Lithium ion battery negative electrode material, preparation method thereof and lithium ion battery

By forming a fluorinated carbon cladding layer on the surface of the silicon-based anode material of lithium-ion batteries, the problem of poor volume expansion and cycle stability of silicon-based anode materials in lithium-ion batteries is solved, and the cycle stability and electrochemical performance of the battery are significantly improved. .

CN119059514APending Publication Date: 2024-12-03SHENZHEN HIGHPOWER TECH CO LTD

Patent Information

Application Number
CN202411051696.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Silicon-based negative electrode material is caused by volume expansion and side reactions in lithium-ion batteries, which affects battery performance.

Method used

The carbon fluoride coating layer is formed on the surface of the silicon-based anode material of lithium-ion batteries. The carbon-coated silicon-based anode material and the fluorine source solution is used to form a fluoride coating layer, improving the interface between the material and the electrolyte solution through solvent heat treatment and calcination. Stability, inhibits volume expansion and side reactions.

Benefits of technology

It significantly improves the cycle stability and electrochemical performance of lithium-ion batteries, extends the battery life, and solves the problems of volume expansion and poor cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059514A_ABST
    Figure CN119059514A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium ion battery negative electrode material, a preparation method thereof and a lithium ion battery. The method comprises the following steps: mixing a carbon-coated silicon-based negative electrode material with ethanol to obtain a first suspension; mixing the first suspension with a fluorine source solution to obtain a second suspension; performing solvent heat treatment on the second suspension; carrying out suction filtration on the second suspension subjected to solvent heat treatment to obtain second powder, and drying the second powder; and calcining the dried second powder to obtain the carbon fluoride coated silicon-based negative electrode material. According to the scheme provided by the invention, the carbon fluoride coating layer can be formed on the surface of the silicon-based negative electrode material of the lithium ion battery, the silicon-based negative electrode material of the lithium ion battery is subjected to interface modification, the interface stability of the silicon-based negative electrode material and the electrolyte is improved, the side reaction of the silicon-based negative electrode material and the electrolyte can be inhibited, and the volume expansion of the silicon-based negative electrode material is inhibited; and the cycling stability and the cycling performance of the lithium ion battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a lithium-ion battery negative electrode material and a preparation method thereof, and a lithium-ion battery. Background Art

[0002] In recent years, silicon-based materials have attracted much attention due to their extremely high theoretical mass specific capacity (about 4200 mAh / g (milliampere-hour per gram)) and are regarded as one of the preferred negative electrode materials for the next generation of lithium-ion batteries.

[0003] Silicon's ability to embed lithium far exceeds that of graphite, and in theory it can significantly increase the energy density of batteries, thereby extending the range of electric vehicles or reducing the size of portable electronic devices. However, silicon-based negative electrodes face major challenges in practical applications. The huge volume expansion (up to 300% or more) of silicon-based negative electrodes in related technologies during the cycle process leads to problems such as material structure destruction, electrode pulverization, electrolyte consumption, and side reactions between silicon and electrolyte, which seriously affect the cycle stability and service life of the battery. Summary of the invention

[0004] In order to solve or partially solve the problems existing in the related art, the present application provides a lithium ion battery negative electrode material and a preparation method thereof, and a lithium ion battery, which can form a carbon fluoride coating layer on the surface of the silicon-based negative electrode material of the lithium ion battery, perform interface modification on the silicon-based negative electrode material of the lithium ion battery, improve the interface stability between the silicon-based negative electrode material and the electrolyte, inhibit the side reaction between the silicon-based negative electrode material and the electrolyte, inhibit the volume expansion of the silicon-based negative electrode material, and improve the cycle stability and cycle performance of the lithium ion battery.

[0005] The first aspect of the present application provides a method for preparing a negative electrode material for a lithium ion battery, the method comprising: mixing the carbon-coated silicon-based negative electrode material with ethanol to obtain a first suspension; mixing the first suspension with a fluorine source solution to obtain a second suspension; subjecting the second suspension to a solvothermal treatment; filtering the second suspension after the solvent thermal treatment to obtain a second powder, and drying the second powder; The dried second powder is calcined to obtain a carbon fluoride-coated silicon-based negative electrode material.

[0006] Preferably, the fluorine source solution is obtained by mixing a fluorine source with ethanol, wherein the fluorine source is ammonium fluoride or 1-butyl-3-methylimidazolium tetrafluoroborate.

[0007] Preferably, the solvothermal treatment of the second suspension comprises: The second suspension is subjected to solvent thermal treatment in a hydrothermal kettle or a hydrothermal box; wherein the temperature of the solvent thermal treatment is 120° C.-180° C., and the insulation time is 4 hours-12 hours.

[0008] Preferably, the step of calcining the dried second powder to obtain a carbon fluoride-coated silicon-based negative electrode material comprises: The dried second powder is calcined under the protection of a protective gas to obtain a carbon fluoride-coated silicon-based negative electrode material; wherein the calcination temperature is 300°C-600°C, the heating rate is 5°C / min-10°C / min, and the calcination time is 6 hours-12 hours.

[0009] Preferably, before mixing the carbon-coated silicon-based negative electrode material with ethanol to obtain the first suspension, the process comprises: Mixing a silicon-based negative electrode material with a polyhydroxy solution to obtain a silicon-based negative electrode material suspension, wherein the silicon-based negative electrode material is a silicon-carbon negative electrode material or a silicon-oxygen negative electrode material; The silicon-based negative electrode material suspension is filtered to obtain a first powder, and the first powder is calcined to obtain a carbon-coated silicon-based negative electrode material.

[0010] Preferably, the calcining of the first powder to obtain a carbon-coated silicon-based negative electrode material comprises: The first powder is calcined in a muffle furnace to obtain a carbon-coated silicon-based negative electrode material; wherein the calcination temperature is 200° C.-300° C., and the calcination time is 2 hours-4 hours.

[0011] Preferably, the polyhydroxy substance is mixed with ethanol to obtain the polyhydroxy solution; wherein the polyhydroxy substance is a polyhydroxy alcohol or a polyhydroxy aldehyde.

[0012] Preferably, the concentration ratio of the silicon-based negative electrode material in the silicon-based negative electrode material suspension, the fluorine source in the fluorine source solution, and the polyhydroxy substance in the polyhydroxy solution is 1:(0.25-4):(0.25-4).

[0013] A second aspect of the present application provides a lithium-ion battery negative electrode material, including a carbon fluoride-coated silicon-based negative electrode material prepared by the above method.

[0014] A third aspect of the present application provides a lithium-ion battery, comprising a negative electrode plate, wherein the negative electrode plate comprises the above-mentioned carbon fluoride-coated silicon-based negative electrode material, or comprises the carbon fluoride-coated silicon-based negative electrode material prepared by the above-mentioned method.

