A silicon-carbon negative electrode material connected by VGCF and a preparation method thereof

The preparation method of silicon carbon negative electrode material connected by VGCF is used to form a hard carbon cladding layer by using solid-phase gas-phase hybrid coating technology, which solves the problem of volume effect and poor conductivity of the negative electrode material of lithium-ion batteries, and significantly improves the service life and capacity of the battery .

CN118738358BActive Publication Date: 2024-11-29GANZHOU RUIFUTE TECHNOLOGY CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411231818.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The graphite capacity of the negative electrode material of existing lithium-ion batteries is close to the theoretical limit. The silicon-carbon material collapses the electrode structure and peels off due to volume effects and poor conductivity, resulting in rapid attenuation of the capacity, limiting the service life of the lithium-ion battery.

Method used

The preparation method of silicon carbon anode material connected by VGCF is used to prepare sub-silicon oxide containing transition metals using micron-scale silicon powder, micron-scale silica powder and nano-scale transition metal powder. Combined with micron-scale graphite, it is coated with solid-phase gas phase mixed coating using solid-phase gas phase. The technology forms a hard carbon cladding layer, reducing volume effects and improving the cyclic stability of the electrodes.

Benefits of technology

It significantly reduces the volume effect of the negative electrode, increases the service life of the lithium-ion battery, and improves the battery capacity and first-time Coulomb efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738358B_ABST
    Figure CN118738358B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of lithium battery electrode materials, and specifically relates to a silicon-carbon negative electrode material connected by VGCF and a preparation method thereof. The preparation method comprises mixing micron-sized silicon powder, micron-sized silicon dioxide powder, and nano-sized transition metal powder to prepare micron-sized silicon oxide powder containing transition metals, then mixing the powder with micron-sized graphite and a granulating agent to obtain a mixture, and finally granulating the mixture by passing a protective gas and a carbon source gas at a high temperature to obtain a silicon-carbon negative electrode material connected by VGCF. The present invention combines solid-phase and gas-phase coating, and bonds micron-sized silicon oxide to graphite through VGCF to form a complete hard carbon coating layer on its surface. The obtained silicon-carbon negative electrode material can significantly reduce the volume effect of the negative electrode, increase the number of cycles, and improve the service life of the lithium-ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium battery electrode materials, and in particular relates to a silicon-carbon negative electrode material connected via VGCF and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have the advantages of high capacity, no memory effect, fast reversible charge and discharge, and high Coulomb efficiency. They are now widely used in 3C products, electric vehicles, and energy storage technologies. At present, graphite, the negative electrode material for commercial lithium-ion batteries, is close to the theoretical capacity of 372mAh / g, and it is difficult to improve it. The theoretical capacity of silicon oxide is 2600mAh / g, which is much higher than graphite. At the same time, compared with graphite negative electrode material, silicon has a higher lithium deintercalation potential, which can effectively avoid the precipitation of lithium during high-rate charge and discharge, and improve battery safety performance. At present, there is no large-scale production of high-capacity silicon-carbon negative electrode materials on the market, so the development of such high-energy-density silicon-carbon negative electrode materials has broad prospects and plays a great role in improving market competitiveness. In addition to its greater energy density advantage, silicon oxide has a volume effect of about 150%, which is significantly better than the volume effect (up to 300%) produced by silicon in the process of alloying with lithium. However, it is still much larger than the 15% expansion rate of graphite, which makes the electrode structure more prone to collapse and the active material to peel off, causing the electrode material to lose electrical contact and resulting in rapid capacity decay. In addition, silicon oxide has poor conductivity and low initial efficiency, which seriously hinders the practical application of silicon oxide as a negative electrode material for lithium-ion batteries.

