A latex plugging agent for drilling fluid and preparation method thereof
By using latex sealing agent composed of latex and other components in the drilling fluid, a cross-linked adhesive and dispersed structure is formed, the problem of poor rheology performance after the drilling fluid is mixed is solved, effective sealing of complex formations is achieved, and the wells are reduced Risk of wall rock collapse.
Patent Information
- Application Number
- CN202211734039.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The latex sealing agent in existing drilling fluid has poor rheology performance after mixing with the drilling fluid, making it difficult to effectively seal the tiny cracks in complex formations, resulting in an increased risk of rock collapse in the well wall.
The latex sealing agent for drilling fluid consisting of latex, esters, acrylic acid, sodium polystyrene sulfonate, nanofillers, tetramethylammonium fluoride, dispersants, stabilizers and solvents is used to form a sealing agent by cross-linking and adhesion. The skeleton is plugged, and the sealing performance is improved through the dispersion and graft structure of nanofillers and stabilizers, enhancing adhesion and matching to rocks.
It significantly improves the rheology and sealing performance of the latex film formation system, can effectively seal the tiny cracks in the well wall formation, reduce the risk of rock collapse in the well wall, and is suitable for drilling fluid applications in complex formations.
Smart Images

Figure BDA0004032527290000081 
Figure BDA0004032527290000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of plugging agents, and more specifically, to a latex plugging agent for drilling fluid and a preparation method thereof. Background Art
[0002] At present, with the progress of oil and gas exploration and development, the formation structures encountered are becoming more and more complex. For example, hard and brittle multi-fracture formations are easy-to-collapse formations often encountered in oil drilling. The characteristics of hydration expansion and dispersion of this formation are that it expands very little after encountering water, and the tendency to disperse into fine particles is also very small. At this time, the drilling fluid pressure in the wellbore is transmitted into the multi-fracture well wall formation, which will cause the pore pressure in the well wall zone to increase. When the stress increases to the destruction limit of the rock, the collapse of the well wall rock will be inevitable.
[0003] Therefore, preventing fluid from entering the cracks in the well wall is the key to preventing collapse. Although many drilling fluids currently have natural wall-building properties, which can prevent fluid or reduce the speed of fluid entry to a certain extent, the pore and crack sizes in the rock profile of a long open hole section vary greatly, and the size and gradation of the solid phase particles in the drilling fluid often make it difficult to seal all formations from a broad spectrum perspective.
[0004] In response to the above problems, technicians have developed latex plugging agents, which have the advantages of low fluorescence level and strong temperature resistance. The Chinese patent application with application publication number CN105884954A discloses a temperature-resistant and salt-resistant latex plugging agent, which is prepared from the following raw materials, including hydrophobic monomers, hydrophilic monomers, emulsifiers, buffers, molecular weight regulators, protective agents, initiators and deionized water; wherein, relative to 100 parts by weight of the hydrophobic monomer, the content of the hydrophilic monomer is 0.5-25 parts by weight, the content of the emulsifier is 0.1-10 parts by weight, the content of the buffer is 0.01-5.5 parts by weight, the content of the molecular weight regulator is 0.01-4.5 parts by weight, the content of the protective agent is 0.01-6.9 parts by weight, and the content of the initiator is 0.01-2.3 parts by weight, which has good plugging and water loss reduction effects.
[0005] The above-mentioned latex plugging agent contains more hydrophobic and emulsified components, which can easily cause the drilling fluid system to foam and become unstable, and the rheological properties to decrease. Summary of the invention
[0006] In order to improve the problem of poor rheological properties of a latex plugging agent after mixing with a drilling fluid, the present application provides a latex plugging agent for drilling fluid and a preparation method thereof.
[0007] In the first aspect, the present application provides a latex plugging agent for drilling fluid, which adopts the following technical solution:
[0008] A latex plugging agent for drilling fluid is mainly prepared from the following raw materials in parts by weight: 80-100 parts of latex, 10-15 parts of esters, 5-12 parts of acrylic acid, 3-6 parts of sodium polystyrene sulfonate, 2-5 parts of nano fillers, 1-2 parts of tetramethylammonium fluoride, 0.5-1 parts of dispersants, 5-10 parts of stabilizers, and 20-35 parts of solvents; the esters are one of vinyl acetate, methyl acrylate, and isooctyl methacrylate; the stabilizer is composed of alkylbenzenesulfonic acid triethanolamine salt, hydroxyethyl urea, and hexamethyldisiloxane in a molar ratio of (5-8):(1.2-1.75):(3-5).
