A 13.9 grade annealing-free hot-rolled cold heading steel wire rod and a manufacturing method thereof

Through high C-containing Ti, Mo chemical components and online salt bath isothermal control technology, tempered pearlite and tempered Sorthiite structures are formed, which solves the high energy consumption and material cost in the manufacturing process of cold heading steel strips in the existing technology. The problem of high and brittle breaking risks has achieved efficient green manufacturing of 13.9-level annealing-free high-strength fastener bolts.

CN118639128BActive Publication Date: 2024-11-19JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118671.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-19
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing cold heading steel strips for grade 13.9 ultra-high strength fasteners require spherical annealing during the manufacturing process, resulting in high energy consumption, large emissions, low efficiency, and strengthening alloys and microalloy components increase material cost and brittle breakage. Risk, it is difficult to meet the needs of annealing-free process.

Method used

Using high C-containing Ti and Mo chemical composition design, combined with online salt bath isothermal control technology, to form microstructures mainly composed of tempered pearlite and tempered cortexite, reduce the amount of alloy, improve the plasticity and strength of the strip, and avoid The emergence of bainite and martensite hard and brittle phases.

Benefits of technology

The 13.9-level annealing-free hot-rolled cold-heading steel strips have been achieved, reducing the risks of drawing and breaking wires and cold heading cracking, improving the yield rate, and adapting to the lightweight and clean development needs of the automobile industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639128B_ABST
    Figure CN118639128B_ABST
Patent Text Reader

Abstract

The invention relates to a 13.9-grade annealing-free hot-rolled cold-heading steel wire rod and a manufacturing method thereof. The invention comprises the following steps: based on a high C-containing Ti and Mo chemical composition, the wire rod is controlled by rolling and spinning to form a wire rod, and then an online salt bath isothermal control is performed, so that the wire rod first passes through a front-stage molten salt, and the wire rod is cooled to a troostite phase region at a cooling rate of ≥43°C / s for isothermal phase transformation, so that austenite is partially transformed into a troostite structure, and then the wire rod is heated and isothermally heated through a rear-stage molten salt, so that untransformed austenite is transformed into a pearlite structure, and at the same time, the troostite structure, the pearlite structure and the carbide are transformed into a spheroidized structure, and finally, the wire rod is slowly cooled through a roller to form a cold-heading steel wire rod having a microstructure including tempered pearlite, tempered troostite, ferrite and quasi-spheroidized carbide, so that the wire rod structure regulation and strength-plasticity matching are achieved, the tensile strength is 1080-1130MPa, and the cross-sectional shrinkage is 51%-56%, and the wire rod is suitable for annealing-free, efficient and green manufacturing of 13.9-grade ultra-high-strength fastener bolts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a 13.9-grade annealing-free hot-rolled cold-heading steel wire rod and a manufacturing method thereof. Background Art

[0002] Bolt fastening is an important connection method for industrial equipment and is widely used in the automotive industry, mechanical equipment, construction and other fields. Cold heading steel, as the parent material of bolts, plays a vital role in the performance of bolts. With the development of new energy vehicles and other application fields, the demand and requirements for cold heading steel wire rods are also increasing. At present, the research and development of cold heading steel wire rods for 13.9 grade ultra-high strength fasteners is mainly concentrated on the basis of medium carbon steel. By increasing the alloy content, adding micro-alloy elements, and adjusting the wire rod structure to contain part of bainite, martensite or all bainite, the strength grade is improved. For example, the 13.9 grade and 14.9 grade delayed fracture resistant high-strength fastener wire rods and their manufacturing methods disclosed in patent CN104046903B adopt a medium C-Si-Mn-Cr-Mo-V-Nb-B-Al composition design, combined with low-temperature spinning, Stelmor slow cooling or fast first and then slow cooling to obtain a bainite-based structure, but on the one hand, the obtained wire rod has insufficient plasticity, which is not suitable for the drawing or cold heading process of bolt manufacturing. A spheroidizing annealing process is also required before the process to improve the cold deformation performance, which brings about problems such as many bolt manufacturing processes, high energy consumption and emissions, and low efficiency. Therefore, in order to adapt to the continuous development needs of the automotive industry towards lightweight and cleanness, it is necessary to develop 13.9 grade annealing-free hot-rolled cold heading steel wire rod to achieve efficient and green manufacturing of ultra-high strength fastener bolts; on the other hand, the content of strengthening alloys and micro-alloy components in the wire rod is relatively high, which increases the material cost. At the same time, the bainite structure as a hard and brittle phase increases the risk of brittle fracture of the wire rod, which is easy to break during the process of steel mill coiling, steel mill transporting coils to downstream, and downstream users uncoiling and unwinding the coils, resulting in waste of raw materials and a decrease in the yield rate, which also limits the application of cold heading steel wire rods.

[0003] Although some annealing-free cold heading steel wire rods have been developed, they are mainly concentrated in cold heading steel wire rods for 8.8~10.9 grade fasteners. The technical difficulties and causes of not meeting the requirements of 13.9 grade fasteners to omit the annealing process include:

[0004] (1) In order to meet the performance level of 13.9 fasteners after annealing-free, drawing, cold heading and tempering processes, a higher strength component system is required, which increases the difficulty of improving the plasticity of cold heading steel wire rods. The annealing-free cold heading steel production design, which uses low-temperature wire drawing and slow cooling after rolling to obtain more deformation-induced ferrite and coarse pearlite to improve the plasticity of the wire rod, will lead to excessive deterioration of the wire rod strength. It is necessary to strengthen it through drawing and cold heading with a large area reduction rate, which further increases the plasticity loss in the process. At the same time, the pearlite structure contains large organizational stress and dislocation density, which has limited effect on improving plasticity. The plasticity of the wire rod is still insufficient, which aggravates the risk of wire breakage during drawing and cracking during cold heading, or it is impossible to reach the final performance level through tempering.

