Positive electrode active material and preparation method thereof, positive electrode plate, secondary battery and electric device
By controlling the structure of the spinel phase and rock salt phase of lithium nickel manganese oxide, combined with phosphate coating, the problem of side reactions between the cathode material and the electrolyte in lithium-ion batteries is solved, and the storage performance and cycle stability of the battery are improved. .
Patent Information
- Application Number
- CN202410957641.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-10-16
AI Technical Summary
In existing lithium-ion batteries, the spinel lithium nickel manganate cathode material undergoes side reactions with the electrolyte under high voltage, resulting in electrolyte consumption and capacity attenuation, and accelerating the capacity loss of the negative electrode and battery.
By controlling the I(111)/I(400) peak intensity ratio of the spinel phase in lithium nickel manganese oxide within the range of 2.5≤I(111)/I(400)≤4, the degree of preference for the (111) plane is improved and stability, combined with the control of the rock salt phase to reduce the oxidative decomposition of high-valent nickel, and through phosphate coating to capture HF and transition metal ions to inhibit their dissolution.
It significantly improves the storage performance and cycle stability of lithium-ion batteries, reduces the oxidative decomposition of the electrolyte and the dissolution of transition metal ions, and extends the service life of the battery.
Smart Images

Figure CN118738374A_ABST
Abstract
Description
[0001] Related Applications
[0002] This application is a divisional application of the Chinese patent application filed on October 16, 2023, with application number CN2023113319584, and entitled "Positive electrode active material and preparation method thereof, positive electrode sheet, secondary battery and electrical device", the full text of which is hereby incorporated by reference. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to a positive electrode active material and a preparation method thereof, a positive electrode sheet, a secondary battery and an electrical device. Background Art
[0004] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.
[0005] In recent years, as the application scope of secondary batteries represented by lithium-ion batteries has become more and more extensive, secondary batteries are widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. As secondary batteries have made great progress, higher requirements have been put forward for their cycle performance and storage performance. Summary of the invention
[0006] The present application provides a positive electrode active material and a preparation method thereof, a positive electrode plate, a secondary battery and an electrical device, which can improve the storage performance of the secondary battery.
[0007] In order to achieve the above-mentioned object, the first aspect of the present application provides a positive electrode active material, including an active substance, wherein the active substance includes lithium nickel manganese oxide, the lithium nickel manganese oxide contains a spinel phase, and the X-ray diffraction analysis spectrum of the lithium nickel manganese oxide has a first diffraction peak at a diffraction angle 2θ of 18°~19°, and a second diffraction peak at a diffraction angle 2θ of 44°~45°, the first diffraction peak corresponds to a crystal plane (111), and the second diffraction peak corresponds to a crystal plane (400); the peak intensity of the first diffraction peak is I (111) , the peak intensity of the second diffraction peak is 1 (400) , I (111) with I (400) Between: 2.5≤I (111) / I (400) ≤4.
[0008] The positive electrode active material provided by the present application includes a lithium nickel manganese oxide containing a spinel phase, wherein I (111) / I (400)When the ratio is controlled within the above range, the preference of the (111) plane can be improved, thereby improving the stacking quality of the (111) plane and thus improving the stability of the spinel phase. The more stable the spinel phase is, the slower the dissolution of transition metal ions (such as manganese ions) in lithium nickel manganese oxide is, and the slower the capacity loss rate of the negative electrode and the battery is, which is beneficial to improving the storage performance of the battery.
[0009] In some embodiments of the present application, the lithium nickel manganese oxide satisfies: 2.8≤I (111) / I (400) ≤3.8.
[0010] In some embodiments of the present application, the lithium nickel manganese oxide satisfies: 3.1≤I (111) / I (400) ≤3.6.
[0011] I (111) / I (400) Being within the above range is beneficial to further improve the stability of the spinel structure, thereby further reducing the dissolution of transition metal ions (such as manganese ions) in lithium nickel manganese oxide, thereby further improving the storage performance of the battery.
[0012] In some embodiments of the present application, the lithium nickel manganese oxide satisfies the chemical formula Li x M y Ni z Mn 2-y-z O 4-k , wherein 0.8≤x≤1.05, 0≤y≤0.2, 0.3≤z≤0.7, -0.1≤k≤0.5, and M includes one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W.
[0013] Lithium nickel manganese oxide satisfies the above chemical formula, and the content x of lithium element is within the above range, which can not only enhance the preference of (111) plane in the spinel structure and improve the stability of the spinel structure, but also ensure the proportion of active lithium ions in lithium nickel manganese oxide and the diffusion channel of active lithium ions, so that the positive electrode active material has sufficient cycle activity.
[0014] In some embodiments of the present application, the lithium nickel manganese oxide satisfies at least one of the following conditions:
[0015] (1) 0.85≤x≤1.02;
[0016] (2)0.01≤y≤0.2.
[0017] In some embodiments of the present application, the lithium nickel manganese oxide satisfies at least one of the following conditions:
[0018] (1) 0.9≤x≤0.99;
[0019] (2)0.02≤y≤0.1.
[0020] In the above chemical formula, the content of M element is within the above range. On the one hand, while ensuring a relatively high lithium content, it can also make I (111) / I (400) At a relatively high level, the preference for the (111) plane in the spinel structure is improved, and the stability of the spinel structure is improved. On the other hand, since the M element itself cannot change its valence and will occupy and reduce the proportion of active lithium ions in lithium nickel manganese oxide, the content of the M element is within the above range, which can ensure that the positive electrode active material has sufficient cycle activity.
[0021] In some embodiments of the present application, the lithium nickel manganese oxide comprises a rock salt phase, and the X-ray diffraction analysis spectrum of the lithium nickel manganese oxide has a third diffraction peak at a diffraction angle 2θ of 43° to 44°, and the peak intensity of the third diffraction peak is 1 RS , the I RS With the I (400) Satisfy between: 0.01≤I RS / I (400) ≤0.2.
[0022] Lithium nickel manganese oxide contains a rock salt phase, and the nickel in the rock salt phase is stable low-valent nickel. RS / I (400) Controlling the content of the rock salt phase within the above range, that is, controlling the content of the rock salt phase within the above range, can effectively reduce the oxidative decomposition of the electrolyte by the high-valent nickel separated from the spinel phase, thereby reducing the oxidation of the electrolyte.
[0023] In some embodiments of the present application, the I RS With the I (400) Satisfy between: 0.02≤I RS / I (400) ≤0.1.
[0024] In some embodiments of the present application, the I RS With the I (400) Between: 0.05≤I RS / I (400) ≤0.1.
[0025] I RS / I (400) Being within the above range is beneficial to further reduce the oxidative decomposition of the electrolyte and further reduce the dissolution of transition metal ions in the spinel phase, thereby further improving the storage performance of the battery.
[0026] In some embodiments of the present application, the lithium nickel manganese oxide satisfies the following conditions: 3.5≤(I (111) +10×I RS ) / I (400) ≤4.4.
[0027] In some embodiments of the present application, the lithium nickel manganese oxide satisfies the following conditions: 3.6≤(I (111) +10×I RS ) / I (400) ≤4.1.
[0028] In lithium nickel manganese oxide, by (I (111) +10×I RS ) / I (400) Controlling within the above range is beneficial to reducing the adverse effects of the spinel phase and rock salt phase on the material capacity and kinetics, and improving the capacity and kinetic performance of the material and battery.
[0029] In some embodiments of the present application, the lithium nickel manganese oxide comprises grains of the spinel phase and grains of the rock salt phase, and the grains of the rock salt phase are covered on at least a portion of the surface of the grains of the spinel phase in the form of a rock salt phase layer.
[0030] Lithium nickel manganese oxide contains spinel phase grains and rock salt phase grains, wherein the spinel phase grains provide a bulk structure for the lithium nickel oxide, and the bulk structure has a relatively high stability, which can make the dissolution of transition metal ions in the lithium nickel manganese oxide relatively slow; while the rock salt phase grains can reduce the oxidative decomposition of the electrolyte by the high-valent nickel formed by separating from the spinel phase, thereby reducing the oxidation of the electrolyte.
[0031] In some embodiments of the present application, the thickness of the rock salt phase layer is 20nm~200nm.
[0032] The thickness of the rock salt phase layer is within the above range, which can improve the battery storage performance while also taking into account long life and capacity.
[0033] In some embodiments of the present application, the active material further includes phosphate, and the mass percentage of the phosphate in the active material is m, 0.2%≤m≤20%.
[0034] Among the active materials, the phosphate ions in the phosphate can both preferentially capture the HF formed by the oxidative decomposition of the electrolyte, reducing the corrosion of the electrolyte to the positive electrode active material; at the same time, they can also capture transition metal ions and inhibit the dissolution of transition metal ions in lithium nickel manganese oxide, thereby improving the storage performance of the battery.
[0035] In some embodiments of the present application, the positive electrode active material satisfies at least one of the following conditions:
[0036] (1) The m satisfies: 0.5%≤m≤10%;
[0037] (2) the phosphate is coated on at least a portion of the surface of the lithium nickel manganese oxide;
[0038] (3) The phosphate includes at least one of orthophosphate, hydrogen phosphate, dihydrogen phosphate, metaphosphate, pyrophosphate, polyphosphate, hypophosphite, phosphite, monofluorophosphate, difluorophosphate and trifluorophosphate containing at least one element of Li, Na, K, Mg, Al, Ti, Zr, La, Ta, Nb, Te, Mo, W, Sb, Ni, Mn, Fe, Co and N.
[0039] Phosphate is coated on at least a portion of the surface of lithium nickel manganese oxide, which can effectively play the role of the aforementioned phosphate in the active material without affecting the phase structure (spinel phase and rock salt phase) of lithium nickel manganese oxide.
[0040] In some embodiments of the present application, the active substance includes particles of the active substance, the particles of the active substance include at least one of single crystal grains and quasi-single crystal grains, and the single crystal grains include at least one of truncated octahedral grains and spherical grains.
[0041] In the particles of the active material, the rock salt phase is mainly distributed on the surface of the particles. Therefore, when the particles of the active material include single crystal grains and / or quasi-single crystal grains, more rock salt phases will be distributed on each surface of the single crystal grains or quasi-single crystal grains, which is more conducive to improving the long-term stability of the positive electrode active material and the battery.
[0042] In some embodiments of the present application, the positive electrode active material satisfies at least one of the following conditions:
[0043] (1) The compaction density P of the positive electrode active material under a pressure of 6 tons satisfies: P ≥ 3 g / cm 3 ;
[0044] (2) The volume average particle size Dv50 of the positive electrode active material satisfies: 2 μm ≤ Dv50 ≤ 20 μm;
[0045] (3) The volume average particle sizes Dv50, Dv90 and Dv10 of the positive electrode active material satisfy the following conditions: 0.8≤(Dv90-Dv10) / Dv50≤2;
[0046] (4) The specific surface area S of the positive electrode active material satisfies: 0 <S≤1m 2 / g;
[0047] (5) The pH value of the positive electrode active material satisfies: 9≤pH≤12.