[0015] The technical solution provided by this application may have the following beneficial effects: The technical solution of the present application can obtain a carbon fluoride-coated silicon-based negative electrode material with a carbon fluoride coating layer, can form a carbon fluoride coating layer on the surface of the silicon-based negative electrode material of a lithium-ion battery, perform interface modification on the silicon-based negative electrode material of the lithium-ion battery, improve the interface stability between the silicon-based negative electrode material and the electrolyte, can inhibit the side reaction between the silicon-based negative electrode material and the electrolyte, inhibit the volume expansion of the silicon-based negative electrode material during the charging and discharging process, improve the cycle stability and cycle performance of the lithium-ion battery, solve the key technical problems such as volume expansion and poor cycle stability faced by silicon-based negative electrode materials in related technologies, and contribute to the advancement of lithium-ion battery technology.

[0016] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The above and other objects, features and advantages of the present application will become more apparent by describing in more detail exemplary embodiments of the present application in conjunction with the accompanying drawings, wherein the same reference numerals generally represent the same components in the exemplary embodiments of the present application.

[0018] Figure 1 It is a schematic diagram of a process for preparing a negative electrode material for a lithium-ion battery shown in an embodiment of the present application; Figure 2 It is another schematic diagram of the process of preparing the negative electrode material of a lithium-ion battery shown in the embodiment of the present application; Figure 3 It is a schematic structural diagram of a carbon fluoride-coated silicon-based negative electrode material in a method for preparing a negative electrode material for a lithium-ion battery shown in an embodiment of the present application; Figure 4 It is a structural schematic diagram of the electrode activation process of the carbon fluoride-coated silicon-based negative electrode material in the method for preparing the negative electrode material for a lithium-ion battery shown in the embodiment of the present application; Figure 5 It is a schematic diagram comparing the capacity retention rates after 200 cycles of half-cells A1, A6-A8 corresponding to Example 1, Example 6-Example 8 and half-cells B1-B4 corresponding to Comparative Examples 1-4 shown in the embodiments of the present application. DETAILED DESCRIPTION

[0019] The embodiments of the present application will be described in more detail below with reference to the accompanying drawings. Although the embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present application more thorough and complete, and to fully convey the scope of the present application to those skilled in the art.

[0020] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0021] It should be understood that although the terms "first", "second", "third", etc. may be used in this application to describe various information, this information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of this application, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0022] The embodiment of the present application provides a method for preparing a negative electrode material for a lithium ion battery, which can form a carbon fluoride coating layer on the surface of a silicon-based negative electrode material for a lithium ion battery, perform interface modification on the silicon-based negative electrode material for a lithium ion battery, improve the interface stability between the silicon-based negative electrode material and the electrolyte, inhibit the side reaction between the silicon-based negative electrode material and the electrolyte, inhibit the volume expansion of the silicon-based negative electrode material, and improve the cycle stability and cycle performance of the lithium ion battery.

[0023] The technical solution of the embodiments of the present application is described in detail below with reference to the accompanying drawings.

[0024] Figure 1 It is a schematic diagram of the process of preparing a negative electrode material for a lithium-ion battery shown in an embodiment of the present application.

[0025] See also Figure 1 , a method for preparing a negative electrode material for a lithium ion battery, comprising: Step 101: Mix the carbon-coated silicon-based negative electrode material with ethanol to obtain a first suspension.

[0026] In one embodiment, the carbon-coated silicon-based negative electrode material can be added into ethanol and stirred to mix evenly to form a first suspension.

[0027] Step 102: Mix the first suspension with a fluorine source solution to obtain a second suspension.

[0028] In one embodiment, the fluorine source solution can be added to the first suspension, and stirred and mixed to form a second suspension.

[0029] Step 103, performing a solvothermal treatment on the second suspension.

[0030] In one embodiment, the second suspension may be subjected to a solvothermal treatment in a hydrothermal kettle or a hydrothermal box to combine the fluorine in the fluorine source solution with the carbon in the carbon coating layer of the carbon-coated silicon-based negative electrode material.

[0031] Step 104, filtering the second suspension after the solvent thermal treatment to obtain a second powder, and drying the second powder.

[0032] In one embodiment, the second suspension after the solvent thermal treatment can be filtered to obtain a second powder of the second suspension after the solvent thermal treatment, and the second powder can be dried.

[0033] Step 105, calcining the dried second powder to obtain a carbon fluoride-coated silicon-based negative electrode material.

[0034] In one embodiment, the dried second powder can be placed in a tubular furnace filled with protective gas for calcination to obtain a carbon fluoride-coated silicon-based negative electrode material.

[0035] The method for preparing a negative electrode material for a lithium-ion battery in the embodiment of the present application can form a carbon fluoride coating layer on the surface of the silicon-based negative electrode material for the lithium-ion battery, perform interface modification on the silicon-based negative electrode material for the lithium-ion battery, improve the interface stability between the silicon-based negative electrode material and the electrolyte, inhibit the side reaction between the silicon-based negative electrode material and the electrolyte, inhibit the volume expansion of the silicon-based negative electrode material, and improve the cycle stability and cycle performance of the lithium-ion battery.

[0036] Figure 2 It is another schematic diagram of the process of preparing negative electrode materials for lithium-ion batteries shown in the embodiment of the present application.

[0037] See also Figure 2 , a method for preparing a negative electrode material for a lithium ion battery, comprising: Step 201, mixing a polyhydroxy substance with ethanol to obtain a polyhydroxy solution.

[0038] In one embodiment, the polyhydroxy substance may be a polyhydroxy alcohol or a polyhydroxy aldehyde. The polyhydroxy substance and ethanol may be used to prepare a polyhydroxy solution, wherein the polyhydroxy alcohol or the polyhydroxy aldehyde is dissolved in the ethanol and stirred to mix uniformly to obtain a polyhydroxy solution; wherein the concentration of the polyhydroxy substance in the polyhydroxy solution is 0.25 mol / L (mole per liter) to 2 mol / L.

[0039] In one embodiment, the molecules of polyhydroxy alcohol and polyhydroxy aldehyde both contain multiple hydroxyl groups. The general chemical formula of polyhydroxy alcohol is C n H 2n+2 O x The general chemical formula of polyhydroxy aldehyde is C n (H2O) m, where x, n and m are different integers, n represents the length of the carbon chain, and x represents the number of hydroxyl groups. Polyhydroxy alcohols can be ethylene glycol (abbreviated as EG, with a chemical formula of (CH2OH)2), glycerol (also known as glycerol, with a chemical formula of C3H8O3), sorbitol (chemical formula of C6H 14 O6), pentaerythritol (chemical formula is C5H 12 O4) or more. The polyhydroxy aldehyde may be glucose (chemical formula C6H 12 O6), fructose (chemical formula is C6H 12 O6), mannose (chemical formula is C6H 12 O6), galactose (chemical formula is C6H 12 O6) or more.

[0040] Step 202 , mixing the silicon-based negative electrode material with the polyhydroxy solution to obtain a silicon-based negative electrode material suspension.

