System and method for dynamically regulating and controlling viscosity of copper ore sulfonium-making slag

By monitoring and analyzing the temperature and composition of the slag in real time, and using programmable logic controllers and mechanical grippers to adjust the amount of pulverized coal and flux, the problem of unstable slag properties in traditional copper ore smelting has been solved, and real-time control of the smelting process has been achieved. and efficient production.

CN118745523APending Publication Date: 2024-10-08KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410967176.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult to accurately control the properties of slag during the traditional copper ore smelting process, resulting in unstable product quality and low efficiency. It lacks real-time adjustment means and relies on manual experience and separate sample delivery for testing, making it impossible to achieve continuity and real-time monitoring of the smelting process.

Method used

A system including a temperature sensor, composition analyzer and programmable logic controller is used to collect and analyze slag temperature and composition data in real time, and dynamically adjust the amount of pulverized coal and flux through a mechanical gripper to achieve closed-loop control of slag viscosity and reduce manual labor. intervention.

Benefits of technology

It achieves real-time control during the smelting process, improves production efficiency and product quality stability, and ensures the stability of the process and easy fault detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745523A_ABST
    Figure CN118745523A_ABST
Patent Text Reader

Abstract

The invention discloses a system and a method for dynamically regulating and controlling viscosity of copper ore matte slag, and belongs to the technical field of metallurgy. The system comprises a temperature sensor, a component analyzer, a mechanical gripper and a programmable logic controller, the programmable logic controller is in data connection with the temperature sensor to obtain temperature data; the component analyzer is in data connection with the programmable logic controller, performs real-time data analysis on the components of the slag, stores the data and transmits the data to the programmable logic controller; the programmable logic controller is in data connection with the mechanical gripper and controls the mechanical gripper to adjust the gripping amount of the pulverized coal and the flux. In the smelting process, the viscosity of the slag and the temperature in the furnace are monitored in real time, the component dosage of pulverized coal and flux is calculated according to the relation between the viscosity of the slag and the temperature and the relation between the viscosity of the slag and the dosage of the flux, the viscosity of the slag is adjusted, the viscosity of the slag is made to be within the set range, and therefore the requirement for closed-loop precise control over the smelted slag is met; the problems that in the traditional smelting process, slag is unstable in property and difficult to control are solved, and the stability of the viscosity of the slag is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a system and method for dynamically regulating the viscosity of copper ore matte slag. Background Art

[0002] Complex copper ore smelting is one of the key links in the copper metallurgical process, in which slag is an important intermediate product. In the traditional smelting process, the properties of slag are often difficult to accurately control, including the physical and chemical properties of slag such as viscosity, density, structure, and slag liquid composition, which leads to problems such as unstable quality of smelting slag products and low efficiency.

[0003] At present, slag control mainly relies on manual experience or post-testing of smelting slag, and most of them adopt separate sample testing, which cannot be adjusted in real time during smelting. There is no real-time performance, slag viscosity feedback lags, and operators are not liberated from production. In addition, the slag temperature is currently measured only by workers holding a temperature gun, which cannot achieve the continuity of the smelting process. Summary of the invention

[0004] In view of the shortcomings of the above-mentioned prior art, the present invention proposes a system and method for dynamically regulating the viscosity of copper mine matte slag. The system and method provided by the present invention can perform real-time regulation during the smelting process, adopt closed-loop control of slag viscosity, without manual intervention, with high work efficiency, and can improve the production efficiency of the enterprise. In addition, the programmable logic controller has the characteristics of strong adaptability and diverse functions, and can meet the needs of various connection methods, thereby ensuring the stability of the production process of the entire process. In addition, the fault display is indicated by a corresponding signal, which is easy to detect the fault.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a system for dynamically controlling the viscosity of copper ore matte slag includes: a temperature sensor, a component analyzer, a mechanical gripper and a programmable logic controller;

[0006] The temperature sensor is used to collect the slag temperature in real time; the component analyzer is used to detect the slag composition in real time; the mechanical gripper is used to grab the coal powder and flux dosage; the programmable logic controller is used to dynamically adjust the slag temperature and flux content into the furnace and adjust the slag properties;

[0007] The programmable logic controller is connected to the temperature sensor data to obtain temperature data; the composition analyzer is connected to the programmable logic controller data to perform real-time data analysis on the composition of the slag, store and transmit it to the programmable logic controller; the programmable logic controller is connected to the mechanical gripper data to control the mechanical gripper to adjust the grabbing amount of coal powder and flux.

