A kind of water-based lithium conductive binder and its preparation method and application

By using a water-based lithium-conducting binder with a Raspberry-type core-shell structure in lithium-ion batteries, combining the organic shell layer and the inorganic core layer, the problem of insufficient lithium ion conduction ability of SBR-type binder is solved, and lithium is significantly improved Dynamic performance and fast charging capability of ion batteries.

CN117050693BActive Publication Date: 2024-11-05SHENZHEN YANYI NEW MATERIALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311025641.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-15
Publication Date
2024-11-05
Estimated Expiration
2043-08-15

AI Technical Summary

Technical Problem

In the negative electrode application of existing SBR type adhesives, the lithium ion conduction capacity is weak, resulting in poor kinetic performance and the inability to achieve fast charging performance.

Method used

Using an aqueous lithium conduction binder with a raspberry-type core-shell structure, the shell layer is an organic polymer with spherical or spherical particles arranged, and the core layer contains lithium conduction material to form an incompletely coated structure to improve lithium ion conduction. ability.

Benefits of technology

The peeling stress and lithium-ion battery ratio performance of the electrode sheet are significantly improved, with peeling stress ranging from 5.72-10.8N/m and the 3C capacity retention rate is 92.74-96.78%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117050693B_ABST
    Figure CN117050693B_ABST
Patent Text Reader

Abstract

The present invention provides an aqueous lithium-conductive binder and a preparation method and application thereof. The aqueous lithium-conductive binder comprises organic-inorganic composite particles with a raspberry-type core-shell structure, wherein the organic-inorganic composite particles comprise an organic shell layer and an inorganic core layer; the shell layer is a polymer distributed on the surface of the core layer and not completely covering the core layer; the core layer is a lithium-conductive material. The aqueous lithium-conductive binder provided by the present invention has high adhesion and lithium-conductive performance, and can significantly improve the peeling stress of a pole piece and the rate performance of a lithium-ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of binders, and in particular relates to a water-based lithium-conductive binder and a preparation method and application thereof. Background Art

[0002] Nowadays, in order to adapt to the needs of future electrification, especially the further development of the mobile phone and electric vehicle industries, the performance improvement of lithium-ion batteries also faces huge challenges. At present, the market not only has higher and higher requirements for the improvement of the energy density of lithium-ion batteries, but also the functional requirements for fast charging are becoming more and more important. The main function of the binder is to connect the electrode active material, the lithium conductor and the electrode current collector so that they have overall connectivity. During the charge and discharge process, the binder effectively maintains the integrity of the electrode structure, ensures that the electrode material can repeatedly insert and remove lithium, and also plays an important role in maintaining the cycle performance. Common binders include polyacrylic acid (PAA), sodium carboxymethyl cellulose / styrene butadiene rubber (CMC / SBR), sodium alginate, chitosan, etc. Among them, SBR-type binders are widely used in negative electrode systems because of their small addition amount in the system and strong bonding between the active material and the current collector.

[0003] CN107394208A discloses a water-based binder, which is composed of polyethylene oxide, an auxiliary binder and a defoamer in a weight ratio of 20-30:0-5:0-5; the molecular weight of the polyethylene oxide is 30w-500w, the solid content of the mixed liquid of polyethylene oxide and deionized water is 5‰-10%, the auxiliary binder is a mixture of one or two of styrene-butadiene rubber, polytetrafluoroethylene, sodium carboxymethyl cellulose, and deionized water, and the solid content of the auxiliary binder is 30%-70%; the defoamer is a mixture of one or more of ethanol, ethylene glycol, and propylene glycol. The water-based binder provided by the technical solution can reduce the investment cost of lithium-ion battery production on the basis of ensuring the basic performance of the battery, and is environmentally friendly, harmless to the human body, increases the contact between the electrode and the solid electrolyte, reduces polarization, and improves the battery rate performance and cycle life.