[0048] In some embodiments of the present application, the positive electrode active material satisfies at least one of the following conditions:
[0049] (1) The compaction density P of the positive electrode active material under a pressure of 6 tons satisfies: 3 g / cm 3 ≤P≤3.5g / cm 3 ;
[0050] (2) The volume average particle size Dv50 of the positive electrode active material satisfies: 3 μm ≤ Dv50 ≤ 15 μm;
[0051] (3) The volume average particle sizes Dv50, Dv90 and Dv10 of the positive electrode active material satisfy the following conditions: 1.0≤(Dv90-Dv10) / Dv50≤1.8;
[0052] (4) The specific surface area S of the positive electrode active material satisfies: 0 <S≤0.7m 2 / g;
[0053] (5) The pH value of the positive electrode active material satisfies: 10≤pH≤12.
[0054] The compaction density of the positive electrode active material of the present application is within the relatively high range mentioned above, which can make the material particles have a morphology that is more conducive to dense stacking, so the pressure required to achieve the same compaction is smaller, and the particles are less likely to break, thereby reducing the risk of particle cracking, reducing the side reactions and transition metal ion dissolution caused by particle cracking.
[0055] The second aspect of the present application also provides a method for preparing a positive electrode active material, comprising:
[0056] A mixture containing a lithium source, a nickel source, and a manganese source is sintered to obtain a positive electrode active material.
[0057] The positive electrode active material includes an active substance, the active substance includes lithium nickel manganese oxide, the lithium nickel manganese oxide contains a spinel phase, the X-ray diffraction analysis spectrum of the lithium nickel manganese oxide has a first diffraction peak at a diffraction angle 2θ of 18° to 19°, and a second diffraction peak at a diffraction angle 2θ of 44° to 45°, the first diffraction peak corresponds to a crystal plane (111), and the second diffraction peak corresponds to a crystal plane (400); the peak intensity of the first diffraction peak is I (111) , the peak intensity of the second diffraction peak is 1 (400) , and I (111) with I (400) Between: 2.5≤I (111) / I (400) ≤4.
[0058] In the above steps, by sintering the mixture containing the lithium source, the nickel source and the manganese source, a lithium nickel manganese oxide satisfying the above conditions can be obtained by sintering, and a spinel phase is formed in the lithium nickel manganese oxide.
[0059] In some embodiments of the present application, the lithium nickel manganese oxide satisfies the chemical formula Li x M y Ni z Mn 2-y-z O 4-k , wherein 0.8≤x≤1.05, 0≤y≤0.2, 0.3≤z≤0.7, -0.1≤k≤0.5, and M includes one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W.
[0060] In some embodiments of the present application, the sintering process includes:
[0061] The mixture is heated to a first sintering temperature T1, maintained at the first sintering temperature T1 for a first preset time t1, and then cooled to room temperature at a first cooling rate v1 to obtain a sintered product.
[0062] By performing the sintering treatment under the conditions of step S110, the spinel phase and the rock salt phase can be formed simultaneously, and by adjusting the first sintering temperature T1 and the first cooling rate v1, the formation and content of the spinel phase and the rock salt phase in the lithium nickel manganese oxide can be adjusted, so that the I (111) / I (400) and I RS / I (400) The values are regulated so that they each satisfy the range provided in the first aspect of the present application.
[0063] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0064] (1) The first sintering temperature T1 satisfies: 900°C≤T1≤1500°C, and T1≥x×1000°C;
[0065] (2) The first preset time t1 satisfies: 1h≤t1≤20h;
[0066] (3) The first cooling rate v1 satisfies: v1 ≥ 10°C / min.
[0067] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0068] (1) The first sintering temperature T1 satisfies: 1000°C ≤ T1 ≤ 1300°C;
[0069] (2) The first preset time t1 satisfies: 2h≤t1≤15h;
[0070] (3) The first cooling rate v1 satisfies: 10°C / min≤v1≤50°C / min.
[0071] During the sintering process, the stable phases at high temperature are spinel phase (Mn-rich part) and rock salt phase (Ni-rich part). Therefore, when T1 is in the relatively high temperature range mentioned above, it is conducive to the formation of spinel phase and rock salt phase, which is also conducive to I (111) / I (400) and I RS / I (400) It can also reduce the abnormal growth of grains, thereby taking into account the cycle storage life and dynamic performance and processing performance.
[0072] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0073] (1) The mixture further comprises an M source;
[0074] The M source includes one or more of oxides, nitric acid compounds, carbonate compounds, hydroxide compounds and acetic acid compounds containing the M element, and the M element includes one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W;
[0075] (2) The lithium source includes one or more of lithium oxide, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium hydroxide, lithium carbonate and lithium nitrate;
[0076] (3) The nickel source includes one or more of nickel oxide, nickel phosphate, nickel acetate, nickel hydroxide, nickel carbonate and nickel nitrate;
[0077] (4) The manganese source includes one or more of manganese oxide, manganese phosphate, manganese acetate, manganese hydroxide, manganese carbonate and manganese nitrate.
[0078] The M element has the function of inducing the preferred orientation of the crystal and forming strong bonds with oxygen or transition metals in lithium nickel manganese oxide. Adding M source to the mixture can promote I 111 / I 400 and I RS / I 400 Reaching the appropriate range mentioned above in this application can better balance capacity and long-term performance.
[0079] In some embodiments of the present application, the sintering process further comprises:
[0080] The material including the sintered product is heated to a second sintering temperature T2, kept at the second sintering temperature T2 for a second preset time t2, and then cooled to room temperature at a second cooling rate v2.
[0081] By performing the sintering treatment under the conditions of step S120, the phosphate and the lithium nickel manganese oxide can be melted and mixed, and by regulating the second sintering temperature T2 and the second cooling rate v2, it is beneficial to achieve the coating of the surface of the lithium nickel manganese oxide with the phosphate, so that the phosphate is coated on at least a portion of the surface of the lithium nickel manganese oxide.
[0082] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0083] (1) The second sintering temperature T2 satisfies: T1-200°C≤T2≤T1, T2≥900°C;
[0084] (2) The second preset time t2 satisfies: 0.5h≤t2≤5h;
[0085] (3) The second cooling rate v2 satisfies: v2 ≥ 10°C / min;
[0086] (4) The material further comprises phosphate, wherein the phosphate comprises at least one of orthophosphate, hydrogen phosphate, dihydrogen phosphate, metaphosphate, pyrophosphate, polyphosphate, hypophosphite, phosphite, monofluorophosphate, difluorophosphate and trifluorophosphate containing at least one element of Li, Na, K, Mg, Al, Ti, Zr, La, Ta, Nb, Te, Mo, W, Sb, Ni, Mn, Fe, Co and N.
[0087] In some embodiments of the present application, the method satisfies at least one of the following conditions:
[0088] (1) The second sintering temperature T2 satisfies: T1-100°C≤T2≤T1, T2≥950°C;
[0089] (2) The second cooling rate v2 satisfies: 10°C / min≤v2≤50°C / min.
[0090] The second sintering temperature T2 is within the above range, which is beneficial to improving the roundness of the lithium nickel manganese oxide grain growth, thereby increasing its compaction density and reducing the specific surface area.
[0091] The third aspect of the present application provides a positive electrode plate, comprising a positive electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode active material of the first aspect of the present application or the positive electrode active material prepared by the method of the second aspect of the present application.
[0092] In some embodiments of the present application, the compaction density P' of the positive electrode active material layer satisfies: P'≥2.9 g / cm 3 .
[0093] In some embodiments of the present application, the compaction density P' of the positive electrode active material layer satisfies: 3 g / cm 3 ≤P'≤3.6g / cm 3 .
[0094] The compaction density of the positive electrode active material layer is within the above range, which is beneficial to improving the volume energy density of the battery cell and reducing side reactions and dissolution of transition metal ions, and also allows sufficient gaps in the positive electrode active material layer to allow the electrolyte to fully infiltrate and maintain normal dynamic performance of the battery.
[0095] The fourth aspect of the present application provides a secondary battery, comprising the positive electrode sheet of the third aspect of the present application.
[0096] A fifth aspect of the present application provides an electrical device, comprising the secondary battery of the fourth aspect of the present application.
[0097] The electric device of the present application includes the secondary battery provided by the present application, and thus has at least the same advantages as the secondary battery.
[0098] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0099] In order to better describe and illustrate the embodiments or examples provided by the present application, reference may be made to one or more drawings. The additional details or examples used to describe the drawings should not be considered as limiting the scope of the disclosed application, the embodiments or examples currently described, and any of the best modes of these applications currently understood. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0100] Figure 1 1 and 2 are X-ray diffraction patterns of the positive electrode active materials of Example 1, Example 2 and Comparative Example 1 of the present application.
[0101] Figure 2 This is a scanning electron microscope image of the positive electrode active material according to one embodiment of the present application.
[0102] Figure 3 This is a transmission electron microscope image of a cross section of a positive electrode active material according to one embodiment of the present application.
[0103] Figure 4 It is a schematic diagram of a battery cell according to an embodiment of the present application.
[0104] Figure 5 for Figure 5 An exploded view of a battery cell according to an embodiment of the present application is shown.
[0105] Figure 6 It is a schematic diagram of a battery module according to one embodiment of the present application.
[0106] Figure 7 A schematic diagram of a battery pack according to an embodiment of the present application.
[0107] Figure 8 for Figure 7 An exploded view of a battery pack according to an embodiment of the present application is shown.
[0108] Fig. 9 FIG. 1 is a schematic diagram of an electrical device using a secondary battery according to an embodiment of the present application as a power source.
[0109] Description of reference numerals:
[0110] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 battery cell; 51 shell; 52 electrode assembly; 53 cover plate; 6 electrical device. DETAILED DESCRIPTION
[0111] Below, some embodiments of the positive electrode active material and preparation method thereof, positive electrode sheet, secondary battery and electric device of the present application are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0112] "Scope" disclosed in the present application can be limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or excluding end values, and any end value can be included or not included independently, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 listed, and if the maximum range values 3,4 and 5 are also listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation for these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to listing the parameter as, for example, integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For example, when a parameter is expressed as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0113] In the present application, "plurality", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0114] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0115] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment or implementation of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments. The "implementation methods" mentioned herein have a similar understanding.
