Dental implant and preparation method thereof
Patent Information
- Application Number
- CN202410624398.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-20
- Publication Date
- 2024-10-01
AI Technical Summary
Existing dental implant materials are prone to fatigue, relaxation, and micro-cracks during long-term use, resulting in poor stability. Bacteria adsorbed on the surface of the material can easily cause inflammation and have poor biological activity, causing implants to fall off.
Titanium metal implants are used, designed into upper, middle and lower sections. The surface of each section has a threaded structure and a hollow structure. The surface is coated with strontium-doped nano-hydroxyapatite and PVA layers. It is prepared through 3D printing and electrolytic deposition technology to improve Biocompatibility and antimicrobial properties.
Enhance the contact area and friction between the implant and bone tissue, reduce the elastic modulus, promote osseointegration, improve the stability and biological activity of the implant, significantly improve the stability and osteogenic effect of the implant, and reduce the risk of inflammation.
Smart Images

Figure CN118718098A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tooth restoration materials, and in particular relates to a tooth implant and a preparation method thereof. Background Art
[0002] At present, dental implants are receiving more and more attention in oral medicine. Dental implants are composed of a dental implant and its supporting superstructure (crown and abutment). Dental implants, also known as artificial tooth roots, are made of artificial materials and surgically implanted into the jawbone of the edentulous area. Through the connection with the artificial tooth root, the retention and support effects are obtained to repair the missing teeth. Among my country's dental implant manufacturing companies, there are many companies engaged in abutment and crown processing, while the research on implants is still in the early stages of development.
[0003] Existing implant materials may become fatigued and loose during long-term use, especially when subjected to chewing pressure, which may cause microcracks, thereby affecting the stability and integrity of the implant; moreover, improper implant structure design may also lead to uneven stress distribution and concentration in a specific area, which may cause the implant thread to loosen the bond with bone tissue and cause the implant to fall off. In addition, the surface of existing implant materials is prone to adsorbing bacteria, forming biofilms and causing infection, which may cause patients to experience symptoms such as allergic reactions or inflammatory reactions. Furthermore, the surface roughness of existing implant materials is not enough, and the biological activity of the material is poor, which may lead to poor bone bonding strength and cause it to fall off. There have been reports in the prior art using titanium as an implant material, but the elastic modulus of titanium is quite different from that of the human jawbone, which will produce a stress shielding effect, causing the implant to loosen, thereby leading to implant failure. Moreover, the bone density of different parts of the jaw is also different. The maxillary bone is mainly cancellous bone, while the mandibular bone is thicker cortical bone. Therefore, the elastic modulus of the bone environment is different in different implant locations, and a simple and unchanging implant structure cannot match the anatomical structure of the human jaw. The existing implant materials still have problems such as long preparation time, high cost, and poor effect. Summary of the invention
[0004] In view of the above-mentioned prior art, the present invention provides a dental implant and a preparation method thereof, so as to solve the technical problems that the existing dental implant materials have poor stability and are prone to inflammation after implantation.
[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is: to provide a dental implant, including a titanium metal main body, the titanium metal main body is divided into an upper section, a middle section and a lower section, the surfaces of the upper section and the lower section have a threaded structure, and the middle section has a hollow structure; the surfaces of the threaded structure and the hollow structure are both coated with functional coatings, and the functional coatings are, from the inside to the outside, a strontium-doped nanohydroxyapatite layer and a PVA layer.
[0006] Based on the above technical solution, the present invention can also be improved as follows.
[0007] Furthermore, the length of the titanium metal body is 12 to 15 mm, and the lengths of the upper section, the middle section and the lower section are the same.
[0008] Furthermore, the thread structure has a nominal diameter of 4 mm, a depth of 2 mm, and a pitch of 2 mm.
[0009] Furthermore, the hollow shape of the hollow structure is a hexagon.
[0010] Furthermore, the porosity of the hollow structure is 60-70%, and the average pore size is 500 μm.