[0041] In one embodiment, the silicon-based negative electrode material can be mixed with the polyhydroxy solution to obtain a silicon-based negative electrode material suspension. The silicon-based negative electrode material can be added to the polyhydroxy solution and stirred by magnetic stirring to obtain a silicon-based negative electrode material suspension; wherein the silicon-based negative electrode material can be a silicon-carbon negative electrode material (SiC) or a silicon-oxygen negative electrode material (SiO).

[0042] Step 203, filtering the silicon-based negative electrode material suspension to obtain a first powder, and calcining the first powder to obtain a carbon-coated silicon-based negative electrode material.

[0043] In one embodiment, the first powder in the silicon-based negative electrode material suspension can be collected by filtration, and the first powder is calcined according to a first calcination process. The first powder after calcination is a carbon-coated silicon-based negative electrode material with a carbon coating layer.

[0044] In a specific embodiment, the first powder can be calcined in a muffle furnace to obtain a carbon-coated silicon-based negative electrode material with a carbon coating layer; wherein the temperature of the muffle furnace is 200°C (degrees Celsius)-300°C, and the calcination holding time is 2 hours-4 hours.

[0045] In one embodiment, the concentration ratio of the silicon-based negative electrode material in the silicon-based negative electrode material suspension, the concentration of the fluorine source in the fluorine source solution, and the concentration of the polyhydroxy substance in the polyhydroxy solution is 1: (0.25-4): (0.25-4). In a specific embodiment, the mass of the silicon-based negative electrode material in the silicon-based negative electrode material suspension can be calculated according to the concentration of the polyhydroxy substance in the polyhydroxy solution, so that the silicon-based negative electrode material added to the polyhydroxy solution has enough polyhydroxy substances to form a carbon coating layer on the surface of the silicon-based negative electrode material, thereby obtaining a carbon-coated silicon-based negative electrode material having a carbon coating layer.

[0046] Step 204 , mixing the carbon-coated silicon-based negative electrode material with ethanol to obtain a first suspension.

[0047] In one embodiment, the calcined first powder can be cooled to room temperature (25°C), the cooled first powder is added to ethanol, and stirred by magnetic stirring to obtain a first suspension; wherein the concentration of the first powder (carbon-coated silicon-based negative electrode material) in the first suspension is 0.5 mol / L-1 mol / L.

[0048] Step 205: Mix the fluorine source and ethanol to obtain a fluorine source solution.

[0049] In one embodiment, a fluorine source and ethanol can be used to prepare a fluorine source solution. The fluorine source is added to the ethanol to dissolve the fluorine source in the ethanol, and the mixture is stirred to obtain a fluorine source solution; wherein the fluorine source can be ammonium fluoride or 1-butyl-3-methylimidazolium tetrafluoroborate, and the concentration of the fluorine source in the fluorine source solution is 0.25 mol / L-2 mol / L.

[0050] In one embodiment, the mass of the carbon-coated silicon-based negative electrode material in the first suspension can be calculated according to the concentration of the carbon-coated silicon-based negative electrode material in the first suspension; the mass of the fluorine source required to obtain the fluorinated carbon-coated silicon-based negative electrode material having a fluorinated carbon coating layer can be calculated according to the mass of the carbon-coated silicon-based negative electrode material in the first suspension; and the fluorine source solution can be prepared according to the mass of the required fluorine source and the concentration of the fluorine source in the fluorine source solution.

[0051] In one embodiment, the ethanol may be anhydrous ethanol with a concentration of 99.5%.

[0052] In another embodiment, the mass of the polyhydroxy substance required to obtain the carbon-coated silicon-based negative electrode material and the concentration of the polyhydroxy substance in the polyhydroxy solution can be calculated according to the mass of the silicon-based negative electrode material to prepare the polyhydroxy solution; the mass of the fluorine source required to obtain the fluorinated carbon-coated silicon-based negative electrode material can be calculated according to the mass of the silicon-based negative electrode material; the fluorine source solution can be prepared according to the mass of the fluorine source required to obtain the fluorinated carbon-coated silicon-based negative electrode material and the concentration of the fluorine source in the fluorine source solution.

[0053] Step 206 , mixing the first suspension with the fluorine source solution to obtain a second suspension.

[0054] In one embodiment, the fluorine source solution may be added dropwise into the first suspension to make the fluorine source in the fluorine source solution more evenly dispersed in the first suspension, and stirred and mixed to obtain the second suspension.

[0055] Step 207, performing a solvothermal treatment on the second suspension.

[0056] In one embodiment, the second suspension may be subjected to a solvent thermal treatment in a hydrothermal kettle or a hydrothermal box; wherein the temperature of the solvent thermal treatment is 120° C.-180° C., and the insulation time is 4 hours-12 hours.

[0057] Step 208, filtering the second suspension after the solvent thermal treatment to obtain a second powder, and drying the second powder.

[0058] In one embodiment, the second suspension after solvent thermal treatment can be cooled to room temperature, the second powder in the second suspension can be collected by suction filtration, and the second powder can be dried in a vacuum oven; wherein the temperature of the vacuum oven is 60°C-120°C.

[0059] Step 209, calcining the dried second powder to obtain a carbon fluoride-coated silicon-based negative electrode material.

[0060] In one embodiment, the dried second powder can be calcined under the protection of a protective gas to obtain a carbon fluoride-coated silicon-based negative electrode material; wherein the calcination temperature is 300°C-600°C, the heating rate is 5°C / min-10°C / min, and the calcination time is 6 hours-12 hours.

[0061] In a specific embodiment, the dried second powder can be placed in a tubular furnace filled with argon atmosphere for calcination and carbonization to remove impurities, thereby obtaining a carbon fluoride-coated silicon-based negative electrode material with a carbon fluoride coating layer; wherein the calcination temperature in the tubular furnace is 300°C-600°C, the heating rate is 5°C / min (degrees Celsius per minute)-10°C / min, and the calcination holding time is 6 hours-12 hours.