[0008] The present invention also claims a method for dynamically controlling the viscosity of copper ore matte slag, comprising the following steps:

[0009] (1) A temperature sensor is installed in the furnace and connected to the programmable logic controller to collect the temperature of the slag in real time;

[0010] (2) Connecting the composition analyzer to the programmable logic controller, initializing the data, and performing real-time data detection and storage of the slag composition;

[0011] (3) A mechanical gripper is set up and connected to a programmable logic controller. The programmable logic controller uses the temperature collected by the temperature sensor and the data of the composition analyzer as the basis. According to the relationship between slag viscosity and slag temperature, slag temperature and coal powder dosage, and slag viscosity and slag composition under the target viscosity, the mechanical gripper is controlled to adjust the gripping of coal powder and flux components to achieve the target slag viscosity.

[0012] As a preferred embodiment of the present invention, in the step (3), according to the slag viscosity and slag temperature, and the slag temperature and coal powder dosage at the target viscosity, the mechanical gripper is controlled to adjust the coal powder grabbing to achieve the target slag viscosity. When the coal powder dosage at the current viscosity is greater than or equal to the coal powder dosage at the target viscosity, there is no need to add coal powder; when the coal powder dosage at the current viscosity is less than the coal powder dosage at the target viscosity, the programmable logic controller controls the mechanical gripper to add coal powder to the smelting furnace in an amount equal to the difference between the target viscosity and the coal powder dosage at the current viscosity.

[0013] As a preferred embodiment of the present invention, the relationship between the slag viscosity and the slag temperature is:

[0014] η 熔渣 =(-1.055×10 -8 )*T 3 +4.294×10 -5 *T 2 +(-0.05891)*T+27.35 (1);

[0015] Where η 熔渣 is the slag viscosity, Pa·s; T is the slag temperature, ℃.

[0016] As a preferred embodiment of the present invention, the relationship between the amount of coal powder g and the temperature T is:

[0017] g = 2.53933T - 2765.1672 (2);

[0018] In the formula, g is the amount of pulverized coal used, kg / h.

[0019] As a preferred embodiment of the present invention, the slag composition includes Al2O3, MgO, SiO2, CaO and FeO, and the relationship between the slag viscosity and the content of Al2O3, MgO, SiO2, CaO and FeO in the slag is:

[0020] The total content of Al2O3, MgO, SiO2, CaO and FeO in the slag, excluding other components, is 100%: h+i+u+n+w=100% (3);

[0021] Al2O3 mass percentage h and viscosity η 熔渣 The calculation relationship is:

[0022] η 熔渣 =5.634×10 -4 *h 2 +0.007039*h+0.1741 (4);

[0023] MgO mass percentage i and viscosity η 熔渣 The calculation relationship is:

[0024] η 熔渣 =-1.219×10 -5 *i 5 +2.059×10 -4 *i 4 +-1.364×10 -3 *i 3 +4.408×10 -3 *i 2

[0025] +-6.931×10 -3 *i+0.2043(5);

[0026] The mass percentage of SiO2 u and viscosity η 熔渣 The calculation relationship is:

[0027] η 熔渣 =4.379×10 -4 *u 2 +-1.059×10 -2 *u+0.1608 (6);

[0028] CaO mass percentage n and viscosity η 熔渣 The calculation relationship is:

[0029] η 熔渣 =-1.162×10 -5 *n 3 +3.621×10 -4 *n 2+-4.375×10 -3 *n+0.2158 (7);

[0030] FeO mass percentage w and viscosity η 熔渣 The calculation relationship is:

[0031] η 熔渣 =-9.177×10 -6 *w 3 +1.607×10 -3 *w 2 +-9.873×10 -2 *w+0.255 (8).

[0032] As a preferred embodiment of the present invention, in the step (3), according to the relationship between the slag viscosity and the slag composition at the target viscosity, the determination of the amount of the flux component to be grasped by the mechanical gripper specifically includes:

[0033] S1: Use a component analyzer to analyze the contents of Al2O3, MgO, SiO2, CaO and FeO in the slag, and then calculate the current viscosity of the slag according to formulas (3)-(8). If the current viscosity is not within the target viscosity range, the programmable logic controller will re-determine the amount of flux component to be added;

[0034] S2: According to formulas (3)-(8), determine the contents of Al2O3, MgO, SiO2, CaO and FeO in the slag at the target viscosity; calculate the total amount of flux at the target viscosity according to the iron-silicon ratio of the slag at the target viscosity; then multiply the contents of Al2O3, MgO, SiO2, CaO and FeO in the slag by the total amount of flux respectively to obtain the addition amounts of Al2O3, MgO, SiO2, CaO and FeO in the flux at the target viscosity;

[0035] S3: The addition amount of Al2O3, MgO, SiO2, CaO and FeO in the flux at the current viscosity is compared with the addition amount of Al2O3, MgO, SiO2, CaO and FeO in the flux at the target viscosity. If the addition amount of one or some components of Al2O3, MgO, SiO2, CaO or FeO in the flux at the current viscosity is less than the addition amount of the corresponding component in the flux at the target viscosity, the programmable logic controller controls the mechanical gripper to add the amount of the component to the melting furnace to be the difference between the addition amount of the component at the target viscosity and the current viscosity;

[0036] S4: If the addition amount of one or some components of Al2O3, MgO, SiO2, CaO or FeO in the flux at the current viscosity is greater than or equal to the addition amount of the corresponding components in the flux at the target viscosity, there is no need to add the corresponding components.