[0009] By adopting the above technical scheme, latex, esters, acrylic acid and solvents are mixed and reacted to form an emulsion-like film-forming system. The latex particles in the film-forming system can cross-link and aggregate to form a plugging skeleton, thereby playing a good plugging role in the cracks in the well wall formation. At the same time, nanofillers, polystyrene, and tetramethylammonium fluoride are evenly dispersed in the film-forming system under the action of the dispersant, and then fill the smaller gaps, improve the density of the plugging skeleton structure, and improve the adhesion and plugging effect of the latex film-forming system on the rock. In addition, the alkylbenzenesulfonic acid triethanolamine salt in the stabilizer is cross-linked and grafted with the film-forming system, and its own large steric hindrance is used to improve the rheological properties of the film-forming system, so that it has a better size matching with the tiny cracks in the formation, and can penetrate deep into the cracks, with a better plugging effect. In addition, hydroxyethyl urea and hexamethyldisiloxane molecules have polar groups such as ether bonds and urea groups, which can assist the stable dispersion of alkylbenzenesulfonic acid triethanolamine salt in the film-forming system, reduce the probability of foaming and segregation of the film-forming system, and have better compatibility when mixed with drilling fluid. They can stably physically and chemically plug microcracks in the well wall formation and improve the stability of the plugging structure.
[0010] Preferably, the alkylbenzenesulfonate triethanolamine salt is at least one of dodecylbenzenesulfonate triethanolamine salt and hexadecylbenzenesulfonate triethanolamine salt.
[0011] By adopting the above technical solution, the type of alkylbenzenesulfonic acid triethanolamine salt is optimized and adjusted, and the appropriate steric hindrance is selected to improve the cross-linking state in the film-forming system, thereby further improving the rheological properties of the film-forming system.
[0012] Preferably, the alkylbenzenesulfonate triethanolamine salt is composed of dodecylbenzenesulfonate triethanolamine salt and hexadecylbenzenesulfonate triethanolamine salt in a molar ratio of (7-15):(3-8).
[0013] By adopting the above technical scheme, the ratio of dodecylbenzenesulfonic acid triethanolamine salt and hexadecylbenzenesulfonic acid triethanolamine salt was further tested to balance the steric hindrance and cohesion performance, improve the interface state of the film-forming system, and enhance the plugging performance of the plugging agent.
[0014] Preferably, the mass ratio of the latex to the stabilizer is (8-10):1.
[0015] By adopting the above technical solution, the ratio of latex to stabilizer is optimized and adjusted, so as to ensure the rheological properties of the latex film-forming system without causing a significant impact on the adhesion and blocking properties, thereby improving the overall comprehensive performance of the blocking agent.
[0016] Preferably, the nanofiller is at least one of nano calcium carbonate, nano barium sulfate, nano calcium sulfate, nano silicon dioxide, and nano zinc oxide.
[0017] By adopting the above technical solution, the types of nanofillers are optimized and adjusted, which can improve the compatibility of nanofillers with the film-forming system and reduce the probability of nanofiller agglomeration. On the other hand, the gradation of nanofillers is improved, which improves the blocking effect of the film-forming system on fine cracks.
[0018] Preferably, the solvent is composed of water, urea and dimethyl sulfoxide in a mass ratio of (10-15):(0.2-0.5):(0.8-1.5).
[0019] By adopting the above technical scheme, testing and adjusting the composition ratio of the solvent, the compatibility of the components in the latex film-forming system is promoted, the stability of the film-forming system is improved, and the rheological properties are not easily reduced due to environmental changes.
[0020] Preferably, the raw materials further include 1.5-2 parts by weight of polyquaternary ammonium salt.
