Negative electrode composite active material and preparation method thereof, negative electrode pole piece and lithium ion battery

The silanol oligomer produced by hydrolysis of silane coupling agent reacts with hydroxylated graphite to form a composite structure of graphite coated silicon active particles, which solves the problems of volume expansion and increased interface impedance of silicon-based anode materials in lithium-ion batteries, and improves the The cycle performance and stability of the battery.

CN119050337AInactive Publication Date: 2024-11-29ENPOWER (PEKING) INC

Patent Information

Application Number
CN202411542513.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silicon-based anode material has problems of volume expansion and increased interface impedance in lithium-ion batteries, resulting in attenuation of cyclic performance.

Method used

The silanol oligomer produced by hydrolysis of silane coupling agent reacts with hydroxylated graphite to form a composite elastic structure with graphite coated with silicon active particles, inhibiting the expansion of silicon volume and protecting the interface, and improving the cell cycle performance.

Benefits of technology

It effectively reduces the reaction between silicon and electrolyte, maintains structural integrity, and improves the circulation performance and cell stability of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050337A_ABST
    Figure CN119050337A_ABST
Patent Text Reader

Abstract

The invention provides a negative electrode composite active material and a preparation method thereof, a negative electrode pole piece and a lithium ion battery. The negative electrode composite active material comprises a negative electrode active material and silanol oligomer modified graphite. The silanol oligomer generated by hydrolysis of the silane coupling agent reacts with the hydroxylated graphite and the silicon active particles to form a composite elastic structure of the graphite coated silicon active particles, so that the side reaction of the silicon active particles and an electrolyte can be effectively inhibited, and the volume expansion of the silicon active particles is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium batteries and relates to a negative electrode composite active material and a preparation method thereof, a negative electrode pole piece and a lithium ion battery. Background Art

[0002] With the development of the new energy electric vehicle industry, the demand for high energy density batteries is becoming more and more urgent. Improving battery capacity, reducing battery quality, and achieving high energy density are the development directions of batteries. The weight of the battery is occupied by the positive and negative electrodes and the electrolyte. At present, the choice of high-capacity positive electrode materials is mainly ternary positive electrode materials. Compared with traditional graphite negative electrode materials (372mAh / g), silicon negative electrode materials have high discharge specific capacity (4200mAh / g) and low discharge potential (0.4 V vs. Li + / Li), favored by the lithium battery industry. Silicon anode has obvious advantages, but there are still some problems that restrict its practical application. Silicon anode has a large volume expansion during the charging and discharging process, silicon-based anode materials crack until they are pulverized and the SEI film ruptures, and the continuous consumption of electrolyte eventually leads to an increase in interface impedance and a decrease in cycle performance.

[0003] Therefore, inhibiting the expansion of the silicon negative electrode and protecting the interface are the key to improving the performance of silicon-based lithium-ion batteries. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a negative electrode composite active material and a preparation method thereof, a negative electrode plate and a lithium ion battery. In the present invention, silanol oligomers generated by hydrolysis of a silane coupling agent react with hydroxylated graphite and silicon active particles to form a composite elastic structure of graphite-coated silicon active particles, which effectively inhibits the volume expansion of silicon during the cycle, protects the interface of the silicon active material, and improves the cycle performance of the battery cell.

[0005] To achieve this object, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a composite active material, wherein the negative electrode composite active material comprises: a negative electrode active material and graphite modified by a silanol oligomer, wherein the mass ratio of the negative electrode active material to the graphite modified by the silanol oligomer is 10:(0.1-10); The silanol oligomer is a product obtained by hydrolyzing a silane coupling agent in an acidic solution or an alkaline solution, wherein the structural formula of the silane coupling agent is Y-(CH 2 ) n -Si-X 3 ; n is an integer of 0-3; X is independently selected from the following hydrolyzable groups: methoxy or ethoxy; Y is selected from the following functional groups: unsaturated alkyl, amino, thiol, acyl or halogen.

[0006] As a preferred embodiment of the present invention, the negative electrode active material includes a silicon negative electrode active material or a mixture of a silicon negative electrode active material and a non-silicon negative electrode active material.

[0007] As a preferred embodiment of the present invention, the silicon negative electrode active material includes any one of silicon, silicon monoxide or silicon carbon, or a combination of at least two of them.