[0037] As a preferred embodiment of the present invention, the flux includes Al2O3, MgO, SiO2, CaO and FeO.

[0038] As a preferred embodiment of the present invention, the relationship between the mass ratio of FeO and SiO2 in the slag and the total amount of flux is calculated as follows:

[0039] Y=3129.95238X 2 -17150.96429X+22870.7194 (9);

[0040] Where Y is the total amount of flux, kg / h; X is the mass ratio of FeO and SiO2 in the slag.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] During the smelting process, the present invention monitors the slag viscosity and the temperature in the furnace in real time, calculates the amount of pulverized coal and the flux component according to the relationship between the slag viscosity and the temperature and the relationship between the slag viscosity and the amount of flux, and adjusts the slag viscosity so that the slag viscosity is within a set range, thereby meeting the requirement of closed-loop precise control of the smelting slag, solving the problem of unstable and difficult-to-control slag properties in the traditional smelting process, and ensuring the stability of the slag viscosity. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 The present invention is a flow chart of a system for dynamically regulating the viscosity of copper ore matte-making slag for dynamically regulating the viscosity of copper ore matte-making slag.

[0044] Figure 2 The present invention is a schematic diagram of a system for dynamically regulating the viscosity of copper ore matte-making slag. DETAILED DESCRIPTION

[0045] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0046] Example 1

[0047] like Figure 2 As shown, a system for dynamically controlling the viscosity of copper ore matte slag includes: a temperature sensor, a component analyzer, a mechanical gripper and a programmable logic controller;

[0048] The temperature sensor is used to collect the slag temperature in real time; the component analyzer is used to detect the slag composition in real time; the mechanical gripper is used to grab the coal powder and flux dosage; the programmable logic controller is used to dynamically adjust the slag temperature and flux content into the furnace and adjust the slag properties;

[0049] The programmable logic controller is connected to the temperature sensor data to obtain temperature data; the composition analyzer is connected to the programmable logic controller data to perform real-time data analysis on the composition of the slag, store and transmit it to the programmable logic controller; the programmable logic controller is connected to the mechanical gripper data to control the mechanical gripper to adjust the grabbing amount of coal powder and flux.

[0050] like Figure 1 As shown, a method for dynamically controlling the viscosity of copper ore matte slag using a system for dynamically controlling the viscosity of copper ore matte slag comprises the following steps:

[0051] (1) The smelting temperature set in the furnace is 1278°C, and the smelting raw materials and the amount of smelting raw materials added are shown in Table 1. The amount of flux added is 1088.60 kg / h, and the amount of coal powder added is 510.57 kg / h. The interval time for adding solvent and coal powder can be added according to actual needs. In this embodiment, the sample is added once every 24 hours.

[0052] Table 1

[0053] Ore type Total amount of ore added / kg Ore proportion / % Imported ore 253000.00 22.81 Mingchuan 23 241500.00 21.77 70 batches of miscellaneous ore 396762.00 35.77 Jinduoli29 195500.00 17.62 Oxidation slag 22483.00 2.03 Total amount of ore fed into the furnace 1109245.00 100.00

[0054] (2) A temperature sensor is installed in the furnace and connected to the programmable logic controller to collect the temperature of the slag in real time.

[0055] (3) Connect the composition analyzer to the programmable logic controller, initialize the data, and store the slag composition in real time. The interval time for slag composition analysis is 0.5 hours, which can be extended or shortened according to actual needs.

[0056] (4) A mechanical gripper is provided and data is connected to a programmable logic controller. Based on the temperature collected by the temperature sensor and the data of the composition analyzer, and according to the relationship between the slag viscosity and temperature, and between the slag viscosity and the slag composition under the target viscosity, the programmable logic controller (PLC) program is operated to control the mechanical gripper to adjust the gripping of the coal powder and the flux composition during the smelting process, so as to ensure that the slag viscosity tends to be stable and reaches the target slag viscosity, which specifically includes:

[0057] S1: Set the target viscosity, use a temperature sensor to collect the temperature of the slag at the current state, use a component analyzer to analyze the content of Al2O3, MgO, SiO2, CaO and FeO in the slag at the current state, and then calculate the current viscosity of the slag according to formulas (3)-(8). Compare whether the current viscosity is within the target viscosity range. If not, the programmable logic controller analyzes the temperature and slag composition and adjusts the dosage. If the current viscosity is the target viscosity, maintain the amount of flux and coal powder added.

