, comprising the following steps:

[0020] S1) Raw material pretreatment: weigh a certain amount of electrolytic copper raw material according to the total mass percentage, clean it with ultrasound, dry it after cleaning and perform preheating treatment; in the step S1, the ultrasonic frequency is controlled at 2.5-5MHz, and after cleaning, it is dried at 100-200°C and kept warm for 1-2 hours for preheating.

[0021] S2) Smelting and deoxidation: the treated electrolytic copper raw material is put into a high-frequency induction furnace, and smelted under the protection of inert gas or nitrogen. After the electrolytic copper raw material in the furnace is completely melted, the smelting temperature is controlled at 1100°C to 1200°C, 0.1 to 0.4% boron is added to the melt, and the melt is stirred for 10 to 20 minutes by an electromagnetic stirring device at the bottom of the furnace, and then kept warm for 2 to 3 hours, so that the molten electrolytic copper raw material undergoes a reduction reaction to deoxidize and generate boron oxide; then it is cast into a tubular mold, cooled and solidified to obtain a deoxidized copper tube; the power of the high-frequency induction furnace is controlled at 15 to 20KW;

[0022] Control of smelting temperature is an important factor affecting the deoxidation effect and the quality of copper tubes. Too high a temperature will lead to the volatilization of boron and excessive deoxidation, while too low a temperature will affect the dissolution and dispersion of boron. The amount of boron added should be determined according to the oxygen content in the electrolytic copper raw material and the required degree of deoxidation. Too much or too little boron will affect the mechanical properties and corrosion resistance of the copper tube.

[0023] The oxygen content in the selected electrolytic copper raw material is measured to be 85-90 ppm; the required boron addition amount is 0.25-0.3%.

[0024] S3) Rolling processing: heating the deoxidized copper tube to 450-500°C to change the structure of boron oxide and generate a directional crystalline structure, laying a foundation for the subsequent hot rolling process; sending the heated deoxidized copper tube to a rolling mill for rolling, and controlling the hot rolling temperature between 350-400°C; obtaining a finished deoxidized copper tube.

[0025] The oxygen content in the electrolytic copper raw material mainly exists in the form of copper oxide. Boron is added to the molten electrolytic copper raw material, and the copper oxide is reduced to copper through the reduction reaction of boron and copper oxide. The reaction generates a by-product of boron oxide. Boron is added to the molten metal, and boron reacts with oxygen to form boron oxide; 3Cu 2O+2B=B2O 3+6Cu.

[0026] Since boron oxide is extremely difficult to crystallize, when the temperature exceeds 450°C and is lower than 1000°C, some double-bonded -B=O groups will appear in the structure of boron oxide, and these groups are polar. Their polarity can well adapt to the structural strengthening characteristics of the grains in the casting and rolling process, causing them to undergo plastic deformation. This deformation will cause dislocation slip inside the grains and rotation of the grains, making the boron oxide grain structure have a certain stability and approach a consistent direction), thereby affecting the isotropic physical properties or chemical properties of the alloy structure. It is worth noting that due to the polarity of boron oxide in this state, it means that the interfacial force between the boron oxide grains and the copper grains can be completely converted into the plastic deformation of the boron oxide grains; it greatly reduces the stress concentration during the rolling process, avoids internal stress, and does not require an annealing process after rolling; it also avoids surface oxidation during the annealing process, reducing the difficulty of processing tubular copper materials.

[0027] The oxygen content of the novel deoxidized copper tube prepared by the present invention is lower than 0.005%, which has met or is close to the requirements of C10100 and C10200 for the oxygen content index in oxygen-free copper. The yield strength is 152.5MPa, the compressive strength is 247.8MPa, and the mechanical properties are significantly better than those of the existing oxygen-free copper tube.

[0028] Experimental plan Experimental purpose: To explore the effect of boron addition on the structure and properties of deoxidized copper tube;

[0029] Experimental steps:

[0030] According to step S1, raw materials are pretreated; according to step S2, smelting and deoxidation are performed, and 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35% and 0.4% of boron are added respectively to obtain seven groups of as-cast deoxidized copper tubes with different contents;

[0031] The seven groups of as-cast deoxidized copper tubes are respectively rolled according to step S3 to form seven groups (Examples 1-7) of finished deoxidized copper tubes with specifications of Φ50 mm×2.4 mm.