[0003] Scientific research shows that vapor-grown carbon fiber (VGCF) has a low resistivity (0.8×10 -4 Ω·cm-1.5×10 -4 Ω·cm), strong tensile strength (2000MPa-5000MPa), and easy to form a good conductive network in the electrode. As mentioned above, the current silicon-carbon negative electrode material still has shortcomings in terms of rapidity and simplicity of preparation. At the same time, in practical applications, due to the large volume effect of the silicon-based negative electrode, the active material peels off and causes the capacity to decay rapidly. Therefore, it is necessary to develop a negative electrode material that can combine VGCF with silicon oxide and graphite to further reduce the negative electrode volume effect and increase the service life of lithium-ion batteries. Summary of the invention

[0004] In view of the above defects or improvement needs of the prior art, the present invention provides a silicon-carbon negative electrode material connected by VGCF and a preparation method thereof. The silicon-carbon negative electrode material can significantly reduce the volume effect of the negative electrode and increase the service life of the lithium-ion battery.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The first object of the present invention is to provide a method for preparing a silicon-carbon negative electrode material connected by VGCF, comprising the following steps:

[0007] S1, mixing micron-sized silicon powder, micron-sized silicon dioxide powder, and nano-sized transition metal powder in a vacuum, evaporating the mixture, and then grinding the mixture using a jet mill to obtain micron-sized silicon oxide powder containing transition metals;

[0008] S2, mixing the micron-sized silicon oxide powder containing transition metal, micron-sized graphite and granulating agent obtained in S1 through a mixer to obtain a mixture;

[0009] S3. The mixture obtained in S2 is introduced with protective gas and carbon source gas at high temperature, and granulated on a drum furnace to obtain a silicon-carbon negative electrode material connected with VGCF.

[0010] The present invention prepares micron-sized silicon oxide containing transition metal by mixing micron-sized silicon powder, micron-sized silicon dioxide powder and nano-sized transition metal powder, and then uses solid-phase gas-phase mixed coating to prepare a silicon-carbon negative electrode material in which graphite and silicon oxide are connected by VGCF in one step, and forms a complete hard carbon coating layer on the surface of the negative electrode. The obtained silicon-carbon negative electrode material significantly reduces the volume effect of the negative electrode and increases the service life of the lithium-ion battery.

[0011] Furthermore, in the above technical solution S1, the nanoscale transition metal powder is one or more of iron, cobalt, and nickel; the micron-sized silicon powder, micron-sized silicon dioxide powder, and nanoscale transition metal powder are mixed in a molar ratio of 1:1:0.00001-0.0001; preferably, the micron-sized silicon powder, micron-sized silicon dioxide powder, and nanoscale transition metal powder are mixed in a molar ratio of 1:1:0.00005.

[0012] Furthermore, in the above technical solution S1, the D50 of the micron-sized transition metal-containing silicon dioxide powder is between 2 μm and 6 μm, and the specific surface area is between 1 m 2 / g-5m 2 / g, the reversible capacity of the button battery test is between 1400mAh / g-1800mAh / g, and the first coulombic efficiency is 60%-70%; the D50 of the micron-sized transition metal-containing silicon oxide powder is preferably between 3μm-4μm, and the specific surface area is 3m 2 / g-4m 2 / g, the button battery tested reversible capacity is between 1500mAh / g-1600mAh / g, and the first coulombic efficiency is 70%.

[0013] Furthermore, in the above technical solution S2, the micron-sized graphite is one or both of artificial graphite and natural graphite, and its D50 is between 12 μm and 16 μm, and its specific surface area is 1 m 2 / g-3m 2 / g, the reversible capacity of the button battery test is between 350mAh / g-365mAh / g, and the first coulomb efficiency is 95%; the preferred micron-sized graphite is artificial graphite, and the D50 is between 14μm-15μm, and the specific surface area is 1m 2 / g-2m 2 / g, the button battery tested reversible capacity is between 355mAh / g-358mAh / g, and the first coulombic efficiency is 95%.

[0014] Furthermore, in the above technical solution S2, the granulating agent is one or more of phenolic resin, asphalt, polyacrylonitrile, polyvinyl alcohol, polyimide, and polyvinylidene fluoride; preferably, the mass ratio of phenolic resin to asphalt is 80-95:5-20.

[0015] Furthermore, in the above technical solution S2, the mixing process of the mixer is: stirring at 600r / min-1000r / min for 5min, stirring at 1000r / min-1800r / min for 10min, and stirring at 2000r / min-3000r / min for 10min; the preferred mixing process is stirring at 800r / min for 5min, stirring at 1500r / min for 10min, and stirring at 2500r / min for 10min.