[0008] As a preferred embodiment of the present invention, the non-silicon negative electrode active material includes graphite and / or hard carbon.

[0009] As a preferred embodiment of the present invention, the mass percentage of silicon element in the mixture of the silicon negative electrode active material and the non-silicon negative electrode active material is 5wt%-70wt%.

[0010] As a preferred embodiment of the present invention, the method for preparing the silanol oligomer modified graphite comprises: mixing a silanol oligomer solution and hydroxylated graphite to prepare the silanol oligomer modified graphite. The concentration of the silanol oligomer solution is 1wt%-10wt%; the mass ratio of the silane coupling agent used in the silanol oligomer solution to the hydroxylated graphite is (0.1-5):1.

[0011] As a preferred embodiment of the present invention, the silane coupling agent is selected from any one or a combination of at least two of the following structural formulas: , , or .

[0012] As a preferred embodiment of the present invention, the pH value of the acidic solution is 4-6.9.

[0013] As a preferred embodiment of the present invention, the pH value of the alkaline solution is 7.1-10.

[0014] As a preferred embodiment of the present invention, the acidic solution includes boric acid and / or oxalic acid.

[0015] As a preferred embodiment of the present invention, the alkaline solution includes any one of lithium hydroxide solution, sodium hydroxide solution or ammonia water, or a combination of at least two of them.

[0016] In a second aspect, the present invention provides a method for preparing the aforementioned negative electrode composite active material, the preparation method comprising: mixing the negative electrode active material with graphite modified by silanol oligomers to obtain the negative electrode composite active material.

[0017] In a third aspect, the present invention provides a negative electrode plate, wherein the negative electrode plate is prepared using the aforementioned negative electrode composite active material.

[0018] In a fourth aspect, the present invention provides a method for preparing the aforementioned negative electrode sheet, the method for preparing the negative electrode sheet comprising: mixing the negative electrode composite active material with a first adhesive, a conductive agent and a second adhesive to obtain a negative electrode slurry, then coating the negative electrode slurry on a current collector, and obtaining a negative electrode sheet through drying, rolling and cutting.

[0019] As a preferred embodiment of the present invention, the first adhesive is lithium polyacrylate.

[0020] As a preferred embodiment of the present invention, the content of the negative electrode composite active material in the negative electrode slurry is 70wt%-97wt%, such as 70wt%, 75wt%, 80wt%, 85wt%, 90wt% or 97wt%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the content of the conductive agent is 0.1wt%-10wt%, such as 0.1wt%, 0.5wt%, 1wt%, 2wt%, 5wt%, 7wt% or 10wt%, etc., but is not limited to the listed values, and the numerical range is Other unlisted values ​​are also applicable; the content of the first adhesive is 0.5wt%-10wt%, for example 0.5wt%, 1wt%, 2wt%, 5wt%, 7wt% or 10wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; the content of the second adhesive is 0.5wt%-10wt%, for example 0.5wt%, 1wt%, 3wt%, 5wt%, 7wt% or 10wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] As a preferred embodiment of the present invention, the conductive agent includes any one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene or carbon nanofibers, or a combination of at least two thereof.

[0022] As a preferred embodiment of the present invention, the second adhesive comprises any one of styrene-butadiene rubber, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid or carboxymethyl chitosan, or a combination of at least two thereof.

[0023] As a preferred embodiment of the present invention, the preparation method of lithium polyacrylate comprises: mixing a polyacrylic acid solution with LiOH and reacting them to obtain lithium polyacrylate.

[0024] As a preferred embodiment of the present invention, the mass ratio of polyacrylic acid to LiOH in the polyacrylic acid solution is (3-3.5):1.

[0025] As a preferred embodiment of the present invention, the concentration of the polyacrylic acid solution is 1wt%-15wt%.

[0026] In a fifth aspect, the present invention provides a lithium-ion battery, wherein the negative electrode plate used in the lithium-ion battery is the aforementioned negative electrode plate.