[0021] By adopting the above technical solution, after adding polyquaternary ammonium salt, its molecule has a hydrophilic main chain and a hydrophobic long chain, and long chain entanglement and association occur in the film-forming system, so that the fluid dynamics volume in the film-forming system is increased, and the rheological properties and plugging properties of the latex film-forming system are further improved.
[0022] In a second aspect, the present application provides a method for preparing a latex plugging agent for drilling fluid, which adopts the following technical solution:
[0023] A method for preparing a latex plugging agent for drilling fluid comprises the following steps:
[0024] S1: uniformly mixing the formulated amount of latex, esters, acrylic acid, tetrabutylammonium fluoride and solvent to prepare a precursor solution;
[0025] S2: Evenly mix the precursor solution, sodium polystyrene sulfonate, nanofiller, dispersant and stabilizer.
[0026] By adopting the above technical scheme, latex, esters, acrylic acid, tetrabutylammonium fluoride and solvent are first mixed to prepare a uniform precursor solution, which is then further mixed and reacted with components such as stabilizers to form a latex film-forming system with good rheological properties, which has a good sealing effect on well wall formation cracks.
[0027] Preferably, step S2 further comprises the step of adding polyquaternary ammonium salt.
[0028] In summary, this application has the following beneficial effects:
[0029] 1. Since the present application adopts a mixed reaction of latex, esters, acrylic acid and solvent to form a latex film-forming system, and a tangled graft structure is formed in the latex film-forming system after adding a stabilizer, the rheological properties and plugging properties of the film-forming system are greatly improved.
[0030] 2. In the present application, it is preferred to use alkylbenzenesulfonic acid triethanolamine salt with suitable steric hindrance to further improve the interface state and rheological properties of the latex film-forming system.
[0031] 3. The latex plugging for drilling fluid prepared by the preparation method of the present application can be used as drilling fluid for complex formations and has good rheological properties and plugging properties. DETAILED DESCRIPTION
[0032] The present application is further described in detail below with reference to the embodiments.
[0033] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.
[0034] Example
[0035] Example 1
[0036] The latex plugging agent for drilling fluid in this embodiment is made of the following raw materials by weight: 100 kg of latex, 10 kg of esters, 5 kg of acrylic acid, 6 kg of sodium polystyrene sulfonate, 2 kg of nanofiller, 1 kg of tetramethylammonium fluoride, 1 kg of dispersant, 5 kg of stabilizer, and 35 kg of solvent; the stabilizer is composed of triethanolamine dodecylbenzenesulfonate, hydroxyethyl urea, and hexamethyldisiloxane in a molar ratio of 5:1.75:3.
[0037] The latex is styrene acrylic latex, the ester is methyl acrylate, the nano filler is nano calcium carbonate, the dispersant is butyl acetate, and the solvent is deionized water.
[0038] The preparation method of the latex plugging agent for drilling fluid of this embodiment comprises the following steps:
[0039] S1: Add the formulated amount of latex, ester, acrylic acid, tetramethylammonium fluoride and solvent into a reaction kettle and mix them evenly, then heat to 80°C and react at a stirring speed of 150 rpm for 20 minutes to obtain a precursor solution;
[0040] S2: Add sodium polystyrene sulfonate, nanofiller, dispersant and stabilizer into the precursor solution and continue stirring for 90 minutes.
[0041] Example 2
[0042] The latex plugging agent for drilling fluid in this embodiment is made of the following raw materials by weight: 80 kg of latex, 15 kg of esters, 12 kg of acrylic acid, 3 kg of sodium polystyrene sulfonate, 5 kg of nanofiller, 2 kg of tetramethylammonium fluoride, 0.5 kg of dispersant, 10 kg of stabilizer, and 20 kg of solvent; the stabilizer is composed of triethanolamine dodecylbenzenesulfonate, hydroxyethyl urea, and hexamethyldisiloxane in a molar ratio of 5:1.75:3.
[0043] The latex is carboxylated nitrile latex, the ester is vinyl acetate, the nanofiller is nano silicon dioxide, the dispersant is xanthan gum, and the solvent is water.