[0062] The method for preparing the negative electrode material for a lithium-ion battery of an embodiment of the present application first utilizes multiple hydroxyl groups of a polyhydroxy alcohol or a polyhydroxy aldehyde to combine the polyhydroxy alcohol or the polyhydroxy aldehyde with a silicon-based negative electrode material through hydrogen bonds through the strong hydrogen bonding of the multiple hydroxyl groups, thereby obtaining a carbon-coated silicon-based negative electrode material having a carbon coating layer, thereby achieving uniform and stable carbon coating on the surface of the silicon-based negative electrode material, and making the carbon coating layer rich in hydroxyl functional groups; then utilizing a solvent thermal reaction to incorporate a fluorine source into the carbon coating layer, and under high temperature and high pressure conditions, the fluorine in the fluorine source more easily replaces the hydroxyl group to form a fluorinated functional group, which is then riveted to the carbon layer; and calcining in a tubular furnace and oxidizing to remove impurities to obtain a product such as Figure 3 The carbon fluoride coated silicon-based negative electrode material shown in the figure comprises a carbon fluoride coating layer 301 and a silicon-based negative electrode material 302 coated by the carbon fluoride coating layer 301; the carbon coating layer of the carbon fluoride coating layer 301 can not only enhance the conductivity of the silicon-based negative electrode material 302, but also inhibit the side reaction between the silicon-based negative electrode material 302 and the electrolyte; secondly, as Figure 4As shown, due to the presence of fluorinated functional groups, during the electrode activation process, the surface of the fluorinated carbon coating layer 301 can form a solid electrolyte membrane (SEI membrane) 401 rich in LiF (lithium fluoride), and the LiF-rich SEI membrane 401 not only has a faster lithium ion transmission speed, but also has a higher interfacial energy, and can even out the lithium ion flux; and the LiF-rich SEI membrane 401 also has good flexibility, and can inhibit the volume expansion of the silicon-based negative electrode material 302 during the charging and discharging process; the lithium-ion battery using the fluorinated carbon-coated silicon-based negative electrode material with the fluorinated carbon coating layer 301 has excellent electrochemical properties, and the fluorinated carbon-coated silicon-based negative electrode material with the fluorinated carbon coating layer 301 can improve the cycle stability and cycle performance of the lithium-ion battery.

[0063] The method for preparing anode materials for lithium-ion batteries in the embodiments of the present application can obtain a carbon fluoride-coated silicon-based cathode material having a carbon fluoride coating layer, can form a carbon fluoride coating layer on the surface of the silicon-based cathode material for lithium-ion batteries, perform interface modification on the silicon-based cathode material for lithium-ion batteries, improve the interface stability between the silicon-based cathode material and the electrolyte, inhibit the side reaction between the silicon-based cathode material and the electrolyte, inhibit the volume expansion of the silicon-based cathode material during the charging and discharging process, improve the cycle stability and cycle performance of the lithium-ion battery, solve the key technical problems such as volume expansion and poor cycle stability faced by silicon-based cathode materials in related technologies, and contribute to the advancement of lithium-ion battery technology.

[0064] The method for preparing a negative electrode material for a lithium-ion battery of an embodiment of the present application can obtain a carbon fluoride-coated silicon-based negative electrode material having a carbon fluoride coating layer. The process for forming the carbon fluoride coating layer is relatively simple and can be easily applied to large-scale production. Moreover, the materials for forming the carbon fluoride coating layer include polyhydroxy alcohols or polyhydroxy aldehydes, ethanol, ammonium fluoride or 1-butyl-3-methylimidazolium tetrafluoroborate, which are easy to obtain and relatively low in price. The preparation of the carbon fluoride-coated silicon-based negative electrode material having a carbon fluoride coating layer will not significantly increase the manufacturing cost and environmental cost of the lithium-ion battery.

[0065] The invention is further described below by means of specific Examples 1-8 and Comparative Examples 1-4.

[0066] Embodiment 1: In Example 1, the concentration ratio of the silicon-carbon negative electrode material in the silicon-carbon negative electrode material suspension, the concentration of pentaerythritol in the polyhydroxy solution, and the concentration of ammonium fluoride in the fluorine source solution is 1:0.8:1.6. 6.8 g of pentaerythritol (C5H 12O4) is added to 100 ml (milliliter) ethanol, and after stirring for 30 minutes (minutes) on a magnetic stirrer (speed of 500 rpm), a polyhydroxy solution is obtained; then 2.5 g of silicon-carbon negative electrode material (SiC) is added to the polyhydroxy solution, mixed and stirred for 2 hours to form a silicon-carbon negative electrode material suspension; the silicon-carbon negative electrode material suspension is filtered to obtain a first powder, and then the wet first powder is calcined in a muffle furnace at 250°C for 2 hours to obtain a calcined first powder, and the calcined first powder is a carbon-coated silicon-carbon negative electrode material rich in hydroxyl groups and has a carbon coating layer; the calcined first powder is added to 50 ml of ethanol and continuously magnetically stirred. The mixture was stirred for 2 hours to obtain a first suspension; 1.85 g of ammonium fluoride was added to 50 ml of ethanol and stirred for 30 min to obtain a fluorine source solution; the fluorine source solution was added dropwise to the first suspension using a rubber-tipped dropper and stirred for 2 hours to obtain a second suspension; the second suspension was transferred to a 100 ml hydrothermal kettle for solvent thermal treatment, the temperature was set to 150 ° C, and the insulation time was 6 hours; after the second suspension after solvent thermal treatment was cooled to room temperature, the second powder in the second suspension was collected by filtration, and the second powder was placed in a vacuum oven at 100 ° C for drying; finally, the dried second powder was placed in a tubular furnace filled with argon atmosphere for calcination at a calcination temperature of 450 ° C, a heating rate of 8 ° C / min, and calcination for 6 hours to carbonize and remove impurities, and finally a fluorinated carbon-coated silicon-carbon negative electrode material with a fluorinated carbon coating layer was obtained, which was named FC-SiC-1.

[0067] FC-SiC-1: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um (micrometer) copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm (millimeter) diameter and a surface density of 1.2 mg / cm 2 (milligrams per square centimeter) ~ 1.5 mg / cm 2 The negative electrode.

[0068] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. Half-cell A1 was assembled in a glove box. The electrolyte of half-cell A1 was 1 mol / L (mole per liter) lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0069] Embodiment 2: In Example 2, the concentration ratio of the silicon-carbon negative electrode material in the silicon-carbon negative electrode material suspension, the concentration of pentaerythritol in the polyhydroxy solution, and the concentration of ammonium fluoride in the fluorine source solution is 1:0.25:0.25. 12 O4) was added to 100 ml of ethanol, and after stirring for 30 minutes with a magnetic stirrer (speed of 500 rpm), a polyhydroxy solution was obtained; then 2.5 g of silicon-carbon negative electrode material (SiC) was added to the polyhydroxy solution, mixed and stirred for 2 hours to form a silicon-carbon negative electrode material suspension; the silicon-carbon negative electrode material suspension was filtered to obtain a first powder, and then the wet first powder was calcined in a muffle furnace at 250°C for 2 hours to obtain a calcined first powder, and the calcined first powder was a carbon-coated silicon-carbon negative electrode material rich in hydroxyl groups and having a carbon coating layer; the calcined first powder was added to 50 ml of ethanol and magnetic stirring was continued for 2 hours. A first suspension was obtained; 0.289 g of ammonium fluoride was added to 50 ml of ethanol and stirred for 30 min to obtain a fluorine source solution; the fluorine source solution was added dropwise to the first suspension using a rubber-tipped dropper and stirred for 2 hours to obtain a second suspension; the second suspension was transferred to a 100 ml hydrothermal kettle for solvent thermal treatment, the temperature was set to 150°C, and the insulation time was 6 hours; after the second suspension after solvent thermal treatment was cooled to room temperature, the second powder in the second suspension was collected by suction filtration, and the second powder was placed in a vacuum oven at 100°C for drying; finally, the dried second powder was placed in a tubular furnace filled with argon atmosphere for calcination, the calcination temperature was 450°C, the heating rate was 8°C / min, and the calcination was performed for 6 hours to carbonize and remove impurities, and finally a fluorinated carbon-coated silicon-carbon negative electrode material with a fluorinated carbon coating layer was obtained, which was named FC-SiC-2.