[0011] The present invention also discloses a method for preparing the dental implant, comprising the following steps:
[0012] S1: Preparation of titanium body by 3D printing;
[0013] S2: dissolving ammonium chloride in ethylene glycol solution to obtain a first electrolyte; then connecting the titanium metal body and the platinum electrode to the anode and cathode of the power supply respectively and immersing them in the first electrolyte, electrolyzing at a voltage of 30 to 40 V for 45 to 90 minutes, and then washing to obtain an intermediate product 1;
[0014] S3: A three-electrode electrolysis system was constructed with the intermediate product 1 as the working electrode, the platinum electrode as the counter electrode, and the saturated calomel electrode as the reference electrode. The second electrolyte was added and the reaction temperature was 2 mA / cm at 55-65 °C. 2 The second electrolyte is a mixed solution of Ca(NO3)2, NH4H2PO4, NaNO3 and SrCl2.
[0015] S4: PVA is dissolved in water to prepare a PVA solution with a concentration of 10%, and then the PVA solution is coated on the surface of the intermediate product 2 by spin coating.
[0016] Furthermore, the ethylene glycol solution is formed by mixing ethylene glycol and water in a volume ratio of 97:3; and the concentration of ammonium chloride in the first electrolyte is 0.5 wt %.
[0017] Furthermore, the pH value of the second electrolyte is 4.3; the concentrations of Ca(NO3)2, NH4H2PO4, NaNO3 and SrCl2 in the second electrolyte are 0.04-0.05 mol / L, 0.02-0.03 mol / L, 0.05-0.2 mol / L and 0.01-0.03 mol / L, respectively.
[0018] Furthermore, the drying temperature in S3 is 60°C.
[0019] Furthermore, the molecular weight of PVA is 85000-124000 g / mol; the spin coating process is: firstly spin coating at a speed of 400-500 rpm for 10-15 s, and then spin coating at a speed of 4000-5000 rpm for 55-65 s.
[0020] The beneficial effects of the present invention are:
[0021] 1. The upper and lower sections of the dental implant in the present invention are threaded structures, which can increase the contact area between the implant and the surrounding tissues, increase friction, and thus enhance the stability of the implant; at the same time, the threaded structure can also effectively prevent the implant from rotating and loosening. The threaded structure also gives the implant excellent self-tapping properties, has mechanical properties that match human cancellous bone, is conducive to the combination of the implant and the alveolar bone, and can significantly improve its stability and firmness compared to traditional implants.
[0022] 2. The middle section of the dental implant in the present invention is a hollow structure, which can reduce the elastic modulus of the implant, making it more compatible with the elastic modulus of the surrounding bone tissue. Moreover, the hollow structure provides a wide space for the growth of osteoblasts, which is conducive to the input of nutrients, the output of metabolites, and the growth of blood vessels, thereby promoting the bone integration process. In addition, the hollow shape of the hollow structure is a regular hexagon, which is different from the circular holes that have been used in the past. The regular hexagonal holes can not only reduce the use of materials, but also have a high degree of symmetry, which can make the force more balanced, which is conducive to improving the stability of the implant.
[0023] 3. The surface of the dental implant of the present invention is coated with a strontium-doped hydroxyapatite layer, which can not only effectively increase the cell adhesion of the implant, but also increase the contact area with human cell tissue, improve the cell adhesion, and further increase the biological activity of the implant. The strontium in the coating affects the differentiation of osteoblasts through the Wnt / β-catenin and TGF-β / smad signaling pathways; and the overall coating material has antibacterial properties, which can effectively solve the defect that other implants are prone to inflammation.
[0024] 4. The preparation method uses software modeling and 3D printing, which has low cost, easy control of pore size and porosity, and can ensure the excellent performance and precise parameter indicators of the implant.
[0025] 5. The dental implant of the present invention exhibits good stability in animal experiments, and its osteogenesis effect and biocompatibility are superior to those of common implants. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a schematic diagram of the structure of the dental implant in the present invention;
[0027] Figure 2 is a cross-sectional view of a dental implant;
[0028] Figure 3 Schematic diagram of an electrolytic preparation device for intermediate product 1;
[0029] Figure 4 HE staining results of rat femur;
[0030] Among them, 1. upper section; 2. middle section; 3. lower section. DETAILED DESCRIPTION
[0031] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.