[0005] (2) Carbon is an economical element that can improve the strength of steel. Replacing strengthening alloys or microalloying elements is beneficial to reducing material costs. However, on the one hand, as the carbon content increases, the risk of secondary cementite precipitation increases. When using low-temperature spinning and Stelmor slow cooling processes, the precipitation temperature interval of secondary cementite is longer, making the network carbides in the steel tend to be continuous and coarsened, destroying the continuity of the matrix, increasing the brittleness of the material, and making the strength of the wire rod under load, especially the toughness, worse, thereby increasing the risk of cracking. The increase in carbon content also increases the temperature of the bainite phase region. When the Stelmor air cooling rate is increased, the air volume is unevenly distributed on the surface of the wire rod. The cloth increases the temperature difference of the wire rod and the risk of precipitation of bainite or even martensite abnormal organization, resulting in a significant decrease in the plasticity and yield rate of the wire rod and an increase in the mechanical fluctuation of the wire rod, which is not conducive to production and use; on the other hand, the existing high-carbon content wire rod is mainly used to obtain a high proportion of bainite organization and improve the strength of the wire rod. Due to the limited cooling control capacity of the Stelmor air cooling line, the wire rod is in a low temperature state during the continuous slow cooling phase transformation and after the bainite organization is incubated. The dislocation density of the obtained bainite organization is relatively high, which makes the final wire rod insufficient in plasticity. The increase of pearlite or ferrite organization also has limited improvement on plasticity, making it difficult for the final wire rod performance to meet the performance level requirements after drawing, cold heading and tempering.

[0006] (3) Compared with V and Nb, Ti is a microalloying element that can improve the plasticity and toughness of wire rods through fine grain strengthening and precipitation strengthening. It can form strong hydrogen traps while strengthening the matrix, and can further improve the hydrogen embrittlement resistance of steel. However, in order to improve the plasticity of cold heading steel wire rods through low-temperature wire drawing and heat preservation and slow cooling, the temperature in the rolling stage is relatively low, which causes the precipitation of deformed austenite, which is not conducive to microalloy precipitation strengthening in the rolling stage. At the same time, under continuous slow cooling after rolling, the time to pass through the precipitation phase temperature range is still relatively short, resulting in fewer or coarser nano-scale precipitates, resulting in waste of alloys and even a decrease in the performance of the final product. Summary of the invention

[0007] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a 13.9-grade annealing-free hot-rolled cold-heading steel wire rod and a manufacturing method thereof, which can reduce the amount of alloy, give play to the role of C and Ti, realize the wire rod structure regulation and the matching of strength and plasticity, and is suitable for the annealing-free, efficient and green manufacturing of 13.9-grade ultra-high strength fastener bolts, which is beneficial to reduce the risk of wire breakage during drawing and cracking during cold heading, and improve the yield rate.

[0008] The technical solution adopted by the present invention to solve its technical problem is:

[0009] A 13.9-grade annealing-free hot-rolled cold-heading steel wire rod, the chemical composition and mass percentage of the cold-heading steel wire rod include: C: 0.72%-0.77%, Si: 0.10%-0.30%, Mn: 0.30%-0.50%, Ti: 0.010%-0.030%, Mo: 0.10%-0.30%, P≤0.015%, S≤0.015%, the rest is Fe and unavoidable impurities, and the microstructure thereof includes a mixed structure consisting of 46%-52% tempered pearlite in volume percentage, 40%-49% tempered troostite in volume percentage, 2%-5% ferrite in volume percentage, and the rest is quasi-spheroidized carbides.

[0010] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:

[0011] (1) Carbon: The carbon element is the main strengthening element of the present invention. It is cheaper than other elements in steel and mainly exists in the form of carbides. It helps to provide the matrix strength of the material through solid solution strengthening and precipitation strengthening, and determines the final hardness and strength of the finished bolt after quenching and tempering. However, it also increases the risk of decarburization and the risk of cementite being distributed in a network along the grain boundary. In addition, if the carbon content is too high, the temperature of the bainite phase region is higher, which is not conducive to microstructure control. Therefore, in order to meet the final performance level requirements of 13.9 grade fasteners, taking into account cold heading performance and easy microstructure control, the mass percentage of carbon is controlled to be 0.75%~0.79%.

[0012] (2) Silicon: The element Si is often added to steel as a deoxidizer during the smelting process. It can improve the strength of the wire rod through solid solution strengthening and inhibit the grain coarsening of the wire rod after passing through the front molten salt. However, excessive silicon will increase the risk of non-metallic inclusions and decarburization, reduce the elongation, cross-sectional shrinkage and toughness of the steel, and deteriorate the cold heading forming performance. Therefore, the mass percentage of Si is controlled to be 0.10%~0.30%.

[0013] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process. It can form carbides and further improve the strength and hardenability of steel through precipitation strengthening and solid solution strengthening. However, too high Mn content will aggravate the segregation during the solidification of the steel billet, resulting in poor uniformity of the steel, increase the tendency of grain coarsening during the heating process of the material, and deteriorate the processing performance and plasticity of the steel. Too high Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.30%~0.50%.

[0014] (4) Titanium: The Ti element can refine the grains through the strain-induced precipitation mechanism during high-temperature rolling, play a role in grain refinement, reduce the work hardening rate of steel, and improve the cold working performance of steel. At the same time, the dispersed precipitation phase of Ti can improve the strength and hydrogen embrittlement resistance of the finished bolts. However, too high a Ti content will increase the cost, and the formation of coarse carbides and inclusions will also reduce the plasticity. Therefore, based on the role of Ti and material cost considerations, the mass percentage of Ti is controlled to be 0.010%~0.030%.

[0015] (5) Molybdenum: The Mo element can strongly improve the hardenability and inhibit the coarsening of the precipitated phase of the material, maximize the strengthening effect of the precipitated phase, and improve the tempering stability of the steel. Mo combined with carbon can form hydrogen traps, which can improve the delayed fracture resistance of the material. However, its cost is extremely high, and it will promote decarburization, easily form ferrite phase or brittle phase, and reduce toughness. Therefore, based on the role of Mo and material cost considerations, the mass percentage of Mo is controlled to be 0.10%~0.30%.

[0016] (6) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.

[0017] The above-mentioned cold heading steel wire rod is designed with high C containing Ti and Mo chemical composition, and the Mn content is relatively low. No alloy components such as Cr, V, Nb, and B are added, which can relatively reduce the material cost. At the same time, the microstructure of the cold heading steel wire rod is mainly tempered pearlite and tempered troostite, containing a small amount of ferrite and quasi-spheroidized carbide. The pearlite structure has better interlamellar spacing and plasticity than the troostite. After the pearlite structure is tempered and transformed into tempered pearlite, the organizational stress and dislocation density are further reduced. The troostite structure has finer interlamellar spacing and higher strength than the pearlite structure. The troostite structure is better than bainite or martensite. The distortion of the body structure is smaller and the dislocation density is lower. After the troostite structure is transformed into tempered troostite through tempering, the dislocation density is further reduced, and the carbide is further transformed into a spheroidized structure. Therefore, compared with the existing cold heading steel wire rod mainly composed of bainite, bainite or martensite, the structure mainly composed of tempered pearlite and tempered troostite retains the strength characteristics of pearlite and troostite. Combined with the solid solution strengthening effect of high C component and the large amount of dispersed precipitation strengthening effect of Ti which inhibits the coarsening of precipitation phase by Mo, the cold heading steel wire rod has the strength that is not inferior to that of the hard and brittle phase structure, but the plasticity is significantly improved.