[0044] The preparation method of the latex plugging agent for drilling fluid of this embodiment comprises the following steps:
[0045] S1: Add the formulated amount of latex, ester, acrylic acid, tetramethylammonium fluoride and solvent into a reaction kettle and mix them evenly, then heat to 90° C. and react at a stirring speed of 200 rpm for 30 minutes to obtain a precursor solution;
[0046] S2: Add sodium polystyrene sulfonate, nanofiller, dispersant and stabilizer into the precursor solution and continue stirring for 150 minutes.
[0047] Example 3
[0048] The latex plugging agent for drilling fluid in this embodiment is made of the following raw materials by weight: 90 kg of latex, 12 kg of esters, 10 kg of acrylic acid, 3.5 kg of sodium polystyrene sulfonate, 3.5 kg of nanofiller, 1.2 kg of tetramethylammonium fluoride, 0.8 kg of dispersant, 8.5 kg of stabilizer, and 25 kg of solvent; the stabilizer is composed of triethanolamine dodecylbenzenesulfonate, hydroxyethyl urea, and hexamethyldisiloxane in a molar ratio of 5:1.75:3.
[0049] The latex is EPDM latex. The ester is isooctyl methacrylate. The nanofiller is nano barium sulfate. The dispersant is guar gum. The solvent is composed of deionized water and urea in a mass ratio of 20:0.3.
[0050] The preparation method of the latex plugging agent for drilling fluid of this embodiment comprises the following steps:
[0051] S1: Add the formulated amount of latex, ester, acrylic acid, tetramethylammonium fluoride and solvent into a reaction kettle and mix them evenly, then heat to 85°C and react at a stirring speed of 180 rpm for 25 minutes to obtain a precursor solution;
[0052] S2: Add sodium polystyrene sulfonate, nanofiller, dispersant and stabilizer into the precursor solution and continue stirring for 120 minutes.
[0053] Example 4
[0054] The difference between the latex plugging agent for drilling fluid in this embodiment and that in embodiment 3 is that the stabilizer in the raw materials is composed of triethanolamine dodecylbenzenesulfonate, hydroxyethyl urea, and hexamethyldisiloxane in a molar ratio of 8:1.2:5, and the rest is the same as in embodiment 3.
[0055] The preparation method of the latex plugging agent for drilling fluid in this embodiment is the same as that in Example 3.
[0056] Example 5
[0057] The difference between the latex plugging agent for drilling fluid in this embodiment and that in embodiment 3 is that the stabilizer in the raw materials is composed of triethanolamine dodecylbenzenesulfonate, hydroxyethyl urea, and hexamethyldisiloxane in a molar ratio of 5.5:1.3:4.2, and the rest is the same as in embodiment 3.
[0058] The preparation method of the latex plugging agent for drilling fluid in this embodiment is the same as that in Example 3.
[0059] Example 6
[0060] The difference between the latex plugging agent for drilling fluid in this embodiment and that in Embodiment 5 is that the alkylbenzenesulfonate triethanolamine salt in the raw material is hexadecylbenzenesulfonate triethanolamine salt, and the rest is the same as that in Embodiment 5.
[0061] The preparation method of the latex plugging agent for drilling fluid in this embodiment is the same as that in Example 5.
[0062] Example 7
[0063] The latex plugging agent for drilling fluid of this embodiment is different from that of Embodiment 5 in that the alkylbenzenesulfonate triethanolamine salt in the raw material is composed of dodecylbenzenesulfonate triethanolamine salt and hexadecylbenzenesulfonate triethanolamine salt in a molar ratio of 7:8, and the rest is the same as that of Embodiment 5.
[0064] The preparation method of the latex plugging agent for drilling fluid in this embodiment is the same as that in Example 5.
[0065] Example 8
[0066] The difference between the latex plugging agent for drilling fluid in this embodiment and that in Embodiment 5 is that the alkylbenzenesulfonate triethanolamine salt in the raw material is composed of dodecylbenzenesulfonate triethanolamine salt and hexadecylbenzenesulfonate triethanolamine salt in a molar ratio of 15:3, and the rest is the same as in Embodiment 5.
[0067] The preparation method of the latex plugging agent for drilling fluid in this embodiment is the same as that in Example 5.
