A device and method for measuring the single ion mass transfer resistance of polyamide membrane
Determination of single ion mass transfer resistance in polyamide films through four-electrode system electrochemical technology solves the problem of difficult to measure single ion transport properties in the prior art, and achieves an in-depth understanding of single ion mass transfer behavior and the efficiency of thin film separation technology promote.
Patent Information
- Application Number
- CN202410985012.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The difficulty in measuring the transport properties of single ions in polyamide membranes, especially the mechanism of salt ions passing through membrane pores, is still a fiercely debated issue, and it is difficult to deeply understand the mass transfer behavior of single ions in the membrane.
Using electrochemical technology based on four-electrode system, cations and anions are driven by electric field to pass through dense subnanoporous polyamide membranes and corresponding ion exchange membranes, single ion mass transfer resistance is determined, and current-potential difference maps and linear fitting are used. Calculate the mass transfer resistance value.
Quantitatively accurate testing of the mass transfer resistance of single ions in polyamide membranes is achieved, and the mass transfer differences of single ions in the membrane is deeply understood, which improves the efficiency and feasibility of thin film separation technology.
Smart Images

Figure CN118518738B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of membrane technology, in particular to a device and a method for measuring the single ion mass transfer resistance of a polyamide membrane. Background Art
[0002] Membrane separation technology, especially the application of reverse osmosis (RO) and nanofiltration (NF) membranes, has become one of the important means to solve the global challenge of freshwater shortage. The development of these membranes, especially thin film composite polyamide (TFC-PA) membranes, has enabled the efficient production of fresh water from wastewater and salt water. This is crucial to meet the growing demand for water in industry, agriculture and households, as these membranes are able to remove a variety of dissolved impurities, including salt ions and other small molecules. Typically, commercial reverse osmosis membranes are prepared by interfacial polymerization of metaphenylenediamine (MPD) with trimesoyl chloride (TMC), while nanofiltration membranes are usually prepared by interfacial polymerization of metaphenylenediamine or piperazine (PIP) with trimesoyl chloride. These composite membranes are usually composed of a top polyamide active layer (20~200nm), a middle polysulfone support (20~50μm) and a polyester backing (50~150μm). In this structure, the polyamide active layer plays the main role of barrier for water and solute transport.
[0003] In order to optimize the performance of polyamide membranes, it is crucial to conduct a detailed study of the ion mass transfer process. The study of ion mass transfer processes usually requires the use of advanced characterization techniques such as quartz crystal microbalance, electrochemical impedance spectroscopy and Rutherford backscattering spectroscopy. These techniques have made significant progress in studying the microscopic mass transfer in the TFC-PA layer. However, it is difficult to measure the transport properties of individual ions in current studies, the presence of ion pairs may affect the behavior of individual ions, and the intrapore diffusion of ions is often overlooked. Therefore, the mechanism of salt ions passing through membrane pores remains a hotly debated issue. Summary of the invention
[0004] In order to solve the characterization requirements of the single ion mass transfer process in the polyamide membrane in the prior art and the defects of the prior art, the present invention proposes a device and method for measuring the single ion mass transfer resistance of the polyamide membrane. The method has the characteristics of high sensitivity, wide applicability and simple operation, and can realize the quantitative characterization of the single ion mass transfer resistance in the membrane. This method provides a new strategy and means for in-depth understanding of the mass transfer behavior of single ions in polyamide membranes.
[0005] The first object of the present invention is to provide a device for measuring the single ion mass transfer resistance of a polyamide membrane, comprising:
[0006] An electrochemical workstation, wherein a first signal terminal of the electrochemical workstation is connected to a working electrode and a recording electrode, and a second signal terminal of the electrochemical workstation is connected to a counter electrode and a reference electrode;
[0007] A measuring cell, the measuring cell comprising a No. 1 electrolytic cell body, a No. 2 electrolytic cell body and a gasket disposed between the No. 1 electrolytic cell body and the No. 2 electrolytic cell body, a polyamide membrane and an ion exchange membrane being disposed on the gasket, the polyamide membrane being located on one side close to the No. 1 electrolytic cell body, and the ion exchange membrane being located on the other side close to the No. 2 electrolytic cell body;
[0008] The first electrolytic cell body has a first cavity, the first cavity is used to hold the solution to be tested, and the working electrode and the recording electrode extend into the first cavity;
[0009] The second electrolytic cell body has a second cavity, and the second cavity is used to contain the solution to be tested, and the counter electrode and the reference electrode extend into the second cavity.