[0032] Example 1
[0033] A dental implant, such as Figure 1 As shown, it includes a titanium metal body, the length of the titanium metal body is 12mm; the titanium metal body is divided into an upper section 1, a middle section 2 and a lower section 3, and the lengths of the upper section 1, the middle section 2 and the lower section 3 are the same; the surface of the upper section 1 and the lower section 2 has a thread structure, and the nominal diameter of the thread in the thread structure is 4mm, the depth is 2mm, and the spacing is 2mm; the middle section 2 has a hollow structure, the hollow shape of the hollow structure is hexagonal, the porosity of the hollow structure is 60%, and the average pore size is 500μm; as shown Figure 2 As shown, the surfaces of the threaded structure and the hollow structure are both covered with functional coatings, and the functional coatings are, from the inside to the outside, a strontium-doped nanohydroxyapatite layer and a PVA layer.
[0034] The dental implant in this embodiment is prepared by the following steps:
[0035] 1. Preparation of titanium metal body
[0036] (1) Design phase: First, mathematical drawing software was used to draw the main structure of the implant with threads on the surface, and the length of the entire implant structure was precisely controlled to be 12 mm. The main structure of the implant was divided into three sections of equal length: upper, middle, and lower. Each section was designed with threads to ensure the stability and functionality of the implant. The nominal diameter of the threads was 4 mm, the spacing was 2 mm, and the depth was 2 mm.
[0037] (2) Middle section processing: The surface threads at the middle section of the implant main structure obtained in step (1) are removed to retain the solid structure; then, a regular hexagonal pore hollow structure is added to the middle section of the implant main structure. This pore structure not only has good connectivity, but also provides sufficient space for cell growth and blood vessel ingrown; at this stage, the porosity (set to 60%) and the average pore diameter (set to 500 um) of the hollow structure are precisely controlled to ensure the effectiveness of the porous structure.
[0038] (3) Model processing: Perform Boolean operations and repair on the overall design model to prepare for printing; ensure the integrity and accuracy of the design model and provide a reliable basis for the subsequent 3D printing process.
[0039] (4) 3D printing: The design model obtained in step (3) was printed using the Hanbang HBD 150 metal 3D printer using the SLM process. The material used for printing was pure titanium powder. The printing parameters of the titanium metal body were laser power of 220W, scanning speed of 350mm / s, scanning spacing of 0.14mm, scanning layer thickness of 0.03mm, and each layer scanning path rotated 67°. 3D printing technology can accurately replicate every detail in the design model, including the threaded structure and porous structure, thereby ensuring the accuracy and functionality of the implant.
[0040] 2. Preparation of functional coating
[0041] (1) Preparation of the first electrolyte: ammonium fluoride is dissolved in an ethylene glycol solution to prepare a first electrolyte with an ammonium fluoride content of 0.5 wt%; the ethylene glycol solution used is a mixture of ethylene glycol and water in a volume ratio of 97:3. Ammonium fluoride plays a key role in the electrolysis process and helps to form a specific surface structure; 3 vol% H2O as a solvent provides the necessary conductivity and stability for the electrolyte; and ethylene glycol is crucial to the physical properties of the electrolyte and the temperature control during the electrolysis process.
[0042] (2) Preparation of intermediate product 1: Figure 3 As shown, the prepared titanium metal body and platinum electrode are connected to the anode and cathode of a power supply respectively. Such a setting ensures that during the electrolysis process, the titanium metal body can act as an anode to receive the action of current; then the titanium metal body and the platinum electrode are immersed in a first electrolyte, the power supply voltage is set to 35V, and electrolysis is performed at this voltage for 1 hour; after the electrolysis is completed, the titanium metal body is taken out and ultrasonically washed in deionized water for 5 minutes to remove the electrolyte residue attached to the surface of the titanium metal body and possible impurities; then, the titanium metal body is naturally air-dried at room temperature to obtain an intermediate product one.