[0018] Similarly, compared with the existing high-carbon steel wire rod mainly composed of troostite, the cold heading steel wire rod uses pearlite and troostite to regulate the plasticity of the wire rod. After tempering state regulation, the reduction of organizational stress and dislocation density enables the plasticity of the cold heading steel wire rod to be further improved, making it more suitable for drawing and cold heading manufacturing of bolts under the annealing-free process. Compared with the existing annealing-free wire rod that improves plasticity by increasing the ferrite content, the cold heading steel wire rod contains only a small amount of ferrite structure, which avoids excessive loss of wire rod strength and thereby ensures that the strength and plasticity of the wire rod are matched.

[0019] In a preferred embodiment, the interlamellar spacing of the tempered pearlite is 155-180 nm, and the interlamellar spacing of the tempered bainite is 80-115 nm. The larger the interlamellar spacing of the tempered pearlite and the tempered bainite, the lower the strength of the cold heading steel wire rod and the higher the plasticity.

[0020] In a preferred embodiment, the network carbide level of the cold heading steel wire rod is level 0, which can effectively eliminate the network carbides, avoid the deterioration of the wire rod performance caused by the network carbides, improve the utilization of carbon elements, and is more suitable for drawing and cold heading.

[0021] In a preferred embodiment, the diameter of the cold heading steel wire rod is 14.0~22.0mm, the tensile strength is 1080~1130MPa, and the cross-sectional shrinkage rate is 51%~56%. The cold heading steel wire rod avoids excessive loss of tensile strength and significantly improves the cross-sectional shrinkage rate. It can effectively reduce the risk of wire breakage during drawing and cracking during cold heading without the spheroidizing annealing process.

[0022] A method for manufacturing a 13.9 grade annealing-free hot-rolled cold-heading steel wire rod, the manufacturing method comprising:

[0023] According to the chemical composition of the 13.9 grade annealing-free hot-rolled cold heading steel wire rod described above, the wire rod is controlled by rolling to produce the wire rod. After the wire rod is spun into a wire rod at a spinning temperature of ≥930°C, it is subjected to online salt bath isothermal control, so that the wire rod first passes through the front section molten salt, and the wire rod is cooled to the sorbite phase region at a cooling rate of ≥43°C / s for isothermal phase transformation, promoting the partial transformation of high-temperature austenite into sorbite structure, and the wire rod is then heated and isothermally increased by the rear section molten salt to transform the untransformed high-temperature austenite into pearlite structure, while promoting the transformation of sorbite structure, pearlite structure and carbide into spheroidized structure, and finally is slowly cooled by a roller to obtain a cold heading steel wire rod having a microstructure including 46% to 52% tempered pearlite by volume, 40% to 49% tempered sorbite by volume, 2% to 5% ferrite by volume, and the rest being a mixed structure composed of quasi-spheroidized carbides.

[0024] The above manufacturing method adopts a high C chemical composition design containing Ti and Mo combined with an online salt bath isothermal control technology to avoid excessively low spinning temperature causing excessively low rolling temperature, which makes it difficult for Ti to precipitate and continuously refine the grains. At the same time, by first passing through the front-stage molten salt direct salt bath after spinning, compared with the Stelmor air-cooled strong cooling process, it can quickly pass through the precipitation temperature range of secondary cementite at a faster cooling rate, effectively eliminate the deterioration effect of network carbides on the wire rod, and form a larger degree of supercooling, so that the wire rod is quickly cooled to the troostite phase region for isothermal transformation, and promote the partial transformation of the high-temperature austenite structure of the wire rod after spinning into a troostite structure with finer lamellar spacing, provide matrix strength and plasticity, and prepare for controlling the proportion of tempered troostite in the structure. Since the molten salt can cover the surface of the wire rod when the wire rod passes through the molten salt and has a high heat exchange capacity, the wire rod and the molten salt exchange heat evenly, and the risk of abnormal bainite or martensite structure caused by excessive temperature difference is avoided.

[0025] Compared with the slow cooling or delayed cooling process after low-temperature spinning to make the wire rod cool continuously, the temperature of the molten salt in the rear section is higher than that of the molten salt in the front section. After the wire rod passes through the molten salt in the front section and then passes through the molten salt in the rear section to be heated and isothermal, the wire rod can reach the pearlite phase transformation temperature range, so that the untransformed high-temperature austenite in the organization is transformed into pearlite or a small amount of inevitable ferrite organization. At the same time, the temperature of the wire rod is kept consistent with that of the molten salt in the rear section for isothermal treatment instead of continuous cooling, which prolongs the isothermal time of the wire rod at a higher temperature, promotes the transformation of troostite and pearlite organizations to spheroidized organizations, reduces organizational stress and dislocation density, and transforms In order to temper the bainite and tempered pearlite structures, the carbides are transformed into spheroidized structures. On the basis of Mo inhibiting the coarsening of the precipitate phase, TiC precipitates are dispersed and precipitated in large quantities on the grain boundaries and dislocations within the grains to avoid their growth and aggregation, maximize the strengthening effect of the dispersed precipitate phase, and then regulate the strength and plasticity of the wire rod. Finally, under the action of roller slow cooling, the high-temperature residual heat after the wire rod passes through the rear section of the molten salt is utilized to promote further toughening of the wire rod structure and further spheroidization of carbides under continuous slow cooling, thereby improving the softening effect of the wire rod and avoiding the strength and excessive loss of the wire rod, and finally realizing the control of the cold heading steel wire rod structure.

[0026] In a preferred embodiment, during the controlled rolling, the heating temperature of the steel billet is controlled to be ≤1120°C before rolling, and the soaking time is 2-3 hours, so as to promote the full dissolution and homogenization of the alloy elements in the steel, and avoid the risks of energy waste, burning, coarsening of original grains and decarburization caused by excessively high heating temperature of the steel billet and long soaking time.

[0027] In a preferred embodiment, during the controlled rolling, the initial rolling temperature is controlled to be 1055~1100℃, the initial rolling reduction is 30%~45%, and the precipitation temperature of Ti is higher than that of Nb and V. Since the direct salt bath after wire drawing can quickly enter the troostite phase region for isothermal transformation, the limitation of low-temperature wire drawing on the production of cold heading steel wire rods is broken. Therefore, in the controlled rolling stage, high-temperature rolling can be used to induce a large amount of Ti-containing precipitation phase to disperse and precipitate to pin the grain boundaries, and a large initial rolling reduction can be used to refine the original austenite, thereby ultimately refining the grains, thereby avoiding the initial rolling temperature being too low, causing the precipitation of Ti to slow down, the rolling speed to be too low, the wear of the rolling mill to increase, and the impact on production efficiency.