[0004] CN111682213A discloses a method for preparing a binder for lithium batteries, the method mainly comprising the following steps: (1) mixing an excess of aromatic diamine and a dibasic acid and heating them to react to generate an aromatic polyamide with amino groups at both ends; (2) subjecting an aromatic diisocyanate and an aromatic polyamide with amino groups at both ends to solution polymerization in an organic solvent to obtain a polyurea polymer; (3) adding the polyurea polymer prepared in step (2) to styrene-butadiene rubber, stirring and dispersing the mixture in an organic solvent to obtain a binder for lithium batteries. The polyurea polymer contained in the binder for lithium batteries provided by the technical solution can well suppress the volume effect of the negative electrode material of the lithium battery and has good bonding performance, and the styrene-butadiene rubber helps to improve the dispersion of the rigid polyurea polymer and improve the energy density of the negative electrode material electrode sheet.

[0005] CN105633411A discloses a composite binder suitable for lithium-ion battery negative electrode materials, the composite binder comprising a main binder and a matching binder, the main binder being partially neutralized polyacrylic acid, and the matching binder being styrene-butadiene rubber. The composite binder provided by the technical solution can significantly improve the electrochemical performance of silicon-based negative electrode materials, consumes less lithium-containing raw materials during preparation, is relatively low in price, is easy to industrialize, and has certain lithium ion conductivity.

[0006] However, the components of SBR type binders are mostly low-polarity components, which have poor affinity with highly polar electrolytes and weak lithium ion conductivity. The lithium ion batteries using it as a negative electrode binder have poor kinetic performance and cannot achieve satisfactory fast charging performance.

[0007] Therefore, it is necessary to develop a binder with good adhesion and better lithium ion conductivity. Summary of the invention

[0008] In view of the shortcomings of the prior art, the present invention aims to provide a water-based lithium-conducting binder and a preparation method and application thereof. The water-based lithium-conducting binder has adhesion and lithium-conducting properties, and can significantly improve the peeling stress of the pole piece and the rate performance of the lithium-ion battery.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides an aqueous lithium-conductive binder, wherein the aqueous lithium-conductive binder comprises organic-inorganic composite particles having a raspberry-type core-shell structure, wherein the organic-inorganic composite particles comprise an organic shell layer and an inorganic core layer;

[0011] The shell layer includes a polymer distributed on the surface of the core layer and not completely covering the core layer;

[0012] The core layer includes a lithium conductive material.

[0013] In the present invention, the raspberry-type core-shell structure refers to a spherical structure with an uneven surface formed by spherical or quasi-spherical particles arranged in the shell, such as Figure 1 shown.

[0014] In the present invention, the shell layer is a polymer distributed on the surface of the core layer and does not completely cover the core layer, which can directly contact the negative electrode or copper foil to provide adhesion; the lithium-conducting material of the core layer is not completely covered by the shell layer, and provides a lithium-conducting transmission channel when in contact with the electrolyte, and has good lithium-ion conductivity.

[0015] Preferably, the polymer is a particle-type polymer, that is, a polymer in the form of particles.

[0016] Preferably, the polymerizable monomer of the polymer is selected from any one of monoethylenically unsaturated monomers, diethylenically unsaturated monomers or triethylenically unsaturated monomers, or a combination of at least two thereof.

[0017] Preferably, the monoethylenically unsaturated monomer includes any one or a combination of at least two of a monoethylenically unsaturated alkyl monomer, a monoethylenically unsaturated haloalkyl monomer, a monoethylenically unsaturated ester monomer, a monoethylenically unsaturated ether monomer, a monoethylenically unsaturated carboxyl monomer, a monoethylenically unsaturated nitrile monomer, a monoethylenically unsaturated amide monomer or a monoethylenically unsaturated aromatic monomer.