[0070] FC-SiC-2: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0071] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. Half-cell A2 was assembled in a glove box. The electrolyte of half-cell A2 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0072] Embodiment 3: In Example 3, the concentration ratio of the silicon-carbon negative electrode material in the silicon-carbon negative electrode material suspension, the concentration of pentaerythritol in the polyhydroxy solution, and the concentration of ammonium fluoride in the fluorine source solution is 1:4:0.25. 12 O4) was added to 100 ml of ethanol, and after stirring for 30 minutes with a magnetic stirrer (speed of 500 rpm), a polyhydroxy solution was obtained; then 2.5 g of silicon-carbon negative electrode material (SiC) was added to the polyhydroxy solution, mixed and stirred for 2 hours to form a silicon-carbon negative electrode material suspension; the silicon-carbon negative electrode material suspension was filtered to obtain a first powder, and then the wet first powder was calcined in a muffle furnace at 250°C for 2 hours to obtain a calcined first powder, and the calcined first powder was a carbon-coated silicon-carbon negative electrode material rich in hydroxyl groups and having a carbon coating layer; the calcined first powder was added to 50 ml of ethanol and magnetic stirring was continued for 2 hours. A first suspension was obtained; 0.289 g of ammonium fluoride was added to 50 ml of ethanol and stirred for 30 min to obtain a fluorine source solution; the fluorine source solution was added dropwise to the first suspension using a rubber-tipped dropper and stirred for 2 hours to obtain a second suspension; the second suspension was transferred to a 100 ml hydrothermal autoclave for solvent thermal treatment, the temperature was set to 150°C, and the insulation time was 6 hours; after the second suspension was cooled to room temperature after solvent thermal treatment, the second powder in the second suspension was collected by suction filtration, and the second powder was placed in a vacuum oven at 100°C for drying; finally, the dried second powder was placed in a tubular furnace filled with argon atmosphere for calcination, the calcination temperature was 450°C, the heating rate was 8°C / min, and the calcination was performed for 6 hours to carbonize and remove impurities, and finally a fluorinated carbon-coated silicon-carbon negative electrode material with a fluorinated carbon coating layer was obtained, which was named FC-SiC-3.

[0073] FC-SiC-3: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0074] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. Half-cell A3 was assembled in a glove box. The electrolyte of half-cell A3 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0075] Embodiment 4: In Example 4, the concentration ratio of the silicon-carbon negative electrode material in the silicon-carbon negative electrode material suspension, the concentration of pentaerythritol in the polyhydroxy solution, and the concentration of ammonium fluoride in the fluorine source solution is 1:0.25:4. 12 O4) was added to 100 ml of ethanol, and stirred for 30 minutes on a magnetic stirrer (speed of 500 rpm) to obtain a polyhydroxy solution; then 2.5 g of silicon-carbon negative electrode material (SiC) was added to the polyhydroxy solution, mixed and stirred for 2 hours to form a silicon-carbon negative electrode material suspension; the silicon-carbon negative electrode material suspension was filtered to obtain a first powder, and then the wet first powder was calcined in a muffle furnace at 250°C for 2 hours to obtain a calcined first powder, and the calcined first powder was a carbon-coated silicon-carbon negative electrode material rich in hydroxyl groups and having a carbon coating layer; the calcined first powder was added to 50 ml of ethanol and magnetically stirred for 2 hours. , obtain a first suspension; add 4.625g of ammonium fluoride to 50ml of ethanol and stir for 30min to obtain a fluorine source solution; use a rubber-tipped dropper to add the fluorine source solution dropwise to the first suspension, stir for 2 hours, and obtain a second suspension; transfer the second suspension to a 100ml hydrothermal kettle for solvent thermal treatment, set the temperature to 150℃, and keep warm for 6 hours; after the second suspension after solvent thermal treatment is cooled to room temperature, filter and collect the second powder in the second suspension, and place the second powder in a vacuum oven at 100℃ for drying; finally, place the dried second powder in a tubular furnace filled with argon atmosphere for calcination, the calcination temperature is 450℃, the heating rate is 8℃ / min, and the calcination is 6 hours, carbonization is carried out and impurities are removed, and finally a fluorinated carbon-coated silicon-carbon negative electrode material with a fluorinated carbon coating layer is obtained, which is named FC-SiC-4.

[0076] FC-SiC-4: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0077] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. Half-cell A4 was assembled in a glove box. The electrolyte of half-cell A4 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0078] Embodiment 5: In Example 5, the concentration ratio of the silicon-carbon negative electrode material in the silicon-carbon negative electrode material suspension, the concentration of pentaerythritol in the polyhydroxy solution, and the concentration of ammonium fluoride in the fluorine source solution is 1:4:4. 12 O4) was added to 100 ml of ethanol, and after stirring for 30 minutes with a magnetic stirrer (speed of 500 rpm), a polyhydroxy solution was obtained; then 2.5 g of silicon-carbon negative electrode material (SiC) was added to the polyhydroxy solution, mixed and stirred for 2 hours to form a silicon-carbon negative electrode material suspension; the silicon-carbon negative electrode material suspension was filtered to obtain a first powder, and then the wet first powder was calcined in a muffle furnace at 250°C for 2 hours to obtain a calcined first powder, and the calcined first powder was a carbon-coated silicon-carbon negative electrode material rich in hydroxyl groups and having a carbon coating layer; the calcined first powder was added to 50 ml of ethanol and magnetic stirring was continued for 2 hours. A first suspension was obtained; 4.625 g of ammonium fluoride was added to 50 ml of ethanol and stirred for 30 min to obtain a fluorine source solution; the fluorine source solution was added dropwise to the first suspension using a rubber-tipped dropper and stirred for 2 hours to obtain a second suspension; the second suspension was transferred to a 100 ml hydrothermal autoclave for solvent thermal treatment, the temperature was set to 150°C, and the insulation time was 6 hours; after the second suspension was cooled to room temperature after solvent thermal treatment, the second powder in the second suspension was collected by suction filtration, and the second powder was placed in a vacuum oven at 100°C for drying; finally, the dried second powder was placed in a tubular furnace filled with argon atmosphere for calcination, the calcination temperature was 450°C, the heating rate was 8°C / min, and the calcination was performed for 6 hours to carbonize and remove impurities, and finally a fluorinated carbon-coated silicon-carbon negative electrode material with a fluorinated carbon coating layer was obtained, which was named FC-SiC-5.