[0027] Compared with the prior art, the present invention has the following beneficial effects: The present invention uses silanol oligomers obtained by hydrolysis of silane coupling agents to coat hydroxylated graphite, and coats the hydroxylated graphite grafted with silanol oligomers on the surface of silicon nanoparticles, thereby reducing the reaction between silicon active particles and electrolytes, and the elastic coating layer can inhibit the volume expansion of silicon. In the subsequent pole piece preparation process, the coated composite structure active material is embedded in a mesh structure containing a lithium polyacrylate binder, further maintaining the structural integrity and improving the battery cell cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic diagram of the structure of the mixed slurry prepared in an embodiment of the present invention; Among them, 1-hydroxylated graphite, 2-silanol oligomers, 3-PAA-Li, and 4-silicon nanoparticles. DETAILED DESCRIPTION

[0029] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0030] The specific implementation mode of the present invention provides a negative electrode composite active material, which includes: a negative electrode active material and graphite modified by a silanol oligomer, wherein the mass ratio of the negative electrode active material to the graphite modified by a silanol oligomer is 10:(0.1~10), for example, 10:0.1, 10:1, 10:2, 10:3, 10:4, 10:5, 10:6, 10:7, 10:8, 10:9 or 10:10, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] The silanol oligomer is a product obtained by hydrolyzing a silane coupling agent in an acidic solution or an alkaline solution, wherein the structural formula of the silane coupling agent is Y-(CH 2 ) n -Si-X 3 ; n is an integer of 0-3, such as 1, 2 or 3; X is independently selected from the following hydrolyzable groups: methoxy or ethoxy, and the three X groups may be the same or different from each other; Y is selected from the following functional groups: unsaturated alkyl, amino, thiol, acyl or halogen.

[0032] The present invention modifies graphite by reacting silanol oligomers produced by hydrolysis of a silane coupling agent with hydroxylated graphite, and then mixes the silanol oligomers with the negative electrode active material (silicon active particles) to form a composite elastic structure of graphite-coated negative electrode active material (silicon active particles), thereby effectively improving the volume expansion of silicon during the cycle, reducing its reaction with the electrolyte, and improving the cycle performance of the battery cell.

[0033] In the present invention, compared with only mixing a silane coupling agent with a negative electrode active material, hydroxylated graphite is reacted with a silane coupling agent and then mixed with a negative electrode active material, and hydroxylated graphite grafted with a silanol oligomer is coated on the surface of silicon nanoparticles, which reduces the reaction between silicon and electrolyte. The elastic coating layer can inhibit the volume expansion of silicon, thereby improving the cycle performance of the battery cell.

[0034] As a preferred embodiment of the present invention, the negative electrode active material includes a silicon negative electrode active material or a mixture of a silicon negative electrode active material and a non-silicon negative electrode active material.

[0035] As a preferred embodiment of the present invention, the silicon negative electrode active material includes any one of silicon, silicon monoxide or silicon carbon, or a combination of at least two of them.

[0036] As a preferred embodiment of the present invention, the non-silicon negative electrode active material includes graphite and / or hard carbon.

[0037] As a preferred embodiment of the present invention, the mass percentage of silicon element in the mixture of the silicon negative electrode active material and the non-silicon negative electrode active material is 5wt%-70wt%, for example, 5wt%, 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt% or 70wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] As a preferred embodiment of the present invention, the preparation method of the silanol oligomer modified graphite includes: preparing the silanol oligomer modified graphite by mixing a silanol oligomer solution and a hydroxylated graphite. Wherein, the concentration of the silanol oligomer solution is 1wt%-10wt%, such as 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; the mass ratio of the silane coupling agent used in the silanol oligomer solution to the hydroxylated graphite is (0.1-5):1, such as 0.1:1, 0.2:1, 0.3:1, 1:1, 2:1, 3:1, 4:1 or 5:1, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] As a preferred embodiment of the present invention, the silane coupling agent is selected from any one or a combination of at least two of the following structural formulas: , , or .

[0040] In the present invention, the silane coupling agent undergoes alcoholization and condensation reaction in an alkaline solution or an acidic solution to generate silanol oligomers, and then the silanol oligomers undergo hydrolysis and condensation reaction with hydroxyl groups on the surface of hydroxylated graphite.

[0041] As a preferred embodiment of the present invention, the pH value of the acidic solution is 4-6.9, such as 4, 4.5, 5, 5.5, 6, 6.5 or 6.9, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0042] As a preferred embodiment of the present invention, the pH value of the alkaline solution is 7.1-10, such as 7.1, 7.5, 8, 8.5, 9, 9.5 or 10, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] As a preferred embodiment of the present invention, the acidic solution includes boric acid and / or oxalic acid.