[0018] Preferably, the diene unsaturated monomer includes any one or a combination of at least two of a diene unsaturated alkyl monomer, a diene unsaturated haloalkyl monomer, a diene unsaturated ester monomer, a diene unsaturated ether monomer, a diene unsaturated carboxyl monomer, a diene unsaturated nitrile monomer, a diene unsaturated amide monomer or a diene unsaturated aromatic monomer.

[0019] Preferably, the triethylenically unsaturated monomer includes any one or a combination of at least two of a triethylenically unsaturated alkyl monomer, a triethylenically unsaturated haloalkyl monomer, a triethylenically unsaturated ester monomer, a triethylenically unsaturated ether monomer, a triethylenically unsaturated carboxyl monomer, a triethylenically unsaturated nitrile monomer, a triethylenically unsaturated amide monomer or a triethylenically unsaturated aromatic monomer.

[0020] Preferably, the polymerizable monomer includes any one or a combination of at least two of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, acrylonitrile, hexene, chlorohexene, allyl polyethylene glycol, acrylic acid, acrylamide, styrene, divinylbenzene, isoprene, chloroisoprene, NN-methylenebisacrylamide, allyl acrylate, allyl methacrylate, ethylene glycol diacrylate, pentaerythritol triacrylate or trimethylolpropane triacrylate.

[0021] Preferably, the lithium-conducting material is spherical lithium-conducting particles.

[0022] Preferably, the spherical lithium-conducting particles include LiPO3, LiAlSiO 4 、LiInO 2 , Li 3 PO 4 , Li 3 BO 3 , Li 2 ZrO 3 、LiF、Li 4 SiO 4 、LiAlO 2 , Li 2 SiO 3 、LiAl(SiO 3 ) 2 、LiAlO 2 , AlF 3 、LiTiO 2 Any one or a combination of at least two of the following:

[0023] Preferably, the particle size of the quasi-spherical lithium-conducting particles is 100-1000 nm, for example, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm or 1000 nm.

[0024] In the present invention, the particle size of the quasi-spherical lithium-conductive particles is 100 to 1000 nm. If the particle size of the quasi-spherical lithium-conductive particles is too small, they will be covered by the polymer of the shell layer, resulting in a decrease in lithium conductivity; if the particle size of the quasi-spherical lithium-conductive particles is too large, the polymer coverage area of ​​the shell layer is small, resulting in a too small bonding area, which reduces the bonding performance.

[0025] Preferably, the mass percentage of the shell layer is 5% to 60%, for example, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%, etc.

[0026] Preferably, the mass percentage of the core layer is 40% to 95%, for example 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90% or 95%, etc.

[0027] In the present invention, the mass percentage of the core layer is 40% to 95%. If the mass percentage of the core layer is too low, it will be covered by the polymer of the shell layer, resulting in a decrease in lithium conductivity; if the mass percentage of the core layer is too high, the polymer coverage area of ​​the shell layer is small, resulting in a too small bonding area, which reduces the bonding performance.

[0028] Preferably, the particle size of the organic-inorganic composite particles is 110 to 1100 nm, for example, 110 nm, 210 nm, 310 nm, 410 nm, 510 nm, 610 nm, 710 nm, 810 nm, 910 nm or 1100 nm.

[0029] In a second aspect, the present invention provides a method for preparing the aqueous lithium-conductive binder as described in the first aspect, the preparation method comprising the following steps: mixing a lithium-conductive material, an emulsifier and water to obtain a core layer suspension; mixing the core layer suspension with a mixture of a polymer monomer, an initiator, an emulsifier and a solvent, and reacting to obtain the aqueous lithium-conductive binder.

[0030] Preferably, the emulsifier comprises sodium dodecyl sulfate (SDS) and / or sodium dodecylbenzene sulfonate (SDBS).

[0031] Preferably, the solvent comprises water.

[0032] Preferably, the initiator comprises persulfate, more preferably ammonium persulfate.

