A thermoplastic polyurethane composition and its preparation method and application
Through the combination of mica powder and wollastonite and the use of epoxy modified silane coupling agent, the problem of long molding cycle of low-hardness thermoplastic polyurethane is solved, the molding cycle is shortened and the hardness change value is reduced, and the production is improved efficiency.
Patent Information
- Application Number
- CN202310378240.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-11
AI Technical Summary
The low-hardness thermoplastic polyurethane has a slow cooling and hardening speed during injection molding, resulting in a long molding cycle and affecting production efficiency.
Mica powder and wollastonite are used as crystallization modifiers, combined with epoxy modified silane coupling agent, and premixed with thermoplastic polyurethane TPU and additives at 150-230°C after baking for 4 hours at 75-85°C. The molding is carried out in a twin-screw extruder, and the combination of mica powder and wollastonite is used to induce the regular arrangement of the polyurethane molecular chains to speed up the crystallization process.
The molding cycle is significantly shortened to below 164s, and the hardness change of TPU at -20℃ and 40℃ is reduced, both below 7A, improving production efficiency.
Smart Images

Figure BDA0004171130260000011 
Figure BDA0004171130260000021 
Figure BDA0004171130260000031
Abstract
Description
Technical Field
[0001] The invention belongs to the field of plastic processing, and particularly relates to a thermoplastic polyurethane composition and a preparation method and application thereof. Background Art
[0002] Thermoplastic polyurethane materials have excellent mechanical properties, resilience, chemical solvent resistance, fatigue resistance, etc. They can be injection molded without vulcanization. They are increasingly used in consumer electronics cushions, car cup holder cushions, office chairs, mobile phone covers, automotive wiring harnesses and other fields.
[0003] Low-hardness thermoplastic polyurethane has excellent elasticity, wear resistance and chemical resistance. In the consumer electronics cushion industry, it replaces silicone and is used in cushion parts to prevent slipping and shock. However, during the injection molding process, low-hardness thermoplastic polyurethane has a slow cooling and hardening speed, and it takes a long time to hold the pressure and cool. The molding cycle is long, which affects production efficiency. Summary of the invention
[0004] In view of the defects of the prior art, the technical problem to be solved by the present invention is to provide a thermoplastic polyurethane composition and a preparation method and application thereof.
[0005] A thermoplastic polyurethane composition of the present invention comprises, by weight:
[0006]
[0007] The crystal modifier is composed of mica powder and wollastonite; the mass ratio of mica powder to wollastonite is (0.5-3):1; the average particle size of mica powder is 200-1000 mesh; the average particle size of wollastonite is 200-600 mesh. The particle size is tested in accordance with GB / T19077-2016.
[0008] The thermoplastic polyurethane TPU is a low-hardness thermoplastic polyurethane TPU with a Shore hardness of 65A-80A. The Shore hardness is tested according to the national standard GB / T 531-2008.
[0009] The content of the crystal modifier in the composition is 0.5 wt%-8 wt%, preferably 1 wt%-6 wt%.
[0010] The content of the silane coupling agent in the composition is 0.04wt%-0.5wt%.
[0011] Preferably, the silane coupling agent is an epoxy-modified silane coupling agent, such as 3-glycidylpropyltrimethoxysilane coupling agent, 3-glycidylpropyltriethoxysilane coupling agent, and the like.
[0012] Preferably, the mass ratio of the mica powder to wollastonite is (0.8-2):1.
[0013] Preferably, the average particle size of the mica powder is 400-800 mesh.
[0014] Preferably, the average particle size of the wollastonite is 300-500 mesh.
[0015] Preferably, the additive is one or more of a flame retardant (such as aluminum diethylphosphinate, inorganic aluminum hypophosphite, resorcinol bisdiphenyl phosphate, etc.), an antioxidant (such as 4.4'-bis(α.α-dimethylbenzyl)diphenylamine, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, etc.), a UV resistant agent (such as 2-(2'-hydroxy-3',5'bis(a,a-dimethylbenzyl)phenyl)benzotriazole, 2-(2-hydroxy-5-methylphenyl)benzotriazole, bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, etc.), carbon black, a pigment (such as azo orange, iron yellow, etc.), a dye (such as ultramarine blue, azo orange, etc.), and a mineral powder (such as calcium carbonate, talc, montmorillonite, etc.).