[0028] In a preferred embodiment, during the controlled rolling, the final rolling temperature is 940-980°C, and the final rolling reduction is 20%-33%, so as to avoid the reduction of nano-scale precipitates caused by too low a final rolling temperature, and utilize the Ti-containing precipitate phase to continuously refine the grains and strengthen the matrix, so that cracks are not easy to initiate and propagate during drawing or cold heading.

[0029] In a preferred embodiment, the temperature of the front-stage molten salt is 460-490°C, and the processing time is 20-40s. The lower the temperature of the front-stage molten salt, the longer the processing time, and the higher the cooling rate, the more the wire rod is transformed into troostite, the finer the spacing between the troostite lamellae, the more the proportion of tempered troostite in the obtained microstructure, the higher the strength of the wire rod, and the lower the plasticity. However, if the temperature is too low, there is a risk of precipitation of abnormal bainite structure. If the time is too long, the content of tempered pearlite in the structure is affected, which is not good for the plasticity of the wire rod. On the contrary, if the temperature of the front-stage molten salt is higher, The shorter the processing time, the smaller the proportion of tempered troostite in the wire rod structure, the coarser the lamellar spacing, the lower the wire rod strength and the higher the plasticity. However, the excessively high temperature of the molten salt in the front stage and the too short processing time are not conducive to the transformation of the austenite structure to the troostite structure, causing excessive loss of wire rod strength. The excessively large troostite lamellar spacing will also increase the difficulty of spheroidization and even the risk of network carbide precipitation. Therefore, the temperature and processing time of the molten salt in the front stage can be further adjusted to control the partial transformation of the austenite structure into the troostite structure with finer lamellar spacing, thereby providing matrix strength and plasticity.

[0030] In a preferred embodiment, the molten salt circulation rate of the front-stage molten salt is 600~800t / h, and the molten salt temperature rise is ≤8°C. A larger molten salt circulation rate is used to control the molten salt temperature rise, maintain the temperature accuracy of the wire rod passing through the front-stage molten salt isotherm, and avoid the occurrence of abnormal bainite structure.

[0031] In a preferred embodiment, the temperature of the molten salt in the latter stage is 525-570°C, and the treatment time is 300-600s. The higher the temperature of the molten salt in the latter stage and the longer the treatment time, the larger the pearlite interlamellar spacing of the untransformed high-temperature austenite, the higher the ferrite content, and the more conducive to the transformation of troostite, pearlite structure and carbide to spheroidized structure, so that the toughening and spheroidizing effects are more obvious, the strength of the wire rod decreases, and the plasticity increases. However, if the temperature of the molten salt in the latter stage is too high, the spacing between the precipitated pearlite lamellae is too large, and the proportion of ferrite is too high, which will cause excessive Strength loss, too long processing time, there is a risk of coarsening of Ti precipitates and agglomeration and growth of quasi-spheroidized carbides, which will lead to a significant loss of strength and plasticity. On the contrary, the lower the temperature of the molten salt in the later stage and the shorter the processing time, the lower the ferrite content and the lower the spacing between the tempered pearlite lamellae, which is not conducive to the transformation of carbides to spheroidized structure, the weaker the toughening and spheroidizing softening effects, the higher the strength of the wire rod and the lower the plasticity. Therefore, the temperature and processing time of the molten salt in the later stage can be further controlled to further regulate the matching of the wire rod structure and strength and plasticity and moderately soften the matrix structure.

[0032] In a preferred embodiment, the molten salt circulation rate of the rear-stage molten salt is 150~250t / h, and the molten salt temperature rise is ≤5°C. A relatively small molten salt circulation rate can be used to control the molten salt temperature rise, maintain the isothermal treatment temperature accuracy of the rear-stage molten salt and reduce the molten salt circulation energy consumption.

[0033] In a preferred embodiment, the roller slow cooling controls the wire rod to be slowly cooled at a cooling rate of 0.3-0.8°C / s, and then coiled. Preferably, the coiling temperature is below 350°C. Further slow cooling can promote further toughening of the wire rod structure and further spheroidization of carbides, thereby improving the softening effect of the wire rod.

[0034] In a preferred embodiment, the roller slow cooling adopts closing the heat preservation cover, or the heat preservation cover is closed and hot air above the salt bath tank of the online salt bath isothermal control is input into the heat preservation cover at the same time, so that the air heat energy of the online salt bath isothermal control can be recycled and utilized, so as to avoid the roller speed being too low under low-speed cooling and affecting the production efficiency, further reduce energy consumption and improve productivity.

[0035] Compared with the prior art, the beneficial effects of the present invention are at least:

[0036] (1) In view of the current situation that the cold heading steel wire rod for 13.9 grade ultra-high strength fasteners still needs spheroidizing annealing, has high energy consumption and emissions, and is limited in application, the present invention adopts a high C-containing Ti and Mo chemical composition design, with a relatively low Mn content, no addition of alloy components such as Cr, V, Nb, and B, and no bainite and martensite hard and brittle phase structure. The microstructure type is a mixed structure composed mainly of tempered pearlite and tempered troostite, a small amount of ferrite and quasi-spheroidized carbide, and the tempered state structure is used to regulate the wire rod structure stress. and dislocation density, significantly improving the plasticity of wire rod, and the product tensile strength Rm can reach 1080~1130MPa, and the cross-sectional shrinkage rate Z can reach 51%~56%. It is used in the manufacture of 13.9 grade annealing-free high-strength fastener bolts and other application fields, which is beneficial to reduce the risk of wire breakage during drawing and cracking during cold heading, improve the yield rate, reduce the waste of raw materials, and realize the efficient and green manufacturing of ultra-high strength fastener bolts, which is beneficial to adapt to the continuous development of the automotive industry towards lightweight and cleanness, and has good market application prospects.

[0037] (2) In view of the fact that the existing cold heading steel wire rod is limited by the Stelmor air cooling line and is difficult to meet the current situation of 13.9 grade annealing-free wire rod manufacturing, the manufacturing method of the present invention is based on high C containing Ti and Mo chemical composition combined with online salt bath isothermal control technology to regulate the microstructure and performance of the hot rolled wire rod. First, the high temperature spinning wire rod is isothermally transformed in the troostite phase region with a large undercooling degree and a fast cooling rate by using the front-end molten salt, which effectively improves the deteriorating effect of the network carbide on the performance of the wire rod and provides matrix strength and plasticity. Then, the rear-end molten salt is used to promote the transformation of the untransformed austenite structure to pearlite, and the transformation of the troostite, pearlite and carbide to spheroidized structure, softening the matrix structure, and slow cooling is used to promote further toughening of the wire rod structure and further spheroidization of the carbide, thereby improving the softening effect of the wire rod and achieving strength and plasticity matching of the wire rod. The role of C and Ti can be effectively exerted and the yield rate can be improved, and the method has good industrial adaptability.