[0010] In some embodiments of the present invention, the end of the working electrode and the end of the counter electrode are formed as a sheet-shaped platinum electrode or a sheet-shaped titanium electrode;
[0011] The reference electrode and the recording electrode are Ag / AgCl electrodes;
[0012] The effective surface area of the polyamide membrane is smaller than the surface area of the sheet-shaped platinum electrode or the sheet-shaped titanium electrode;
[0013] The effective surface area of the polyamide membrane is 1-4 cm 2 .
[0014] In some embodiments of the present invention, the recording electrode is located on a side close to the polyamide membrane, and the reference electrode is located on a side away from the ion exchange membrane;
[0015] A cover plate is respectively arranged on the top of the No. 1 electrolytic cell body and the No. 2 electrolytic cell body, and a first through hole and a second through hole are provided on the cover plate. Threaded sleeves are arranged in the first through hole and the second through hole, and one of the threaded sleeves is used for installing the working electrode and / or the counter electrode, and a Luggin capillary is arranged in the other threaded sleeve, and the reference electrode and / or the recording electrode is arranged in the Luggin capillary.
[0016] In some embodiments of the present invention, the Luggin capillary is an L-type sand core salt bridge or an L-type Luggin capillary;
[0017] The distance between the elbow outlet of the Luggin capillary and the surface of the polyamide membrane is 1-2 mm.
[0018] In some embodiments of the present invention, it further comprises:
[0019] The fixing rods include four fixing rods, and the four fixing rods pass through the gasket to connect the first electrolytic cell body and the second electrolytic cell body.
[0020] The second object of the present invention is to provide a method for measuring the single ion mass transfer resistance of a polyamide membrane using the device, comprising the following steps:
[0021] S1, providing the device described in any one of the above items, attaching a polyamide membrane to the ion exchange membrane of the device, and injecting a solution to be tested into the No. 1 electrolytic cell body and the No. 2 electrolytic cell body of the device;
[0022] S2, starting the electrochemical workstation of the device, measuring the current-potential difference spectrum of a single ion across the membrane, and obtaining the cation / anion mass transfer resistance value by fitting the slope calculation.
[0023] In some embodiments of the present invention, before using the ion exchange membrane, the ion exchange membrane is immersed in the test solution for 12 to 72 hours;
[0024] The polyamide membrane is a composite polyamide membrane. Before using the composite polyamide membrane, the composite polyamide membrane is immersed in an alcohol solution for 30 to 120 minutes or
[0025] Soaking the composite polyamide membrane in ultrapure water for 12 to 72 hours;
[0026] The alcohol solution is one or more of ethanol, methanol, and isopropanol, and the volume fraction of the alcohol solution is 10% to 40%.
[0027] In some embodiments of the present invention, the concentration of the test solution is 0.01 mM to 1000 mM;
[0028] The cation in the solution to be tested is Li + 、Na + , K + , Rb + , Cs + NH4 + , Ca 2+ Mg 2+ , Ba 2+ One or more of;
[0029] The anion in the solution to be tested is Cl - 、SO4 2- 、NO3 - PO4 3- 、CO3 2- and ClO4 - One or more of .
[0030] In some embodiments of the present invention, the working voltage of the electrochemical workstation is -50mV~50mV, and the scanning rate is 0.1mV / s~100mV / s.
[0031] In some embodiments of the present invention, the working current of the electrochemical workstation is -0.1 mA / cm 2 ~1mA / cm 2 , the application time is 20~60s.
[0032] The above technical solution of the present invention has the following advantages compared with the prior art:
[0033] The present invention uses an electrochemical technology based on a four-electrode system to test the separated polyamide membrane. By using the electric field as the driving force, cations and anions are separated and passed through a dense sub-nanoporous polyamide membrane and a corresponding ion exchange membrane, thereby achieving a quantitative and accurate test of the mass transfer resistance of a single ion. The linear fitting data processing process used is simple and effective, and has good detection stability. This method helps to deeply understand the mass transfer differences of single ions in polyamide membranes, and provides a new strategy and method for clarifying and regulating the ion mass transfer process in polyamide membranes. This research is expected to deepen the understanding of ion transfer in the membrane separation process, thereby further improving the efficiency and feasibility of membrane separation technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0035] Figure 1 is a structural schematic diagram of measuring the single ion mass transfer resistance of a polyamide membrane according to an embodiment of the present invention;
[0036] Figure 2 The linear voltammetric curve of the mass transfer resistance of the polyamide membrane to potassium ions in potassium chloride is measured by the method of Example 2;
[0037] Figure 3 The linear voltammetric curve of the mass transfer resistance of the polyamide membrane to chloride ions in potassium chloride is measured by the method of Example 3;
[0038] Figure 4 The linear voltammetric curve of the mass transfer resistance of the polyamide membrane to chloride ions in potassium chloride is measured by the method of Example 4;
[0039] Figure 5 The linear voltammetric curve of the mass transfer resistance of the polyamide membrane to chloride ions in potassium chloride is measured using the method of Example 5.