[0068] Example 9
[0069] The difference between the latex plugging agent for drilling fluid in this embodiment and that in Embodiment 8 is that the nano filler in the raw material is composed of nano calcium sulfate and nano zinc oxide in a mass ratio of 2:1, and the rest is the same as that in Embodiment 8.
[0070] The preparation method of the latex plugging agent for drilling fluid in this embodiment is the same as that in Example 8.
[0071] Example 10
[0072] The difference between the latex plugging agent for drilling fluid in this embodiment and that in Embodiment 9 is that the solvent in the raw materials is composed of water, urea, and dimethyl sulfoxide in a mass ratio of 15:2:0.8, and the rest is the same as that in Embodiment 9.
[0073] The preparation method of the latex plugging agent for drilling fluid in this embodiment is the same as that in Example 9.
[0074] Embodiment 11
[0075] The difference between the latex plugging agent for drilling fluid in this embodiment and that in Embodiment 9 is that the solvent in the raw materials is composed of water, urea, and dimethyl sulfoxide in a mass ratio of 10:3.5:1.5, and the rest is the same as that in Embodiment 9.
[0076] The preparation method of the latex plugging agent for drilling fluid in this embodiment is the same as that in Example 9.
[0077] Example 12
[0078] The difference between the latex plugging agent for drilling fluid in this embodiment and that in Example 10 is that the raw materials further include 1.5 kg of polyquaternary ammonium salt, which is polyquaternary ammonium salt 10, and the rest is the same as in Example 10.
[0079] The preparation method of the latex plugging agent for drilling fluid of this embodiment comprises the following steps:
[0080] S1: Add the formulated amount of latex, ester, acrylic acid, tetramethylammonium fluoride and solvent into a reaction kettle and mix them evenly, then heat to 85°C and react at a stirring speed of 180 rpm for 25 minutes to obtain a precursor solution;
[0081] S2: Add sodium polystyrene sulfonate, nanofiller, dispersant, stabilizer and polyquaternary ammonium salt into the precursor solution and continue stirring for 120 minutes to obtain the product.
[0082] Example 13
[0083] The difference between the latex plugging agent for drilling fluid in this embodiment and that in Example 10 is that the raw materials further include 2 kg of polyquaternary ammonium salt, which is polyquaternary ammonium salt 10, and the rest is the same as in Example 10.
[0084] The preparation method of the latex plugging agent for drilling fluid of this embodiment comprises the following steps:
[0085] S1: Add the formulated amount of latex, ester, acrylic acid, tetramethylammonium fluoride and solvent into a reaction kettle and mix them evenly, then heat to 85°C and react at a stirring speed of 180 rpm for 25 minutes to obtain a precursor solution;
[0086] S2: Add sodium polystyrene sulfonate, nanofiller, dispersant, stabilizer and polyquaternary ammonium salt into the precursor solution and continue stirring for 120 minutes to obtain the product.
[0087] Comparative Example
[0088] Comparative Example 1
[0089] The latex plugging agent for drilling fluid in this comparative example is made of the following raw materials by weight: 105kg of latex, 10kg of esters, 5kg of acrylic acid, 6kg of sodium polystyrene sulfonate, 2kg of nano filler, 1kg of tetramethylammonium fluoride, 1kg of dispersant, and 35kg of solvent.
[0090] The latex is styrene acrylic latex, the ester is methyl acrylate, the nano filler is nano calcium carbonate, and the dispersant is butyl acetate.
[0091] The preparation method of the latex plugging agent for drilling fluid in this comparative example comprises the following steps:
[0092] S1: Add the formulated amount of latex, ester, acrylic acid, tetramethylammonium fluoride and solvent into a reaction kettle and mix them evenly, then heat to 80°C and react at a stirring speed of 150 rpm for 20 minutes to obtain a precursor solution;
[0093] S2: Add sodium polystyrene sulfonate, nanofiller and dispersant into the precursor solution and continue stirring for 90 minutes.