[0033] Preferably, in the core layer suspension, based on 100 parts by mass of the lithium conductive material, the mass fraction of the emulsifier is 0.05-5 parts, for example, 0.05 parts, 0.1 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts, etc., and the mass fraction of the solvent is 50-5000 parts, for example, 50 parts, 100 parts, 200 parts, 500 parts, 800 parts, 1000 parts, 2000 parts, 3000 parts, 4000 parts, 4500 parts or 5000 parts, etc.

[0034] Preferably, in the mixed solution of the polymerization monomer, initiator, emulsifier and solvent of the polymer, based on 100 parts by mass of the polymerization monomer, the mass fraction of the initiator is 0.05-5 parts (for example, 0.05 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts, etc.), the mass fraction of the emulsifier is 0.05-5 parts (for example, 0.05 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts, etc.), and the mass fraction of the solvent is 50-5000 parts, for example, 50 parts, 100 parts, 200 parts, 500 parts, 800 parts, 1000 parts, 2000 parts, 3000 parts, 4000 parts, 4500 parts or 5000 parts, etc.

[0035] Preferably, the mixing is to add a mixed solution of polymer monomers, initiators, emulsifiers and solvents into the core layer suspension for mixing.

[0036] Preferably, the reaction temperature is 60-80°C (e.g., 60°C, 62°C, 65°C, 67°C, 70°C, 75°C, 78°C, 79°C or 80°C), and the reaction time is 1-12h (e.g., 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h or 12h, etc.).

[0037] Preferably, the reaction further comprises a neutralization step after completion.

[0038] In a third aspect, the present invention provides a battery electrode, wherein the battery electrode comprises the aqueous lithium-conductive binder as described in the first aspect.

[0039] Preferably, the battery electrode comprises a current collector and a coating disposed on the current collector, and the coating comprises the aqueous lithium-conductive binder as described in the first aspect.

[0040] Preferably, the battery electrode is a negative electrode.

[0041] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the aqueous lithium-conductive binder as described in the first aspect or the battery electrode as described in the third aspect.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The aqueous lithium-conducting binder provided by the present invention realizes the bonding effect through the organic shell layer, the inorganic core layer can provide higher lithium-conducting performance, the organic shell layer and the inorganic core layer form a raspberry-shaped core-shell structure, which increases the lithium ion transmission channel and can significantly improve the peeling stress of the pole piece and the rate performance of the lithium-ion battery. The peeling stress of the pole piece made of the aqueous lithium-conducting binder is 5.72-10.8N / m, and the 3C capacity retention rate of the prepared lithium-ion battery is 92.74-96.78%. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 is a schematic diagram of the raspberry-shaped core-shell structure;

[0045] Among them, 1-shell, 2-core;

[0046] Figure 2 A scanning electron microscope image of the water-based lithium-conducting binder provided in Example 1;

[0047] Figure 3 A schematic diagram of the structure of the aqueous lithium-conducting binder provided in Comparative Example 1;

[0048] Among them, 1-core layer, 2-shell layer. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0050] Example 1

[0051] This embodiment provides a water-based lithium-conductive binder and a preparation method thereof. The preparation method of the water-based lithium-conductive binder is as follows:

[0052] 100g of lithium conductive material (LiF, particle size of 500nm), 1g of emulsifier (sodium dodecyl sulfate) and 100g of solvent (water) were mixed and added into a reactor. The stirring was started at 300rpm and the dispersion was carried out for 4 hours to obtain a core layer suspension. Then, a mixture of 100g of polymerization monomer (methyl methacrylate), 1g of initiator (ammonium persulfate), 1g of emulsifier (sodium dodecyl sulfate) and 100g of solvent (water) was added. The mixture was dripped into the reactor at a uniform speed within 1 hour, and then the reaction was continued at 70°C for 4 hours to obtain a water-based lithium conductive binder.

[0053] The mass percentage of the shell layer of the aqueous lithium-conductive binder is 50%, and the mass percentage of the core layer is 50%.

