Preparation method of high-efficiency aldehyde removal liquid, product and application thereof
By using microcapsule-encapsulated nano zinc oxide particles, the problem of white spots and damage easily occurring on the surface of organic furniture by photocatalytic formaldehyde removers has been solved, achieving the effect of highly efficient formaldehyde removal without leaving white spots.
Patent Information
- Application Number
- CN202310911079.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-24
- Publication Date
- 2025-10-17
- Estimated Expiration
- 2043-07-24
AI Technical Summary
Existing photocatalytic formaldehyde removal agents tend to produce white spots when sprayed on organic furniture surfaces and can damage the organic materials. They are difficult to use universally on different furniture surfaces without leaving white spots.
The photocatalytically active nano-zinc oxide particles are encapsulated in microcapsules. By modifying the surface of the nano-zinc oxide and using microcapsule encapsulation technology, the damage to the organic substrate material caused by the photocatalytic oxidation reaction is avoided. Furthermore, the microcapsule particles are supported by a three-dimensional network structure to ensure that they do not leave white spots on the surface of furniture made of different materials.
It achieves efficient formaldehyde removal from furniture surfaces of different materials without leaving white spots or damaging organic materials, and exhibits good stability.
Smart Images

Figure FT_1 
Figure SMS_1
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the field of catalysis, and relates to a preparation method of high-efficiency formaldehyde removal liquid, the product and application thereof, in particular to high-efficiency formaldehyde removal liquid which is suitable for different material furniture surfaces and does not leave white spots and does not damage organic material furniture. BACKGROUND
[0002] The materials such as plywood, composite floor, door, wardrobe and cabinet used in home decoration will release formaldehyde. Due to the special irritating taste of formaldehyde, the human body will produce various uncomfortable symptoms when contacting formaldehyde gas with a certain concentration. The national standard GB50325-2020 "Code for Indoor Environmental Pollution Control of Civil Building Engineering" stipulates that the concentration of formaldehyde in the indoor environment should be lower than 0.08 mg / m 3 . The common methods for removing formaldehyde in the indoor environment include ventilation, activated carbon adsorption or green plant adsorption, and photocatalyst type formaldehyde removal agent products. Ventilation cannot fundamentally eliminate formaldehyde, and the adsorption rate of activated carbon or green plants is slow. The photocatalyst type formaldehyde removal agent product is used more and more widely because of high formaldehyde removal efficiency and safety and environmental protection. The photocatalyst type formaldehyde removal agent product usually uses the photocatalytic effect of semiconductor materials such as zinc oxide, cadmium sulfide, carbonized nitrogen, bismuth oxide, oxide and titanium dioxide to remove formaldehyde. When light (ultraviolet) irradiates the semiconductor particles, electrons are released from the surface of the semiconductor particles, generating holes. The generated holes take electrons from the surrounding hydroxide ions (OH - ) and the like to generate OH· free radicals. OH· free radicals have strong oxidizing power and decompose formaldehyde by taking electrons from formaldehyde. Because of the photocatalytic degradation characteristics, the product is sprayed on the surface of furniture, especially the surface of organic materials such as fabric and leather, which will damage these materials. Therefore, during construction, it is often required to cover the leather sofa, wool carpet and the like before construction. In addition, in order to obtain high formaldehyde removal efficiency, the size of the semiconductor material particles in the photocatalyst type formaldehyde removal agent is usually in the submicron or even nanometer scale, so that the characteristics of nanometer materials can be better played, and then high photocatalytic activity is obtained. However, because the semiconductor material particles are in a dispersed state in the product, after being sprayed on the surface of the construction object, the solvent in the product volatilizes and dries, and the semiconductor material particles will deposit on the surface of the construction object, that is, the so-called white spots are generated. For furniture articles with surface pores such as wallpaper, sofa and carpet, the above-mentioned white spots will penetrate into them and are difficult to remove, thereby affecting the appearance. Therefore, there is a need in the market for a high-efficiency formaldehyde removal agent which can be used on different material furniture surfaces without leaving white spots and does not damage organic material furniture. SUMMARY
[0003] The application aims to provide a preparation method of high-efficiency formaldehyde removal liquid which is suitable for different material furniture surfaces and does not leave white spots and does not damage organic material furniture.