[0116] Those skilled in the art will appreciate that, in the methods of each embodiment or example, the order in which each step is written does not mean a strict order of execution and does not constitute any limitation on the implementation process, and the detailed order of execution of each step should be determined by its function and possible internal logic. If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) can be added to the method in any order, for example, the method may include steps (a), (b) and (c), or steps (a), (c) and (b), or steps (c), (a) and (b), etc.
[0117] In the present application, in the open technical features or technical solutions described by the words "contain", "include", "comprise", etc., unless otherwise specified, additional members other than the listed members are not excluded, and it can be regarded as providing both closed features or solutions consisting of the listed members and open features or solutions including additional members in addition to the listed members. For example, A includes a1, a2 and a3. Unless otherwise specified, it may also include other members or may not include additional members. It can be regarded as providing both the feature or solution of "A consists of a1, a2 and a3" and the feature or solution of "A not only includes a1, a2 and a3, but also includes other members". In the present application, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.
[0118] In this application, "optionally", "optional", and "optional" mean optional, that is, any one of the two parallel schemes of "yes" or "no". If there are multiple "options" in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "option" is independent.
[0119] At present, spinel nickel manganese oxide LiNi 0.5 Mn 1.5 O 4 When the positive electrode material is used in a full battery, due to its ultra-high lithium deintercalation potential (4.7V vs Li / Li+) and oxidation of high-valent Ni, the positive electrode material and the electrolyte undergo serious side reactions, and the electrolyte is consumed to produce a large amount of gas, which increases the risk of cell swelling and accelerates capacity decay. At the same time, the spinel nickel manganese oxide positive electrode material undergoes transition metal ions (such as manganese ions) dissolution due to its unstable structure, and the dissolved transition metal ions will deposit on the negative electrode surface, destroying the SEI film, accelerating the capacity decay of the negative electrode and the battery, and ultimately leading to a decrease in battery storage performance.
[0120] In order to solve the above technical problems, the present application proposes a positive electrode active material, which can reduce the oxidation consumption of electrolyte by the positive electrode by regulating the crystal structure of the positive electrode active material, and stabilize the material structure itself to significantly reduce the dissolution of transition metal ions in the material, thereby improving the storage performance of the battery. The positive electrode active material will be described in more detail below.
[0121] In a first aspect, the present application provides a positive electrode active material, which includes an active substance, wherein the active substance includes lithium nickel manganese oxide, the lithium nickel manganese oxide contains a spinel phase, and the X-ray diffraction analysis spectrum of the lithium nickel manganese oxide has a first diffraction peak at a diffraction angle 2θ of 18°~19°, and a second diffraction peak at a diffraction angle 2θ of 44°~45°, wherein the first diffraction peak corresponds to a crystal plane (111), and the second diffraction peak corresponds to a crystal plane (400); the peak intensity of the first diffraction peak is I (111) , the peak intensity of the second diffraction peak is 1 (400) , I (111) with I (400) Between: 2.5≤I (111) / I (400) ≤4.0.
[0122] It can be understood that in the X-ray diffraction analysis spectrum of the above lithium nickel manganese oxide, the first diffraction peak and the second diffraction peak both correspond to the spinel phase of the lithium nickel manganese oxide, that is, the first diffraction peak and the second diffraction peak are both peaks of the spinel phase.
[0123] It can be understood that the above-mentioned “active material” refers to a material that can provide activity to the positive electrode active material and realize battery energy conversion.
[0124] In some embodiments, I (111) / I (400) It can be 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0 or a range consisting of any of the above values.
[0125] The positive electrode active material provided in the present application includes a lithium nickel manganese oxide containing a spinel phase, and the first preferred growth crystal plane of the lithium nickel manganese oxide (LNMO) is the (111) plane, that is, the atoms spread and grow layer by layer along the (111) plane, so the stacking quality of the (111) plane determines the stability of the crystal structure. A spinel LNMO grain can have multiple (111) planes (eight side surfaces in the octahedral grain shape) growing synchronously at the same time, and form (a00) side surfaces after contacting each other, so that the (111) plane can be used as the "basal plane" of the spinel phase, and the (a00) plane can be used as the "end face" of the spinel phase. Therefore, in the XRD spectrum of lithium nickel manganese oxide, the ratio of the peak intensity of the "basal plane" (111) to the peak intensity of the end face (a00) is 1 (111) / I (a00) It can indicate the preference of the crystal plane (111). In the XRD spectrum of conventional spinel structured lithium nickel manganese oxide, the (111) and (400) peaks are two of the three strongest peaks, so this application selects I (111) / I (400) As an indicator of the degree of preference of the (111) face. (111) / I (400) When the ratio is controlled within the above range, the preference of the (111) plane can be improved, thereby improving the stacking quality of the (111) plane and thus improving the stability of the spinel phase. The more stable the spinel phase is, the slower the dissolution of transition metal ions (such as manganese ions) in lithium nickel manganese oxide is, and the slower the capacity loss rate of the negative electrode and the battery is, which is beneficial to improving the storage performance of the battery.
[0126] In some embodiments, the lithium nickel manganese oxide satisfies: 2.8≤I (111) / I (400) ≤3.8.
[0127] In some embodiments, the lithium nickel manganese oxide satisfies: 3.1≤I (111) / I (400) ≤3.6.
[0128] In the XRD spectrum of spinel lithium nickel manganese oxide, I (111) / I (400) Being within the above range is beneficial to further improve the stability of the spinel structure, thereby further reducing the dissolution of transition metal ions (such as manganese ions) in lithium nickel manganese oxide, thereby further improving the storage performance of the battery.
[0129] The X-ray diffraction analysis spectrum is well known in the art and can be tested by methods known in the art. For example, the X-ray diffraction analysis spectrum of the positive electrode active material can be measured using CuKα1 radiation with reference to JIS K 0131-1996 General Rules for X-ray Diffraction Analysis.
[0130] In some embodiments, the lithium nickel manganese oxide satisfies the chemical formula Li x M y Ni z Mn 2-y-z O 4-k , wherein 0.8≤x≤1.05, 0≤y≤0.2, 0.3≤z≤0.7, -0.1≤k≤0.5, and M includes one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W.
[0131] In some embodiments, the content x of lithium in the lithium nickel manganese oxide may be 0.8, 0.85, 0.9, 0.95, 1.0, 1.05 or any range thereof.
[0132] In the positive electrode active material provided in the present application, the lithium nickel manganese oxide satisfies the above chemical formula, and the content x of the lithium element is within the above range, which can not only enhance the preference for the (111) face in the spinel structure and improve the stability of the spinel structure; but also ensure the proportion of active lithium ions in the lithium nickel manganese oxide and the diffusion channel of active lithium ions, so that the positive electrode active material has sufficient cycle activity.
[0133] In addition, in lithium nickel manganese oxide, the close-packed plane of oxygen or transition metal ions (such as manganese ions) is the (111) plane; and when lithium nickel manganese oxide satisfies the above chemical formula, the M element in the chemical formula can form a strong bond with oxygen or transition metal ions and improve the preference for the (111) plane.
[0134] In some embodiments, 0.85≤x≤1.02. For example, x can be 0.85, 0.88, 0.91, 0.93, 0.95, 0.97, 0.99, 1.01, 1.02, or any range thereof.
[0135] In some embodiments, 0.9≤x≤0.99. For example, x can be 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99 or any range thereof.
[0136] In the lithium nickel manganese oxide, the content x of the lithium element is within the above range, which can further improve the stability of the spinel structure and enable the positive electrode active material to have sufficient cycle activity.
[0137] In some embodiments, the content y of the M element in the lithium nickel manganese oxide may be 0, 0.01, 0.02, 0.04, 0.06, 0.08, 0.1, 0.12, 0.14, 0.16, 0.18, 0.2 or any range thereof.
[0138] In the above chemical formula, the content of M element is within the above range. On the one hand, while ensuring a relatively high lithium content, it can also make I (111) / I (400) At a relatively high level, the preference for the (111) plane in the spinel structure is improved, and the stability of the spinel structure is improved. On the other hand, since the M element itself cannot change its valence and will occupy and reduce the proportion of active lithium ions in lithium nickel manganese oxide, the content of the M element is within the above range, which can ensure that the positive electrode active material has sufficient cycle activity.
[0139] In some embodiments, 0.01≤y≤0.2. For example, y may be 0.01, 0.03, 0.05, 0.07, 0.09, 0.11, 0.13, 0.15, 0.17, 0.19, 0.2, or any range thereof.
[0140] In some embodiments, 0.02≤y≤0.1. For example, y may be 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, or any range thereof.
[0141] In lithium nickel manganese oxide, the content y of the M element is within the above range, which can further improve the stability of the spinel structure while enabling the positive electrode active material to have sufficient cycle activity, thereby better balancing the capacity and long-term performance of the positive electrode active material.
[0142] In some embodiments, the lithium nickel manganese oxide comprises a rock salt phase, and the X-ray diffraction analysis spectrum of the lithium nickel manganese oxide has a third diffraction peak at a diffraction angle 2θ of 43° to 44°, and the peak intensity of the third diffraction peak is 1 RS , the I RS With the I (400) Satisfy between: 0.01≤I RS / I (400) ≤0.2.
[0143] It can be understood that in the X-ray diffraction analysis spectrum of the above lithium nickel manganese oxide, the third diffraction peak corresponds to the rock salt phase of the lithium nickel manganese oxide, that is, the third diffraction peak is a peak of the rock salt phase.
[0144] In some embodiments, I RS / I (400) It can be 0.01, 0.03, 0.05, 0.07, 0.09, 0.11, 0.13, 0.15, 0.17, 0.19, 0.2 or within a range consisting of any of the above values.
[0145] Lithium nickel manganese oxide contains a rock salt phase, wherein the nickel in the rock salt phase is stable low-valent nickel. RS / I (400) Controlling the content of the rock salt phase within the above range, that is, controlling the content of the rock salt phase within the above range, can effectively reduce the oxidative decomposition of the electrolyte by the high-valent nickel separated from the spinel phase, and reduce the oxidation of the electrolyte; at the same time, the reduction in the oxidative decomposition of the electrolyte can also reduce the dissolution of transition metal ions in the spinel phase, thereby reducing the attenuation of the negative electrode and battery capacity and improving the storage performance of the battery.
[0146] Further, in lithium nickel manganese oxide, by (111) / I (400) and I RS / I (400) By controlling each of them within the corresponding range, the stability of the spinel phase is improved, its oxidation at high voltage (such as 4.7V) and the dissolution of transition metal ions are reduced, while the oxidative decomposition of the electrolyte is reduced, and the dissolution of transition metal ions is further reduced, thereby effectively improving the storage performance of the battery.