[0038] (3) The manufacturing method of the present invention breaks the limitation of low-temperature wire drawing on the manufacturing of cold heading steel wire rod. By inducing a large amount of Ti-containing precipitate phase to disperse and precipitate to pin the grain boundaries through high-temperature rolling, the Ti-containing precipitate phase is used to continuously refine the grains, and Mo is used to inhibit the coarsening of the material precipitate phase. The strengthening effect of the precipitate phase is maximized, which can improve the strength and hydrogen embrittlement resistance of the finished bolt. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0040] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0041] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;

[0042] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0043] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:

[0044] A preferred embodiment of the manufacturing method of the 13.9 grade annealing-free hot-rolled cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.72%, Si: 0.3%, Mn: 0.45%, Ti: 0.013%, Mo: 0.21%, P: 0.014%, S: 0.011%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online salt bath isothermal control → roller slow cooling → coiling, specifically:

[0045] The controlled rolling is used to heat a steel billet of 220 mm×220 mm through a heating furnace to promote full dissolution and homogenization of alloy elements in the steel and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 20 mm through a rolling line. The high-temperature rolling induces a large amount of Ti-containing precipitation phase to disperse and precipitate to pin the grain boundaries, and finally plays a role in refining the grains. Specifically: the heating temperature of the steel billet is controlled to be 1100°C, the soaking time is 2.5h, the initial rolling temperature is 1080°C, the initial rolling reduction is 36%, the final rolling temperature is 960°C, and the final rolling reduction is 25%.

[0046] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on the roller and transported along the roller. Through the appropriate spinning temperature, the wire rod is prevented from precipitating network carbides in the spinning stage, the grain refinement effect is continued, and favorable conditions are created for the formation of a large undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 940°C.

[0047] The online salt bath isothermal control adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller through the first salt bath tank, i.e., the front molten salt, and is quickly cooled to the molten salt temperature of the front molten salt, so that the wire rod is cooled at a cooling rate of 46°C / s, and the high-temperature spinning wire rod is controlled to quickly pass through the precipitation temperature range of secondary cementite, and isothermal phase transformation is carried out in the troostite phase region with a large undercooling degree and a fast cooling rate, so as to promote the partial transformation of high-temperature austenite into troostite structure, provide matrix strength and plasticity, and the wire rod passing through the front molten salt passes through the second salt bath. The tank, i.e. the rear section, is heated isothermally to transform the untransformed high-temperature austenite into pearlite structure, while promoting the transformation of troostite structure, pearlite structure and carbide into spheroidized structure, softening the matrix structure, so as to ensure the strength and plasticity matching of the wire rod. Specifically: the temperature of the front section molten salt is 460°C, the processing time is 40s, the molten salt circulation volume is 800t / h, and the molten salt temperature rise is ≤8°C; the temperature of the rear section molten salt is 525°C, the processing time is 300s, the molten salt circulation volume is 180t / h, and the molten salt temperature rise is ≤5°C.

[0048] The roller slow cooling process is closed with an insulation cover, and the wire rod coming out of the second salt bath tank is transported into the insulation cover by rollers. At the same time, the hot air generated above the two salt bath tanks is transported into the insulation cover as hot air for slow cooling. The slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides. Specifically: the wire rod is controlled to be slowly cooled at a cooling rate of 0.3°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 320°C. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as follows Figure 1 shown.

[0049] Comparative Example 1:

[0050] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of controlled rolling → low-temperature wire drawing → Stelmor insulation and slow cooling → coiling, specifically: the heating temperature of the steel billet is controlled to be 1050°C, the soaking time is 3h, the initial rolling temperature is 1030°C, the final rolling temperature is 910°C, the wire drawing temperature is 890°C, the Stelmor insulation and slow cooling adopts closing all fans and insulation covers, and the wire rod is conveyed by rollers. The wire rod completes phase change at a cooling rate of 1.2°C / s in the cover, and the finished wire rod is obtained after coiling off the line.

[0051] Comparative Example 2:

[0052] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to a process flow of controlled rolling → spinning → Stelmor rapid cooling → roller slow cooling → coiling. Specifically: the Stelmor rapid cooling is performed by opening 1~7# fans at 35%, so that the wire rod is cooled to 680°C at a cooling rate of 3.5°C / s; the roller slow cooling is performed by closing all fans and insulation covers, so that the wire rod completes a phase change at a cooling rate of 1.3°C / s in the cover, and the finished wire rod is obtained after coiling off the line.

[0053] Comparative Example 3:

[0054] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of controlled rolling → low-temperature wire spinning → Stelmor rapid cooling → roller slow cooling, specifically: controlling the heating temperature of the steel billet to be 1075°C, the soaking time to be 3h, the initial rolling temperature to be 150°C, the final rolling temperature to be 930°C, the wire spinning temperature to be 910°C, the Stelmor rapid cooling is performed by opening 1~6# fans at 80%, so that the wire rod is cooled to 710°C at a cooling rate of 7.4°C / s, the roller slow cooling is performed by closing all fans and insulation covers, so that the wire rod completes phase change in the cover at a cooling rate of 0.9°C / s, and the finished wire rod is obtained after going offline.

[0055] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organization and performance testing: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:

[0056] Table 1. Comparison of wire rod structure and properties by different manufacturing methods

[0057]

[0058] From the comparison results of Example 1 and Comparative Example 1, it can be seen that the design based on high C containing Ti and Mo chemical composition is not conducive to inducing Ti precipitation and grain refinement in the rolling stage compared with the low temperature spinning and slow cooling process. Although the pearlite + ferrite soft phase structure is obtained, the precipitation temperature interval time of the secondary cementite is longer, which makes the network carbide in the steel tend to be continuous and coarsened, destroying the continuity of the matrix, increasing the brittleness of the material, and improving the plasticity of the wire rod to a limited extent. The present invention combines the online salt bath isothermal control technology, first using the front section molten salt The high-temperature spinning wire rod is controlled to undergo isothermal transformation in the troostite phase region with a large undercooling degree and a fast cooling rate, which can effectively improve the deteriorating effect of network carbides on the performance of the wire rod, provide matrix strength and plasticity, and then use the subsequent molten salt to promote the transformation of the untransformed austenite structure to pearlite, and the transformation of the troostite, pearlite structure and carbide to spheroidized structure, soften the matrix structure, and use slow cooling to promote further toughening of the wire rod structure and further spheroidization of carbides, which can effectively play the role of C and Ti, improve the yield rate, and regulate the structure and performance of the hot-rolled wire rod.