[0016] Furthermore, in the above technical solution S2, the mass ratio of the micron-sized transition metal-containing silicon dioxide powder, micron-sized graphite and granulating agent is 3-10:90-95:1-10; preferably, the mass ratio of the micron-sized transition metal-containing silicon dioxide powder, micron-sized graphite and granulating agent is 7:93:5.

[0017] Furthermore, in the above technical solution S3, the carbon source gas is one or more of ethylene, propylene, acetylene, ethane, and propane.

[0018] Furthermore, in the above technical solution S3, the drum furnace granulation process is: angular velocity 0.3r / min-1r / min, heating 700℃-1200℃, constant temperature 4h-10h, preferably angular velocity 0.4r / min-0.5r / min, heating 800℃-1000℃, constant temperature 6h-8h; the volume ratio of the carbon source gas and the protective gas is 10-30:70-90; the protective gas is one or more of helium, argon, and neon, and the volume ratio of ethylene and argon is preferably 20:80.

[0019] The second object of the present invention is to provide a silicon-carbon negative electrode material connected by VGCF prepared by the above preparation method, wherein the D50 of the silicon-carbon negative electrode material is between 13 μm and 18 μm, and the specific surface area is between 1 m 2 / g-2m 2 / g, the reversible capacity of the button battery test is between 380mAh / g-500mAh / g, and the first coulomb efficiency is 90%-95%; the D50 of the preferred silicon-carbon negative electrode material is between 15μm-16μm, and the specific surface area is 1m 2 / g-2m 2 / g, the button battery tested reversible capacity is between 400mAh / g-450mAh / g, and the first coulombic efficiency is 93%-95%.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention uses micron-sized silicon powder and micron-sized silicon dioxide as raw materials, and dopes the obtained micron-sized silicon dioxide with transition metals as catalysts, so as to prepare for improving the subsequent reaction rate; then the solid carbon is pre-mixed with the above raw materials, and then the carbon source gas and the protective gas are introduced, the solid phase and the gas phase are combined for mixed coating, and conditions are provided for the growth of gas-phase VCGF in an environment with sufficient carbon source, the micron-sized silicon oxide is bonded to the graphite, and a complete hard carbon coating layer is formed on its surface, which can effectively inhibit volume expansion.

[0022] 2. The silicon-carbon negative electrode material prepared by the present invention not only has high capacity and initial efficiency, but also significantly reduces the volume effect of the negative electrode, increases the number of cycles, and improves the service life of the lithium-ion battery.

[0023] 3. The raw materials used in the preparation method of the present invention are abundant and extensive, the sources of micron-sized graphite and carbon sources are sufficient and low-priced, and the obtained silicon-carbon negative electrode material has excellent performance and good market competitiveness. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 Schematic diagram of the structure of the silicon-carbon negative electrode material prepared in an embodiment of the present invention.

[0026] Figure 2 This is the charge and discharge curve of the silicon-carbon material half-cell test in Example 1 of the present invention.

[0027] Figure 3 It is a comparison chart of the cycle test data of Examples 1 to 3 of the present invention and Comparative Examples 1 to 2.

[0028] Figure 4 This is an electron microscope image of the silicon-carbon material of Example 1 of the present invention, wherein a is a secondary electron image (20500×) and b is a backscattered electron image (20500×).

[0029] Figure 5 These are electron microscope images of the silicon-carbon material of Comparative Example 1 of the present invention, where a (5000×) and b (20000×). DETAILED DESCRIPTION

[0030] The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials involved in the following examples are common commercial products and can be purchased from the market unless otherwise specified.

[0031] The above-mentioned technical features of the present invention and the technical features specifically described below (such as implementation cases) can be combined with each other to form a new or preferred technical solution.

[0032] The raw materials involved in the embodiments of the present invention are either existing commercially available products or can be prepared according to existing methods, and the testing methods are industry methods.