[0016] Additives can be added selectively according to actual conditions.
[0017] Preferably, by weight, the components include:
[0018]
[0019] The amount of additives is added according to actual conditions.
[0020] A method for preparing the thermoplastic polyurethane composition of the present invention comprises:
[0021] (1) Weighing each component by weight, mixing the crystal modifier and the silane coupling agent, and baking at 75-85° C. for 4 h to obtain a premix;
[0022] (2) mixing thermoplastic polyurethane TPU with premix and additives;
[0023] (3) The mixed material is fed into a twin-screw extruder by weight-loss metering, extruded at 150-230° C., granulated and dried to obtain a thermoplastic polyurethane composition.
[0024] In the step (3), the length-to-diameter ratio of the twin-screw extruder is 36-60 / 1, and the residence time of the material in the screw is 40-90 seconds.
[0025] An application of the thermoplastic polyurethane composition described in claim 1 of the present invention in the field of consumer products, such as cable plugs, shoe soles, cable sheaths, washers, etc.
[0026] The compound use of mica powder and wollastonite within the particle size range of the present invention can induce regular arrangement of thermoplastic polyurethane molecular chains, accelerate the crystallization of thermoplastic polyurethane, thereby accelerating the molding cycle, and at the same time can reduce the hardness change value of TPU material at -20°C and 40°C.
[0027] Beneficial Effects
[0028] The thermoplastic polyurethane composition of the present invention has a short molding cycle, as low as below 164s, and reduces the hardness change value of TPU at -20°C and 40°C, and the hardness change value is below 7A. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0030] 1. Source of raw materials:
[0031] Thermoplastic polyurethane TPU-1: HF-1065AP, produced by Zhejiang Huafeng Thermoplastic Polyurethane Co., Ltd., tested according to GB / T 531-2008, Shore hardness is 65A;
[0032] Thermoplastic polyurethane TPU-2: HF-3080A, produced by Zhejiang Huafeng Thermoplastic Polyurethane Co., Ltd., tested according to GB / T 531-2008, Shore hardness is 80A;
[0033] Silane coupling agent-1: KH-560, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, produced by Nanjing Shuguang Silane Chemical Co., Ltd., epoxy-modified silane coupling agent;
[0034] Silane coupling agent-2: JH-A110, 3-aminopropyltriethoxysilane, produced by Jingzhou Jianghan Fine Chemical Co., Ltd., non-epoxy modified silane coupling agent;
[0035]
[0036] Crystal modifier-1 is mica powder-1 and wollastonite-1 in a mass ratio of 1:1;
[0037] Crystal modifier-2 is mica powder-1 and wollastonite-1 in a mass ratio of 0.8:1;
[0038] Crystal modifier-3 is mica powder-1 and wollastonite-1 in a mass ratio of 2:1;
[0039] Crystal modifier-4 is mica powder-1 and wollastonite-1 in a mass ratio of 3:1;
[0040] Crystal modifier-5 is mica powder-1 and wollastonite-2 in a mass ratio of 1:1;
[0041] Crystal modifier-6 is mica powder-1 and wollastonite-3 in a mass ratio of 1:1;
[0042] Crystal modifier-7 is mica powder-2 and wollastonite-1 in a mass ratio of 1:1;
[0043] Crystal modifier-8 is mica powder-3 and wollastonite-1 in a mass ratio of 1:1;
[0044] Crystal modifier-9 is mica powder-1 and wollastonite-4 in a mass ratio of 1:1;
[0045] The crystal modifier-10 is mica powder-4 and wollastonite-1 in a mass ratio of 1:1;
[0046] The crystal modifier-11 is mica powder-1 and wollastonite-1 in a mass ratio of 5:1.
[0047] The additives are antioxidant tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester, ultraviolet light absorber 2-(2'-hydroxy-3',5'bis(a,a-dimethylbenzyl)phenyl)benzotriazole and carbon black in a mass ratio of 2:3:5.