[0004] The object of the present application is achieved by the following solution:
[0005] A preparation method of high-efficiency aldehyde removal liquid, characterized by adopting microcapsule coated photocatalytic active nano-zinc oxide particles, which can play the function of removing formaldehyde and avoid the damage of photocatalytic oxidation reaction to the base organic material due to the isolation of the microcapsule wall material, comprising the following steps:
[0006] 1) Surface modification of nano-zinc oxide: under stirring conditions, 50.0 parts by weight of nano-zinc oxide powder is added into the same weight of anhydrous ethanol, after the nano-zinc oxide powder is uniformly dispersed, the temperature is raised to 75-80 ℃, 0.5-1.0 parts by weight of titanate coupling agent is added under stirring conditions, and the reaction is carried out for 1-2 h. After natural cooling to room temperature, the solid material is filtered and dried in an oven at 60-80 ℃ for 10-12 h to recover the modified nano-zinc oxide powder.
[0007] 2) Preparation of microcapsule water dispersion liquid coated with modified nano-zinc oxide: 2.0-5.0 parts by weight of modified nano-zinc oxide powder prepared in step 1) is mixed with 8.0-15.0 parts by weight of a mixture of methyl methacrylate, butyl acrylate and acrylic acid to form an oil phase, then the oil phase is added to a water phase formed by 1.6-3.8 parts by weight of emulsifier and 76.0-88.3 parts by weight of deionized water, emulsified to obtain an oil / water emulsion; the oil / water emulsion is heated to 80-85 ℃, 0.1-0.2 parts by weight of initiator potassium persulfate is added dropwise, and the polymerization reaction is carried out for 2-4 h, and then the temperature is naturally cooled to room temperature to obtain a microcapsule water dispersion liquid coated with modified nano-zinc oxide.
[0008] 3) Preparation of aldehyde removal liquid: 20.0-50.0 parts by weight of the microcapsule water dispersion liquid coated with modified nano-zinc oxide prepared in step 2), 0.1-0.2 parts by weight of isomeric alcohol polyoxyethylene ether, 0.2-0.4 parts by weight of triethanolamine, 0.5-1.0 parts by weight of water-soluble resin, 0.1-0.2 parts by weight of sodium carboxymethyl cellulose and 48.2-79.1 parts by weight of deionized water are stirred uniformly to obtain the aldehyde removal liquid.
[0009] The titanate coupling agent is a chelated titanate.
[0010] The emulsifier is a mixture of OP-10 and SDS, and the mass ratio of OP-10 to SDS is 4-2:1.
[0011] The water-soluble resin is polyvinylpyrrolidone.
[0012] The particle size D90 of the microcapsule coated with modified nano-zinc oxide in the aldehyde removal liquid is 200-300 nm.
[0013] The application also provides the high-efficiency aldehyde removal liquid prepared by any of the above methods.
[0014] The application also provides application of the high-efficiency aldehyde removal liquid in furniture formaldehyde removal, which is used for furniture surfaces of different materials without leaving white spots and does not damage organic material furniture.
[0015] The laser particle size instrument is used to test the particle size of the aldehyde removal liquid prepared in the examples. The aldehyde removal performance of the aldehyde removal liquid is evaluated according to the light industry standard QB / T2761-2006 “Method for testing purification effect of indoor air purification products”, and the residual situation of the aldehyde removal liquid on the surface of the cloth sofa after use and the damage to the surface of the leather sofa are observed by naked eyes.
[0016] Compared with the prior art, the application has the following advantages:
[0017] 1. The aldehyde removal liquid of the application uses microcapsules to coat the photocatalytically active nano-zinc oxide particles, which can play the function of removing formaldehyde and avoid damage to the substrate organic material caused by photocatalytic oxidation reaction due to the isolation of the microcapsule wall material.
[0018] 2. The microcapsules in the aldehyde removal liquid have a suitable size and are not easy to penetrate into the interior of porous materials such as fabrics and wood, so they can be easily wiped clean and will not cause white spot residues affecting the appearance.
[0019] 3. The application uses water-soluble resin polyvinylpyrrolidone and sodium carboxymethyl cellulose to construct a three-dimensional network structure, which can well support the microcapsule particles, and the aldehyde removal liquid has good stability. BRIEF DESCRIPTION OF DRAWINGS
[0020] Figure 1 The particle size distribution curve of the microcapsules coated with modified nano-zinc oxide in the aldehyde removal liquid prepared in Example 1 is shown in the figure. DETAILED DESCRIPTION
[0021] The technical solutions of the application will be further described below according to specific examples. The protection scope of the application is not limited to the following examples, and these examples are listed only for illustrative purposes and do not limit the application in any way.