[0044] As a preferred embodiment of the present invention, the alkaline solution includes any one of lithium hydroxide solution, sodium hydroxide solution or ammonia water, or a combination of at least two of them.

[0045] In the present invention, the acidic or alkaline solution is used to facilitate the modification and hydrolysis of the silane coupling agent.

[0046] In a second aspect, the specific implementation of the present invention also provides a method for preparing the aforementioned negative electrode composite active material, the preparation method comprising: mixing the negative electrode active material with graphite modified by silanol oligomers to obtain the negative electrode composite active material.

[0047] In a third aspect, the specific implementation method of the present invention also provides a negative electrode plate, which is prepared by using the above-mentioned negative electrode composite active material.

[0048] In a fourth aspect, the specific implementation of the present invention also provides a method for preparing the aforementioned negative electrode sheet, the method for preparing the negative electrode sheet comprising: mixing the negative electrode composite active material with the first binder, the conductive agent and the second binder to obtain a negative electrode slurry, coating the negative electrode slurry on the current collector, and drying, rolling and cutting to obtain a negative electrode sheet. The drying, rolling, cutting and other preparation processes are all conventional preparation methods in the art.

[0049] As a preferred embodiment of the present invention, the preparation method comprises: mixing the negative electrode composite active material with the first adhesive to form a mixture, then mixing it with the conductive agent and the second adhesive to obtain a negative electrode slurry, then coating the negative electrode slurry on the current collector, and obtaining a negative electrode sheet through drying, rolling and cutting.

[0050] In the present invention, the first binder is added to the negative electrode composite active material to further strengthen the elastic structure formed on the surface of the silicon active particles.

[0051] As a preferred embodiment of the present invention, the first adhesive is lithium polyacrylate (PAA-Li).

[0052] As a preferred embodiment of the present invention, the content of negative electrode composite active material in the negative electrode slurry is 70wt%-97wt%, the content of conductive agent is 0.1wt%-10wt%, the content of first binder is 0.5wt%-10wt%, and the content of second binder is 0.5wt%-10wt%.

[0053] As a preferred embodiment of the present invention, the conductive agent includes any one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene or carbon nanofibers, or a combination of at least two thereof.

[0054] As a preferred embodiment of the present invention, the second adhesive comprises any one of styrene-butadiene rubber, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid or carboxymethyl chitosan, or a combination of at least two thereof.

[0055] As a preferred embodiment of the present invention, the preparation method of lithium polyacrylate comprises: mixing a polyacrylic acid solution with LiOH and reacting them to obtain lithium polyacrylate.

[0056] As a preferred embodiment of the present invention, the mass ratio of polyacrylic acid to LiOH in the polyacrylic acid solution is (3-3.5):1, for example, 3:1, 3.1:1, 3.2:1, 3.3:1, 3.4:1 or 3.5:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] The first binder used in the present invention is lithium polyacrylate, which can reduce internal resistance and has a lithium supplement effect compared to polyacrylic acid.

[0058] As a preferred embodiment of the present invention, the concentration of the polyacrylic acid solution is 1wt%-15wt%, for example, 1wt%, 2wt%, 3wt%, 5wt%, 8wt%, 10wt%, 12wt% or 15wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] In a fifth aspect, the specific implementation of the present invention also provides a lithium-ion battery, wherein the negative electrode plate used in the lithium-ion battery is the aforementioned negative electrode plate.

[0060] The following are typical but non-limiting embodiments of the present invention: Embodiment 1:

[0061] The present embodiment provides a negative electrode composite active material and a preparation method thereof, wherein the negative electrode composite active material comprises: a negative electrode active material and graphite modified by a silanol oligomer, wherein the preparation method of the graphite modified by a silanol oligomer comprises: preparing a boric acid solution containing 1wt%, adding a silane coupling agent to the boric acid solution to make the concentration of the silane coupling agent 1.5wt%, then adding 5wt% hydroxylated graphite and stirring for 24h to obtain a graphite particle solution modified by a silanol oligomer, wherein the structure of the silane coupling agent is .