[0054] Examples 2 to 14 adopt the same preparation method as Example 1, except for the raw materials, content and process parameters, as shown in Tables 1 and 2.

[0055] Table 1

[0056]

[0057]

[0058] Table 2

[0059]

[0060]

[0061] Comparative Example 1

[0062] This comparative example provides a water-based lithium-conductive binder and a preparation method thereof. The preparation method of the water-based lithium-conductive binder is as follows:

[0063] 100g of lithium conductive material (LiF, particle size of 500nm), 1g of emulsifier (sodium dodecyl sulfate) and 100g of solvent (water) were mixed and added into a reactor. Stirring was started at 300rpm and dispersed for 4h to obtain a core layer suspension. Then, a mixture of 100g of polymerization monomer (methyl methacrylate), 1g of emulsifier (sodium dodecyl sulfate) and 100g of solvent (water) was added, and 1g of initiator (ammonium persulfate) was added. The temperature was then raised and maintained at 70°C for 4h to obtain a water-based lithium conductive binder.

[0064] Comparative Example 2

[0065] This comparative example provides a water-based lithium-conductive binder and a preparation method thereof. The preparation method of the water-based lithium-conductive binder is as follows:

[0066] (1) A mixture of 100 g of polymerization monomer (methyl methacrylate), 1 g of initiator (ammonium persulfate), 1 g of emulsifier (sodium dodecyl sulfate) and 200 g of solvent (water) was maintained at 70° C. and reacted for 4 h to obtain a polymethyl methacrylate emulsion.

[0067] (2) Add 100 g of lithium-conducting material (LiF, particle size of 500 nm) to the above-mentioned polymethyl methacrylate emulsion, start stirring at 300 rpm, and disperse to obtain an aqueous lithium-conducting binder.

[0068] Comparative Example 3

[0069] This comparative example provides a binder, which is an SBR binder sourced from Shenzhen Yanyi New Materials Co., Ltd.

[0070] Application Example 1

[0071] This application example provides a negative electrode sheet and a lithium-ion battery including the negative electrode sheet. The preparation methods of the negative electrode sheet and the lithium-ion battery including the negative electrode sheet are as follows.

[0072] A negative electrode plate, comprising a current collector (Cu foil) and a coating arranged on the current collector, wherein the coating comprises a negative electrode active material (silicon oxide material SiO-450, produced by B&T New Energy Materials Co., Ltd., with a silicon content of 10%), carbon black SP, a binder and a thickener (sodium carboxymethyl cellulose).

[0073] The above-mentioned binder is the aqueous lithium-conductive binder provided in Example 1.

[0074] The method for preparing the negative electrode plate is as follows:

[0075] The negative electrode active material, carbon black SP, binder and thickener were mixed in a mass ratio of 96.5:1.0:1.0:1.5, added into deionized water at a solid content of 40 wt%, and stirred to make a uniform negative electrode slurry. After passing through a 100 mesh sieve, the slurry was coated on the negative electrode current collector Cu foil, dried, and rolled with a roller at 10×10 4 The negative electrode sheet is rolled by a load per unit length of N / m to obtain the negative electrode sheet.

[0076] A lithium-ion battery, comprising a positive electrode plate, the above-mentioned negative electrode plate, a separator and an electrolyte (EC:EMC:DEC volume ratio = 1:1:1, containing 1.0M LiPF 6 The preparation method is as follows:

[0077] (1) Preparation of positive electrode sheet: The positive electrode active material (lithium iron phosphate material), carbon black SP, and binder (PVDF) were mixed at a mass ratio of 96.5:2.0:2.5, and N-methylpyrrolidone was added at a ratio of 50 wt% of the system solid content and stirred to make a uniform positive electrode slurry. After passing through a 100-mesh sieve, the slurry was coated on the positive electrode current collector Al foil, and then dried. The slurry was rolled using a roller at a speed of 10×10 4 The positive electrode sheet is obtained by rolling with a unit length load of N / m.