[0079] FC-SiC-5: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0080] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. Half-cell A5 was assembled in a glove box. The electrolyte of half-cell A5 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0081] Half-cells A1-A5 were electrochemically tested at room temperature (25°C). The charge and discharge regime was 0.1C / 0.1C for the first 3 weeks, followed by 0.5C / 0.5C for 200 weeks. The voltage range was 0.005V-2V, and 1C=1800 mA / g.

[0082] Embodiment 6: In Example 6, the concentration ratio of the silicon oxide negative electrode material in the silicon oxide negative electrode material suspension, the concentration of pentaerythritol in the polyhydroxy solution, and the concentration of ammonium fluoride in the fluorine source solution is 1:0.8:1.6. 6.8 g of pentaerythritol (C5H 12 O4) was added to 100 ml of ethanol, and after stirring for 30 minutes with a magnetic stirrer (speed of 500 rpm), a polyhydroxy solution was obtained; then 3.75 g of silicon oxide negative electrode material (SiO) was added to the polyhydroxy solution, mixed and stirred for 2 hours to form a silicon oxide negative electrode material suspension; the silicon oxide negative electrode material suspension was filtered to obtain a first powder, and then the wet first powder was calcined in a muffle furnace at 250°C for 2 hours to obtain a calcined first powder, and the calcined first powder was a carbon-coated silicon oxide negative electrode material rich in hydroxyl groups and having a carbon coating layer; the calcined first powder was added to 50 ml of ethanol and continuously magnetically stirred for 2 hours. to obtain a first suspension; 1.85 g of ammonium fluoride was added to 50 ml of ethanol and stirred for 30 min to obtain a fluorine source solution; the fluorine source solution was added dropwise to the first suspension using a rubber-tipped dropper and stirred for 2 hours to obtain a second suspension; the second suspension was transferred to a 100 ml hydrothermal kettle for solvent thermal treatment, the temperature was set to 150 ° C, and the time was 6 hours; after the second suspension after solvent thermal treatment was cooled to room temperature, the second powder in the second suspension was collected by suction filtration, and the second powder was placed in a vacuum oven at 100 ° C for drying; finally, the dried second powder was placed in a tubular furnace filled with argon atmosphere for calcination, the calcination temperature was 450 ° C, the heating rate was 8 ° C / min, and the calcination was 6 hours, carbonization was carried out and impurities were removed, and finally a fluorinated carbon-coated silicon oxygen negative electrode material with a fluorinated carbon coating layer was obtained, which was named FC-SiO.

[0083] FC-SiO: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare a negative electrode slurry. The negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0084] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was an 18 um thick polypropylene (PP) separator. Half-cell A6 was assembled in a glove box. The electrolyte of half-cell A6 was 1 mol / L (mole per liter) lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0085] Half-cell A6 was electrochemically tested at room temperature with a charge and discharge regime of 0.1C / 0.1C for the first 3 weeks, followed by 0.5C / 0.5C for 200 cycles, with a voltage range of 0.005 V -2 V and 1C=1500 mA / g.

[0086] Embodiment 7: In Example 7, the concentration of the silicon-carbon negative electrode material in the silicon-carbon negative electrode material suspension, the concentration of glucose in the polyhydroxy solution, and the concentration of 1-butyl-3-methylimidazolium tetrafluoroborate (C8H 15 N2BF4) concentration ratio is 1:0.8:0.85. 9g glucose (C6H 12 O6, polyhydroxy aldehyde) is added to 100 ml of ethanol, and after stirring for 30 minutes on a magnetic stirrer (speed of 500 rpm), a polyhydroxy solution is obtained; then 2.5 g of silicon-carbon negative electrode material (SiC) is added to the polyhydroxy solution, mixed and stirred for 2 hours to form a silicon-carbon negative electrode material suspension; the silicon-carbon negative electrode material suspension is filtered to obtain a first powder, and then the wet first powder is calcined in a muffle furnace at 200°C for 3 hours to obtain a calcined first powder, and the calcined first powder is a carbon-coated silicon-carbon negative electrode material rich in hydroxyl groups and having a carbon coating layer; the calcined first powder is added to 50 ml of ethanol, and magnetic stirring is continued for 2 hours to obtain a first suspension; 6 g of 1-butyl-3-methylimidazole tetrafluoroborate is added to 50 ml of ethanol and stirred for 30 minutes to obtain a fluorine source solution; a rubber-tipped dropper is used to drop the fluorine source solution dropwise Add it to the first suspension and stir for 2 hours to obtain a second suspension; transfer the second suspension to a 100 ml hydrothermal autoclave for solvent thermal treatment, set the temperature to 180°C, and the time to 8 hours; after the second suspension after solvent thermal treatment is cooled to room temperature, filter and collect the second powder in the second suspension, and place the second powder in a vacuum oven at 80°C for drying; finally, place the dried second powder in a tubular furnace filled with argon atmosphere for calcination at a calcination temperature of 600°C, a heating rate of 5°C / min, and calcination for 6 hours to carbonize and remove impurities, and finally obtain a fluorinated carbon-coated silicon-carbon negative electrode material with a fluorinated carbon coating layer, which is named FC-SiC-7.

[0087] FC-SiC-7: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0088] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. The half-cell A7 was assembled in a glove box. The electrolyte of the half-cell A7 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0089] Embodiment 8: In Example 8, the concentration ratio of the silicon-carbon negative electrode material in the silicon-carbon negative electrode material suspension, the concentration of sorbitol in the polyhydroxy solution, and the concentration of 1-butyl-3-methylimidazolium tetrafluoroborate in the fluorine source solution is 1:0.8:0.85. 14 O6) was added to 100 ml of ethanol, and stirred for 30 minutes on a magnetic stirrer (speed of 500 rpm) to obtain a polyhydroxy solution; then 2.5 g of silicon-carbon negative electrode material (SiC) was added to the polyhydroxy solution, mixed and stirred for 2 hours to form a silicon-carbon negative electrode material suspension; the silicon-carbon negative electrode material suspension was filtered to obtain a first powder, and then the wet first powder was calcined in a muffle furnace at 250°C for 2.5 hours to obtain a calcined first powder, and the calcined first powder was a carbon-coated silicon-carbon negative electrode material rich in hydroxyl groups and having a carbon coating layer; the calcined first powder was added to 50 ml of ethanol, and magnetic stirring was continued for 2 hours to obtain a first suspension; 6 g of 1-butyl-3-methylimidazole tetrafluoroborate was added to 50 ml of ethanol and stirred for 30 minutes to obtain a fluorine source solution; a rubber-tipped dropper was used to drop the fluorine source solution dropwise The reaction mixture was added into the first suspension and stirred for 2 hours to obtain a second suspension; the second suspension was transferred to a 100 ml hydrothermal autoclave for solvent thermal treatment, the temperature was set to 140°C, and the time was 6 hours; after the second suspension after solvent thermal treatment was cooled to room temperature, the second powder in the second suspension was collected by filtration, and the second powder was placed in a vacuum oven at 120°C for drying; finally, the dried second powder was placed in a tubular furnace filled with argon atmosphere for calcination, the calcination temperature was 400°C, the heating rate was 10°C / min, and the calcination was carried out for 12 hours to carbonize and remove impurities, and finally a fluorinated carbon-coated silicon-carbon negative electrode material with a fluorinated carbon coating layer was obtained, which was named FC-SiC-8.