[0022] Example 1
[0023] A high-efficiency aldehyde removal liquid is prepared by using microcapsules to coat photocatalytically active nano-zinc oxide particles, which can play the function of removing formaldehyde and avoid damage to the substrate organic material caused by photocatalytic oxidation reaction due to the isolation of the microcapsule wall material, according to the following steps:
[0024] 1) Surface modification of nano-zinc oxide:
[0025] Under stirring condition, 50.0 parts by weight of nano-zinc oxide powder was added into equal weight of anhydrous ethanol, and after the nano-zinc oxide powder was uniformly dispersed, the temperature was raised to 75 ℃, and under stirring condition, 0.5 parts by weight of titanate coupling agent KR-138S was added, and reacted for 1 h; after natural cooling to room temperature, the solid substance was filtered, and dried in a 60 ℃ oven for 12 h, to recover the modified nano-zinc oxide powder;
[0026] 2) Preparation of microcapsule water dispersion of coated modified nano-zinc oxide:
[0027] 2.0 parts by weight of the modified nano-zinc oxide powder prepared in step 1) was uniformly mixed with a mixture of 3.0 parts by weight of methyl methacrylate, 3.0 parts by weight of butyl acrylate and 2.0 parts by weight of acrylic acid to form an oil phase, and then the oil phase was added into an aqueous phase formed by 1.3 parts by weight of emulsifier OP-10 and 0.3 parts by weight of SDS and 88.3 parts by weight of deionized water, to obtain an oil / water emulsion; the oil / water emulsion was heated to 85 ℃, and 0.1 parts by weight of initiator potassium persulfate was added dropwise, and polymerized for 2 h, and then naturally cooled to room temperature, to obtain a microcapsule water dispersion of coated modified nano-zinc oxide;
[0028] 3) Preparation of aldehyde removal liquid: 50.0 parts by weight of the microcapsule water dispersion of coated modified nano-zinc oxide prepared in step 2), 0.2 parts by weight of isomeric alcohol polyoxyethylene ether, 0.4 parts by weight of triethanolamine, 1.0 parts by weight of water-soluble resin, 0.1 parts by weight of sodium carboxymethyl cellulose and 48.2 parts by weight of deionized water were uniformly stirred, to obtain an aldehyde removal liquid. The particle size distribution curve of the microcapsule water of coated modified nano-zinc oxide in the prepared aldehyde removal liquid is shown in Figure 1 .
[0029] The aldehyde removal liquid obtained in the example is suitable for furniture surfaces of different materials without leaving white spots.
[0030] Example 2
[0031] A high-efficiency aldehyde removal liquid was prepared according to the following steps, which were similar to those in step of example 1.
[0032] 1) Surface modification of nano-zinc oxide:
[0033] Under stirring condition, 50.0 parts by weight of nano-zinc oxide powder was added into equal weight of anhydrous ethanol, and after the nano-zinc oxide powder was uniformly dispersed, the temperature was raised to 75 ℃, and under stirring condition, 1.0 parts by weight of titanate coupling agent was added, and reacted for 2 h; after natural cooling to room temperature, the solid substance was filtered, and dried in an 80 ℃ oven for 10 h, to recover the modified nano-zinc oxide powder;
[0034] 2) Preparation of microcapsule water dispersion of coated modified nano-zinc oxide:
[0035] 5.0 parts by weight of the modified nano-zinc oxide powder prepared in step 1) was mixed with a mixture of 5.0 parts by weight of methyl methacrylate, 5.0 parts by weight of butyl acrylate and 5.0 parts by weight of acrylic acid to form an oil phase, which was then added to an aqueous phase formed by 2.5 parts by weight of OP-10 and 1.3 parts by weight of SDS as emulsifiers and 76.1 parts by weight of deionized water, emulsified to obtain an oil / water emulsion; the oil / water emulsion was heated to 80 ℃, and 0.2 parts by weight of initiator potassium persulfate was added dropwise, and the polymerization reaction was carried out for 4 h, and then naturally cooled to room temperature to obtain a microcapsule water dispersion of modified nano-zinc oxide coated with;
[0036] 3) Preparation of aldehyde removal liquid: 20.0 parts by weight of the microcapsule water dispersion of modified nano-zinc oxide coated with prepared in step 2), 0.1 parts by weight of isomeric alcohol polyoxyethylene ether, 0.2 parts by weight of triethanolamine, 0.5 parts by weight of water-soluble resin, 0.2 parts by weight of sodium carboxymethyl cellulose and 79.1 parts by weight of deionized water were stirred uniformly to obtain an aldehyde removal liquid.