[0147] In some embodiments, the I RS With the I (400) Satisfy between: 0.02≤I RS / I (400) ≤0.1. For example, I RS / I (400) It can be 0.02, 0.04, 0.06, 0.08, 0.1 or within a range consisting of any of the above values.
[0148] In some embodiments, the I RS With the I (400) Between: 0.05≤I RS / I (400) ≤0.1. For example, I RS / I (400) It can be 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or within a range consisting of any of the above values.
[0149] I RS / I (400) Being within the above range is beneficial to further reduce the oxidative decomposition of the electrolyte and further reduce the dissolution of transition metal ions in the spinel phase, thereby further improving the storage performance of the battery.
[0150] In some embodiments, the lithium nickel manganese oxide satisfies the following conditions: 3.5≤(I (111) +10×I RS ) / I (400) ≤4.4. For example, (I (111)+10×I RS ) / I (400) It can be 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4 or within a range consisting of any of the above values.
[0151] In lithium nickel manganese oxide, by (I (111) +10×I RS ) / I (400) Controlling within the above range is beneficial to reducing the adverse effects of the spinel phase and rock salt phase on the material capacity and kinetics, and improving the capacity and kinetic performance of the material and battery.
[0152] In some embodiments, the lithium nickel manganese oxide satisfies the following conditions: 3.6≤(I (111) +10×I RS ) / I (400) ≤4.1. For example, (I (111) +10×I RS ) / I (400) It can be 3.6, 3.65, 3.7, 3.75, 3.8, 3.85, 3.9, 3.95, 4, 4.05, 4.1 or within a range consisting of any of the above values.
[0153] (I (111) +10×I RS ) / I (400) Being within the above range is beneficial to further reduce the adverse effects of the spinel phase and rock salt phase on the material capacity and kinetics, and further improve the capacity and kinetic performance of the material and battery.
[0154] In some embodiments, the lithium nickel manganese oxide comprises grains of the spinel phase and grains of the rock salt phase, wherein the grains of the rock salt phase are covered on at least a portion of the surface of the grains of the spinel phase in the form of a rock salt phase layer (see Figure 3 ).
[0155] Lithium nickel manganese oxide contains spinel phase grains and rock salt phase grains, wherein the spinel phase grains provide a bulk structure for the lithium nickel oxide, and the bulk structure has a relatively high stability, which can make the dissolution of transition metal ions in the lithium nickel manganese oxide relatively slow; while the rock salt phase grains can reduce the oxidative decomposition of the electrolyte by the high-valent nickel formed by separating from the spinel phase, thereby reducing the oxidation of the electrolyte.
[0156] At the same time, the grains of the rock salt phase are covered on at least part of the surface of the grains of the spinel phase in the form of a rock salt phase layer. That is, when the rock salt phase is on the surface of the lithium nickel manganese oxide, the lithium nickel manganese oxide can keep the nickel on the surface in a relatively low valence state after charging, which can further reduce the oxidation of the electrolyte and thereby improve the storage performance of the battery.
[0157] In some embodiments, the thickness of the rock salt phase layer is 20 nm to 200 nm. For example, the thickness of the rock salt phase layer can be 20 nm, 40 nm, 60 nm, 80 nm, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, 200 nm or within the range of any of the above values. Optionally, the thickness of the rock salt phase layer is 50 nm to 100 nm.
[0158] The thickness of the rock salt phase layer is within the above range, which can improve the battery storage performance while also taking into account long life and capacity.
[0159] The thickness of the rock salt phase layer is well known in the art and can be tested by methods known in the art, for example, by using a transmission electron microscope (TEM, model: Hitachi, JEM-2100F).
[0160] In some embodiments, the active material further comprises phosphate.
[0161] Among the active materials, the phosphate ions in the phosphate can both preferentially capture the HF formed by the oxidative decomposition of the electrolyte, reducing the corrosion of the electrolyte to the positive electrode active material; at the same time, they can also capture transition metal ions and inhibit the dissolution of transition metal ions in lithium nickel manganese oxide, thereby improving the storage performance of the battery.
[0162] In some embodiments, the mass percentage of the phosphate in the active material is m, 0.2%≤m≤20%. For example, m can be 0.2%, 0.5%, 0.8%, 1%, 3%, 5%, 7%, 9%, 10%, 12%, 14%, 16%, 18%, 20% or any range thereof.
[0163] The mass percentage of phosphate in the active material is well known in the art and can be tested by methods known in the art. For example, it can be tested by inductively coupled plasma (ICP, such as Optima 5300 DV) with reference to EPA 6010D-2014 inductively coupled plasma atomic emission spectrometry.
[0164] In some embodiments, m satisfies: 0.5%≤m≤10%. For example, m can be 0.5%, 0.7%, 0.9%, 1%, 2%, 4%, 6%, 8%, 10% or a range divided by any of the above values. Optionally, m satisfies: 1%≤m≤5%.
[0165] The mass percentage of phosphate in the active material is within the above range, which is beneficial to further reduce the corrosion of the electrolyte to the positive electrode active material; at the same time, it further inhibits the dissolution of transition metal ions in the lithium nickel manganese oxide, thereby further improving the storage performance of the battery.
[0166] In some embodiments, the phosphate is coated on at least a portion of the surface of the lithium nickel manganese oxide.
[0167] Phosphate is coated on at least a portion of the surface of lithium nickel manganese oxide, which can effectively play the role of the aforementioned phosphate in the active material without affecting the phase structure (spinel phase and rock salt phase) of lithium nickel manganese oxide.
[0168] In some embodiments, the phosphate includes but is not limited to at least one of orthophosphate, hydrogen phosphate, dihydrogen phosphate, metaphosphate, pyrophosphate, polyphosphate, hypophosphite, phosphite, monofluorophosphate, difluorophosphate and trifluorophosphate containing at least one element of Li, Na, K, Mg, Al, Ti, Zr, La, Ta, Nb, Te, Mo, W, Sb, Ni, Mn, Fe, Co and N (nitrogen).
[0169] In some embodiments, the active material includes particles of the active material, and the particles of the active material include at least one of single crystal grains and quasi-single crystal grains.
[0170] In the particles of the active material, the rock salt phase is mainly distributed on the surface of the particles. Therefore, when the particles of the active material include single crystal grains and / or quasi-single crystal grains, more rock salt phases will be distributed on each surface of the single crystal grains or quasi-single crystal grains, which is more conducive to improving the long-term stability of the positive electrode active material and the battery.
[0171] In some embodiments, the single crystal grains include at least one of truncated octahedral grains and spherical grains (see Figure 2 ). The shapes of truncated octahedral grains and spherical grains are more resistant to pressure, which is beneficial for the positive electrode active material to obtain a higher compaction density and reduce its cracking.
[0172] In some embodiments, the compaction density P of the positive electrode active material under 6 tons of pressure satisfies: P ≥ 3 g / cm 3 .
[0173] In some embodiments, the compaction density P of the positive electrode active material under 6 tons of pressure satisfies: 3 g / cm 3 ≤P≤3.5g / cm 3 For example, P can be 3 g / cm 3 , 3.1g / cm 3 , 3.2g / cm 3 , 3.3g / cm3 , 3.4g / cm 3 , 3.5g / cm 3 Or within the range of any of the above values. Optionally, P satisfies: 3.1 g / cm 3 ≤P≤3.4g / cm 3 .
[0174] In the positive electrode active material, particle cracking will expose unstable fresh interfaces, accelerate side reactions and transition metal ion dissolution. The compaction density of the positive electrode active material of the present application is within the relatively high range mentioned above, which can make the material particles have a morphology that is more conducive to dense stacking, so the pressure required to achieve the same compaction is smaller, and the particles are less likely to break, thereby reducing the risk of particle cracking and reducing the occurrence of side reactions and transition metal ion dissolution caused by particle cracking. In addition, the relatively high compaction density is conducive to improving the volume energy density of battery cells and batteries.
[0175] The compaction density of the positive electrode active material under 6 tons of pressure is well known in the art and can be tested by methods known in the art. For example, it can be tested by an electronic pressure tester, such as the UTM7305 electronic pressure tester, with reference to GB / T24533-2009 standard. Accurately weigh about 1g of the sample and add a bottom area of 1.327cm 2 In the mold, a pressure device is used to apply 6 tons of pressure to the sample and keep it at this pressure for 30 seconds before removing the pressure. Then the height of the sample is measured and the compaction density of the material can be obtained through the formula P=m / (1.327×h). In the formula, P represents the compaction density of the material, m represents the mass of the sample, and h represents the height of the sample after 6 tons of pressure is applied and kept at this pressure for 30 seconds before removing the pressure.
[0176] In some embodiments, the volume average particle size Dv50 of the positive electrode active material satisfies: 2μm≤Dv50≤20μm. For example, Dv50 may be 2μm, 4μm, 6μm, 8μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, or within a range consisting of any of the above values.
[0177] In some embodiments, the volume average particle size Dv50 of the positive electrode active material satisfies: 3μm≤Dv50≤15μm. For example, Dv50 may be 3μm, 5μm, 7μm, 9μm, 11μm, 13μm, 15μm, or within a range consisting of any of the above values. Optionally, Dv50 satisfies: 5μm≤Dv50≤10μm.
[0178] The volume average particle size Dv50 of the positive electrode active material is within the above range, which can better regulate parameters such as the crystal structure, oxygen defects and specific surface area of the positive electrode active material, thereby improving its cycle performance.
[0179] The volume average particle size Dv50 of the positive electrode active material is well known in the art and can be measured by methods known in the art. For example, it can be measured with a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd., UK, with reference to the particle size distribution laser diffraction method of GB / T 19077-2016.
[0180] In some embodiments, the volume average particle sizes Dv50, Dv90 and Dv10 of the positive electrode active material satisfy: 0.8≤(Dv90-Dv10) / Dv50≤2. For example, (Dv90-Dv10) / Dv50 may be 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2 or within a range consisting of any of the above values.
[0181] In some embodiments, the volume average particle size Dv50, Dv90 and Dv10 of the positive electrode active material satisfies: 1≤(Dv90-Dv10) / Dv50≤1.8. For example, (Dv90-Dv10) / Dv50 can be 1, 1.1, 1.3, 1.5, 1.7, 1.8 or within the range of any of the above values. Optionally, Dv50, Dv90 and Dv10 satisfy: 1.2≤(Dv90-Dv10) / Dv50≤1.5.
[0182] The larger the (Dv90-Dv10) / Dv50 is, the wider the particle size distribution of the positive electrode material is, that is, the greater the difference between large and small particles. (Dv90-Dv10) / Dv50 is within the above range, which is conducive to obtaining a higher compaction density while better taking into account the relatively small specific surface area, thereby helping to improve the volume energy density of the material.