[0090] FC-SiC-8: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0091] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. The half-cell A8 was assembled in a glove box. The electrolyte of the half-cell A8 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0092] Half-cells A7-A8 were electrochemically tested at room temperature. The charge and discharge regime was 0.1C / 0.1C for the first 3 weeks, followed by 0.5C / 0.5C for 200 cycles. The voltage range was 0.005 V -2 V, and 1C=1800 mA / g.

[0093] Comparative Example 1: In Comparative Example 1, SiC: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare a negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 hours, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0094] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. The half-cell B1 was assembled in a glove box. The electrolyte of the half-cell B1 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0095] Half-cell B1 was electrochemically tested at room temperature with a charge and discharge regime of 0.1C / 0.1C for the first 3 weeks, followed by 0.5C / 0.5C for 200 cycles, with a voltage range of 0.005 V -2 V and 1C=1800 mA / g.

[0096] Comparative Example 2: In Comparative Example 2, 6.8 g of pentaerythritol (C5H 12 O4) is added to 100 ml of ethanol, and after stirring for 30 minutes with a magnetic stirrer (speed of 500 rpm), a polyhydroxy solution is obtained; then 2.5 g of silicon-carbon negative electrode material (SiC) is added to the polyhydroxy solution, and the mixture is mixed and stirred for 2 hours to form a silicon-carbon negative electrode material suspension; the silicon-carbon negative electrode material suspension is filtered to obtain a first powder, and then the wet first powder is calcined in a muffle furnace at 250°C for 2 hours to obtain a calcined first powder; finally, the calcined first powder is placed in a tubular furnace filled with argon atmosphere for calcination at a calcination temperature of 450°C, a heating rate of 8°C / min, and a calcination time of 6 hours to carbonize and remove impurities, and finally a carbon-coated silicon-carbon negative electrode material with a carbon coating layer is obtained, which is named C-SiC.

[0097] C-SiC: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80 °C for 12 h, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode.

[0098] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. The half-cell B2 was assembled in a glove box. The electrolyte of the half-cell B2 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0099] Half-cell B2 was electrochemically tested at room temperature with a charge and discharge regime of 0.1C / 0.1C for the first 3 weeks, followed by 0.5C / 0.5C for 200 cycles, with a voltage range of 0.005 V -2 V and 1C=1800 mA / g.

[0100] Comparative Example 3: In Comparative Example 3, SiO2: carbon black: lithium carboxymethyl cellulose (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare a negative electrode slurry; the negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80°C for 12 h, and then compacted using a roller press and punched into a sheet with a diameter of 12 mm and a surface density of 1.2 mg / cm 2 ~1.5mg / cm 2 The negative electrode.

[0101] The negative electrode was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. Half-cell B3 was assembled in a glove box. The electrolyte of half-cell B3 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0102] Half-cell B3 was electrochemically tested at room temperature with a charge and discharge regime of 0.1C / 0.1C for the first 3 weeks, followed by 0.5C / 0.5C for 200 cycles, with a voltage range of 0.005 V -2 V and 1C=1500 mA / g.

[0103] Comparative Example 4: In Comparative Example 4, 6.8 g of pentaerythritol (C5H 12 O4) was added to 100 ml of ethanol and stirred for 30 minutes on a magnetic stirrer (speed of 500 rpm) to obtain a polyhydroxy solution; then 3.75 g of silicon oxide negative electrode material (SiO) was added to the polyhydroxy solution and stirred for 2 hours to form a silicon oxide negative electrode material suspension; the silicon oxide negative electrode material suspension was filtered to obtain a first powder, and then the wet first powder was calcined in a muffle furnace at 250°C for 2 hours, and finally the first powder was placed in a tubular furnace filled with argon atmosphere for calcination at a calcination temperature of 450°C, a heating rate of 8°C / min, and calcination for 6 hours to carbonize and remove impurities to obtain a carbon-coated silicon oxide negative electrode material with a carbon coating layer, which was named C-SiO.

[0104] C-SiO: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 to prepare the negative electrode slurry. The negative electrode slurry was evenly coated on a 10 um copper foil, dried in a vacuum oven at 80 °C for 12 h, and then compacted using a roller press and punched into a 12 mm diameter and 1.2 mg / cm surface density copper foil. 2 ~1.5 mg / cm 2 The negative electrode sheet was used as the working electrode, lithium metal as the counter electrode, and the separator was a 18 um thick polypropylene (PP) separator. The half-cell B4 was assembled in a glove box. The electrolyte of the half-cell B4 was a 1 mol / L lithium hexafluorophosphate (LiPF6) solution, and the solvent of the electrolyte was ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0105] Half-cell B4 was electrochemically tested at room temperature with a charge and discharge regime of 0.1C / 0.1C for the first 3 weeks, followed by 0.5C / 0.5C for 200 cycles, with a voltage range of 0.005 V -2 V and 1C=1500 mA / g.

[0106] The test data of the electrochemical tests of half-cells A1-A8 and half-cells B1-B4 are shown in Tables 1 and Figure 5 shown.

[0107] Table 1:

[0108] See Table 1 and Figure 5 The capacity retention rate after 200 cycles of the half-cells A1-A8 corresponding to Examples 1-8 is significantly better than the capacity retention rate after 200 cycles of the half-cells B1-B4 corresponding to Comparative Examples 1-4. The half-cells A1-A8 using the carbon fluoride coated silicon-based negative electrode material having a carbon fluoride coating layer have excellent electrochemical properties. The battery cycle stability and cycle performance of the half-cells A1-A8 are improved. The lithium-ion battery using the carbon fluoride coated silicon-based negative electrode material having a carbon fluoride coating layer can improve the cycle stability and cycle performance of the lithium-ion battery.

[0109] Referring to Table 1, according to the capacity retention rates after 200 cycles of half-cells A1-A8 corresponding to Examples 1-8, half-cell B2 corresponding to Comparative Example 2, and half-cell B4 corresponding to Comparative Example 4, a carbon coating layer is formed on the surface of the silicon-based negative electrode material using a polyhydroxy substance. Although the carbon coating layer can avoid the contact between the silicon-based negative electrode material and the electrolyte, inhibit the side reaction between the silicon-based negative electrode material and the electrolyte, and improve the capacity retention rates after 200 cycles of the half-cells B2 corresponding to Comparative Example 2 and the half-cell B4 corresponding to Comparative Example 4, the capacity retention rates after 200 cycles of the half-cells A1-A8 corresponding to Examples 1-8 using the fluorinated carbon coated silicon-based negative electrode material having a fluorinated carbon coating layer are significantly better than the capacity retention rates after 200 cycles of the half-cells B2 corresponding to Comparative Example 2 and the half-cells B4 corresponding to Comparative Example 4. Therefore, a fluorinated carbon coating is formed on the surface of the silicon-based negative electrode material, and half-cell A1 of the fluorinated carbon coated silicon-based negative electrode material having a fluorinated carbon coating layer is used. -A8, has more excellent electrochemical properties, the battery cycle stability and cycle performance of half-cell A1-A8 have been significantly improved, and the lithium-ion battery uses a carbon-fluorinated silicon-based negative electrode material with a carbon-fluorinated coating layer, which can significantly improve the cycle stability and cycle performance of the lithium-ion battery.