[0043] (3) Preparation of the second electrolyte: First, dissolve Ca(NO3)2 and NH4H2PO4 in 50 ml of deionized water, respectively, and then pour the resulting solution into a 500 ml beaker, then add NaNO3 to the beaker, and select dilute HNO3 and ammonia water to adjust the pH value of the solution to 4.3; then add SrCl2 to the beaker, slowly stir until the materials are completely dissolved, and then adjust the volume to 500 ml to obtain the second electrolyte; the concentrations of Ca(NO3)2, NH4H2PO4, NaNO3 and SrCl2 in the obtained second electrolyte are 0.042 mol / L, 0.025 mol / L, 0.1 mol / L and 0.02 mol / L, respectively.
[0044] (4) Preparation of intermediate product 2: A three-electrode electrolysis system was constructed with intermediate product 1 as the working electrode, platinum electrode as the counter electrode, and saturated calomel electrode (SCE) as the reference electrode, with the spacing between the electrodes being 3 cm. 100 ml of the second electrolyte was added and the electrolyte was charged at 2 mA / cm2 in a water bath at 60 °C. 2 The electrolytic deposition was carried out at a current density of 60 minutes, and then the electrolyte was replaced and the deposition was continued under the same deposition conditions; the above operation was repeated 4 times to complete the deposition of the strontium-doped nanohydroxyapatite layer; the sample was then taken out, rinsed with deionized water, and placed in an oven to dry at a temperature of 60°C to obtain intermediate product 2.
[0045] (5) Preparation of the final product: polyvinyl alcohol (PVA) with a molecular weight of 100,000 g / mol was dissolved in distilled water at 90°C, and the mixture was stirred continuously for 4 h by magnetic stirring to ensure that the PVA was completely dissolved, thereby obtaining a 10% (m / v) PVA solution; the PVA solution was then gradually stirred and cooled to 50°C, 0.2 mL of the PVA solution was accurately transferred using a pipette, and the solution was evenly coated on the surface of the intermediate product 2 using a spin coating process. The spin coating process was specifically as follows: first, the sample was spin-coated at a speed of 400 rpm for 10 seconds to allow the PVA solution to be initially distributed on the sample surface; then, the speed was increased to 4000 rpm, and the spin coating was continued for 60 seconds to ensure that the PVA solution could evenly and tightly cover the surface of the nanostructured sample.
[0046] Example 2
[0047] A dental implant, such as Figure 1 As shown, it includes a titanium metal body, the length of the titanium metal body is 15mm; the titanium metal body is divided into an upper section 1, a middle section 2 and a lower section 3, and the lengths of the upper section 1, the middle section 2 and the lower section 3 are the same; the surface of the upper section 1 and the lower section 2 has a thread structure, and the nominal diameter of the thread in the thread structure is 4mm, the depth is 2mm, and the spacing is 2mm; the middle section 2 has a hollow structure, the hollow shape of the hollow structure is hexagonal, the porosity of the hollow structure is 65%, and the average pore size is 500μm; as shown Figure 2As shown, the surfaces of the threaded structure and the hollow structure are both covered with functional coatings, and the functional coatings are, from the inside to the outside, a strontium-doped nanohydroxyapatite layer and a PVA layer.
[0048] The dental implant in this embodiment is prepared by the following steps:
[0049] 1. Preparation of titanium metal body
[0050] (1) Design phase: First, mathematical drawing software was used to draw the main structure of the implant with threads on the surface, and the length of the entire implant structure was precisely controlled to be 15 mm. The main structure of the implant was divided into three sections of equal length: upper, middle, and lower. Each section was designed with threads to ensure the stability and functionality of the implant. The nominal diameter of the threads was 4 mm, the spacing was 2 mm, and the depth was 2 mm.
[0051] (2) Middle section processing: The surface threads at the middle section of the implant main structure obtained in step (1) are removed to retain the solid structure; then, a regular hexagonal pore hollow structure is added to the middle section of the implant main structure. This pore structure not only has good connectivity, but also provides sufficient space for cell growth and blood vessel ingrown; at this stage, the porosity (set to 65%) and the average pore diameter (set to 500 um) of the hollow structure are precisely controlled to ensure the effectiveness of the porous structure.
[0052] (3) Model processing: Perform Boolean operations and repair on the overall design model to prepare for printing; ensure the integrity and accuracy of the design model and provide a reliable basis for the subsequent 3D printing process.