[0040] Reference numerals:
[0041] 1. No. 1 electrolytic cell body; 2. No. 2 electrolytic cell body; 3. Working electrode; 4. Recording electrode; 5. Counter electrode; 6. Luggin capillary; 7. Threaded sleeve; 8. Gasket; 9. Fixing rod; 10. Cover plate; 11. Measuring cell; 12. Polyamide membrane; 13. Ion exchange membrane; 14. Electrochemical workstation; 15. Reference electrode. DETAILED DESCRIPTION
[0042] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0043] The first object of the present invention is to provide a device for measuring the single ion mass transfer resistance of a polyamide membrane, comprising an electrochemical workstation 14 and a measuring cell 11, wherein the first signal end of the electrochemical workstation 14 is connected to a working electrode 3 and a recording electrode 4, and the second signal end of the electrochemical workstation 14 is connected to a counter electrode 5 and a reference electrode 15; the measuring cell 11 comprises a No. 1 electrolytic cell body 1, a No. 2 electrolytic cell body 2 and a gasket 8 arranged between the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2, a polyamide membrane 12 and an ion exchange membrane 13 are arranged on the gasket 8, the polyamide membrane 12 is located on one side close to the No. 1 electrolytic cell body 1, and the ion exchange membrane 13 is located on the other side close to the No. 2 electrolytic cell body 2; the No. 1 electrolytic cell body 1 has a first cavity, the first cavity is used to hold a solution to be tested, and the working electrode 3 and the recording electrode 4 extend into the first cavity; the No. 2 electrolytic cell body 2 has a second cavity, the second cavity is used to hold a solution to be tested, and the counter electrode 5 and the reference electrode 15 extend into the second cavity. That is, the separated polyamide membrane 12 is tested by using an electrochemical technique based on a four-electrode system. By using an electric field as a driving force, cations and anions are separated and passed through the dense sub-nanoporous polyamide membrane 12 and the corresponding ion exchange membrane 13, thereby achieving a quantitative and accurate test of the mass transfer resistance of a single ion. The device of the present invention is simple and effective to operate and has good detection stability.
[0044] In some embodiments of the present invention, the cavity length L of the No. 1 electrolytic cell body 1 or the No. 2 electrolytic cell body 2 is 40-70 mm, the width B is 30-50 mm, and the height H is 40-80 mm. The No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2 can be made of acrylic material, for example.
[0045] In some embodiments of the present invention, the ends of the working electrode 3 and the counter electrode 5 are formed as sheet-like platinum electrodes or sheet-like titanium electrodes; the reference electrode 15 and the recording electrode 4 are Ag / AgCl electrodes; the effective surface area of the polyamide membrane 12 is smaller than the surface area of the sheet-like platinum electrode or sheet-like titanium electrode. This is because the effective surface area of the polyamide membrane 12 is smaller than the surface area of the sheet-like platinum electrode or sheet-like titanium electrode, which helps to ensure the uniform transfer of ions on the membrane. As an embodiment of the present invention, the effective surface area of the polyamide membrane 12 is 1~4 cm 2 .
[0046] In some embodiments of the present invention, the recording electrode 4 is located on the side close to the polyamide membrane 12, and the reference electrode 15 is located on the side away from the ion exchange membrane 13; the tops of the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2 are respectively provided with a cover plate 10, and a first through hole and a second through hole are provided on the cover plate 10, and threaded sleeves 7 are provided in the first through hole and the second through hole, wherein one threaded sleeve 7 is used to install the working electrode 3 and / or the counter electrode 5, and a Luggin capillary 6 is provided in the other threaded sleeve 7, and the reference electrode 15 and / or the recording electrode 4 are provided in the Luggin capillary 6. Fixing the reference electrode 15 and / or the recording electrode 4 by the Luggin capillary 6 and the threaded sleeve 7 can enhance the stability of the recording point during the test.