[0059] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with improving the air-cooling strength after spinning, the improvement on the web carbon level is limited, the obtained troostite lamellae have a larger spacing and a lower content, and the wire rod is in a low-temperature state during the continuous slow cooling phase transformation and after the troostite structure is incubated. The dislocation density of the obtained troostite structure is relatively high, resulting in insufficient plasticity of the final wire rod. The present invention uses the tempered state structure to regulate the wire rod structure stress and dislocation density, which can significantly improve the plasticity of the wire rod.

[0060] From the comparison results of Example 1 and Comparative Example 3, it can be seen that compared with further improving the air-cooling strength after spinning, bainite structure appears. Bainite structure as a hard and brittle phase increases the risk of brittle fracture of wire rods, and is easy to break during coiling in the steel plant, transportation of coils to downstream by the steel plant, and uncoiling and unwinding of coils by downstream users, resulting in waste of raw materials and a decrease in the yield rate. The present invention does not contain bainite and martensite hard and brittle phase structures, which is beneficial to reducing the risk of wire breakage during drawing and cracking during cold heading, and improving the yield rate. Embodiment 2:

[0061] A preferred embodiment of the manufacturing method of the 13.9 grade annealing-free hot-rolled cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.75%, Si: 0.1%, Mn: 0.3%, Ti: 0.023%, Mo: 0.3%, P: 0.01%, S: 0.012%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online salt bath isothermal control → roller slow cooling → coiling, specifically:

[0062] The controlled rolling is used to heat a steel billet of 220 mm×220 mm through a heating furnace to promote full dissolution and homogenization of alloy elements in the steel and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 16 mm through a rolling line. The high-temperature rolling induces a large amount of Ti-containing precipitation phase to disperse and precipitate to pin the grain boundaries, and finally plays a role in refining the grains. Specifically: the heating temperature of the steel billet is controlled to be 1110°C, the soaking time is 2.5h, the initial rolling temperature is 1090°C, the initial rolling reduction is 40%, the final rolling temperature is 970°C, and the final rolling reduction is 29%.

[0063] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on the roller and transported along the roller. Through the appropriate spinning temperature, the wire rod is prevented from precipitating network carbides in the spinning stage, the grain refinement effect is continued, and favorable conditions are created for the formation of a large undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 950°C.

[0064] The online salt bath isothermal control adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller through the first salt bath tank, i.e., the front molten salt, and is quickly cooled to the molten salt temperature of the front molten salt, so that the wire rod is cooled at a cooling rate of 45°C / s, and the high-temperature spinning wire rod is controlled to quickly pass through the precipitation temperature range of secondary cementite, and isothermal phase transformation is carried out in the troostite phase region with a large undercooling degree and a fast cooling rate, so as to promote the partial transformation of high-temperature austenite into troostite structure, provide matrix strength and plasticity, and the wire rod passing through the front molten salt passes through the second salt bath. The tank, i.e. the rear section, is heated isothermally to transform the untransformed high-temperature austenite into pearlite structure, while promoting the transformation of troostite structure, pearlite structure and carbide into spheroidized structure, softening the matrix structure, so as to ensure the strength and plasticity matching of the wire rod. Specifically: the temperature of the front section molten salt is 475°C, the processing time is 25s, the molten salt circulation volume is 700t / h, and the molten salt temperature rise is ≤8°C; the temperature of the rear section molten salt is 536°C, the processing time is 500s, the molten salt circulation volume is 150t / h, and the molten salt temperature rise is ≤5°C.

[0065] The roller slow cooling process is closed with an insulation cover, and the wire rod coming out of the second salt bath tank is transported into the insulation cover by rollers. At the same time, the hot air generated above the two salt bath tanks is transported into the insulation cover as hot air for slow cooling. The slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides. Specifically: the wire rod is controlled to be slowly cooled at a cooling rate of 0.4°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 335°C. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as shown below Figure 2 shown.

[0066] Comparative Example 4:

[0067] A method for manufacturing a wire rod, which differs from that of Example 2 in that, specifically: the heating temperature of the steel billet is controlled to be 1070°C, the soaking time is 3h, the initial rolling temperature is 1040°C, the final rolling temperature is 920°C, the spinning temperature is 900°C, the wire rod after spinning passes through a front-stage molten salt, the wire rod is controlled to be cooled at a cooling rate of 40°C / s, and the finished wire rod is obtained after being rolled off the line.

[0068] Comparative Example 5:

[0069] A method for manufacturing wire rod, which differs from Example 2 in that: specifically: the wire rod after spinning passes through a front-stage molten salt, and the wire rod is controlled to be cooled at a cooling rate of 48°C / s. The temperature of the front-stage molten salt is 455°C, the processing time is 45s, the molten salt circulation rate is 850t / h, and the finished wire rod is obtained after being rolled off the line.

[0070] Comparative Example 6:

[0071] A method for manufacturing wire rod, which differs from Example 2 in that: specifically: the wire rod after spinning passes through a front-stage molten salt, and the wire rod is controlled to be cooled at a cooling rate of 44°C / s. The temperature of the front-stage molten salt is 495°C, and the processing time is 15s. The finished wire rod is obtained after being rolled off the line. Embodiment 3:

[0072] A preferred embodiment of the manufacturing method of the 13.9 grade annealing-free hot-rolled cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.77%, Si: 0.15%, Mn: 0.5%, Ti: 0.01%, Mo: 0.25%, P: 0.013%, S: 0.012%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online salt bath isothermal control → roller slow cooling → coiling, specifically:

[0073] The controlled rolling is used to heat a steel billet of 220 mm×220 mm through a heating furnace to promote full dissolution and homogenization of alloy elements in the steel and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 22 mm through a rolling line. The high-temperature rolling induces a large amount of Ti-containing precipitation phase to disperse and precipitate to pin the grain boundaries, and finally plays a role in refining the grains. Specifically: the heating temperature of the steel billet is controlled to be 1085°C, the soaking time is 3h, the initial rolling temperature is 1055°C, the initial rolling reduction is 30%, the final rolling temperature is 940°C, and the final rolling reduction is 20%.

[0074] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on the roller and transported along the roller. Through the appropriate spinning temperature, the wire rod is prevented from precipitating network carbides in the spinning stage, the grain refinement effect is continued, and favorable conditions are created for the formation of a large undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 930°C.