[0048] The additives used in the examples and the parallel comparative examples are all the same commercially available products.
[0049] 2. Preparation methods of embodiments and comparative examples
[0050] After the crystal modifier and silane coupling agent are mixed in a high-speed mixer, they are baked at 80°C for 4 hours to obtain a powder premix; the thermoplastic polyurethane TPU, the powder premix and the additives are put into a high-speed mixer for mixing; the mixed materials are fed into a twin-screw extruder by weightless metering, extruded at 150-230°C, granulated and dried to obtain a thermoplastic polyurethane composition. The length-to-diameter ratio of the twin-screw extruder used is 36-60 / 1, and the material stays in the screw for 40-90 seconds.
[0051] 3. Test standards and methods
[0052] Forming speed evaluation method:
[0053] The thermoplastic polyurethane composition was injection molded into a 40*10*5mm block. Under the same injection molding process conditions, the cooling time was changed. The shortest cooling time when the part could be demoulded normally without deformation was recorded as t. The molding speed was judged by comparing the t value.
[0054] Hardness change:
[0055] The hardness test is carried out in accordance with GB / T 531-2008.
[0056] -20℃ hardness test standard and method: After placing the sample at -20℃ for 4 hours, refer to GB / T 531-2008 to test the hardness;
[0057] Test standard and method for 40℃ hardness value: Place the sample at 40℃ for 4h and then test the hardness in accordance with GB / T 531-2008.
[0058] Table 1 Example ratio (weight parts) and performance effect data
[0059]
[0060]
[0061] Table 2 is the example ratio (weight parts) and performance effect data
[0062]
[0063] Table 3 is the ratio (weight parts) and performance effect data of the comparative example
[0064]
[0065]
[0066] In Examples 1-15 of the present invention, a silane coupling agent and a crystal modifier are used together, and the crystal modifier is compounded with mica powder having a particle size of 200-1000 mesh and wollastonite having a particle size of 200-600 mesh, which can significantly shorten the molding cycle to less than 164 seconds, and reduce the hardness change value of TPU at -20°C and 40°C to less than 7A;
[0067] It can be seen from Examples 1 and 3 that the epoxy-modified silane coupling agent is better than the non-epoxy-modified silane coupling agent.
Claims
1. A thermoplastic polyurethane composition, It is characterized in that By weight, the components include: The crystal modifier is composed of mica powder and wollastonite; wherein the mass ratio of mica powder to wollastonite is (0.5-3):1; The average particle size of the mica powder is 200-1000 meshes; the average particle size of the wollastonite is 200-600 meshes.
2. The composition according to claim 1, It is characterized in that The silane coupling agent is an epoxy-modified silane coupling agent.
3. The composition according to claim 1, It is characterized in that The mass ratio of the mica powder to wollastonite is (0.8-2):
1.
4. The composition according to claim 1, It is characterized in that The average particle size of the mica powder is 400-800 meshes.
5. The composition according to claim 1, It is characterized in that The average particle size of the wollastonite is 300-500 meshes.
6. The composition according to claim 1, It is characterized in that The additive is one or more of flame retardants, antioxidants, UV resistant agents, carbon black, pigments, dyes, and mineral powders.
7. The composition according to claim 1, It is characterized in that By weight, the components include:
8. A method for preparing the thermoplastic polyurethane composition according to claim 1, include: (1) Weighing each component by weight, mixing the crystal modifier and the silane coupling agent, and baking at 75-85° C. for 1-4 hours to obtain a premix; (2) mixing thermoplastic polyurethane TPU with premix and additives; (3) The mixed material is fed into a twin-screw extruder by weight-loss metering, extruded at 150-230° C., granulated and dried to obtain a thermoplastic polyurethane composition.
9. The preparation method according to claim 8, It is characterized in that In the step (3), the length-to-diameter ratio of the twin-screw extruder is 36-60 / 1, and the residence time of the material in the screw is 40-90 seconds.
10. Use of the thermoplastic polyurethane composition according to claim 1 in the field of consumer products.