[0033] Example 1

[0034] A method for preparing a silicon-carbon negative electrode material connected by VGCF comprises the following steps:

[0035] S1. Mix micron-sized silicon powder, micron-sized silicon dioxide powder and nano-sized transition metal powder in a molar ratio of 1:1:0.00005, evaporate them in a vacuum to prepare silicon oxide containing transition metals, and then grind the prepared silicon oxide containing transition metals using a jet mill to obtain a silicon oxide with a D50 between 3 μm and 4 μm and a specific surface area of ​​3 m 2 / g-4m 2 / g, the reversible capacity of button cell test is between 1500mAh / g-1600mAh / g, and the first coulombic efficiency is 70% for micron-sized silicon oxide powder containing transition metals;

[0036] S2, the micron-sized silicon oxide powder containing transition metals prepared in S1, micron-sized artificial graphite (D50 between 14μm-15μm, specific surface area between 1m 2 / g-2m 2 / g, the button battery test reversible capacity is between 355mAh / g-358mAh / g, the first coulomb efficiency is 95%) and granulating agent (phenolic resin: asphalt mass ratio is 90:10) are put into a mixer according to a mass ratio of 7:93:5, and the mixing process is 800r / min for 5min, 1500r / min for 10min, and 2500r / min for 10min to obtain a mixture;

[0037] S3, put the mixture prepared in S2 into a drum furnace, raise the temperature to 800℃-1000℃ at an angular speed between 0.4r / min-0.5r / min, keep the temperature constant for 6h-8h, introduce ethylene:argon gas with a volume ratio of 20:80 to carry out granulation process, and obtain VGCF connected silicon-carbon negative electrode material, wherein D50 is between 15μm-16μm and the specific surface area is 1m 2 / g-2m 2 / g, the button battery tested reversible capacity is between 436mAh / g-442mAh / g, and the first coulombic efficiency is between 93%-95%.

[0038] The schematic diagram of the structure of the silicon-carbon negative electrode material prepared in the embodiment of the present invention is as follows Figure 1 shown.

[0039] Example 2

[0040] A method for preparing a silicon-carbon negative electrode material connected by VGCF comprises the following steps:

[0041] S1. Mix micron-sized silicon powder, micron-sized silicon dioxide powder and nano-sized transition metal powder in a molar ratio of 1:1:0.00001, evaporate them in a vacuum to prepare silicon oxide containing transition metals, and then grind the prepared silicon oxide containing transition metals using a jet mill to obtain a silicon oxide with a D50 between 5 μm and 6 μm and a specific surface area of ​​1 m 2 / g-3m 2 / g, the reversible capacity of button cell test is between 1600mAh / g-1700mAh / g, and the first coulombic efficiency is 70% for micron-sized silicon oxide powder containing transition metals;

[0042] S2, the micron-sized transition metal-containing silicon oxide powder and micron-sized artificial graphite (D50 between 15μm-16μm, specific surface area between 1m 2 / g-2m 2 / g, the button battery test reversible capacity is between 358mAh / g-365mAh / g, the first coulomb efficiency is 95%) and granulating agent (phenolic resin: asphalt mass ratio is 90:10) are put into a mixer according to a mass ratio of 7:93:10, and the mixing process is 600r / min for 5min, 1800r / min for 10min, and 3000r / min for 10min to obtain a mixture;

[0043] S3, put the mixture prepared in S2 into a drum furnace, raise the temperature to 800℃-1000℃ at an angular speed between 0.4r / min-0.5r / min, keep the temperature constant for 6h-8h, introduce ethylene:argon gas with a volume ratio of 30:70 to carry out granulation process, and obtain VGCF connected silicon-carbon negative electrode material, wherein D50 is between 16μm-18μm, and the specific surface area is 1m 2 / g-2m 2 / g, the button battery tested reversible capacity is between 442mAh / g-449mAh / g, and the first coulombic efficiency is between 94%-95%.