[0078] (2) Assembly of lithium-ion battery: The positive electrode sheet, the separator (PE porous polymer film, purchased from Shenzhen Xingyuan Material Technology Co., Ltd.), and the negative electrode sheet are wound in order to obtain a battery cell. The battery cell is packaged with an aluminum plastic film, baked to remove water, and then injected with electrolyte. After vacuum packaging, shelving, formation, secondary sealing, shaping and other processes, the lithium-ion battery is obtained.

[0079] Application Examples 2 to 14 and Comparative Application Examples 1 to 3 adopt the same preparation method as Application Example 1, except that the binder is replaced by the aqueous lithium-conductive binder provided by Examples 2 to 14, the aqueous lithium-conductive binder provided by Comparative Examples 1 to 2, or the binder provided by Comparative Example 3, respectively.

[0080] The negative electrode sheets and lithium-ion batteries provided in the application examples and comparative application examples were subjected to the following performance tests:

[0081] (1) Adhesion performance: The negative electrode sheet was cut into strips of 20 cm × 2.5 cm. The current collector side was bonded to a 1 mm thick steel plate with double-sided tape. A transparent tape was pasted on the coating layer side. The coating layer was peeled off in a 180° direction at a speed of 100 mm / min using a tensile testing machine. The peeling stress was measured and used as the basis for judging the adhesion performance. The greater the peeling stress, the better the adhesion strength of the water-based lithium conductive binder.

[0082] (2) The rate performance test of lithium-ion batteries is as follows:

[0083] Initial adjustment: Charge the lithium-ion batteries provided in the application examples and comparative application examples to 4.2V at a constant current of 0.33C, then charge at a constant voltage to a cut-off current of 0.02C, and discharge at 0.33C to 2.5V; leave for 5 minutes, charge at a constant current of 0.33C to 4.2V, then charge at a constant voltage to a cut-off current of 0.02C, and discharge at 0.33C to 2.5V.

[0084] Rate performance test: At 25°C, the initially adjusted lithium-ion battery is charged to 4.2V at 0.5C constant current, then charged to a cut-off current of 0.02C at constant voltage, left for 5 minutes, then discharged to 2.5V at 1C constant current, left for 5 minutes, and the 1C discharge capacity is measured. Then, it is charged to 4.2V at 0.5C constant current, then charged to a cut-off current of 0.02C at constant voltage, left for 5 minutes, then discharged to 2.5V at 3C constant current, left for 5 minutes, and the discharge capacity at 3C rate is measured.

[0085] 3C capacity retention rate (%) = 100% × (3C discharge capacity / 1C discharge capacity).

[0086] The test results are shown in Table 3.

[0087] Table 3

[0088] Peel stress (N / m) 3C capacity retention rate (%) Application Example 1 8.75 95.17 Application Example 2 10.8 94.48 Application Example 3 9.55 94.97 Application Example 4 8.70 95.36 Application Example 5 7.85 95.75 Application Example 6 7.00 96.14 Application Example 7 6.15 96.53 Application Example 8 6.03 96.78 Application Example 9 6.93 95.72 Application Example 10 6.08 96.11 Application Example 11 10.39 93.76 Application Example 12 5.95 95.87 Application Example 13 9.43 92.74 Application Example 14 5.72 96.50 Comparative application example 1 5.01 92.31 Comparative Application Example 2 3.15 93.04 Comparative Application Example 3 7.00 88.07

[0089] According to the test results in Table 3, the peeling stress of the negative electrode sheet made of the aqueous lithium conductive binder provided in Examples 1 to 14 is 5.72-10.8 N / m, and the 3C capacity retention rate of the prepared lithium ion battery is 92.74-96.78%. The aqueous lithium conductive binder provided in Example 1 is a raspberry-type core-shell structure, and its scanning electron microscope image is as follows Figure 2 shown.