[0075] The online salt bath isothermal control adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller through the first salt bath tank, i.e., the front molten salt, and is quickly cooled to the molten salt temperature of the front molten salt, so that the wire rod is cooled at a cooling rate of 43°C / s, and the high-temperature spinning wire rod is controlled to quickly pass through the precipitation temperature range of secondary cementite, and isothermal phase transformation is carried out in the troostite phase region with a large undercooling degree and a fast cooling rate, so as to promote the partial transformation of high-temperature austenite into troostite structure, provide matrix strength and plasticity, and the wire rod passing through the front molten salt passes through the second salt bath. The tank, i.e. the rear section, is heated isothermally to transform the untransformed high-temperature austenite into pearlite structure, while promoting the transformation of troostite structure, pearlite structure and carbide into spheroidized structure, softening the matrix structure, so as to ensure the strength and plasticity matching of the wire rod. Specifically: the temperature of the front section molten salt is 490°C, the processing time is 20s, the molten salt circulation volume is 600t / h, and the molten salt temperature rise is ≤8°C; the temperature of the rear section molten salt is 570°C, the processing time is 400s, the molten salt circulation volume is 250t / h, and the molten salt temperature rise is ≤5°C.

[0076] The roller slow cooling process is closed with a heat preservation cover, and the wire rod coming out of the second salt bath tank is conveyed by a roller into the heat preservation cover for slow cooling treatment. The slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides. Specifically: the wire rod is controlled to be slowly cooled at a cooling rate of 0.8°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 340°C. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as follows Figure 3 shown.

[0077] Comparative Example 7:

[0078] A method for manufacturing a wire rod, which differs from Example 3 in that: specifically: the temperature of the rear-stage molten salt is 585° C., the processing time is 610 s, and the finished wire rod is obtained after the coil is rolled off the line.

[0079] Comparative Example 8:

[0080] A method for manufacturing a wire rod, which differs from the manufacturing method of Example 3 in that: specifically: the processing time is 700s, and the finished wire rod is obtained after the coil is rolled off the line.

[0081] Comparative Example 9:

[0082] A method for manufacturing a wire rod, which differs from Example 3 in that: specifically: the temperature of the rear-stage molten salt is 520° C., the processing time is 250 s, and the finished wire rod is obtained after the coil is rolled off the line. Embodiment 4:

[0083] A preferred embodiment of the manufacturing method of the 13.9 grade annealing-free hot-rolled cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.73%, Si: 0.22%, Mn: 0.38%, Ti: 0.03%, Mo: 0.1%, P: 0.015%, S: 0.015%, and the rest are Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online salt bath isothermal control → roller slow cooling → coiling, specifically:

[0084] The controlled rolling is used to heat a steel billet of 220 mm×220 mm through a heating furnace to promote full dissolution and homogenization of alloy elements in the steel and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 14 mm through a rolling line. The high-temperature rolling induces a large amount of Ti-containing precipitation phase to disperse and precipitate to pin the grain boundaries, and finally plays a role in refining the grains. Specifically: the heating temperature of the steel billet is controlled to be 1120°C, the soaking time is 2h, the initial rolling temperature is 1100°C, the initial rolling reduction is 45%, the final rolling temperature is 980°C, and the final rolling reduction is 33%.

[0085] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on the roller and transported along the roller. Through the appropriate spinning temperature, the wire rod is prevented from precipitating network carbides in the spinning stage, the grain refinement effect is continued, and favorable conditions are created for the formation of a large undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 960°C.

[0086] The online salt bath isothermal control adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller through the first salt bath tank, i.e., the front molten salt, and is quickly cooled to the molten salt temperature of the front molten salt, so that the wire rod is cooled at a cooling rate of 46°C / s, and the high-temperature spinning wire rod is controlled to quickly pass through the precipitation temperature range of secondary cementite, and isothermal phase transformation is carried out in the troostite phase region with a large undercooling degree and a fast cooling rate, so as to promote the partial transformation of high-temperature austenite into troostite structure, provide matrix strength and plasticity, and the wire rod passing through the front molten salt passes through the second salt bath. The tank, i.e. the rear section, heats the molten salt isothermally to transform the untransformed high-temperature austenite into pearlite structure, while promoting the transformation of troostite structure, pearlite structure and carbide into spheroidized structure, softening the matrix structure, so as to ensure the strength and plasticity matching of the wire rod. Specifically: the temperature of the front section molten salt is 482°C, the processing time is 30s, the molten salt circulation volume is 760t / h, and the molten salt temperature rise is ≤8°C; the temperature of the rear section molten salt is 552°C, the processing time is 600s, the molten salt circulation volume is 200t / h, and the molten salt temperature rise is ≤5°C.

[0087] The roller slow cooling process is closed with an insulation cover, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment. The slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides. Specifically: the wire rod is controlled to be slowly cooled at a cooling rate of 0.6°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 315°C. After packaging and storage, the finished cold heading steel wire rod is obtained.

[0088] Comparative Example 10:

[0089] A method for manufacturing a wire rod, which differs from Example 4 in that the method is manufactured according to a process flow of controlled rolling → spinning → online salt bath isothermal control → air cooling → coiling. Specifically: the air cooling process uses a heat preservation cover to open, and a roller conveys the wire rod coming out of the second salt bath tank, and the wire rod is controlled to cool at a rate of 1.8°C / s, and the finished wire rod is obtained after coiling off the line.

[0090] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 10 were subjected to organization and performance testing: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:

[0091] Table 2. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods

[0092]

[0093] It can be seen from the results of Examples 1 to 4 that the present invention can achieve a tensile strength Rm of 1080 to 1130 MPa and a cross-sectional shrinkage Z of 51 to 56%, and is used in the manufacture of 13.9-grade annealing-free high-strength fastener bolts and other application fields, achieving efficient and green manufacturing of ultra-high-strength fastener bolts, and has good market application prospects.

[0094] From the comparison results of Example 2 and Comparative Example 4, it can be seen that the low-temperature spinning causes the rolling temperature to be too low, which makes it difficult for Ti to precipitate and continuously refine the grains, and is not conducive to the formation of a large degree of supercooling to control the formation of sorbite; from the comparison results of Example 2 and Comparative Example 5, it can be seen that the lower the temperature of the front-stage molten salt, the longer the treatment time, and the higher the cooling rate, the more the wire rod is transformed into sorbite, the finer the spacing between the sorbite lamellae, the more the proportion of tempered sorbite in the obtained microstructure, the wire rod strength increases, and the plasticity decreases, but the treatment time is too long, which affects the tempered pearlite content in the organization, which is not conducive to the plasticity of the wire rod; from the comparison results of Example 2 and Comparative Example 6, it can be seen that the temperature of the front-stage molten salt is too high and the treatment time is too short, which is not conducive to the transformation of austenite structure to sorbite structure, and will cause excessive loss of wire rod strength. Excessive spacing between sorbite lamellae will also increase the difficulty of spheroidization and even the risk of precipitation of network carbides.