[0062] The preparation method of the negative electrode composite active material comprises: adding silicon nanoparticles to a graphite particle solution modified by a silanol oligomer to make the concentration of the silicon nanoparticles in the solution be 10wt%, and mechanically stirring to obtain the negative electrode composite active material. Embodiment 2:

[0063] This embodiment provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method are the same as those in Example 1, except that the concentration of the silane coupling agent in the boric acid solution is 2 wt %. Embodiment 3:

[0064] This embodiment provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method are the same as those in Example 1, except that the concentration of the silane coupling agent in the boric acid solution is 2.5 wt %. Embodiment 4:

[0065] This embodiment provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method are the same as those in Example 1, except that the concentration of the silane coupling agent in the boric acid solution is 5 wt %. Embodiment 5:

[0066] This embodiment provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method are the same as those in Example 1, except that the concentration of the silane coupling agent in the boric acid solution is 10 wt %. Embodiment 6:

[0067] This embodiment provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method are the same as those in Example 1, except that the concentration of the silane coupling agent in the boric acid solution is 0.5 wt %. Embodiment 7:

[0068] This embodiment provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method are the same as those in Example 1, except that the silane coupling agent used is . Embodiment 8:

[0069] This embodiment provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method are the same as those in Example 1, except that the silane coupling agent used is . Embodiment 9:

[0070] This embodiment provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method are the same as those in Example 1, except that the silane coupling agent used is .

[0071] Comparative Example 1: This comparative example provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method of the negative electrode composite active material are the same as those in Example 2, except that the silane coupling agent used in the negative electrode composite active material does not undergo a hydrolysis reaction in the boric acid solution, that is, the silane coupling agent and hydroxylated graphite are directly added.

[0072] Comparative Example 2: This comparative example provides a negative electrode active material, which includes only silicon nanoparticles.

[0073] Comparative Example 3: This comparative example provides a negative electrode composite active material and a preparation method thereof. The composition and preparation method of the negative electrode composite active material are the same as those in Example 2, except that the negative electrode composite active material does not include hydroxylated graphite.

[0074] The negative electrode composite active material prepared in Examples 1-9 is used to prepare a negative electrode plate and a lithium-ion soft-pack battery. The preparation method of the negative electrode plate is as follows: (1) The negative electrode composite active material, PAA-Li, CNT, CMC, and SBR were prepared in a mass ratio of 96:0.5:0.78:1:1.72; (2) The negative electrode composite active material is mixed with the PAA-Li solution to make the concentration of PAA-Li 2wt%, and stirred evenly to obtain a mixed slurry. The structure of the mixed slurry is as follows: Figure 1 As shown; (3) Add CMC to the mixed slurry and stir for 4 hours until the CMC is completely mixed and evenly mixed; continue to add CNT to the above solution and stir for 30 minutes until the CNT is completely dispersed and evenly mixed; finally add SBR and stir for 2 hours until it is evenly mixed; (4) The slurry prepared in the above steps is coated on a copper foil, and then dried, rolled and cut to finally prepare a negative electrode sheet with a pole piece area length × width = 57*52 mm and a tab area length × width = 10*5 mm for standby use.

[0075] Similarly, the negative electrode plates were prepared using the negative electrode composite active materials prepared in Comparative Examples 1-4 in the same manner.

[0076] Preparation of positive electrode sheet: Mix the positive electrode ternary active material NMC811, conductive carbon black (Super P), and polyvinylidene fluoride (PVDF) in a weight ratio of 90:5:5, add N-methylpyrrolidone (NMP) as a solvent, and prepare a slurry with a solid content of 70wt%, and stir evenly. The slurry is evenly coated on aluminum foil, and through drying, rolling, and cutting, a positive electrode sheet with a specification of 55*50mm in the sheet area length × width and 10*5mm in the tab area length × width is prepared for standby use.

[0077] Preparation of lithium-ion soft pack batteries: The negative electrode sheet, the positive electrode sheet and the separator are wound to obtain a battery cell, the battery cell is placed in an aluminum-plastic film and then packaged, an electrolyte is injected, and then sealed in sequence, and a lithium-ion secondary battery is obtained through processes such as infiltration, formation, and exhaust.

[0078] The performance of lithium-ion soft-pack batteries prepared using the negative electrode sheets prepared using the negative electrode compositions described in Examples 1-9 and Comparative Examples 1-4 was tested. The test results are shown in Table 1.