[0110] Referring to Table 1, the capacity retention rate after 200 cycles of the half-cells A2-A5 corresponding to Examples 2-5 is significantly better than the capacity retention rate after 200 cycles of the half-cells B1-B2 corresponding to Comparative Examples 1-2. When the concentration of the polyhydroxy substance in the polyhydroxy solution and the concentration of the fluorine source in the fluorine source solution are determined, the polyhydroxy solution has sufficient polyhydroxy substances and the fluorine source solution has sufficient fluorine sources, a fluorinated carbon coating layer can be formed on the surface of the silicon-based negative electrode material. The half-cells A2-A5 using the fluorinated carbon-coated silicon-based negative electrode material having the fluorinated carbon coating layer have excellent electrochemical properties, and the battery cycle stability and cycle performance of the half-cells A2-A5 are improved. The lithium-ion battery uses the fluorinated carbon-coated silicon-based negative electrode material having the fluorinated carbon coating layer to improve the cycle stability and cycle performance of the lithium-ion battery.

[0111] Referring to Table 1, according to the capacity retention rates after 200 cycles of the half-cells A2-A5 corresponding to Examples 2-5, the capacity retention rate after 200 cycles of the half-cell A4 corresponding to Example 4 is better than the capacity retention rate after 200 cycles of the half-cell A2 corresponding to Example 2, and the capacity retention rate after 200 cycles of the half-cell A5 corresponding to Example 5 is better than the capacity retention rate after 200 cycles of the half-cell A3 corresponding to Example 3. When the concentration of the polyhydroxy substance in the polyhydroxy solution is determined, that is, the mass of the polyhydroxy substance in the polyhydroxy solution is determined, the concentration of the fluorine source in the fluorine source solution is increased. The degree, that is, the quality of the fluorine source, can form a fluorinated carbon coating layer on the surface of the silicon-based negative electrode material, and the fluorinated carbon coating layer can have more fluorinated functional groups, so that the half-cells A4 and A5 using the fluorinated carbon coating layer of the carbon-coated silicon-based negative electrode material with more fluorinated functional groups have more excellent electrochemical properties, and the battery cycle stability and cycle performance of the half-cells A4 and A5 are further improved. The lithium-ion battery uses the fluorinated carbon coating layer of the carbon-coated silicon-based negative electrode material with more fluorinated functional groups, which can better improve the cycle stability and cycle performance of the lithium-ion battery.

[0112] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing a negative electrode material for a lithium ion battery, characterized in that: include: mixing the carbon-coated silicon-based negative electrode material with ethanol to obtain a first suspension; mixing the first suspension with a fluorine source solution to obtain a second suspension; subjecting the second suspension to a solvothermal treatment; filtering the second suspension after the solvent thermal treatment to obtain a second powder, and drying the second powder; The dried second powder is calcined to obtain a carbon fluoride-coated silicon-based negative electrode material.

2. The method according to claim 1, characterized in that: The fluorine source solution is obtained by mixing a fluorine source with ethanol, wherein the fluorine source is ammonium fluoride or 1-butyl-3-methylimidazolium tetrafluoroborate.

3. The method according to claim 1, characterized in that The step of subjecting the second suspension to solvothermal treatment comprises: The second suspension is subjected to solvent thermal treatment in a hydrothermal kettle or a hydrothermal box; wherein the temperature of the solvent thermal treatment is 120° C.-180° C., and the insulation time is 4 hours-12 hours.

4. The method according to claim 1, characterized in that The step of calcining the dried second powder to obtain a carbon fluoride-coated silicon-based negative electrode material comprises: The dried second powder is calcined under the protection of a protective gas to obtain a carbon fluoride-coated silicon-based negative electrode material; wherein the calcination temperature is 300°C-600°C, the heating rate is 5°C / min-10°C / min, and the calcination time is 6 hours-12 hours.

5. The method according to claim 2, characterized in that: Before the carbon-coated silicon-based negative electrode material is mixed with ethanol to obtain a first suspension, the method comprises: Mixing a silicon-based negative electrode material with a polyhydroxy solution to obtain a silicon-based negative electrode material suspension, wherein the silicon-based negative electrode material is a silicon-carbon negative electrode material or a silicon-oxygen negative electrode material; The silicon-based negative electrode material suspension is filtered to obtain a first powder, and the first powder is calcined to obtain a carbon-coated silicon-based negative electrode material.

6. The method according to claim 5, characterized in that The step of calcining the first powder to obtain a carbon-coated silicon-based negative electrode material comprises: The first powder is calcined in a muffle furnace to obtain a carbon-coated silicon-based negative electrode material; wherein the calcination temperature is 200° C.-300° C., and the calcination time is 2 hours-4 hours.

7. The method according to claim 5, characterized in that: The polyhydroxy substance is mixed with ethanol to obtain the polyhydroxy solution; wherein the polyhydroxy substance is polyhydroxy alcohol or polyhydroxy aldehyde.

8. The method according to claim 7, characterized in that: The concentration ratio of the silicon-based negative electrode material in the silicon-based negative electrode material suspension, the fluorine source in the fluorine source solution, and the polyhydroxy substance in the polyhydroxy solution is 1: (0.25-4): (0.25-4).

9. A negative electrode material for a lithium ion battery, characterized in that: The invention comprises a fluorinated carbon-coated silicon-based negative electrode material prepared by the method according to any one of claims 1 to 8.

10. A lithium ion battery, characterized in that: It comprises a negative electrode plate, wherein the negative electrode plate comprises the carbon fluoride-coated silicon-based negative electrode material according to claim 9, or comprises the carbon fluoride-coated silicon-based negative electrode material prepared by the method according to any one of claims 1-8.

Citation Information

Patent Citations

  • Modified silicon-carbon material as well as preparation method and application thereof

    CN111276675A

  • Silicon-based composite material as well as preparation method and application thereof

    CN113451561A

  • Negative electrode material and preparation method thereof, negative electrode plate and secondary battery

    CN115101731A

  • Preparation method and application of silicon fluoride carbon negative electrode material

    CN115799474A

  • Nano silicon-carbon composite material, preparation method thereof and lithium ion battery negative plate

    CN115939342A

Cited By

  • Surface modification method of silicon-carbon negative electrode material, modified silicon-carbon negative electrode material, negative electrode plate and lithium ion battery