[0183] The volume average particle size Dv90 of the positive electrode active material refers to the value at which 90% of the particles in the volume-based particle size distribution of the positive electrode active material have a particle size smaller than this value; Dv10 refers to the value at which 10% of the particles in the volume-based particle size distribution of the positive electrode active material have a particle size smaller than this value. Both Dv90 and Dv10 can be tested using methods known in the art, for example, they can be measured using a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd., UK, with reference to the particle size distribution laser diffraction method of GB / T19077-2016.
[0184] In some embodiments, the specific surface area S of the positive electrode active material satisfies: <S≤1m2 / g. For example, S can be 0.1m 2 / g,0.2m 2 / g,0.4m 2 / g,0.6m 2 / g,0.8m 2 / g,1m 2 / g or within a range consisting of any of the above values.
[0185] In some embodiments, the specific surface area S of the positive electrode active material satisfies: <S≤0.7m 2 / g. For example, S can be 0.1m 2 / g,0.2m 2 / g,0.3m 2 / g,0.4m 2 / g,0.5m 2 / g,0.6m 2 / g,0.7m 2 / g or within the range of any of the above values. Optionally, S satisfies: 0.1m 2 / g≤S≤0.5m 2 / g.
[0186] The specific surface area of the positive electrode active material is within the above range, which is beneficial to slowing down the occurrence of side reactions on its surface, thereby improving its long-term performance.
[0187] The specific surface area of the positive electrode active material is a well-known meaning in the art and can be tested by methods known in the art. For example, according to the gas adsorption BET method of GB / T 19587-2004, after the sample is heated and degassed, the adsorption amount of the gas on the solid surface under different adsorption pressures is measured at a constant low temperature, and the monolayer adsorption amount of the sample is obtained based on the BET multilayer adsorption theory and its formula, thereby calculating the specific surface area per unit mass of the solid sample.
[0188] In some embodiments, the pH value of the positive electrode active material satisfies: 9≤pH≤12. The pH value may be 9, 10, 11, 12 or within a range consisting of any of the above values.
[0189] In some embodiments, the pH value of the positive electrode active material satisfies: 10≤pH≤12. For example, the pH value may be 10, 10.5, 11, 11.5, 12, or within a range of any of the above values. Optionally, the pH value satisfies: 10.5≤pH≤11.5.
[0190] The pH of the positive electrode active material is within the above range, indicating that there is an appropriate amount of alkaline groups in the material, which can neutralize the strong acid (such as hydrofluoric acid) generated under high voltage (such as 4.7V) to reduce the damage to the surface of the positive electrode active material; it will not affect the processing performance of the material, and will not cause the material to deteriorate battery performance due to the impact on processing performance (such as easy moisture absorption, reaction with binder, etc.).
[0191] The pH value of the positive electrode active material is well known in the art and can be tested by methods known in the art. For example, referring to GB / T 9724-2007 General Rules for Determination of pH Value of Chemical Reagents, the sample and DI water are mixed into a solution at a fixed ratio of 1:9 and sealed on a magnetic stirrer for 30 minutes. After stirring, the conical flask is placed in a 25°C water bath thermostat, and the pH of the mixture is measured using a pH meter after standing for 1.5 hours.
[0192] In a second aspect, the present application provides a method for preparing a positive electrode active material, which is used to prepare the positive electrode active material of the first aspect of the present application, and may include the following steps:
[0193] S10, sintering a mixture comprising a lithium source, a nickel source, and a manganese source to obtain a positive electrode active material, wherein the positive electrode active material comprises an active substance, the active substance comprises lithium nickel manganese oxide, the lithium nickel manganese oxide comprises a spinel phase, and an X-ray diffraction analysis spectrum of the lithium nickel manganese oxide has a first diffraction peak at a diffraction angle 2θ of 18° to 19°, and a second diffraction peak at a diffraction angle 2θ of 44° to 45°, the first diffraction peak corresponds to a crystal plane (111), and the second diffraction peak corresponds to a crystal plane (400); the peak intensity of the first diffraction peak is 1 (111) , the peak intensity of the second diffraction peak is 1 (400) , and I (111) with I (400) Between: 2.5≤I (111) / I (400) ≤4.
[0194] In the above steps, by sintering the mixture containing the lithium source, the nickel source and the manganese source, a lithium nickel manganese oxide satisfying the above conditions can be obtained by sintering, and a spinel phase is formed in the lithium nickel manganese oxide.
[0195] In some embodiments, the lithium nickel manganese oxide satisfies the chemical formula Li x M y Ni z Mn 2-y-z O 4-k, wherein 0.8≤x≤1.05, 0≤y≤0.2, 0.3≤z≤0.7, -0.1≤k≤0.5, and M includes one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W.
[0196] It should be noted that the chemical formula satisfied by the lithium nickel manganese oxide can be pre-designed according to the target components actually required before the step of preparing the positive electrode active material, and then the positive electrode active material can be prepared in turn according to the pre-designed target components.
[0197] In some embodiments, the sintering process in step S10 may further include the following steps:
[0198] S110, heating the mixture to a first sintering temperature T1, maintaining the mixture at the first sintering temperature T1 for a first preset time t1, and then cooling the mixture to room temperature at a first cooling rate v1 to obtain a sintered product.
[0199] By performing the sintering treatment under the conditions of step S110, the spinel phase and the rock salt phase can be formed simultaneously, and by adjusting the first sintering temperature T1 and the first cooling rate v1, the formation and content of the spinel phase and the rock salt phase in the lithium nickel manganese oxide can be adjusted, so that the I (111) / I (400) and I RS / I (400) The values are regulated so that they each satisfy the range provided in the first aspect of the present application.
[0200] In some embodiments, the first sintering temperature T1 satisfies: 900° C.≤T1≤1500° C., and T1≥x×1000° C. For example, T1 may be 900° C., 1000° C., 1100° C., 1200° C., 1300° C., 1400° C., 1500° C., or any range thereof.
[0201] During the sintering process, the stable phases at high temperature are spinel phase (Mn-rich part) and rock salt phase (Ni-rich part). Therefore, when T1 is in the relatively high temperature range mentioned above, it is conducive to the formation of spinel phase and rock salt phase, which is also conducive to I (111) / I (400) and I RS / I (400)The increase of the temperature of the lithium nickel manganese oxide can be reduced; and the abnormal growth of the grains can be reduced, thereby taking into account the cycle storage life and the dynamic performance and processing performance. At the same time, the lithium content x in the lithium nickel manganese oxide, that is, the content of the lithium source in the mixture in step S10, will affect the formation of the spinel phase and the rock salt phase. By making T1 ≥ x × 1000 ° C, the minimum temperature of the first sintering treatment can still be kept at a relatively high level, thereby promoting the formation of the spinel phase and the rock salt phase.
[0202] In some embodiments, the first sintering temperature T1 satisfies: 1000°C≤T1≤1300°C. For example, T1 may be 1000°C, 1050°C, 1150°C, 1250°C, 1300°C or any range thereof. Optionally, 1000°C≤T1≤1200°C.
[0203] In some embodiments, the first preset time t1 satisfies: 1h≤t1≤20h. For example, t1 can be 1h, 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h or any range thereof.
[0204] In some embodiments, the first preset time t1 satisfies: 2h≤t1≤15h. For example, t1 can be 2h, 3h, 5h, 7h, 9h, 11h, 13h, 15h or any range thereof.
[0205] In some embodiments, the first cooling rate v1 satisfies: v1 ≥ 10°C / min.
[0206] In some embodiments, the first cooling rate v1 satisfies: 10°C / min≤v1≤50°C / min. For example, v1 can be 10°C / min, 20°C / min, 30°C / min, 40°C / min, 50°C / min, or any range thereof.
[0207] The first cooling rate v1 is within the above range, which is beneficial to suppress the reduction of the rock salt phase caused by annealing, thereby promoting I RS / I (400) improvement.
[0208] In some embodiments, the mixture further comprises an M source; the M source comprises one or more of oxides, nitric acid compounds, carbonate compounds, hydroxide compounds and acetic acid compounds containing the M element, and the M element comprises one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W.
[0209] The M element has the function of inducing the preferred orientation of the crystal and forming strong bonds with oxygen or transition metals in lithium nickel manganese oxide. Adding M source to the mixture can promote I 111 / I 400 and I RS / I 400 Reaching the appropriate range mentioned above in this application can better balance capacity and long-term performance.
[0210] In some embodiments, the lithium source includes, but is not limited to, one or more of lithium oxide, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium hydroxide, lithium carbonate, and lithium nitrate.
[0211] In some embodiments, the nickel source includes, but is not limited to, one or more of nickel oxide, nickel phosphate, nickel acetate, nickel hydroxide, nickel carbonate, and nickel nitrate.
[0212] In some embodiments, the manganese source includes, but is not limited to, one or more of manganese oxide, manganese phosphate, manganese acetate, manganese hydroxide, manganese carbonate, and manganese nitrate.
[0213] In some embodiments, after step S110, the sintering process in step S10 may further include the following steps:
[0214] S120, raising the temperature of the material including the sintered product to a second sintering temperature T2, maintaining the temperature at the second sintering temperature T2 for a second preset time t2, and then cooling the temperature at a second cooling rate v2 to room temperature.
[0215] It can be understood that the "room temperature" in steps S110 and S120 refers to 20°C to 30°C, and further, can be 25°C.
[0216] In some embodiments, the material in step S120 may further include phosphate.
[0217] In some embodiments, the phosphate includes but is not limited to at least one of orthophosphate, hydrogen phosphate, dihydrogen phosphate, metaphosphate, pyrophosphate, polyphosphate, hypophosphite, phosphite, monofluorophosphate, difluorophosphate and trifluorophosphate containing at least one element of Li, Na, K, Mg, Al, Ti, Zr, La, Ta, Nb, Te, Mo, W, Sb, Ni, Mn, Fe, Co and N (nitrogen).
[0218] By performing the sintering treatment under the conditions of step S120, the phosphate and the lithium nickel manganese oxide can be melted and mixed, and by regulating the second sintering temperature T2 and the second cooling rate v2, it is beneficial to achieve the coating of the surface of the lithium nickel manganese oxide with the phosphate, so that the phosphate is coated on at least a portion of the surface of the lithium nickel manganese oxide.
[0219] The spinel phase and the rock salt phase can be formed at the same time, and by adjusting the first sintering temperature T1 and the first cooling rate v1, the formation and content of the spinel phase and the rock salt phase in the lithium nickel manganese oxide can be adjusted, so that the I (111) / I (400) and I RS / I (400) The values are regulated so that they each satisfy the range provided in the first aspect of the present application.
[0220] In some embodiments, the second sintering temperature T2 satisfies: T1-200°C≤T2≤T1, T2≥900°C.