[0079] The applicant declares that the present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A negative electrode composite active material, characterized in that: The negative electrode composite active material comprises: a negative electrode active material and graphite modified by silanol oligomers, wherein the mass ratio of the negative electrode active material to the graphite modified by silanol oligomers is 10:(0.1-10); The silanol oligomer is a product obtained by hydrolyzing a silane coupling agent in an acidic solution or an alkaline solution, wherein the structural formula of the silane coupling agent is Y-(CH2) n -Si-X3; n is an integer of 0-3; X is independently selected from the following hydrolyzable groups: methoxy or ethoxy; Y is selected from the following functional groups: unsaturated alkyl, amino, mercapto, acyl or halogen.

2. The negative electrode composite active material according to claim 1, characterized in that: The negative electrode active material includes a silicon negative electrode active material or a mixture of a silicon negative electrode active material and a non-silicon negative electrode active material; The silicon negative electrode active material includes any one of silicon, silicon monoxide or silicon carbon or a combination of at least two of them; the non-silicon negative electrode active material includes graphite and / or hard carbon; the mass percentage of silicon element in the mixture of the silicon negative electrode active material and the non-silicon negative electrode active material is 5wt%-70wt%.

3. The negative electrode composite active material according to claim 1, characterized in that: The preparation method of the silanol oligomer modified graphite comprises: mixing a silanol oligomer solution and hydroxylated graphite to prepare the silanol oligomer modified graphite; wherein the concentration of the silanol oligomer solution is 1wt%-10wt%; and the mass ratio of the silane coupling agent used in the silanol oligomer solution to the hydroxylated graphite is (0.1-5):

1.

4. The negative electrode composite active material according to claim 1, characterized in that: The silane coupling agent is selected from any one or a combination of at least two of the following structural formulas: , , or ; The pH value of the acidic solution is 4-6.9; the pH value of the alkaline solution is 7.1-10.

5. The negative electrode composite active material according to claim 1, characterized in that: The acidic solution includes boric acid and / or oxalic acid; The alkaline solution includes any one of lithium hydroxide solution, sodium hydroxide solution or ammonia solution, or a combination of at least two of them.

6. A method for preparing a negative electrode composite active material according to any one of claims 1 to 5, characterized in that: The preparation method comprises: mixing the negative electrode active material with graphite modified by silanol oligomer to obtain the negative electrode composite active material.

7. A negative electrode plate, characterized in that: The negative electrode plate is prepared by using the negative electrode composite active material according to any one of claims 1 to 5.

8. A method for preparing a negative electrode sheet as claimed in claim 7, characterized in that: The method for preparing the negative electrode sheet comprises: The negative electrode composite active material is mixed with the first binder, the conductive agent and the second binder to obtain a negative electrode slurry, and the negative electrode slurry is coated on the current collector, and the negative electrode sheet is obtained after drying, rolling and cutting; Wherein, the first adhesive is lithium polyacrylate; The negative electrode slurry contains 70wt%-97wt% of the negative electrode composite active material, 0.1wt%-10wt% of the conductive agent, 0.5wt%-10wt% of the first binder, and 0.5wt%-10wt% of the second binder. The conductive agent includes any one or a combination of at least two of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene or carbon nanofibers; The second adhesive includes any one of styrene-butadiene rubber, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid or carboxymethyl chitosan, or a combination of at least two thereof.

9. The preparation method according to claim 8, characterized in that: The preparation method of lithium polyacrylate comprises: mixing a polyacrylic acid solution with LiOH and reacting to obtain lithium polyacrylate; the mass ratio of polyacrylic acid to LiOH in the polyacrylic acid solution is (3-3.5):1; and the concentration of the polyacrylic acid solution is 1wt%-15wt%.

10. A lithium ion battery, characterized in that: The negative electrode plate used in the lithium-ion battery is the negative electrode plate according to claim 7.

Citation Information

Patent Citations

  • Silicon / graphite composite anode material and preparation method thereof

    CN104319367A

  • Modified silicon-based negative electrode material, preparation method thereof, and lithium ion battery

    CN110504441A

  • Silicon-containing negative electrode, preparation method thereof and lithium ion battery

    CN118299576A

  • Negative plate and battery

    CN118676308A

  • Negative electrode slurry and preparation method thereof, negative electrode plate and preparation method thereof, and lithium ion battery

    CN118738395A

Cited By

  • Composite silicon-carbon negative electrode material and preparation method thereof

    CN122417832A