[0044] Example 3

[0045] A method for preparing a silicon-carbon negative electrode material connected by VGCF comprises the following steps:

[0046] S1. Mix micron-sized silicon powder, micron-sized silicon dioxide powder and nano-sized transition metal powder in a molar ratio of 1:1:0.0001, evaporate them in a vacuum to prepare silicon oxide containing transition metals, and then grind the prepared silicon oxide containing transition metals using a jet mill to obtain a silicon oxide with a D50 between 2 μm and 3 μm and a specific surface area of ​​4 m 2 / g-5m 2 / g, the reversible capacity of button cell test is between 1600mAh / g-1700mAh / g, and the first coulombic efficiency is 70% for micron-sized silicon oxide powder containing transition metals;

[0047] S2, the micron-sized transition metal-containing silicon oxide powder and micron-sized artificial graphite (D50 between 12μm-14μm, specific surface area between 1m 2 / g-3m 2 / g, the button battery test reversible capacity is between 350mAh / g-355mAh / g, the first coulomb efficiency is 95%) and granulating agent (phenolic resin: asphalt mass ratio is 90:10) are put into a mixer according to a mass ratio of 7:93:5, and the mixing process is 1000r / min for 5min, 1500r / min for 10min, and 2000r / min for 10min to obtain a mixture;

[0048] S3, put the mixture prepared in S2 into a drum furnace, raise the temperature to 800℃-1000℃ at an angular speed between 0.4r / min-0.5r / min, keep the temperature constant for 6h-8h, introduce ethylene:argon gas with a volume ratio of 20:80 to carry out granulation process, and obtain VGCF connected silicon-carbon negative electrode material, wherein D50 is between 15μm-16μm and the specific surface area is 1m 2 / g-2m 2 / g, the button battery tested reversible capacity is between 430mAh / g-436mAh / g, and the first coulombic efficiency is between 93%-94%.

[0049] Comparative Example 1

[0050] A method for preparing a silicon-carbon negative electrode material comprises the following steps:

[0051] S1. Mix micron-sized silicon powder, micron-sized silicon dioxide powder and nano-sized transition metal powder in a molar ratio of 1:1:0.00005, evaporate them in a vacuum to prepare silicon oxide containing transition metals, and then grind the prepared silicon oxide containing transition metals using a jet mill to obtain a silicon oxide with a D50 between 3 μm and 4 μm and a specific surface area of ​​3 m 2 / g-4m 2 / g, the reversible capacity of button cell test is between 1500mAh / g-1600mAh / g, and the first coulombic efficiency is 70% for micron-sized silicon oxide powder containing transition metals;

[0052] S2, the micron-sized silicon oxide powder containing transition metals prepared in S1, micron-sized artificial graphite (D50 between 14μm-15μm, specific surface area between 1m 2 / g-2m 2 / g, the button battery test reversible capacity is between 355mAh / g-358mAh / g, and the first coulomb efficiency is 95%), put into the mixer according to the mass ratio of 7:93, and stir at 800r / min for 5min, 1500r / min for 10min, and 2500r / min for 10min to obtain a mixture;

[0053] S3, put the mixture prepared in S2 into a drum furnace, raise the temperature to 800℃-1000℃ at an angular speed between 0.4r / min-0.5r / min, keep the temperature constant for 6h-8h, introduce ethylene:argon gas with a volume ratio of 20:80 to carry out granulation process, and obtain a carbon-coated silicon-carbon negative electrode material, wherein D50 is between 14μm-16μm and the specific surface area is 1m 2 / g-2m 2 / g, the button battery tested reversible capacity is between 440mAh / g-446mAh / g, and the first coulombic efficiency is between 93%-94%.

[0054] Comparative Example 2

[0055] A method for preparing a silicon-carbon negative electrode material comprises the following steps:

[0056] S1. Mix micron-sized silicon powder and micron-sized silicon dioxide powder in a molar ratio of 1:1, evaporate them in a vacuum to prepare silicon oxide containing transition metals, and then grind the prepared silicon oxide containing transition metals using a jet mill to obtain a D50 of 3 μm-4 μm and a specific surface area of ​​3 m 2 / g-4m 2 / g, the reversible capacity of button cell test is 1500mAh / g-1600mAh / g, and the micron-sized silicon oxide powder containing transition metals has a Coulombic efficiency of 70% for the first time;