[0047] In some embodiments of the present invention, a rotary stirrer may be disposed at the bottom of the first electrolytic cell body 1 and the second electrolytic cell body 2 respectively to maintain a stable state of the solution to be tested on both sides of the polyamide membrane 12 .
[0048] In some embodiments of the present invention, the Luggin capillary 6 is an L-shaped sand core salt bridge or an L-shaped Luggin capillary 6; the distance between the elbow outlet of the Luggin capillary 6 and the surface of the polyamide membrane 12 is 1-2 mm.
[0049] In some embodiments of the present invention, a fixing rod 9 is further included, and the fixing rod 9 includes four fixing rods, and the four fixing rods 9 pass through the gasket 8 to connect the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2. The No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2 are connected by the fixing rod 9, and the connection is used to install the gasket 8, which plays a role of fixed connection on the one hand, and plays a guiding role on the other hand, so as to improve the installation accuracy of the polyamide membrane 12 and the ion exchange membrane 13 on the No. 1 electrolytic cell body 1, the No. 2 electrolytic cell body 2 and the gasket 8.
[0050] The second object of the present invention is to provide a method for measuring the single ion mass transfer resistance of a polyamide membrane, comprising the following steps: S1, providing a device as described in any of the above items, attaching a polyamide membrane 12 to the ion exchange membrane 13 of the device, and injecting a solution to be tested into the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2 of the device; S2, starting the electrochemical workstation 14 of the device, measuring the current-potential difference spectrum of a single ion across the membrane, and obtaining the cation / anion mass transfer resistance value by fitting the slope calculation.
[0051] The working mechanism of the device for measuring the single ion mass transfer resistance of the polyamide membrane of the present invention is as follows: a positive potential can be applied to the working electrode 3 by using an electrochemical workstation 14. At this time, the ion exchange membrane 13 selects a cation exchange membrane. The positively charged ions in the solution to be tested pass through the dense sub-nanopore polyamide membrane 12 and the cation exchange membrane under the action of the electric field, and migrate to the counter electrode 5. The potential difference change on both sides of the membrane is recorded by the Ag / AgCl reference electrode 15 in the Luggin capillary 6. The slope fitting is performed on the obtained current-potential difference spectrum. The derivative of the slope is the resistance of cation transmembrane mass transfer. Under the same conditions, , with a cation exchange membrane as a control; a negative potential can also be applied to the working electrode 3 using an electrochemical workstation 14. At this time, the ion exchange membrane 13 selects an anion exchange membrane. The negatively charged ions in the solution to be tested pass through the dense sub-nanopore polyamide membrane 12 and the anion exchange membrane under the action of the electric field, and migrate to the counter electrode 5. The change in the potential difference on both sides of the membrane is recorded by the Ag / AgCl reference electrode 15 in the Luggin capillary 6. The slope of the obtained current-potential difference spectrum is fitted, and the derivative of the slope is the resistance to transmembrane mass transfer of anions. Under the same conditions, an anion exchange membrane is used as a control.
[0052] In some embodiments of the present invention, step S1 further includes: before using the ion exchange membrane 13, immersing the ion exchange membrane 13 in the solution to be tested for 12 to 72 hours;
[0053] The polyamide membrane 12 is a composite polyamide membrane. Before using the composite polyamide membrane, the composite polyamide membrane is immersed in an alcohol solution for 30 to 120 minutes or
[0054] The composite polyamide membrane was immersed in ultrapure water for 12 to 72 h;
[0055] The alcohol solution is one or more of ethanol, methanol and isopropanol, and the volume fraction of the alcohol solution is 10% to 40%.
[0056] In step S1, the installation steps of the device are specifically as follows: (1) preparing the polyamide membrane 12: bonding the polyamide membrane 12 or the soaked polyamide composite membrane and the ion exchange membrane 13 soaked in the test solution, and sandwiching them between the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2; (2) adding the test solution: adding the test solution to the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2 respectively, ensuring that the test solution completely covers the end of the working electrode 3 and the end of the counter electrode 5; (3) installing the electrodes: connecting the sheet platinum electrode or sheet titanium electrode and the Ag / AgCl recording electrode 4 located at the end of the working electrode 3 to the first signal terminal of the electrochemical workstation 14, and connecting the sheet platinum electrode or sheet titanium electrode and the Ag / AgCl reference electrode 15 located at the end of the counter electrode 5 to the second signal terminal of the electrochemical workstation 14.