[0094] Comparative Example 2
[0095] The latex plugging agent for drilling fluid in this comparative example is made of the following raw materials by weight: 100 kg of latex, 10 kg of esters, 5 kg of acrylic acid, 6 kg of sodium polystyrene sulfonate, 2 kg of nanofiller, 1 kg of tetramethylammonium fluoride, 1 kg of dispersant, 5 kg of stabilizer, and 35 kg of solvent; the stabilizer is triethanolamine dodecylbenzenesulfonate.
[0096] The latex is styrene acrylic latex, the ester is methyl acrylate, the nano filler is nano calcium carbonate, and the dispersant is butyl acetate.
[0097] The preparation method of the latex plugging agent for drilling fluid in this comparative example comprises the following steps:
[0098] S1: Add the formulated amount of latex, ester, acrylic acid, tetramethylammonium fluoride and solvent into a reaction kettle and mix them evenly, then heat to 80°C and react at a stirring speed of 150 rpm for 20 minutes to obtain a precursor solution;
[0099] S2: Add sodium polystyrene sulfonate, nanofiller, dispersant and stabilizer into the precursor solution and continue stirring for 90 minutes.
[0100] Comparative Example 3
[0101] The latex plugging agent for drilling fluid in this comparative example is made of the following raw materials by weight: 100 kg of latex, 10 kg of esters, 5 kg of acrylic acid, 6 kg of sodium polystyrene sulfonate, 2 kg of nano filler, 1 kg of tetramethylammonium fluoride, 1 kg of dispersant, 5 kg of stabilizer, and 35 kg of solvent; the stabilizer is composed of hydroxyethyl urea and hexamethyldisiloxane in a molar ratio of 1.75:3.
[0102] The latex is styrene acrylic latex, the ester is methyl acrylate, the nano filler is nano calcium carbonate, and the dispersant is butyl acetate.
[0103] The preparation method of the latex plugging agent for drilling fluid in this comparative example comprises the following steps:
[0104] S1: Add the formulated amount of latex, ester, acrylic acid, tetramethylammonium fluoride and solvent into a reaction kettle and mix them evenly, then heat to 80°C and react at a stirring speed of 150 rpm for 20 minutes to obtain a precursor solution;
[0105] S2: Add sodium polystyrene sulfonate, nanofiller, dispersant and stabilizer into the precursor solution and continue stirring for 90 minutes.
[0106] Comparative Example 4
[0107] The latex plugging agent for drilling fluid in this comparative example is made of the following raw materials by weight: 100 kg of latex, 10 kg of esters, 5 kg of acrylic acid, 6 kg of sodium polystyrene sulfonate, 2 kg of nano filler, 1 kg of tetramethylammonium fluoride, 1 kg of dispersant, 5 kg of stabilizer, and 35 kg of solvent; the stabilizer is composed of triethanolamine dodecylbenzenesulfonate and hydroxyethyl urea in a molar ratio of 5:1.75.
[0108] The latex is styrene acrylic latex, the ester is methyl acrylate, the nano filler is nano calcium carbonate, and the dispersant is butyl acetate.
[0109] The preparation method of the latex plugging agent for drilling fluid in this comparative example is the same as that in Example 1.
[0110] Comparative Example 5
[0111] The latex plugging agent for drilling fluid in this comparative example is made of the following raw materials by weight: 100 kg of latex, 10 kg of esters, 5 kg of acrylic acid, 6 kg of sodium polystyrene sulfonate, 2 kg of nano filler, 1 kg of tetramethylammonium fluoride, 1 kg of dispersant, 5 kg of stabilizer, and 35 kg of solvent; the stabilizer is OP-10.
[0112] The latex is styrene acrylic latex, the ester is methyl acrylate, the nano filler is nano calcium carbonate, and the dispersant is butyl acetate.
[0113] The preparation method of the latex plugging agent for drilling fluid in this comparative example is the same as that in Example 1.
[0114] Comparative Example 6
[0115] The difference between the latex plugging agent for drilling fluid in this comparative example and that in Example 5 is that the alkylbenzenesulfonate triethanolamine salt in the raw material is composed of dodecylbenzenesulfonate triethanolamine salt and hexadecylbenzenesulfonate triethanolamine salt in a molar ratio of 5:9, and the rest is the same as in Example 5.