[0057] S2, the micron-sized silicon oxide powder containing transition metals prepared in S1, micron-sized artificial graphite (D50 between 14μm-15μm, specific surface area between 1m 2 / g-2m 2 / g, the button battery test reversible capacity is between 355mAh / g-358mAh / g, the first coulomb efficiency is 95%) and granulating agent (phenolic resin: asphalt mass ratio is 90:10) are put into a mixer according to a mass ratio of 7:93:5, and the mixing process is 800r / min for 5min, 1500r / min for 10min, and 2500r / min for 10min to obtain a mixture;

[0058] S3, put the mixture prepared in S2 into a drum furnace, heat it to 800℃-1000℃ at an angular speed of 0.4r / min-0.5r / min, and keep it at a constant temperature for 6h-8h to perform a granulation process to obtain a carbon-coated silicon-carbon negative electrode material, wherein D50 is between 15μm-16μm and the specific surface area is 1m 2 / g-2m 2 / g, the button battery tested reversible capacity is between 439mAh / g-445mAh / g, and the first coulombic efficiency is between 94%-95%.

[0059] Test example

[0060] In order to detect the performance of the silicon-carbon negative electrode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2 for lithium-ion batteries, tests were performed using a half-cell test method, a 18650 steel shell full battery, a scanning electron microscope, and a specific surface area and porosity analyzer.

[0061] (1) The half-cell test method is to use the silicon-carbon materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2 as negative electrode active materials to prepare slurry, and the slurry ratio is active material: SP: SWCNT: CMC: SBR = 95.6%: 0.5%: 0.1%: 1.5%: 2.3%, and then coat the slurry on copper foil and vacuum dry for 12 hours to make a negative electrode sheet. The electrolyte is purchased commercially, the separator is a PE film, and the lithium sheet is the counter electrode. The half-cell is assembled in a glove box. A constant current charge and discharge experiment is carried out in the LAND battery test system. The charge and discharge voltage is limited to 0.005V-2V, and a computer-controlled charge and discharge cabinet is used for data collection and control. Among them, the charge and discharge curve of the silicon-carbon material half-cell test in Example 1 is as follows Figure 2 The comparison results of the buckling performance of Example 1 to Example 3 and Comparative Example 1 to Comparative Example 2 are shown in Table 1.

[0062] Table 1. Test results of power-on performance

[0063]

[0064] From the test results in Table 1, it can be seen that in Comparative Example 1, no granulating agent was added for solid phase coating, and in Comparative Example 2, no ethylene and argon were added for gas phase coating. The battery capacity and first effect test results of the prepared silicon-carbon material were basically consistent with those of Examples 1 to 3, indicating that the generation of VGCF has little effect on the battery capacity and first effect.

[0065] (2) The batteries made of silicon-carbon materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to cycle tests for comparison. The test conditions were as shown in Table 2:

[0066] Table 2 Cyclic test conditions

[0067]

[0068] Cyclic test data comparison Figure 3 As shown, it can be seen that the silicon-carbon materials prepared in Examples 1 to 3 have higher cycle performance, among which Example 1 has the best cycle performance, indicating that the hard carbon coating layer formed by solid-gas phase mixed coating is beneficial to reducing the volume effect of the negative electrode material; while in Comparative Examples 1 and 2, since a hard carbon coating layer cannot be formed, the cycle performance is poor. Although the reversible specific capacity data of Comparative Examples 1 and 2 are good, the cycle performance is poor, affecting the overall performance.

[0069] (3) The electron microscope images of the silicon-carbon materials of Example 1 and Comparative Example 1 are compared. Figure 4-Figure 5 As shown. Among them, Figure 4The electron microscope images of the silicon-carbon material of Example 1 (a is a secondary electron image, b is a backscattered electron image), it can be seen that the micron-sized silicon dioxide is bound to the graphite surface by VGCF; Figure 5 This is the electron microscope image of the silicon-carbon material in Comparative Example 2. It can be seen that its micron-sized silicon oxide and graphite are not well combined together. It is probably because there is no hard carbon coating layer formed on its surface, which causes the material to expand during the charge and discharge process of the electrode, resulting in structural collapse and peeling of the active material.