[0057] In step S2, the measurement steps are specifically as follows: (1) Setting the working parameters of the electrochemical workstation 14: Setting the experimental parameters on the electrochemical workstation 14, applying a working voltage or a working current, the working voltage of the electrochemical workstation 14 is -50mV~50mV, the scanning rate is 0.1mV / s~100mV / s, and the working current of the electrochemical workstation 14 is -0.1mA / cm 2 ~1mA / cm 2 , the application time is 20~60s; (2) Recording data: Record the obtained current-potential difference spectrum; (3) Data analysis: Perform linear fitting and calculate the mass transfer resistance value of cations or anions through the fitting slope.
[0058] In some embodiments of the present invention, the concentration of the solution to be tested is 0.01 mM to 1000 mM; the cation in the solution to be tested is Li + 、Na + , K + , Rb + , Cs + NH4 + , Ca 2+ Mg 2+ , Ba 2+ One or more of; the anion in the test solution is Cl - 、SO4 2- 、NO3 - PO4 3- 、CO3 2- and ClO4 - One or more of . Specific embodiments
[0060] Example 1
[0061] like Figure 1As shown, a schematic diagram of the structure of a device for measuring the mass transfer resistance of a single ion of a polyamide membrane is provided in this embodiment, comprising an electrochemical workstation 14 and a measuring cell 11, wherein a first signal end of the electrochemical workstation 14 is connected to a working electrode 3 and a recording electrode 4, and a second signal end of the electrochemical workstation 14 is connected to a counter electrode 5 and a reference electrode 15; the measuring cell 11 comprises a No. 1 electrolytic cell body 1, a No. 2 electrolytic cell body 2 and a gasket 8 arranged between the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell body 2, a polyamide membrane 12 and an ion exchange membrane 13 are arranged on the gasket 8, the polyamide membrane 12 is located on one side close to the No. 1 electrolytic cell body 1, and the ion exchange membrane 13 is located on the other side close to the No. 2 electrolytic cell body 2; the No. 1 electrolytic cell body 1 has a first cavity, the first cavity is used to hold a solution to be tested, and the working electrode 3 and the recording electrode 4 extend into the first cavity; the No. 2 electrolytic cell body 2 has a second cavity, the second cavity is used to hold a solution to be tested, and the counter electrode 5 and the reference electrode 15 extend into the second cavity.
[0062] Among them, the end of the working electrode 3 and the end of the counter electrode 5 are made of platinum sheets with a size of 3 cm × 3 cm, which are placed on the outside of the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell, respectively. The Luggin capillary 6 is a commercial L-type sand core salt bridge. The Ag / AgCl recording electrode 4 and the Ag / AgCl reference electrode 15 are placed in the corresponding Luggin capillary 6, respectively. At the same time, the Luggin capillary 6 is filled with potassium chloride with a concentration of 3 M. The Luggin capillary 6 is located on the inside of the No. 1 electrolytic cell body 1 and the No. 2 electrolytic cell, respectively. The No. 1 electrolytic cell body 1, the polyamide membrane 12 on the gasket 8 and the ion exchange membrane 13, and the No. 2 electrolytic cell body 2 are connected by four fixing rods 9, thereby forming a measuring cell 11 of a four-electrode system. It is worth noting that the platinum sheet, the outlet of the Luggin capillary 6, the polyamide film and the center of the ion exchange membrane 13 are kept on the same horizontal line to ensure the accuracy and reliability of the experiment.
[0063] Example 2
[0064] This embodiment specifically provides a method for measuring the mass transfer resistance of a polyamide membrane to potassium ions, and the specific steps are as follows:
[0065] (1) The commercial NF90 polyamide membrane was soaked in 25% v / v isopropanol for 30 min and then washed with ultrapure water three times, each time for 8 h. Subsequently, the non-woven fabric support layer of the commercial NF90 polyamide membrane was peeled off; the CMX cation exchange membrane was soaked in 50 mM KCl solution for 24 h; and the non-woven fabric support layer of the commercial NF90 polyamide membrane was bonded to the soaked CMX cation exchange membrane.
[0066] (2) Add 50 mL of 50 mM KCl solution to each of the No. 1 and No. 2 electrolytic cells, ensuring that the solution completely covers the 3 cm × 3 cm platinum sheet.