[0095] From the comparison results of Example 3 and Comparative Example 7, it can be seen that the higher the temperature of the molten salt in the latter stage and the longer the treatment time, the larger the interlamellar spacing of the pearlite transformed from the untransformed high-temperature austenite, the increased ferrite content, and the more conducive to the transformation of troostite, pearlite structure and carbide to spheroidized structure, making the toughening and spheroidizing effects more obvious; from the comparison results of Example 3 and Comparative Example 8, it can be seen that if the treatment time is too long, there is a risk of coarsening of Ti precipitates and agglomeration and growth of quasi-spheroidized carbides, which will lead to a significant loss of strong and plastic properties; from the comparison results of Example 3 and Comparative Example 9, it can be seen that the lower the temperature of the molten salt in the latter stage and the shorter the treatment time, it is not conducive to the transformation of carbides to spheroidized structure, the toughening and spheroidizing softening effects are weaker, the strength of the wire rod increases, and the plasticity decreases.

[0096] From the comparison results of Example 4 and Comparative Example 10, it can be seen that under the slow cooling effect of the roller, the high-temperature residual heat after the wire rod passes through the rear molten salt can be utilized to promote further toughening of the wire rod structure and further spheroidization of carbides under continuous slow cooling, thereby improving the softening effect of the wire rod.

[0097] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A 13.9 grade annealing-free hot-rolled cold heading steel wire rod, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.72% to 0.77%, Si: 0.10% to 0.30%, Mn: 0.30% to 0.50%, Ti: 0.010% to 0.030%, Mo: 0.10% to 0.30%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities, and its microstructure includes 46% to 52% by volume of tempered pearlite, 40% to 49% by volume of tempered troostite, 2% to 5% by volume of ferrite, and the rest are a mixed structure composed of quasi-spheroidized carbides; The manufacturing method comprises: controlling the rolling production of wire rods according to the chemical composition of the 13.9 grade annealing-free hot-rolled cold heading steel wire rods, spinning the wire rods at a spinning temperature of ≥930°C, performing online salt bath isothermal control, allowing the wire rods to first pass through the front section of molten salt, cooling the wire rods at a cooling rate of ≥43°C / s to the sorbite phase region for isothermal phase transformation, promoting the transformation of part of austenite into sorbite structure, and then passing through the rear section of molten salt to heat up isothermally, so that the untransformed austenite is transformed into a pearlite structure. The method comprises the following steps: preparing a cold heading steel wire rod having a microstructure of tempered pearlite, tempered troostite, ferrite and quasi-spheroidized carbide, and preparing the cold heading steel wire rod having a mixed microstructure of tempered pearlite, tempered troostite, ferrite and quasi-spheroidized carbide. The temperature of the molten salt in the front section is 460-490°C, and the treatment time is 20-40s; the temperature of the molten salt in the rear section is 525-570°C, and the treatment time is 300-600s.

2. The 13.9 grade annealing-free hot-rolled cold heading steel wire rod according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 155-180 nm, the interlamellar spacing of the tempered troostite is 80-115 nm, and the network carbide level of the cold heading steel wire rod is level 0.

3. The 13.9 grade annealing-free hot-rolled cold heading steel wire rod according to claim 1 or 2, characterized in that: The cold heading steel wire rod has a diameter of 14.0-22.0 mm, a tensile strength of 1080-1130 MPa, and a cross-sectional shrinkage of 51%-56%.

4. A method for manufacturing 13.9 grade annealing-free hot-rolled cold heading steel wire rod, characterized in that: The manufacturing method thereof comprises: According to the chemical composition controlled rolling production line of the 13.9 grade annealing-free hot-rolled cold heading steel wire rod as claimed in claim 1, after the wire rod is spun into a wire rod at a spinning temperature of ≥930°C, an online salt bath isothermal control is performed, so that the wire rod first passes through the front section molten salt, and the wire rod is cooled at a cooling rate of ≥43°C / s to the sorbite phase region for isothermal phase transformation, promoting the partial transformation of austenite into sorbite structure, and then the wire rod is heated and isothermally heated through the rear section molten salt to transform the untransformed austenite into pearlite structure, while promoting the transformation of sorbite structure, pearlite structure and carbon structure. The cold heading steel wire rod is a mixed structure composed of 46% to 52% tempered pearlite, 40% to 49% tempered troostite, 2% to 5% ferrite and the rest quasi-spheroidized carbides; the temperature of the front section molten salt is 460 to 490°C, and the processing time is 20 to 40s; the temperature of the rear section molten salt is 525 to 570°C, and the processing time is 300 to 600s.

5. The method for manufacturing 13.9 grade annealing-free hot-rolled cold heading steel wire rod according to claim 4, characterized in that: During the controlled rolling, the heating temperature of the steel billet is controlled to be ≤1120°C before rolling, and the soaking time is 2-3h.

6. The method for manufacturing 13.9 grade annealing-free hot-rolled cold heading steel wire rod according to claim 4, characterized in that: During the controlled rolling, the initial rolling temperature is controlled to be 1055-1100° C., the initial rolling reduction is controlled to be 30%-45%, the final rolling temperature is controlled to be 940-980° C., and the final rolling reduction is controlled to be 20%-33%.

7. The method for manufacturing 13.9 grade annealing-free hot-rolled cold heading steel wire rod according to claim 4, characterized in that: The molten salt circulation volume of the front-stage molten salt is 600-800 t / h, and the molten salt temperature rise is ≤8°C; the molten salt circulation volume of the rear-stage molten salt is 150-250 t / h, and the molten salt temperature rise is ≤5°C.

8. The method for manufacturing 13.9 grade annealing-free hot-rolled cold heading steel wire rod according to claim 4, characterized in that: The roller slow cooling controls the wire rod to be slowly cooled at a cooling rate of 0.3-0.8°C / s.

9. The method for manufacturing 13.9 grade annealing-free hot-rolled cold heading steel wire rod according to claim 8, characterized in that: The roller slow cooling adopts the method of closing the heat preservation cover, or the heat preservation cover is closed and hot air above the salt bath tank of the online salt bath isothermal control is input into the heat preservation cover.