[0116] The preparation method of the latex plugging agent for drilling fluid in this comparative example is the same as that in Example 5.
[0117] Performance testing
[0118] 1) The physical and chemical performance indicators of the drilling fluid latex plugging agent of Examples 1-13 were tested, and the test results are shown in Table 1.
[0119] A. Appearance
[0120] Place an appropriate amount of sample into a clean and dry 50mL colorimetric tube, visually inspect its color and state against a white background, and record it.
[0121] B. Determination of pH value
[0122] Use a glass rod to drop the sample onto the pH test paper, compare the reading with the standard color scale, and record it.
[0123] C. Determination of density
[0124] Density is measured according to GB / T 6750.
[0125] D. Electrolyte stability
[0126] Add 50.00 g NaCl and 200 mL deionized water into a beaker, stir with a glass rod to dissolve, add 5.00 g NSEAL sample, stir evenly, then put into a test tube, let stand at 90 ° C for 2 h, and observe the electrolyte stability.
[0127] E. Sand bed plugging test
[0128] Measure 400 ml of deionized water, add 16 g of sodium chloride, stir at high speed for 20 min, add 16 g of experimental bentonite, stir at high speed for 20 min, and let it stand for 24 hours to prepare the base slurry.
[0129] 400 ml of base slurry was measured and added with 8 ml of the above-mentioned latex plugging agent for drilling fluid, and stirred at high speed for 20 min. The sand bed plugging permeability loss was measured on the FA sand bed plugging instrument.
[0130] Table 1 Physical and chemical performance index test data of latex plugging agent for drilling fluid of Examples 1-13
[0131]
[0132]
[0133] 2) Drilling fluid was prepared according to GB / T5005-2010 standard, and the latex plugging agents for drilling fluid of Examples 1-13 and Comparative Examples 1-6 were added respectively. Then, the plugging performance was tested according to GB / T16783.1-2014, wherein AV is the apparent viscosity; FL is the plugging instrument leakage under the condition of 60 min / 3000 psi. The test results are shown in Table 2.
[0134] Table 2 Plugging performance test data of latex plugging agents for drilling fluids of Examples 1-13 and Comparative Examples 1-6
[0135] Serial number AV(mpa·s) FL(ml) Example 1 5.2 46 Example 2 5.5 60 Example 3 5.0 41 Example 4 5.1 45 Example 5 4.6 32 Example 6 4.8 38 Example 7 4.3 32 Example 8 4.0 29 Example 9 4.0 25 Example 10 3.2 17 Embodiment 11 3.5 20 Example 12 2.9 13 Example 13 2.5 10 Comparative Example 1 9.5 106 Comparative Example 2 7.7 85 Comparative Example 3 6.5 62 Comparative Example 4 7.0 73 Comparative Example 5 8.1 93 Comparative Example 6 4.5 30
[0136] It can be seen from the analysis of Examples 1-3, Examples 4-5 and Comparative Examples 1-5 and combined with Table 1 that the composition ratio of the latex plugging agent is optimized and adjusted, and the addition of the stabilizer can effectively improve the rheological properties and plugging properties of the drilling fluid-plugging agent mixed system. It can be seen that the apparent viscosity of Example 3 is reduced by about 47% compared with Comparative Example 1 without adding a stabilizer. In addition, the plugging instrument leakage under the condition of 60min / 3000psi is only 41ml, and the plugging state is very good. In addition, it can be seen from the analysis of Examples 4-5 and Comparative Examples 2-4 that when alkylbenzenesulfonic acid triethanolamine salt is used alone, it may be unevenly distributed in the latex film-forming system due to the effect of steric hindrance, resulting in a decrease in the rheological properties of the film-forming system. After adding hydroxyethyl urea and hexamethyldisiloxane, the winding and grafting of alkylbenzenesulfonic acid triethanolamine salt in the film-forming system are effectively promoted, and the rheological properties and interface bonding state of the latex film-forming system are improved. It can be seen that compared with Comparative Example 2, the apparent viscosity of Example 5 is reduced by about 40%. Moreover, compared with the conventional stabilizer OP-10, the apparent viscosity of Example 5 decreased by about 43%.