[0053] (4) 3D printing: The design model obtained in step (3) was printed using the Hanbang HBD 150 metal 3D printer using the SLM process. The material used for printing was pure titanium powder. The printing parameters of the titanium metal body were laser power of 220W, scanning speed of 350mm / s, scanning spacing of 0.14mm, scanning layer thickness of 0.03mm, and each layer scanning path rotated 67°. 3D printing technology can accurately replicate every detail in the design model, including the threaded structure and porous structure, thereby ensuring the accuracy and functionality of the implant.
[0054] 2. Preparation of functional coating
[0055] (1) Preparation of the first electrolyte: ammonium fluoride is dissolved in an ethylene glycol solution to prepare a first electrolyte with an ammonium fluoride content of 0.5 wt%; the ethylene glycol solution used is a mixture of ethylene glycol and water in a volume ratio of 97:3. Ammonium fluoride plays a key role in the electrolysis process and helps to form a specific surface structure; 3 vol% H2O as a solvent provides the necessary conductivity and stability for the electrolyte; and ethylene glycol is crucial to the physical properties of the electrolyte and the temperature control during the electrolysis process.
[0056] (2) Preparation of intermediate product 1: Figure 3 As shown, the prepared titanium metal body and platinum electrode are connected to the anode and cathode of the power supply respectively. Such a setting ensures that during the electrolysis process, the titanium metal body can act as an anode to receive the action of current; then the titanium metal body and the platinum electrode are immersed in the first electrolyte, the power supply voltage is set to 30V, and electrolysis is performed at this voltage for 90 minutes; after the electrolysis is completed, the titanium metal body is taken out and ultrasonically washed in deionized water for 5 minutes to remove the electrolyte residue attached to the surface of the titanium metal body and possible impurities; then, the titanium metal body is naturally air-dried at room temperature to obtain an intermediate product one.
[0057] (3) Preparation of the second electrolyte: First, dissolve Ca(NO3)2 and NH4H2PO4 in 50 ml of deionized water, respectively, and then pour the resulting solution into a 1000 ml beaker, then add NaNO3 to the beaker, and select dilute HNO3 and ammonia water to adjust the pH value of the solution to 4.3; then add SrCl2 to the beaker, slowly stir until the materials are completely dissolved, and then adjust the volume to 600 ml to obtain the second electrolyte; the concentrations of Ca(NO3)2, NH4H2PO4, NaNO3 and SrCl2 in the obtained second electrolyte are 0.04 mol / L, 0.03 mol / L, 0.05 mol / L and 0.03 mol / L, respectively.
[0058] (4) Preparation of intermediate product 2: A three-electrode electrolysis system was constructed with intermediate product 1 as the working electrode, platinum electrode as the counter electrode, and saturated calomel electrode (SCE) as the reference electrode, with the spacing between the electrodes being 3 cm. 100 ml of the second electrolyte was added and the electrolyte was charged at 2 mA / cm2 in a water bath at 55 °C. 2 The electrolytic deposition was carried out at a current density of 70 minutes, and then the electrolyte was replaced and the deposition was continued under the same deposition conditions; the above operation was repeated 5 times to complete the deposition of the strontium-doped nanohydroxyapatite layer; the sample was then taken out, rinsed with deionized water, and placed in an oven to dry at 60°C to obtain intermediate product 2.
[0059] (5) Preparation of the final product: polyvinyl alcohol (PVA) with a molecular weight of 85,000 g / mol was dissolved in distilled water at 90°C, and the mixture was stirred continuously for 4 h by magnetic stirring to ensure that the PVA was completely dissolved, thereby obtaining a 10% (m / v) PVA solution; the PVA solution was then gradually stirred and cooled to 50°C, 0.2 mL of the PVA solution was accurately transferred using a pipette, and the solution was evenly coated on the surface of the intermediate product 2 using a spin coating process. The spin coating process was specifically as follows: first, the sample was spin-coated at a speed of 350 rpm for 12 seconds to allow the PVA solution to be initially distributed on the sample surface; then, the speed was increased to 4,500 rpm, and the spin coating was continued for 55 seconds to ensure that the PVA solution could evenly and tightly cover the surface of the nanostructured sample.