[0032] The seven groups of embodiments were subjected to pressure tests to measure the yield strength and compressive strength;

[0033] The seven groups of embodiments were subjected to hardness tests to measure the Vickers hardness;

[0034] For the CK group: the unrolled cast deoxidized copper tubes with 0.3% boron content were subjected to pressure test and hardness test respectively; the yield strength, compressive strength and Vickers hardness were measured.

[0035] According to the experimental data, the influence of yield strength, compressive strength, Vickers hardness and boron content is obtained; as shown in Table 1 below:

[0036] Table 1

[0037]

[0038] Experimental conclusion:

[0039] From the data in Table 1, it can be seen that with the increase of boron content, in Example 4 (0.25% boron), the yield strength and compressive strength of the finished deoxidized copper tube both show a significant jump, and the Vickers hardness remains basically unchanged, indicating that at a boron content of 0.25-0.3%, the deoxidation effect of the electrolytic copper can be effectively achieved, and the boron oxide crystals produced can maximize the yield strength and compressive strength of the deoxidized copper.

[0040] According to the data comparison between Example 4 and the CK group, it is shown that after heating above 450°C and rolling, the boron oxide crystals rotate and approach consistent directionality and stability. The boron oxide crystals in this state have a significant strengthening effect on deoxidized copper. The present invention is based on this discovery to prepare a high-pressure resistant deoxidized copper tube. The performance indicators of the deoxidized copper tube prepared by the process of the present invention meet the requirements of GB / T17791-2017 "Seamless Copper Tubes for Air Conditioning and Refrigeration Equipment". Provide a new type of copper tube with excellent performance such as high pressure resistance, corrosion resistance, crack resistance, and long service life for the industrial refrigeration field with higher environmental requirements using R410A refrigerant.

[0041] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that changes may be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a high-pressure resistant deoxidized copper tube, characterized in that: The following steps are included: S1) Raw material pretreatment: weigh a certain amount of electrolytic copper raw material according to the total mass percentage, clean it with ultrasound, dry it after cleaning and perform preheating treatment; S2) smelting and deoxidation: putting the treated electrolytic copper raw material into a high-frequency induction furnace, smelting under the protection of inert gas or nitrogen, and after all the electrolytic copper raw material in the furnace is melted, controlling the smelting temperature at 1100° C. to 1200° C., adding boron to the melt, stirring the melt at the bottom of the furnace with an electromagnetic stirring device for 10-20 minutes and then keeping the melt warm for 2 to 3 hours, so that the molten electrolytic copper raw material undergoes a reduction reaction to deoxidize and generate boron oxide; then casting it into a tubular mold, cooling and solidifying it to obtain a deoxidized copper tube; S3) Processing and forming: hot extrusion or hot rolling is used to process the cast deoxidized copper tube to obtain a finished deoxidized copper tube of a desired size and shape; The measured value of oxygen content in the selected electrolytic copper raw material is 85-90 ppm; the required boron addition amount is 0.25-0.3%.

2. The method for preparing a high-pressure resistant deoxidized copper tube according to claim 1, characterized in that: In the step S1, the ultrasonic frequency is controlled at 2.5-5 MHz, and after cleaning, the product is dried at 100-200° C. and kept warm for 1-2 hours for preheating.

3. The method for preparing a high-pressure resistant deoxidized copper tube according to claim 1, characterized in that: The power of the high frequency induction furnace is controlled at 15-20KW.

4. The method for preparing a high-pressure resistant deoxidized copper tube according to claim 1, characterized in that: The process steps of step 3) are as follows: heating the deoxidized copper tube to 450-500°C to change the structure of the boron oxide and generate a directional crystalline structure; sending the heated deoxidized copper tube to a rolling mill for rolling, with the hot rolling temperature controlled at 350-400°C; and obtaining a finished deoxidized copper tube.