[0067] (3) Connect the platinum sheet at the end of the working electrode and the Ag / AgCl recording electrode to the first signal terminal of the electrochemical workstation, and connect the platinum sheet at the end of the counter electrode and the Ag / AgCl reference electrode to the second signal terminal of the electrochemical workstation.
[0068] (4) Set the experimental parameters on the electrochemical workstation and use linear sweep voltammetry to determine the current and potential difference spectra of potassium ions across the membrane; set the test parameters to a starting voltage of 0 mV and an ending voltage of 5 mV, respectively, and a scan rate of 0.5 mV / s; perform the test three times in a row until the test system is stable.
[0069] (5) The current-potential difference spectrum (scatter plot) obtained was recorded by an electrochemical workstation and linearly fitted; the mass transfer resistance of potassium ions was calculated by the derivative of the fitting slope; under the same conditions, the mass transfer resistance of potassium ions containing only CMX cation exchange membrane was measured, and the difference between the two resistances was the transmembrane resistance of potassium ions passing through the commercial NF90 polyamide membrane; the test results are shown in Figure 2 .
[0070] pass Figure 2 It can be found that the slope of the commercial NF90 polyamide membrane bonded to the CMX cation exchange membrane is smaller than the slope of the CMX cation exchange membrane alone. Through linear fitting analysis, it is found that the mass transfer resistance of the commercial NF90 polyamide membrane to potassium ions is 32.7 Ω cm 2 .
[0071] Example 3
[0072] This embodiment provides a method for measuring the mass transfer resistance of a polyamide membrane to chloride ions, and the specific steps are as follows:
[0073] (1) The commercial NF90 polyamide membrane was soaked in 25% v / v isopropanol for 30 min and then washed with ultrapure water three times, each time for 8 h. Subsequently, the non-woven fabric support layer of the commercial NF90 polyamide membrane was peeled off; the AMX anion exchange membrane was soaked in 50 mM KCl solution for 28 h; and the non-woven fabric support layer of the commercial NF90 polyamide membrane was bonded to the soaked AMX anion exchange membrane.
[0074] (2) Add 50 mL of 50 mM KCl solution to each of the No. 1 and No. 2 electrolytic cells, making sure that the solution completely covers the 3 cm × 3 cm platinum sheet.
[0075] (3) Connect the platinum sheet at the end of the working electrode and the Ag / AgCl recording electrode to the first signal terminal of the electrochemical workstation, and connect the platinum sheet at the end of the counter electrode and the Ag / AgCl reference electrode to the second signal terminal of the electrochemical workstation.
[0076] (4) Set the experimental parameters on the electrochemical workstation and use linear sweep voltammetry to determine the current and potential difference spectra of chloride ions across the membrane; set the test parameters to a starting voltage of 0 mV and an ending voltage of -5 mV, respectively, and a scan rate of 0.5 mV / s; perform the test three times in a row until the test system is stable.
[0077] (5) The obtained current-potential difference spectrum (scatter plot) was recorded by an electrochemical workstation and linearly fitted; the mass transfer resistance of chloride ions was calculated by the derivative of the fitting slope; under the same conditions, the mass transfer resistance of chloride ions containing only AMX anion exchange membrane was measured, and the difference between the two resistances was the transmembrane resistance of chloride ions passing through the commercial NF90 polyamide membrane; the test results are shown in Figure 3 .
[0078] pass Figure 3 It can be found that the slope of the commercial NF90 polyamide membrane bonded with the AMX anion exchange membrane is smaller than the slope of the AMX anion exchange membrane alone. The mass transfer resistance of the commercial NF90 polyamide membrane to chloride ions is 28.2 Ωcm through linear fitting. 2 .
[0079] Example 4
[0080] This embodiment provides a method for measuring the mass transfer resistance of a polyamide membrane to sodium ions, and the specific steps are as follows:
[0081] (1) The commercial NF90 polyamide membrane was soaked in 25% v / v isopropanol for 30 min, and then washed with ultrapure water three times, each time for 8 h. Subsequently, the non-woven fabric support layer of the commercial NF90 polyamide membrane was peeled off; the CMX cation exchange membrane was soaked in 100 mM Na2SO4 solution for 24 h; and the non-woven fabric support layer of the commercial NF90 polyamide membrane was bonded to the soaked CMX cation exchange membrane.