[0221] In some embodiments, the second sintering temperature T2 satisfies: T1-100°C≤T2≤T1, T2≥950°C.
[0222] The second sintering temperature T2 is within the above range, which is beneficial to improving the roundness of the lithium nickel manganese oxide grain growth, thereby increasing its compaction density and reducing the specific surface area.
[0223] In some embodiments, the second preset time t2 satisfies: 0.5h≤t2≤5h. For example, t2 can be 0.5h, 1h, 2h, 3h, 4h, 5h or any range thereof.
[0224] In some embodiments, the second cooling rate v2 satisfies: v2 ≥ 10°C / min.
[0225] In some embodiments, the second cooling rate v2 satisfies: 10°C / min≤v2≤50°C / min. For example, v2 can be 10°C / min, 20°C / min, 30°C / min, 40°C / min, 50°C / min, or any range thereof.
[0226] In some embodiments, the material in step S120 may further include a nickel-containing compound. Adding the nickel-containing compound in step 120 is beneficial to further promote the formation of the rock salt phase layer.
[0227] In some embodiments, the nickel-containing compound includes but is not limited to one or more of nickel oxide, nickel phosphate, nickel acetate, nickel hydroxide, nickel carbonate and nickel nitrate.
[0228] In addition, the secondary battery and the electric device of the present application will be described below with reference to the drawings as appropriate.
[0229] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0230] Positive electrode
[0231] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer arranged on at least one surface of the positive electrode current collector, and the positive electrode active material layer includes the positive electrode active material of the first aspect of the present application or the positive electrode active material prepared by the method of the second aspect of the present application.
[0232] In some embodiments, the compaction density P' of the positive electrode active material layer satisfies: P'≥2.9 g / cm 3 .
[0233] In some embodiments, the compaction density P' of the positive electrode active material layer satisfies: 3 g / cm 3 ≤P'≤3.6g / cm 3 For example, P' can be 3 g / cm 3 , 3.1g / cm 3 , 3.2g / cm 3 , 3.3g / cm 3 , 3.4g / cm 3 , 3.5g / cm 3 , 3.6g / cm 3 Or within the range of any of the above values. Optionally, P' satisfies: 3.1 g / cm 3 ≤P'≤3.5g / cm 3 .
[0234] The compaction density of the positive electrode active material layer is within the above range, which is beneficial to improving the volume energy density of the battery cell and reducing side reactions and dissolution of transition metal ions, and also allows sufficient gaps in the positive electrode active material layer to allow the electrolyte to fully infiltrate and maintain normal dynamic performance of the battery.
[0235] As a non-limiting example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode active material layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0236] In some of the embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be obtained by forming a metal material on a polymer material substrate. In the positive electrode current collector, non-limiting examples of the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In the positive electrode current collector, non-limiting examples of the polymer material substrate may include one or more of substrates such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0237] In some of the embodiments, the positive electrode active material may also use other positive electrode active materials for batteries that are well known in the art. As non-limiting examples, other positive electrode active materials may include one or more of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxides (such as LiCoO 2 ), one or more of lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and modified compounds thereof. Non-limiting examples of lithium phosphates containing an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. Non-limiting examples of lithium cobalt oxides may include LiCoO 2 Non-limiting examples of lithium nickel oxides may include LiNiO 2 Non-limiting examples of lithium manganese oxides may include LiMnO 2 、LiMn 2 O 4 etc.; Non-limiting examples of lithium nickel cobalt manganese oxides may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 (Also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O 2 (Also referred to as NCM 523 )、LiNi 0.5Co 0.25 Mn 0.25 O 2 (Also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O 2 (Also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O 2 (Also referred to as NCM 811 ) etc. Non-limiting examples of lithium nickel cobalt aluminum oxide may include LiNi 0.85 Co 0.15 Al 0.05 O 2 .
[0238] As the Li content in the positive electrode material changes, how to define the subscript of Li in the general formula:
[0239] For ternary materials:
[0240] Li x (Ni a Co b Mn c ) 1-d M d O 2-y A y , x is 0.2-1.2;
[0241] Li x A a (Ni a Co b Mn c ) 1-d M d O 2-y A y , x+a is 0.2-1.2.
[0242] For lithium manganese iron phosphate materials:
[0243] Li a Mn 1-y B y P 1-z C z O 4-n D n , a is 0-1.1;
[0244] Li a A x Mn 1-y B y P1-z C z O 4-n D n , a+x is 0-1.1.
[0245] The above limitation on x includes the molar content of Li under different charge and discharge states of the battery (usually the battery voltage is between 2-5V).
[0246] It is understandable that the battery will be accompanied by lithium (Li) deintercalation and consumption during the charging and discharging process, and the content of Li in the positive electrode plate is different when the battery is discharged to different states. In the enumeration of positive electrode materials in this application, unless otherwise specified, the content of Li is the initial state of the material. The positive electrode material is applied to the positive electrode plate in the battery system, and after the charge and discharge cycle, the content of Li in the positive electrode material contained in the plate usually changes. Among them, the content of Li can be measured by molar content, but is not limited to this. Regarding "the content of Li is the initial state of the material", the initial state of the material refers to the state before the material is added to the positive electrode slurry. It is understandable that new materials obtained by appropriate modification on the basis of the listed positive electrode materials are also within the scope of positive electrode materials. The aforementioned appropriate modification refers to acceptable modification methods for positive electrode materials, and non-limiting examples include coating modification.
[0247] In the list of positive electrode materials in this application, the content of oxygen (O) is only a theoretical state value. The release of oxygen from the lattice will cause the molar content of oxygen to change, and the actual content of O will fluctuate. Among them, the content of O can be measured by molar content, but is not limited to this.
[0248] In some embodiments, the positive electrode active material may also include at least one of the following materials: one or more of sodium transition metal oxides, polyanionic compounds, and Prussian blue compounds. However, the present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for sodium ion batteries may also be used.
[0249] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal may include one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Non-limiting examples of sodium transition metal oxides may include Na x MO 2 , where M may include one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.
[0250] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO 4 ) n-A class of compounds with anionic units. Transition metals may include one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y may be one or more of P, S and Si; n represents (YO 4 ) n- valence state.
[0251] The polyanionic compound can also be a compound having sodium ions, transition metal ions, tetrahedral (YO 4 ) n- A class of compounds of anion units and halogen anions. Transition metals may include one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y may be one or more of P, S and Si, and n represents (YO 4 ) n- valence state; the halogen can be one or more of F, Cl and Br.
[0252] The polyanionic compound can also be a compound having sodium ions, tetrahedral (YO 4 ) n- Anion unit, polyhedral unit (ZO y ) m+ and an optional halogen anion. Y can be one or more of P, S and Si, and n represents (YO 4 ) n- valence state; Z represents a transition metal, which may include one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; m represents (ZO y ) m+ valence state; the halogen can be one or more of F, Cl and Br.
[0253] The polyanionic compound may include NaFePO 4 、Na 3 V 2 (PO 4 ) 3 (Sodium vanadium phosphate, referred to as NVP), Na 4 Fe 3 (PO 4 ) 2 (P 2 O 7 ), NaM'PO 4 F and Na 3 (VO y ) 2 (PO 4 ) 2 F 3-2y (0≤y≤1) or more. Among them, NaM'PO4 M' in F may include one or more of V, Fe, Mn and Ni.
[0254] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ). The transition metal may include one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Non-limiting examples of Prussian blue compounds may include Na a Me b Me' c (CN) 6 , wherein Me and Me' can each independently be one or more of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.
[0255] In some embodiments, the positive electrode active material layer may further include a binder. As non-limiting examples, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0256] In some embodiments, the positive electrode active material layer may further include a conductive agent. As non-limiting examples, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0257] In some of the embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent to form a positive electrode slurry; the positive electrode slurry is coated on at least one side of the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained. The type of solvent can be selected from but not limited to any one of the aforementioned embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode collector coated with the positive electrode slurry can be on a single surface of the positive electrode collector or on both surfaces of the positive electrode collector. The solid content of the positive electrode slurry can be 40wt%~80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000-25000mPa·s. When the positive electrode slurry is coated, the coating unit surface density on a dry weight basis (excluding the solvent) can be 15-35 mg / cm 2 The compaction density of the positive electrode can be 3.0~3.6 g / cm 3 , can be selected as 3.3~3.5 g / cm 3 .
[0258] Negative electrode
[0259] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.
[0260] As a non-limiting example, the negative electrode current collector has two surfaces opposite to each other in its own thickness direction, and the negative electrode active material layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0261] In some of the embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be obtained by forming a metal material on a polymer material substrate. In the negative electrode current collector, non-limiting examples of the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In the negative electrode current collector, non-limiting examples of the polymer material substrate may include one or more of substrates such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0262] In some of the embodiments, the negative electrode active material may adopt the negative electrode active material for batteries known in the art. As a non-limiting example, the negative electrode active material may include one or more of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may include one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include one or more of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0263] In some embodiments, the negative electrode active material layer may further include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0264] In some embodiments, the negative electrode active material layer may further include a conductive agent, which may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0265] In some of the embodiments, the negative electrode active material layer may further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0266] In some of the embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (a non-limiting example of the solvent is deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on at least one side of the surface of the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained. The surface of the negative electrode collector coated with the negative electrode slurry can be on a single surface of the negative electrode collector or on both surfaces of the negative electrode collector. The solid content of the negative electrode slurry can be 40wt%~60wt%. The viscosity of the negative electrode slurry at room temperature can be adjusted to 2000-10000mPa·s. When coating the negative electrode slurry, the coating unit surface density on a dry weight basis (excluding the solvent) can be 75-220 g / m 2 The compaction density of the negative electrode sheet can be 1.0 g / cm 3 ~ 1.8 g / cm 3 .
[0267] Electrolytes
[0268] The electrolyte has the function of conducting ions between the positive electrode and the negative electrode. The present application has no particular restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0269] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0270] In some embodiments, the electrolyte salt may include lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium perchlorate (LiClO 4 ) and lithium hexafluoroarsenate (LiAsF 6 ), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO 2 F 2 ), one or more of lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorooxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0271] In some embodiments, the solvent may include ethylene carbonate (EC, ), propylene carbonate (PC, )、ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate ( ), fluoroethylene carbonate (FEC), methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0272] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0273] In some embodiments, the additive in the electrolyte may include, but is not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), and the like.
[0274] Isolation film
[0275] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0276] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0277] In some embodiments, the isolation film has a thickness of 6-40 μm, and optionally 12-20 μm.
[0278] In some of the embodiments, the positive electrode sheet, the negative electrode sheet and the separator can be formed into an electrode assembly by a winding process or a lamination process.