[0060] Example 3
[0061] A dental implant, such as Figure 1 As shown, it includes a titanium metal body, the length of the titanium metal body is 12mm; the titanium metal body is divided into an upper section 1, a middle section 2 and a lower section 3, and the lengths of the upper section 1, the middle section 2 and the lower section 3 are the same; the surface of the upper section 1 and the lower section 2 has a thread structure, and the nominal diameter of the thread in the thread structure is 4mm, the depth is 2mm, and the spacing is 2mm; the middle section 2 has a hollow structure, the hollow shape of the hollow structure is hexagonal, the porosity of the hollow structure is 70%, and the average pore size is 500μm; as shown Figure 2 As shown, the surfaces of the threaded structure and the hollow structure are both covered with functional coatings, and the functional coatings are, from the inside to the outside, a strontium-doped nanohydroxyapatite layer and a PVA layer.
[0062] The dental implant in this embodiment is prepared by the following steps:
[0063] 1. Preparation of titanium metal body
[0064] (1) Design phase: First, mathematical drawing software was used to draw the main structure of the implant with threads on the surface, and the length of the entire implant structure was precisely controlled to be 12 mm. The main structure of the implant was divided into three sections of equal length: upper, middle, and lower. Each section was designed with threads to ensure the stability and functionality of the implant. The nominal diameter of the threads was 4 mm, the spacing was 2 mm, and the depth was 2 mm.
[0065] (2) Middle section processing: The surface threads at the middle section of the implant main structure obtained in step (1) are removed to retain the solid structure; then, a regular hexagonal pore hollow structure is added to the middle section of the implant main structure. This pore structure not only has good connectivity, but also provides sufficient space for cell growth and blood vessel ingrown; at this stage, the porosity (set to 70%) and the average pore diameter (set to 500 um) of the hollow structure are precisely controlled to ensure the effectiveness of the porous structure.
[0066] (3) Model processing: Perform Boolean operations and repair on the overall design model to prepare for printing; ensure the integrity and accuracy of the design model and provide a reliable basis for the subsequent 3D printing process.
[0067] (4) 3D printing: The design model obtained in step (3) was printed using the Hanbang HBD 150 metal 3D printer using the SLM process. The material used for printing was pure titanium powder. The printing parameters of the titanium metal body were laser power of 220W, scanning speed of 350mm / s, scanning spacing of 0.14mm, scanning layer thickness of 0.03mm, and each layer scanning path rotated 67°. 3D printing technology can accurately replicate every detail in the design model, including the threaded structure and porous structure, thereby ensuring the accuracy and functionality of the implant.
[0068] 2. Preparation of functional coating
[0069] (1) Preparation of the first electrolyte: ammonium fluoride is dissolved in an ethylene glycol solution to prepare a first electrolyte with an ammonium fluoride content of 0.5 wt%; the ethylene glycol solution used is a mixture of ethylene glycol and water in a volume ratio of 97:3. Ammonium fluoride plays a key role in the electrolysis process and helps to form a specific surface structure; 3 vol% H2O as a solvent provides the necessary conductivity and stability for the electrolyte; and ethylene glycol is crucial to the physical properties of the electrolyte and the temperature control during the electrolysis process.
[0070] (2) Preparation of intermediate product 1: Figure 3 As shown, the prepared titanium metal body and platinum electrode are connected to the anode and cathode of a power supply respectively. Such a setting ensures that during the electrolysis process, the titanium metal body can act as an anode to receive the action of current; then the titanium metal body and the platinum electrode are immersed in a first electrolyte, the power supply voltage is set to 40V, and electrolysis is performed at this voltage for 45 minutes; after the electrolysis is completed, the titanium metal body is taken out and ultrasonically washed in deionized water for 5 minutes to remove the electrolyte residue attached to the surface of the titanium metal body and possible impurities; then, the titanium metal body is naturally air-dried at room temperature to obtain an intermediate product one.