[0082] (2) Add 50 mL of 100 mM Na2SO4 solution to each of the No. 1 and No. 2 electrolytic cells, ensuring that the solution completely covers the 3 cm × 3 cm platinum sheet.
[0083] (3) Connect the platinum sheet at the end of the working electrode and the Ag / AgCl recording electrode to the first signal terminal of the electrochemical workstation, and connect the platinum sheet at the end of the counter electrode and the Ag / AgCl reference electrode to the second signal terminal of the electrochemical workstation.
[0084] (4) Set the experimental parameters on the electrochemical workstation and use linear sweep voltammetry to determine the current and potential difference spectra of sodium ions across the membrane; set the test parameters to a starting voltage of 0 mV and an ending voltage of 5 mV, respectively, and a scan rate of 0.5 mV / s; perform the test three times in a row until the test system is stable.
[0085] (5) The obtained current-potential difference spectrum (scatter plot) was recorded by an electrochemical workstation and linearly fitted; the mass transfer resistance of sodium ions was calculated by the derivative of the fitting slope; under the same conditions, the mass transfer resistance of sodium ions containing only CMX cation exchange membrane was measured, and the difference between the two resistances was the transmembrane resistance of sodium ions passing through the commercial NF90 polyamide membrane; the test results are shown in Figure 4 .
[0086] pass Figure 4 It can be found that the slope of the commercial NF90 polyamide membrane bonded to the CMX cation exchange membrane is smaller than the slope of the CMX cation exchange membrane alone. The mass transfer resistance of the commercial NF90 polyamide membrane to sodium ions is 14.3Ω cm-1 through linear fitting analysis. 2 .
[0087] Example 5
[0088] This embodiment provides a method for measuring the mass transfer resistance of a polyamide membrane to sulfate ions, and the specific steps are as follows:
[0089] (1) The commercial NF90 polyamide membrane was soaked in 25% v / v isopropanol for 30 min, and then washed with ultrapure water three times, each time for 8 h. Subsequently, the non-woven fabric support layer of the commercial NF90 polyamide membrane was peeled off; the AMX anion exchange membrane was soaked in 100 mM Na2SO4 solution for 24 h; and the non-woven fabric support layer of the commercial NF90 polyamide membrane was bonded to the soaked AMX anion exchange membrane.
[0090] (2) Add 50 mL of 100 mM Na2SO4 solution to each of the No. 1 and No. 2 electrolytic cells, ensuring that the solution completely covers the 3 cm × 3 cm platinum sheet.
[0091] (3) Connect the platinum sheet at the end of the working electrode and the Ag / AgCl recording electrode to the first signal terminal of the electrochemical workstation, and connect the platinum sheet at the end of the counter electrode and the Ag / AgCl reference electrode to the second signal terminal of the electrochemical workstation.
[0092] (4) Set the experimental parameters on the electrochemical workstation and use linear sweep voltammetry to determine the current and potential difference spectra of sulfate ions across the membrane; set the test parameters to a starting voltage of 0 mV and an ending voltage of -5 mV, respectively, and a scan rate of 0.5 mV / s; perform the test three times in a row until the test system is stable.
[0093] (5) The obtained current-potential difference spectrum (scatter plot) was recorded by an electrochemical workstation and linearly fitted; the mass transfer resistance of sulfate ions was calculated by the derivative of the fitting slope; under the same conditions, the mass transfer resistance of sulfate ions containing only AMX anion exchange membrane was measured; the difference between the two resistances was the transmembrane resistance of sulfate ions passing through the commercial NF90 polyamide membrane. The test results are shown in Figure 5 .
[0094] pass Figure 5 It can be found that the slope of the commercial NF90 polyamide membrane bonded with the AMX anion exchange membrane is smaller than the slope of the AMX anion exchange membrane alone. The mass transfer resistance of the commercial NF90 polyamide membrane to sulfate ions is 19.4Ω cm-1 through linear fitting. 2 .