[0279] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0280] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and further, non-limiting examples of plastic can include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0281] The secondary battery includes at least one battery cell. The secondary battery may include one or more battery cells.
[0282] In this application, unless otherwise specified, "battery cell" refers to a basic unit that can realize the mutual conversion of chemical energy and electrical energy, and further, generally speaking, at least includes a positive electrode sheet, a negative electrode sheet and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting active ions between the positive electrode sheet and the negative electrode sheet.
[0283] The present application has no particular limitation on the shape of the battery cell, which may be cylindrical, square or any other shape. Figure 4 The battery cell 5 is a square structure as an example.
[0284] In some of these embodiments, reference Figure 5 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to actual needs.
[0285] The secondary battery may be a battery module 4 or a battery pack 1 .
[0286] The battery module includes at least one battery cell. The number of battery cells contained in the battery module can be one or more, and those skilled in the art can select a suitable number according to the application and capacity of the battery module.
[0287] Figure 6 4 is an example of a battery module. Figure 6 In the battery module 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 5 may be fixed by fasteners.
[0288] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of battery cells 5 are received in the receiving space.
[0289] In some of the embodiments, the battery modules may be assembled into a battery pack. The battery pack may contain one or more battery modules. Those skilled in the art may select a suitable number according to the application and capacity of the battery pack.
[0290] Figure 7 and Figure 8 1 is a battery pack 1 as an example. Figure 7 and Figure 8 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0291] In addition, the present application also provides an electrical device, which includes a secondary battery provided by the present application. The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but are not limited thereto.
[0292] As an electrical device, a secondary battery can be selected according to its usage requirements.
[0293] Fig. 9 The power consumption device 6 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the power consumption device's requirements for high power and high energy density of secondary batteries, a battery pack or a battery module can be used.
[0294] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0295] Example
[0296] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If the techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0297] Example 1
[0298] (1) Preparation of positive electrode active materials
[0299] By target component Li 0.95 Ni 0.5 Mn 1.5 O 4-k Weigh the corresponding stoichiometric ratio of Li 2 CO 3 、NiO、Mn 3 O 4 The powder is then mixed evenly to obtain a mixture powder of the raw materials.
[0300] The mixture powder was subjected to a first sintering treatment (first sintering), that is, the temperature was raised to 1100°C in an air atmosphere and kept at this temperature for 6 hours, and then cooled to room temperature at a rate of 20°C / min to obtain a sintered product, and the positive electrode active material Li 0.95 Ni 0.5 Mn 1.5 O 3.8 .
[0301] (2) Preparation of positive electrode
[0302] The positive electrode active material of step (1) is mixed with conductive carbon black (Super P) and PVDF in a weight ratio of 96:2.5:1.5, and an appropriate amount of solvent N-methylpyrrolidone (NMP) is added and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry is coated on both sides of the positive electrode current collector aluminum foil, and dried after coating to obtain a positive electrode sheet. The loading of the positive electrode active material on one side of the positive electrode current collector is 0.016 g / cm 2 .
[0303] (3) Preparation of negative electrode sheet
[0304] The negative electrode active material artificial graphite, conductive agent carbon black (Super P), binder styrene butadiene rubber, and thickener sodium carboxymethyl cellulose were fully stirred and mixed in a proper amount of solvent deionized water at a mass ratio of 96:1:1:2 to form a uniform negative electrode slurry; the negative electrode slurry was evenly coated on the double-sided surface of the negative electrode current collector copper foil, and after drying and cold pressing, the negative electrode sheet was obtained. The loading amount of negative electrode active material on one side of the negative electrode current collector is 0.007g / cm 2 .
[0305] (4) Isolation film
[0306] A 12μm thick polypropylene isolation film was selected.
[0307] (5) Preparation of electrolyte
[0308] The organic solvent is a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), wherein the volume ratio of EC, EMC and DEC is 20:20:60. In an argon atmosphere glove box with a water content of <10 ppm, a fully dried lithium salt LiPF 6 Dissolve in an organic solvent and mix well to obtain an electrolyte, wherein the concentration of the lithium salt is 1 mol / L.
[0309] (6) Preparation of batteries
[0310] The positive electrode sheet, separator, and negative electrode sheet prepared above are placed in order, with the separator placed between the positive and negative electrode sheets to play a role of isolation, processed into shape, and packaged in an aluminum-plastic bag. The electrolyte is injected, and the packaging is followed by forming the capacity to obtain a soft-pack battery.
[0311] Embodiments 2 to 38
[0312] The preparation of the positive electrode active materials and batteries in Examples 2 to 38 is similar to that in Example 1, except that the relevant parameters of the positive electrode active materials are adjusted. The specific parameters are detailed in Tables 1 and 2 below.
[0313] Embodiment 39
[0314] The preparation of the positive electrode active material and the battery in Example 39 is similar to that in Example 1, except that after obtaining the sintered product in step (1), the sintered product is mechanically mixed with lithium phosphate. The specific parameters are shown in Table 1 below.
[0315] Embodiment 40
[0316] The preparation of the positive electrode active material and the battery in Example 40 is similar to that in Example 1, except that after the sintered product is obtained in step (1), the sintered product is evenly mixed with lithium phosphate and then subjected to a second sintering treatment (second sintering) to achieve the coating of the sintered product with lithium phosphate. The specific parameters are detailed in Tables 1 and 2 below.
[0317] Embodiments 41 to 49
[0318] The preparation of the positive electrode active materials and batteries in Examples 41 to 49 is similar to that in Example 41, except that the type and content of phosphate are changed. The specific parameters are detailed in Tables 1 and 2 below.
[0319] Embodiment 50-51
[0320] The preparation of the positive electrode active material and the battery in Examples 50-51 is similar to that in Example 1, except that after the sintered product is obtained in step (1), the sintered product is evenly mixed with nickel oxide equivalent to 2% by mass of the sintered product and then subjected to a second sintering treatment (second sintering). Specific parameters are shown in Tables 1 and 2 below.
[0321] Embodiment 52-53
[0322] The preparation of the positive electrode active material and the battery in Examples 52-53 is similar to that in Example 1, except that after the sintered product is obtained in step (1), the sintered product is evenly mixed with nickel oxide equivalent to 5% by mass of the sintered product and then subjected to a second sintering treatment (second sintering). Specific parameters are shown in Tables 1 and 2 below.
[0323] Comparative Examples 1 to 4
[0324] The preparation of the positive electrode active materials and batteries in Comparative Examples 1 to 4 is similar to that in Example 1, except that the parameters of the lithium nickel manganese oxide in the positive electrode active material are adjusted. The specific parameters are shown in Tables 1 and 2 below.
[0325] The parameters of the positive electrode active materials and their preparation processes of the above-mentioned Examples 1 to 53 and Comparative Examples 1 to 4 are shown in the following Tables 1 and 2, where " / " indicates that there is no corresponding value. In Table 1, the amount of phosphate added is calculated as a percentage of the mass of the sintered product; for example, the 3% addition in Example 39 represents 3% of the mass of the sintered product.
[0326] Table 1
[0327]
[0328]
[0329]
[0330] Table 2
[0331]
[0332]
[0333]
[0334] In addition, the positive electrode active materials and batteries obtained in the above Examples 1 to 53 and Comparative Examples 1 to 4 were subjected to performance tests, respectively. The test results are shown in Table 3 below.
[0335] Test Section
[0336] (1) X-ray diffraction analysis test
[0337] Referring to JIS K 0131-1996 X-ray diffraction analysis method general rules, CuKα1 rays were used to measure the X-ray diffraction analysis spectrum of the positive electrode active material. The model used was Bruker D8 Discover, and the XRD test analysis conditions were: Cu target, scanning voltage of 40kV, current of 40mA, and scanning range of 10°~90°. In order to reduce the error of spectrum fitting, the instrument measurement step size was 0.02° and the scanning speed was 2° / min.
[0338] (2) Morphology test
[0339] The morphology of the positive electrode active materials was tested using a scanning electron microscope (model: ZEISS sigma 300) and a transmission electron microscope (model: Hitachi, JEM-2100F).
[0340] (3) High temperature full charge storage performance test
[0341] The battery is fully charged at a constant current of 0.3C to a voltage of 4.9V, and then charged at a constant voltage of 4.9V to a current of 0.05C. The battery is fully discharged at a constant current of 0.33C to a voltage of 3.0V. After full charge and standing for 5 minutes, the fully discharged capacity is the discharge capacity of the battery. Dividing this capacity by the mass of the positive electrode active material in the battery is the discharge gram capacity Cn of the positive electrode active material.
[0342] After fully charging the battery at 25°C, place it in a 45°C oven and let it stand. Take it out and fully discharge it every 10 days. Then do a full charge and discharge at 25°C to extract Cn. Then fully charge it again and continue to store it at 45°C. The storage ends when the discharge capacity Cn decays to 100mAh / g (125mAh / g is the benchmark level of the capacity of conventional spinel nickel manganese oxide (LNMO), and 80% is the life end condition generally recognized in the industry). The total storage time at 45°C after full charge is the high-temperature full charge storage time, and this high-temperature full charge storage time can represent the high-temperature full charge storage performance of the battery.
[0343] Table 3
[0344]
[0345]
[0346]
[0347] Comparing Examples 1 to 53 with Comparative Examples 1 to 4, it can be seen that when the X-ray diffraction peak intensity of the positive electrode active material in Comparative Examples 1 to 4 is (111) / I (400) When it is not within the protection scope of this application, the storage life of the battery is significantly reduced, indicating that this application will(111) / I (400) Controlling within the corresponding protection range is beneficial to improving the storage performance of the battery.
[0348] The above description of various embodiments tends to emphasize the differences between the various embodiments. The same or similar aspects can be referenced to each other, and for the sake of brevity, they will not be repeated herein.
[0349] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A positive electrode active material, characterized in that: The invention comprises an active material, wherein the active material comprises a lithium nickel manganese oxide, wherein the lithium nickel manganese oxide comprises a spinel phase and a rock salt phase, wherein an X-ray diffraction analysis spectrum of the lithium nickel manganese oxide has a first diffraction peak at a diffraction angle 2θ of 18° to 19°, a second diffraction peak at a diffraction angle 2θ of 44° to 45°, and a third diffraction peak at a diffraction angle 2θ of 43° to 44°, wherein the first diffraction peak corresponds to a crystal plane (111), and the second diffraction peak corresponds to a crystal plane (400); The peak intensity of the first diffraction peak is 1 (111) , the peak intensity of the second diffraction peak is 1 (400) , I (111) with I (400) Between: 2.5≤I (111) / I (400) ≤4; The lithium nickel manganese oxide satisfies the chemical formula Li x M y Ni z Mn 2-y-z O 4-k , wherein 0.8≤x≤1.05, 0≤y≤0.2, 0.3≤z≤0.7, -0.1≤k≤0.5, and M includes one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W.