[0090] Compared with Example 1, if the particle size of the lithium-conductive material is too small (Example 11), the 3C capacity retention rate of the prepared lithium-ion battery decreases and the lithium conductivity performance decreases; if the particle size of the lithium-conductive material is too large (Example 12), the peeling stress decreases and the bonding force of the aqueous lithium-conductive binder decreases, proving that the aqueous lithium-conductive binder prepared using lithium-conductive materials in a specific particle size range has better performance.

[0091] Compared with Example 1, if the mass percentage of the core layer is too small (Example 13), the 3C capacity retention rate of the prepared lithium-ion battery decreases and the lithium conductivity performance decreases; if the mass percentage of the core layer is too large (Example 14), the peeling stress decreases and the bonding force of the aqueous lithium-conductive binder decreases, proving that the performance of the aqueous lithium-conductive binder obtained by controlling the mass percentage of the core layer within a specific range is better.

[0092] Compared with Example 1, if a mixture of a polymerizable monomer, an emulsifier and a solvent is added to the core layer suspension, and then an initiator is added, the prepared aqueous lithium conductive binder (Comparative Example 1) is a fully coated core-shell structure, and the shell layer is uniformly coated on the outer surface of the core layer, such as Figure 3 As shown, 1 represents the core layer formed by the lithium conductive material, and 2 represents the shell layer formed by the polymerization of methyl methacrylate. Then, the peeling stress and the 3C capacity retention rate of the prepared lithium-ion battery are both reduced.

[0093] Compared with Example 1, if the polymethyl methacrylate emulsion and the lithium conductive material are mixed to prepare an aqueous lithium conductive binder (Comparative Example 2), the peeling stress and the 3C capacity retention rate of the prepared lithium ion battery are both reduced.

[0094] Compared with Example 1, if a commercially available SBR binder is used (Comparative Example 3), the peel stress and the 3C capacity retention rate of the prepared lithium ion battery are both reduced.

[0095] The applicant declares that the present invention illustrates a water-based lithium-conducting binder and its preparation method and application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A water-based lithium-conducting binder, characterized in that: The aqueous lithium-conducting binder comprises organic-inorganic composite particles having a raspberry-shaped core-shell structure, wherein the organic-inorganic composite particles comprise an organic shell layer and an inorganic core layer; The shell layer includes a polymer distributed on the surface of the core layer and not completely covering the core layer; The core layer includes a lithium conductive material; The lithium-conducting material comprises spherical lithium-conducting particles; The spherical lithium-conducting particles include any one of LiPO3, LiAlSiO4, LiInO2, Li3PO4, Li3BO3, Li2ZrO3, LiF, Li4SiO4, Li2SiO3, LiAl(SiO3)2, LiAlO2, AlF3, and LiTiO2, or a combination of at least two thereof; The particle size of the quasi-spherical lithium-conducting particles is 100-1000 nm; The mass percentage of the shell layer is 5% to 60%; The mass percentage of the core layer is 40% to 95%; The polymer is a particle-type polymer; The polymerizable monomer of the polymer is selected from any one or a combination of at least two of a monoethylenically unsaturated monomer, a diethylenically unsaturated monomer or a triethylenically unsaturated monomer; The monoethylenically unsaturated monomer includes any one or a combination of at least two of a monoethylenically unsaturated alkyl monomer, a monoethylenically unsaturated haloalkyl monomer, a monoethylenically unsaturated ester monomer, a monoethylenically unsaturated ether monomer, a monoethylenically unsaturated carboxyl monomer, a monoethylenically unsaturated nitrile monomer, a monoethylenically unsaturated amide monomer or a monoethylenically unsaturated aromatic monomer; The diethylenically unsaturated monomers include any one or a combination of at least two of diethylenically unsaturated alkyl monomers, diethylenically unsaturated haloalkyl monomers, diethylenically unsaturated ester monomers, diethylenically unsaturated ether monomers, diethylenically unsaturated carboxyl monomers, diethylenically unsaturated nitrile monomers, diethylenically unsaturated amide monomers or diethylenically unsaturated aromatic monomers; The triethylenically unsaturated monomers include any one or a combination of at least two of triethylenically unsaturated alkyl monomers, triethylenically unsaturated halogenated alkyl monomers, triethylenically unsaturated ester monomers, triethylenically unsaturated ether monomers, triethylenically unsaturated carboxyl monomers, triethylenically unsaturated nitrile monomers, triethylenically unsaturated amide monomers or triethylenically unsaturated aromatic monomers.