[0095] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A device for measuring the single ion mass transfer resistance of a polyamide membrane, characterized in that: include: An electrochemical workstation (14), wherein a first signal terminal of the electrochemical workstation (14) is connected to a working electrode (3) and a recording electrode (4), and a second signal terminal of the electrochemical workstation (14) is connected to a counter electrode (5) and a reference electrode (15); A measuring cell (11), the measuring cell (11) comprising a first electrolytic cell body (1), a second electrolytic cell body (2), and a gasket (8) disposed between the first electrolytic cell body (1) and the second electrolytic cell body (2), a polyamide membrane (12) and an ion exchange membrane (13) being disposed on the gasket (8), the polyamide membrane (12) being located on one side close to the first electrolytic cell body (1), and the ion exchange membrane (13) being located on the other side close to the second electrolytic cell body (2); The first electrolytic cell body (1) has a first cavity, the first cavity is used to contain a solution to be tested, and the working electrode (3) and the recording electrode (4) extend into the first cavity; The second electrolytic cell body (2) has a second cavity, the second cavity is used to contain the solution to be tested, and the counter electrode (5) and the reference electrode (15) extend into the second cavity; The recording electrode (4) is located on a side close to the polyamide membrane (12), and the reference electrode (15) is located on a side away from the ion exchange membrane (13).
2. The device for measuring the single ion mass transfer resistance of a polyamide membrane according to claim 1, characterized in that: The end of the working electrode (3) and the end of the counter electrode (5) are formed as a sheet-shaped platinum electrode or a sheet-shaped titanium electrode; The reference electrode (15) and the recording electrode (4) are Ag / AgCl electrodes; The effective surface area of the polyamide membrane (12) is smaller than the surface area of the sheet-shaped platinum electrode or the sheet-shaped titanium electrode; The effective surface area of the polyamide membrane (12) is 1 to 4 cm 2 .
3. The device for measuring the single ion mass transfer resistance of a polyamide membrane according to claim 1, characterized in that: A cover plate (10) is provided on the top of the first electrolytic cell body (1) and the second electrolytic cell body (2), respectively. A first through hole and a second through hole are provided on the cover plate (10). Threaded sleeves (7) are provided in the first through hole and the second through hole. One of the threaded sleeves (7) is used to install the working electrode (3) and / or the counter electrode (5). A Luggin capillary (6) is provided in the other threaded sleeve (7). The reference electrode (15) and / or the recording electrode (4) are provided in the Luggin capillary (6).
4. The device for measuring the single ion mass transfer resistance of a polyamide membrane according to claim 3, characterized in that: The Luggin capillary (6) is an L-shaped sand core salt bridge or an L-shaped Luggin capillary; The distance between the elbow outlet of the Luggin capillary (6) and the surface of the polyamide membrane (12) is 1 to 2 mm.
5. The device for measuring the single ion mass transfer resistance of a polyamide membrane according to claim 1, characterized in that: Also includes: A fixing rod (9), wherein the fixing rod (9) comprises four fixing rods, and the four fixing rods (9) pass through the gasket (8) to connect the first electrolytic cell body (1) and the second electrolytic cell body (2).
6. A method for determining the single ion mass transfer resistance of a polyamide membrane, characterized in that: The following steps are involved: S1, providing the device according to any one of claims 1 to 5, attaching a polyamide membrane (12) to the ion exchange membrane (13) of the device, and injecting a solution to be tested into the first electrolytic cell body (1) and the second electrolytic cell body (2) of the device; S2, starting the electrochemical workstation (14) of the device, measuring the current-potential difference spectrum of a single ion across the membrane, and obtaining the cation / anion mass transfer resistance value by fitting the slope calculation.
7. The method according to claim 6, characterized in that The step S1 further comprises: Before using the ion exchange membrane (13), immersing the ion exchange membrane (13) in the solution to be tested for 12 to 72 hours; The polyamide membrane (12) is a composite polyamide membrane. Before using the composite polyamide membrane, the composite polyamide membrane is immersed in an alcohol solution for 30 to 120 minutes or Soaking the composite polyamide membrane in ultrapure water for 12 to 72 hours; The alcohol solution is one or more of ethanol, methanol, and isopropanol, and the volume fraction of the alcohol solution is 10% to 40%.
8. The method according to claim 6, characterized in that The concentration of the solution to be tested is 0.01mM~1000mM; The cation in the solution to be tested is Li + 、Na + , K + , Rb + , Cs + NH4 + , Ca 2+ Mg 2+ , Ba 2+ One or more of; The anion in the solution to be tested is Cl - 、SO4 2- 、NO3 - PO4 3- 、CO3 2- and ClO4 - One or more of .
9. The method according to claim 6, characterized in that The working voltage of the electrochemical workstation (14) is -50mV~50mV, and the scanning rate is 0.1mV / s~100mV / s.
10. The method according to claim 6, characterized in that The working current of the electrochemical workstation (14) is -0.1 mA / cm 2 ~1mA / cm 2 , the application time is 20~60s.