[0037] The aldehyde removal liquid obtained in this example is suitable for different material furniture surfaces without leaving white spots.
[0038] Example 3
[0039] An efficient aldehyde removal liquid is prepared by using microcapsules to coat nano-zinc oxide particles with photocatalytic activity, which can remove formaldehyde while avoiding damage to the substrate organic material caused by photocatalytic oxidation due to the isolation of the microcapsule wall material, according to the following steps:
[0040] 1) Surface modification of nano-zinc oxide:
[0041] Under stirring conditions, 50.0 parts by weight of nano-zinc oxide powder was added to the same weight of anhydrous ethanol, and after the nano-zinc oxide powder was uniformly dispersed, it was heated to 80 ℃, and 0.7 parts by weight of titanium ester coupling agent was added under stirring conditions, and the reaction was carried out for 1.5 h; after natural cooling to room temperature, the solid material was filtered and dried in a 70 ℃ oven for 11 h to recover the modified nano-zinc oxide powder;
[0042] 2) Preparation of microcapsule water dispersion of modified nano-zinc oxide coated with:
[0043] The modified nano-zinc oxide powder prepared in step 1) is mixed with a mixture of 4.0 parts by weight of methyl methacrylate, 4.0 parts by weight of butyl acrylate and 4.3 parts by weight of acrylic acid to form an oil phase, which is then added to an aqueous phase formed by 2.1 parts by weight of OP-10, 0.7 parts by weight of SDS emulsifier and 81.25 parts by weight of deionized water, emulsified to obtain an oil / water emulsion; the oil / water emulsion is heated to 80 DEG C, and 0.15 parts by weight of initiator potassium persulfate is added dropwise, and the polymerization reaction is carried out for 3 hours, and then the reaction system is naturally cooled to room temperature to obtain a microcapsule water dispersion of modified nano-zinc oxide coated with the modified nano-zinc oxide;
[0044] 3) Preparation of aldehyde removal liquid: 28.6 parts by weight of the microcapsule water dispersion of modified nano-zinc oxide coated with the modified nano-zinc oxide prepared in step 2), 0.15 parts by weight of isomeric alcohol polyoxyethylene ether, 0.3 parts by weight of triethanolamine, 0.7 parts by weight of water-soluble resin, 0.15 parts by weight of sodium carboxymethyl cellulose and 70.1 parts by weight of deionized water are stirred uniformly to obtain an aldehyde removal liquid.
[0045] The aldehyde removal liquid obtained in the example is suitable for different material furniture surfaces without leaving white spots.
[0046] The aldehyde removal liquid prepared in examples 1-3 is subjected to particle size test by using a laser particle size analyzer; the aldehyde removal performance of the aldehyde removal liquid is evaluated according to the light industry standard QB / T 2761-2006 "Method for testing the purification effect of indoor air purification products"; at the same time, the residual situation of the aldehyde removal liquid on the surface of a cloth sofa after use is observed by naked eyes, and the damage to the surface of a leather sofa is observed, and the data are shown in Table 1:
[0047]
[0048] It can be seen that the aldehyde removal liquid provided by the application has high formaldehyde removal effect, is suitable for different material furniture surfaces without leaving white spots, and has no damage to organic material furniture.
[0049] Those skilled in the art should note that the embodiments described in the application are only exemplary, and various other alternatives, changes and improvements can be made within the scope of the application. Thus, the application is not limited to the above-described embodiments, but is only limited by the claims.