[0071] (3) Preparation of the second electrolyte: First, dissolve Ca(NO3)2 and NH4H2PO4 in 50 ml of deionized water, respectively, and then pour the resulting solution into a 1000 ml beaker, then add NaNO3 to the beaker, and select dilute HNO3 and ammonia water to adjust the pH value of the solution to 4.3; then add SrCl2 to the beaker, slowly stir until the materials are completely dissolved, and then adjust the volume to 600 ml to obtain the second electrolyte; the concentrations of Ca(NO3)2, NH4H2PO4, NaNO3 and SrCl2 in the obtained second electrolyte are 0.05 mol / L, 0.02 mol / L, 0.2 mol / L and 0.01 mol / L, respectively.
[0072] (4) Preparation of intermediate product 2: A three-electrode electrolysis system was constructed with intermediate product 1 as the working electrode, platinum electrode as the counter electrode, and saturated calomel electrode (SCE) as the reference electrode, with the spacing between the electrodes being 3 cm. 100 ml of the second electrolyte was added and the electrolyte was charged at 2 mA / cm2 in a water bath at 65 °C. 2 The electrolytic deposition was carried out at a current density of 45 minutes, and then the electrolyte was replaced and the deposition was continued under the same deposition conditions; the above operation was repeated 6 times to complete the deposition of the strontium-doped nanohydroxyapatite layer; the sample was then taken out, rinsed with deionized water, and placed in an oven to dry at 60°C to obtain intermediate product 2.
[0073] (5) Preparation of the final product: polyvinyl alcohol (PVA) with a molecular weight of 124,000 g / mol was dissolved in distilled water at 90°C, and the mixture was stirred continuously for 4 h by magnetic stirring to ensure that the PVA was completely dissolved, thereby obtaining a 10% (m / v) PVA solution; the PVA solution was then gradually stirred and cooled to 50°C, 0.2 mL of the PVA solution was accurately transferred using a pipette, and the solution was evenly coated on the surface of the intermediate product 2 using a spin coating process. The spin coating process was specifically as follows: first, the sample was spin-coated at a speed of 450 rpm for 8 seconds to allow the PVA solution to be initially distributed on the sample surface; then, the speed was increased to 3500 rpm, and the spin coating was continued for 65 seconds to ensure that the PVA solution could evenly and tightly cover the surface of the nanostructured sample.
[0074] Experimental example
[0075] The dental implants prepared in the three embodiments of the present invention have similar performances. Taking Embodiment 1 as an example, the performance of the related products is described.
[0076] The bone defect experiment in rats was used to verify the osteogenic performance of the implant of the present invention. All surgical and experimental procedures were approved by the ethical principles of animal research adopted by the Animal Use Ethics Committee of Chengdu University.
[0077] Ten 8-week-old rats were selected, 8 of which were in the experimental group (new implant material group) and the remaining 2 were used as blank control group.
[0078] First, prepare the mouse plate, surgical instruments, alcohol, iodine, cotton swabs, etc. The implant is selected as a cylindrical shape with a height of 3mm. The high-temperature sterilization box is set at 50℃ for 12 hours to sterilize the implant material. 10% chloral hydrate (4ml / kg) is used for intraperitoneal injection anesthesia, and drilling is performed near the trochanter of the femoral head on both sides of the rat, with a diameter of 3mm. The periosteum needs to be fully stripped before drilling. After connecting the 3mm hollow drill bit to the electric drill, drill at a low speed (≤1500rpm). During the drilling process, the assistant uses saline drip (1 drop / 2s) to cool down. The action is gentle during drilling to avoid drilling through the bone tissue completely. When drilling is close to penetration, use a stripper to perform blunt separation along the periphery of the circular defect to avoid damage to the blood vessels and tissues under the femur. Take out the prepared implant material, bury the implant accurately in the drilling site, rinse the surgical field with saline, and after probing for no active bleeding, use No. 0 line to close the subcutaneous muscle and skin incision layer by layer. After the operation, the rats were placed in a 30℃ constant temperature table in a lateral position for anesthesia recovery. After they were fully awake, they were returned to the breeding cage for continued feeding and penicillin was drip-fed for three consecutive days to prevent infection.