2. The positive electrode active material according to claim 1, characterized in that The lithium nickel manganese oxide satisfies: 2.8≤I (111) / I (400) ≤3.
8.
3. The positive electrode active material according to claim 1 or 2, characterized in that: The lithium nickel manganese oxide satisfies: 3.1≤I (111) / I (400) ≤3.
6.
4. The positive electrode active material according to any one of claims 1 to 3, characterized in that: The lithium nickel manganese oxide satisfies at least one of the following conditions: (1)0.85≤x≤1.02; (2)0.01≤y≤0.2。 5. The positive electrode active material according to any one of claims 1 to 4, characterized in that: The lithium nickel manganese oxide satisfies at least one of the following conditions: (1)0.9≤x≤0.99; (2)0.02≤y≤0.1。 6. The positive electrode active material according to any one of claims 1 to 5, characterized in that: The peak intensity of the third diffraction peak is 1 RS , the I RS With the I (400) Satisfy between: 0.01≤I RS / I (400) ≤0.
2.
7. The positive electrode active material according to claim 6, characterized in that I RS With the I (400) Satisfy between: 0.02≤I RS / I (400) ≤0.
1.
8. The positive electrode active material according to claim 6 or 7, characterized in that: I RS With the I (400) Between: 0.05≤I RS / I (400) ≤0.
1.
9. The positive electrode active material according to any one of claims 6 to 8, characterized in that: The lithium nickel manganese oxide satisfies the following conditions: 3.5≤(I (111) +10×I RS ) / I (400) ≤4.
4.
10. The positive electrode active material according to any one of claims 6 to 9, characterized in that: The lithium nickel manganese oxide satisfies the following conditions: 3.6≤(I (111) +10×I RS ) / I (400) ≤4.
1.
11. The positive electrode active material according to any one of claims 1 to 10, characterized in that: The lithium nickel manganese oxide comprises crystal grains of the spinel phase and crystal grains of the rock salt phase, and the crystal grains of the rock salt phase cover at least a portion of the surface of the crystal grains of the spinel phase in the form of a rock salt phase layer.
12. The positive electrode active material according to claim 11, characterized in that The thickness of the rock salt phase layer is 20nm~200nm.
13. The positive electrode active material according to any one of claims 1 to 12, characterized in that: The active material further includes phosphate, and the mass percentage of the phosphate in the active material is m, 0.2%≤m≤20%.
14. The positive electrode active material according to claim 13, characterized in that Satisfy at least one of the following conditions: (1) The m satisfies: 0.5%≤m≤10%; (2) the phosphate is coated on at least a portion of the surface of the lithium nickel manganese oxide; (3) The phosphate includes at least one of orthophosphate, hydrogen phosphate, dihydrogen phosphate, metaphosphate, pyrophosphate, polyphosphate, hypophosphite, phosphite, monofluorophosphate, difluorophosphate and trifluorophosphate containing at least one element of Li, Na, K, Mg, Al, Ti, Zr, La, Ta, Nb, Te, Mo, W, Sb, Ni, Mn, Fe, Co and N.
15. The positive electrode active material according to any one of claims 1 to 14, characterized in that: The active material includes particles of the active material, the particles of the active material include at least one of single crystal grains and quasi-single crystal grains, and the single crystal grains include at least one of truncated octahedral grains and spherical grains.
16. The positive electrode active material according to any one of claims 1 to 15, characterized in that: Satisfy at least one of the following conditions: (1) The compaction density P of the positive electrode active material under a pressure of 6 tons satisfies: P ≥ 3 g / cm 3 ; (2) The volume average particle size Dv50 of the positive electrode active material satisfies: 2 μm ≤ Dv50 ≤ 20 μm; (3) The volume average particle sizes Dv50, Dv90 and Dv10 of the positive electrode active material satisfy the following conditions: 0.8≤(Dv90-Dv10) / Dv50≤2; (4) The specific surface area S of the positive electrode active material satisfies: 0 <S≤1m 2 / g; (5) The pH value of the positive electrode active material satisfies: 9≤pH≤12.
17. The positive electrode active material according to any one of claims 1 to 16, characterized in that: Satisfy at least one of the following conditions: (1) The compaction density P of the positive electrode active material under a pressure of 6 tons satisfies: 3 g / cm 3 ≤P≤3.5g / cm 3 ; (2) The volume average particle size Dv50 of the positive electrode active material satisfies: 3 μm ≤ Dv50 ≤ 15 μm; (3) The volume average particle sizes Dv50, Dv90 and Dv10 of the positive electrode active material satisfy the following conditions: 1.0≤(Dv90-Dv10) / Dv50≤1.8; (4) The specific surface area S of the positive electrode active material satisfies: 0 <S≤0.7m 2 / g; (5) The pH value of the positive electrode active material satisfies: 10≤pH≤12.
18. A method for preparing a positive electrode active material, characterized in that: include: A mixture containing a lithium source, a nickel source, and a manganese source is sintered to obtain a positive electrode active material. The positive electrode active material includes an active substance, the active substance includes lithium nickel manganese oxide, the lithium nickel manganese oxide includes a spinel phase and a rock salt phase, the X-ray diffraction analysis spectrum of the lithium nickel manganese oxide has a first diffraction peak at a diffraction angle 2θ of 18° to 19°, a second diffraction peak at a diffraction angle 2θ of 44° to 45°, and a third diffraction peak at a diffraction angle 2θ of 43° to 44°, the first diffraction peak corresponds to a crystal plane (111), and the second diffraction peak corresponds to a crystal plane (400); the peak intensity of the first diffraction peak is 1 (111) , the peak intensity of the second diffraction peak is 1 (400) , and I (111) with I (400) Between: 2.5≤I (111) / I (400) ≤4; the lithium nickel manganese oxide satisfies the chemical formula Li x M y Ni z Mn 2-y-z O 4-k , wherein 0.8≤x≤1.05, 0≤y≤0.2, 0.3≤z≤0.7, -0.1≤k≤0.5, and M includes one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W.
19. The method according to claim 18, characterized in that The sintering process comprises: The mixture is heated to a first sintering temperature T1, maintained at the first sintering temperature T1 for a first preset time t1, and then cooled to room temperature at a first cooling rate v1 to obtain a sintered product.
20. The method according to claim 19, characterized in that Satisfy at least one of the following conditions: (1) The first sintering temperature T1 satisfies: 900°C≤T1≤1500°C, and T1≥x×1000°C; (2) The first preset time t1 satisfies: 1h≤t1≤20h; (3) The first cooling rate v1 satisfies: v1 ≥ 10°C / min.
21. The method according to claim 19 or 20, characterized in that Satisfy at least one of the following conditions: (1) The first sintering temperature T1 satisfies: 1000°C ≤ T1 ≤ 1300°C; (2) The first preset time t1 satisfies: 2h≤t1≤15h; (3) The first cooling rate v1 satisfies: 10°C / min≤v1≤50°C / min.
22. The method according to any one of claims 18 to 21, characterized in that: Satisfy at least one of the following conditions: (1) The mixture further comprises an M source; The M source includes one or more of oxides, nitric acid compounds, carbonate compounds, hydroxide compounds and acetic acid compounds containing the M element, and the M element includes one or more of B, Si, P, S, Nb, Mo, Ru, Te, Ce, Ta and W; (2) The lithium source includes one or more of lithium oxide, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium hydroxide, lithium carbonate and lithium nitrate; (3) The nickel source includes one or more of nickel oxide, nickel phosphate, nickel acetate, nickel hydroxide, nickel carbonate and nickel nitrate; (4) The manganese source includes one or more of manganese oxide, manganese phosphate, manganese acetate, manganese hydroxide, manganese carbonate and manganese nitrate.
23. The method according to any one of claims 19 to 22, characterized in that: The sintering process also includes: The material including the sintered product is heated to a second sintering temperature T2, kept at the second sintering temperature T2 for a second preset time t2, and then cooled to room temperature at a second cooling rate v2.
24. The method according to claim 23, characterized in that Satisfy at least one of the following conditions: (1) The second sintering temperature T2 satisfies: T1-200°C≤T2≤T1, T2≥900°C; (2) The second preset time t2 satisfies: 0.5h≤t2≤5h; (3) The second cooling rate v2 satisfies: v2 ≥ 10°C / min; (4) The material further comprises phosphate, wherein the phosphate comprises at least one of orthophosphate, hydrogen phosphate, dihydrogen phosphate, metaphosphate, pyrophosphate, polyphosphate, hypophosphite, phosphite, monofluorophosphate, difluorophosphate and trifluorophosphate containing at least one element of Li, Na, K, Mg, Al, Ti, Zr, La, Ta, Nb, Te, Mo, W, Sb, Ni, Mn, Fe, Co and N.
25. The method according to claim 23 or 24, characterized in that Satisfy at least one of the following conditions: (1) The second sintering temperature T2 satisfies: T1-100°C≤T2≤T1, T2≥950°C; (2) The second cooling rate v2 satisfies: 10°C / min≤v2≤50°C / min.
26. A positive electrode plate, characterized in that: The invention comprises a positive electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 17 or the positive electrode active material prepared by the method according to any one of claims 18 to 25.
27. The positive electrode sheet according to claim 26, characterized in that: The compaction density P' of the positive electrode active material layer satisfies: P'≥2.9g / cm 3 .
28. The positive electrode sheet according to claim 26 or 27, characterized in that: The compaction density P' of the positive electrode active material layer satisfies: 3 g / cm 3 ≤P'≤3.6g / cm 3 .
29. A secondary battery, characterized in that: Comprising the positive electrode sheet as described in any one of claims 26-28.
30. An electrical device, characterized in that: Includes the secondary battery as claimed in claim 29.
Citation Information
Patent Citations
Positive electrode active material and preparation method thereof, positive electrode plate, secondary battery and electric device
CN117080419A
Positive active material of non-aqueous electrolytic secondary battery and non-aqueous electrolytic secondary battery containing said material
CN1352471A
Spinel type lithium manganese oxide and method for manufacturing the same
JP2008156163A
Nonaqueous electrolyte battery, positive electrode active material to be used therein, and process for production thereof
WO2011089697A1
Cited By
Lithium nickel manganese oxide positive electrode material, preparation method thereof and battery
CN119370911A
A lithium nickel manganese oxide positive electrode material and preparation method thereof and battery
CN119370911B
Positive active material and preparation method thereof, positive pole piece, secondary battery and electric device
CN120895615A
Positive electrode plate and use thereof
WO2026114067A1
Positive electrode active material and preparation method therefor, positive electrode sheet, and battery
WO2026144165A1