[0070] In summary, the present invention adopts a combination of solid-phase and gas-phase coating, bonds micron-sized silicon oxide and graphite together through VGCF, and forms a complete hard carbon coating layer on its surface. The obtained silicon-carbon negative electrode material has not only high capacity and initial efficiency after testing, but also can significantly reduce the volume effect of the negative electrode, increase the number of cycles, and improve the service life of the lithium-ion battery; without solid-gas mixed coating, a hard carbon coating layer cannot be formed on the surface, and the cycle performance is poor.

[0071] Finally, it should be emphasized that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a silicon-carbon negative electrode material connected by VGCF, characterized in that: The silicon-carbon negative electrode material is obtained by bonding micron-sized silicon dioxide and graphite together through VGCF, and forming a complete hard carbon coating layer on the surface thereof. The specific preparation method includes the following steps: S1. Mix micron-sized silicon powder, micron-sized silicon dioxide powder and nano-sized transition metal powder in a vacuum, evaporate them, and then grind them using a jet mill to obtain micron-sized silicon oxide powder containing transition metal; the nano-sized transition metal powder is one or more of iron, cobalt and nickel; the micron-sized silicon powder, micron-sized silicon dioxide powder and nano-sized transition metal powder are mixed in a molar ratio of 1:1:0.00001-0.0001; the D50 of the micron-sized silicon oxide powder containing transition metal is between 2 μm and 6 μm; S2, mixing the micron-sized silicon dioxide powder containing transition metals, micron-sized graphite and granulating agent obtained in S1 through a mixer to obtain a mixture; the D50 of the micron-sized graphite is between 12 μm and 16 μm; the granulating agent is one or more of phenolic resin, asphalt, polyacrylonitrile, polyvinyl alcohol, polyimide and polyvinylidene fluoride; the mass ratio of the micron-sized silicon dioxide powder containing transition metals, micron-sized graphite and granulating agent is 3-10:90-95:1-10; S3. The mixture obtained in S2 is introduced with protective gas and carbon source gas at high temperature, and a granulation process is performed on a drum furnace to obtain a silicon-carbon negative electrode material connected with VGCF, wherein the drum furnace granulation process is: angular velocity 0.3r / min-1r / min, heating 700℃-1200℃, constant temperature 4h-10h; the volume ratio of the carbon source gas to the protective gas is 10-30:70-90.

2. The preparation method according to claim 1, characterized in that: In S1, the specific surface area of ​​the micron-sized transition metal-containing silicon dioxide powder is 1 m 2 / g-5m 2 / g, the button battery tested reversible capacity is between 1400mAh / g-1800mAh / g, and the first coulombic efficiency is 60%-70%.

3. The preparation method according to claim 1, characterized in that: In S2, the micron-sized graphite is one or both of artificial graphite and natural graphite, with a specific surface area of ​​1m 2 / g-3m 2 / g, the button battery tested reversible capacity is between 350mAh / g-365mAh / g, and the first coulombic efficiency is 95%.

4. The preparation method according to claim 1, characterized in that: In S2, the mixing process of the mixer is: stirring at 600 r / min-1000 r / min for 5 min, stirring at 1000 r / min-1800 r / min for 10 min, and stirring at 2000 r / min-3000 r / min for 10 min.

5. The preparation method according to claim 1, characterized in that: In S3, the carbon source gas is one or more of ethylene, propylene, acetylene, ethane, and propane.

6. The preparation method according to claim 1, characterized in that: In S3, the protective gas is one or more of helium, argon, and neon.

7. A silicon-carbon negative electrode material connected by VGCF obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The D50 of the silicon-carbon negative electrode material is between 13 μm and 18 μm, and the specific surface area is 1 m 2 / g-2m 2 / g, the button battery tested reversible capacity is between 380mAh / g-500mAh / g, and the first coulombic efficiency is 90%-95%.

Citation Information

Patent Citations

  • Silicon monoxide composite negative electrode material, preparation method thereof and lithium ion battery

    CN111082006A

  • Amorphous carbon-silicon-carbon nanofiber-graphite composite material as well as preparation method and application thereof