[0079] The samples were collected at the eighth and tenth weeks after surgery. Rats were killed by cervical dislocation, and the femurs of the rats were dissected and washed with saline. After fixation for 48 hours, the samples were demineralized for 45 days, and the solution was changed three times a week. After demineralization, the samples were washed in water for 1 hour, dehydrated with anhydrous ethanol, and embedded with xylene and paraffin. The 4.0 μm sections were mounted on slides and stained with hematoxylin and eosin (HE) for histomorphological evaluation. Ten images of each bone sample were analyzed using Image J software. The experimental data are expressed as mean ± standard deviation. The experimental results were repeated at least three times in parallel. The differences between the two groups were evaluated by one-way analysis of variance or post hoc t-test Bonferroni test. Probability values such as *P<0.05, **P<0.01, ***P<0.001 were considered statistically significant.
[0080] The results of histological HE staining are as follows Figure 4 As shown, it can be seen from the figure that in the experimental group (the group implanted with the implant of the present invention), the newly formed bone dark-stained tissue is significantly more than that in the control group, demonstrating that the implant has excellent bone-forming ability.
[0081] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.
Claims
1. A dental implant, characterized in that: It comprises a titanium metal body, which is divided into an upper section, a middle section and a lower section. The surfaces of the upper section and the lower section have threaded structures, and the middle section has a hollow structure. The surfaces of the threaded structure and the hollow structure are both covered with functional coatings, and the functional coatings are sequentially composed of a strontium-doped nanohydroxyapatite layer and a PVA layer from the inside to the outside.
2. The dental implant according to claim 1, characterized in that: The length of the titanium metal body is 12-15 mm, and the lengths of the upper section, the middle section and the lower section are the same.
3. The dental implant according to claim 2, characterized in that: The thread structure has a nominal diameter of 4 mm, a depth of 2 mm, and a pitch of 2 mm.
4. The dental implant according to claim 1, characterized in that: The hollow shape of the hollow structure is hexagonal.
5. The dental implant according to claim 4, characterized in that: The porosity of the hollow structure is 60-70%, and the average pore diameter is 500 μm.
6. The method for preparing a dental implant according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: Preparation of titanium body by 3D printing; S2: dissolving ammonium fluoride in ethylene glycol solution to obtain a first electrolyte; then connecting the titanium metal body and the platinum electrode to the anode and cathode of the power supply respectively and immersing them in the first electrolyte, electrolyzing at a voltage of 30 to 40 V for 45 to 90 minutes, and then washing to obtain an intermediate product 1; S3: A three-electrode electrolysis system was constructed with the intermediate product 1 as the working electrode, the platinum electrode as the counter electrode, and the saturated calomel electrode as the reference electrode. The second electrolyte was added and the reaction temperature was 2 mA / cm at 55-65 °C. 2 The second electrolyte is a mixed solution of Ca(NO3)2, NH4H2PO4, NaNO3 and SrCl2; and the second electrolyte is a mixed solution of Ca(NO3)2, NH4H2PO4, NaNO3 and SrCl2. S4: PVA is dissolved in water to prepare a PVA solution with a concentration of 10%, and then the PVA solution is coated on the surface of the intermediate product 2 by spin coating.
7. The preparation method according to claim 6, characterized in that: The ethylene glycol solution is formed by mixing ethylene glycol and water in a volume ratio of 97:3; the concentration of ammonium fluoride in the first electrolyte is 0.5wt%.
8. The preparation method according to claim 6, characterized in that: The pH value of the second electrolyte is 4.3; the concentrations of Ca(NO3)2, NH4H2PO4, NaNO3 and SrCl2 in the second electrolyte are 0.04-0.05 mol / L, 0.02-0.03 mol / L, 0.05-0.2 mol / L and 0.01-0.03 mol / L, respectively.
9. The preparation method according to claim 6, characterized in that: The drying temperature in S3 is 60°C.
10. The preparation method according to claim 6, characterized in that: The molecular weight of the PVA is 85000-124000 g / mol; the spin coating process is: firstly spin coating at a speed of 350-450 rpm for 8-12 s, and then spin coating at a speed of 3500-4500 rpm for 55-65 s.