[0137] Analysis of Examples 6-8 and Comparative Example 6 in combination with Table 1 shows that further optimization and adjustment of alkylbenzenesulfonic acid triethanolamine salt improves the rheological properties and plugging properties of the latex film-forming system, and the apparent viscosity of Example 8 decreases by about 12.5% compared with Comparative Example 6.
[0138] It can be seen from the analysis of Example 9, Example 10-11, and Example 12-13 in combination with Table 1 that the composition ratio of the nanofiller is optimized, and urea and dimethyl sulfoxide are added to the solvent to promote the compatibility of the components of the film-forming system, so that it has better matching with the cracks in the well wall formation. And after adding the polyquaternary ammonium salt, long chain entanglement and association are promoted in the film-forming system, so that the fluid mechanics volume in the film-forming system is increased. It can be seen that compared with Example 8, the apparent viscosity of Example 13 has decreased by about 37.5, and the plugging instrument leakage under the condition of 60min / 3000psi has decreased by about 65.5%. The plugging performance and rheological properties are better, and it is very suitable for compounding with drilling fluids of various complex formations.
[0139] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A latex plugging agent for drilling fluid, characterized in that: The invention is mainly prepared from the following raw materials in parts by weight: 80-100 parts of latex, 10-15 parts of esters, 5-12 parts of acrylic acid, 3-6 parts of sodium polystyrene sulfonate, 2-5 parts of nano fillers, 1-2 parts of tetramethylammonium fluoride, 0.5-1 parts of dispersants, 5-10 parts of stabilizers, and 20-35 parts of solvents; the esters are one of vinyl acetate, methyl acrylate, and isooctyl methacrylate; the stabilizers are composed of alkylbenzene sulfonic acid triethanolamine salt, hydroxyethyl urea, and hexamethyldisiloxane in a molar ratio of (5-8):(1.2-1.75):(3-5); The latex is any one of styrene acrylic latex, carboxylated nitrile latex, and EPDM latex; The nano filler is at least one of nano calcium carbonate, nano barium sulfate, nano calcium sulfate, nano silicon dioxide, and nano zinc oxide; The raw materials also include 1.5-2 parts by weight of polyquaternary ammonium salt.
2. A latex plugging agent for drilling fluid according to claim 1, characterized in that: The alkylbenzenesulfonate triethanolamine salt is at least one of dodecylbenzenesulfonate triethanolamine salt and hexadecylbenzenesulfonate triethanolamine salt.
3. A latex plugging agent for drilling fluid according to claim 2, characterized in that: The alkylbenzenesulfonic acid triethanolamine salt is composed of dodecylbenzenesulfonic acid triethanolamine salt and hexadecylbenzenesulfonic acid triethanolamine salt in a molar ratio of (7-15):(3-8).
4. The latex plugging agent for drilling fluid according to claim 1, characterized in that: The mass ratio of the latex to the stabilizer is (8-10):
1.
5. The latex plugging agent for drilling fluid according to claim 1, characterized in that: The solvent is composed of water, urea and dimethyl sulfoxide in a mass ratio of (10-15):(0.2-0.5):(0.8-1.5).
6. A method for preparing a latex plugging agent for drilling fluid according to any one of claims 1 to 5, characterized in that: The steps include: S1: uniformly mixing the formulated amount of latex, esters, acrylic acid, tetrabutylammonium fluoride and solvent to prepare a precursor solution; S2: The precursor solution, sodium polystyrene sulfonate, nanofiller, dispersant and stabilizer are mixed evenly; The step S2 also includes the step of adding polyquaternary ammonium salt.
Citation Information
Patent Citations
Temperature-resistant and salt-resistant latex blocking agent and preparation method thereof
CN105884954A
Preparation method of shale micro / nano particle plugging agent for water-base drilling fluids
CN104762071A
Resin type nanoparticle latex blocking agent for drilling fluids and preparation method of blocking agent
CN105462568A
Preparation method of latex plugging agent for drilling fluids, and drilling fluid
CN109666465A
Nanometer latex micro-crack plugging agent, and preparation method thereof
CN110330955A