Claims
1. A method for preparing an efficient formaldehyde removal solution, characterized in that: By using microcapsules to encapsulate nano zinc oxide particles with photocatalytic activity, while performing the formaldehyde removal function, the isolation of the microcapsule wall material prevents the photocatalytic oxidation reaction from damaging the base organic material. The process includes the following steps: 1) Surface modification of nano zinc oxide: 50.0 parts by weight of nano zinc oxide powder was added to an equal part by weight of anhydrous ethanol under stirring. After the nano zinc oxide powder was evenly dispersed, the temperature was raised to 75-80°C, and 0.5-1.0 parts by weight of a titanate coupling agent was added under stirring. The mixture was reacted for 1-2 hours. After naturally cooling to room temperature, the solid was filtered to obtain a solid substance, which was placed in an oven at 60-80°C and dried for 10-12 hours to obtain the modified nano zinc oxide powder. 2) Preparation of aqueous dispersion of microcapsules coated with modified nano zinc oxide: 2.0-5.0 parts by weight of the modified nano-zinc oxide powder prepared in step 1) and 8.0-15.0 parts by weight of a mixture of methyl methacrylate, butyl acrylate, and acrylic acid are uniformly mixed to form an oil phase, and then the oil phase is added to an aqueous phase formed by 1.6-3.8 parts by weight of an emulsifier and 76.0-88.3 parts by weight of deionized water, and emulsified to obtain an oil / water emulsion; the oil / water emulsion is heated to 80-85°C, and 0.1-0.2 parts by weight of potassium persulfate as an initiator is added dropwise, and a polymerization reaction is carried out for 2-4 hours, and the mixture is naturally cooled to room temperature to obtain an aqueous dispersion of microcapsules coated with the modified nano-zinc oxide; 3) Preparation of formaldehyde removal solution: 20.0-50.0 parts by weight of the aqueous dispersion of microcapsules coated with modified nano-zinc oxide prepared in step 2), 0.1-0.2 parts by weight of isomeric alcohol polyoxyethylene ether, 0.2-0.4 parts by weight of triethanolamine, 0.5-1.0 parts by weight of a water-soluble resin, 0.1-0.2 parts by weight of sodium carboxymethyl cellulose, and 48.2-79.1 parts by weight of deionized water are uniformly stirred to obtain a formaldehyde removal solution; The titanate coupling agent is a chelate titanate; The emulsifier is a mixture of OP-10 and SDS, and the mass ratio of OP-10 to SDS is 4 to 2:1; The water-soluble resin is polyvinyl pyrrolidone.
2. The method for preparing a high-efficiency aldehyde-removing liquid according to claim 1, wherein The particle size D90 of the microcapsules coated with modified nano zinc oxide in the formaldehyde removal solution is 200-300 nm.
3. The method for preparing the high-efficiency formaldehyde removal solution according to any one of claims 1 to 2, characterized in that: Prepare as follows: 1) Surface modification of nano zinc oxide: 50.0 parts by weight of nano-zinc oxide powder was added to an equal part by weight of anhydrous ethanol under stirring. After the nano-zinc oxide powder was evenly dispersed, the temperature was raised to 80°C, and 0.7 parts by weight of a titanate coupling agent was added under stirring. The mixture was reacted for 1.5 hours. After naturally cooling to room temperature, the solid was filtered and dried in a 70°C oven for 11 hours to recover the modified nano-zinc oxide powder. 2) Preparation of aqueous dispersion of microcapsules coated with modified nano zinc oxide: 3.5 parts by weight of the modified nano-zinc oxide powder prepared in step 1) were uniformly mixed with a mixture of 4.0 parts by weight of methyl methacrylate, 4.0 parts by weight of butyl acrylate, and 4.3 parts by weight of acrylic acid to form an oil phase, and then the oil phase was added to an aqueous phase formed by 2.1 parts by weight of OP-10, 0.7 parts by weight of SDS emulsifier, and 81.25 parts by weight of deionized water, and emulsified to obtain an oil / water emulsion; the oil / water emulsion was heated to 80° C., and 0.15 parts by weight of potassium persulfate as an initiator was added dropwise, and the polymerization reaction was carried out for 3 hours. The mixture was then naturally cooled to room temperature to obtain an aqueous dispersion of microcapsules coated with modified nano-zinc oxide; 3) Preparation of formaldehyde removal solution: 28.6 parts by weight of the aqueous dispersion of microcapsules coated with modified nano-zinc oxide prepared in step 2), 0.15 parts by weight of isomeric alcohol polyoxyethylene ether, 0.3 parts by weight of triethanolamine, 0.7 parts by weight of a water-soluble resin, 0.15 parts by weight of sodium carboxymethyl cellulose and 70.1 parts by weight of deionized water were stirred uniformly to obtain a formaldehyde removal solution.
4. A highly efficient formaldehyde removal solution, characterized in that Prepared according to any one of claims 1 to 3.
5. An application of the high-efficiency formaldehyde removal liquid according to claim 4 in removing formaldehyde from furniture, which does not leave white spots on the surfaces of furniture made of different materials and does not damage furniture made of organic materials.
Citation Information
Patent Citations
Formaldehyde removal liquid added with biological enzyme aid, and preparation method thereof
CN110743357A
Preparation method of polyurethane for photocatalytic degradation of formaldehyde