2. The aqueous lithium-conducting binder according to claim 1, characterized in that: The polymerizable monomers include any one or a combination of at least two of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, acrylonitrile, hexene, chlorohexene, allyl polyethylene glycol, acrylic acid, acrylamide, styrene, divinylbenzene, isoprene, chloroisoprene, NN-methylenebisacrylamide, allyl acrylate, allyl methacrylate, ethylene glycol diacrylate, pentaerythritol triacrylate or trimethylolpropane triacrylate.

3. The aqueous lithium-conducting binder according to claim 1, characterized in that: The particle size of the organic-inorganic composite particles is 110-1100 nm.

4. The method for preparing an aqueous lithium-conducting binder according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: mixing a lithium conductive material, an emulsifier and a solvent to obtain a core layer suspension; mixing the core layer suspension with a mixed solution of a polymer monomer, an initiator, an emulsifier and a solvent, and reacting to obtain the water-based lithium conductive binder; The mixing is to add the mixed liquid of the polymer monomer, initiator, emulsifier and solvent dropwise into the core layer suspension for mixing.

5. The preparation method according to claim 4, characterized in that: The emulsifier includes sodium dodecyl sulfate and / or sodium dodecylbenzene sulfonate.

6. The preparation method according to claim 4, characterized in that: The solvent includes water.

7. The preparation method according to claim 4, characterized in that: The initiator includes a persulfate.

8. The preparation method according to claim 7, characterized in that: The initiator is ammonium persulfate.

9. The preparation method according to claim 4, characterized in that: In the core layer suspension, based on 100 parts by weight of the lithium conductive material, the mass fraction of the emulsifier is 0.05-5 parts, and the mass fraction of the solvent is 50-5000 parts.

10. The preparation method according to claim 4, characterized in that: In the mixed solution of the polymer monomer, initiator, emulsifier and solvent, based on 100 parts by mass of the polymer monomer, the mass fraction of the initiator is 0.05-5 parts, the mass fraction of the emulsifier is 0.05-5 parts, and the mass fraction of the solvent is 50-5000 parts.

11. The preparation method according to claim 4, characterized in that: The reaction temperature is 60-80° C., and the reaction time is 1-12 h.

12. The preparation method according to claim 4, characterized in that: After the reaction is completed, a neutralization step is also included.

13. A battery pole piece, characterized in that: The battery pole piece includes the aqueous lithium-conductive binder as described in any one of claims 1-3.

14. The battery pole piece according to claim 13, characterized in that: The battery pole piece includes a current collector and a coating disposed on the current collector, wherein the coating includes the aqueous lithium-conductive binder according to any one of claims 1 to 3.

15. The battery pole piece according to claim 13, characterized in that: The battery pole piece is a negative pole piece.

16. A lithium ion battery, characterized in that: The lithium-ion battery comprises the aqueous lithium-conductive binder according to any one of claims 1 to 3 or the battery pole piece according to any one of claims 13 to 15.

Citation Information

Patent Citations

  • Composite binding agent applicable for silicon-based negative electrode material of lithium ion battery, preparation method of composite binding agent and negative electrode material

    CN105633411A

  • Water-based adhesive and production method of lithium battery pole piece applying same

    CN107394208A

  • Preparation method of binder for lithium battery

    CN111682213A

  • Lithium ion power battery composite anode material and preparation method thereof

    CN107293732A

  • Secondary battery

    CN111710869A