[0058] S2: According to formulas (3)-(8), determine the contents of Al2O3, MgO, SiO2, CaO and FeO in the slag at the target viscosity; calculate the total amount of flux at the target viscosity according to the mass ratio of FeO and SiO2 in the slag at the target viscosity through formula (9); then, multiply the contents of Al2O3, MgO, SiO2, CaO and FeO in the slag by the total amount of flux respectively to obtain the addition amount of Al2O3, MgO, SiO2, CaO and FeO in the flux at the target viscosity.

[0059] The slag components include Al2O3, MgO, SiO2, CaO, FeO and others. The present invention only considers Al2O3, MgO, SiO2, CaO and FeO components related to viscosity. Therefore, the total content of Al2O3, MgO, SiO2, CaO and FeO in the slag is 100%: h+i+u+n+w=100% (3);

[0060] The relationship between slag viscosity and the contents of Al2O3, MgO, SiO2, CaO and FeO in the slag is:

[0061] Al2O3 mass percentage h and viscosity η 熔渣 The calculation relationship is:

[0062] η 熔渣 =5.634×10-4*h 2 +0.007039*h+0.1741 (4);

[0063] MgO mass percentage i and viscosity η 熔渣 The calculation relationship is:

[0064] η 熔渣 =-1.219×10 -5 *i^5+2.059×10 -4 *i 4 +-1.364×10 -3 *i 3 +4.408×10 -3 *i 2

[0065] +-6.931×10 -3 *i+0.2043(5);

[0066] The mass percentage of SiO2 u and viscosity η 熔渣 The calculation relationship is:

[0067] η 熔渣 =4.379×10 -4 *u 2 +-1.059×10-2 *u+0.1608 (6);

[0068] CaO mass percentage n and viscosity η 熔渣 The calculation relationship is:

[0069] η 熔渣 =-1.162×10 -5 *n 3 +3.621×10 -4 *n 2 +-4.375×10 -3 *n+0.2158 (7);

[0070] FeO mass percentage w and viscosity η 熔渣 The calculation relationship is:

[0071] η 熔渣 =-9.177×10 -6 *w 3 +1.607×10 -3 *w 2 +-9.873×10 -2 *w+0.255 (8).

[0072] The relationship between the mass ratio of FeO and SiO2 in the slag and the total amount of flux is:

[0073] Y=3129.95238X 2 -17150.96429X+22870.7194 (9);

[0074] Where Y is the total amount of flux, kg / h; X is the mass ratio of FeO and SiO2 in the slag.

[0075] S3: The addition amounts of Al2O3, MgO, SiO2, CaO and FeO in the flux at the current viscosity are compared with the addition amounts of Al2O3, MgO, SiO2, CaO and FeO in the flux at the target viscosity. If the addition amount of one or some components of Al2O3, MgO, SiO2, CaO or FeO in the flux at the current viscosity is less than the addition amount of the corresponding components in the flux at the target viscosity, the programmable logic controller controls the mechanical gripper to add the amount of the component to the smelting furnace to be the difference between the addition amount of the component at the target viscosity and the current viscosity.

[0076] S4: If the addition amount of one or some components of Al2O3, MgO, SiO2, CaO or FeO in the flux at the current viscosity is greater than or equal to the addition amount of the corresponding components in the flux at the target viscosity, there is no need to add the corresponding components.

[0077] S5: The slag temperature at the target viscosity is calculated by the relationship between the slag viscosity and the slag temperature (1), and then the amount of coal powder added at the target viscosity is calculated according to the relationship between the coal powder dosage g and the temperature T (2); when the coal powder dosage at the current viscosity is greater than or equal to the coal powder dosage at the target viscosity, there is no need to add coal powder; when the coal powder dosage at the current viscosity is less than the coal powder dosage at the target viscosity, the programmable logic controller controls the mechanical gripper to add coal powder to the smelting furnace in an amount equal to the difference between the coal powder dosage at the target viscosity and the coal powder dosage at the current viscosity.

[0078] The relationship between the slag viscosity and the slag temperature is:

[0079] η 熔渣 =(-1.055×10 -8 )*T 3 +4.294×10 -5 *T 2 +(-0.05891)*T+27.35 (1);

[0080] Where η 熔渣 is the slag viscosity, and T is the slag temperature.

[0081] The relationship between the amount of coal powder g and the temperature T is:

[0082] g = 2.53933T - 2765.1672 (2);

[0083] In the formula, g is the amount of pulverized coal used, kg / h.

[0084] S6: In order to achieve the purpose of slag viscosity being the target viscosity, the programmable logic controller (PLC) adjusts the gripping amount of the mechanical gripper within the unit response time (i.e., analyzing the slag composition at intervals of 0.5h). At the same time, the programmable logic controller (PLC) will consume the amount of coal powder corresponding to the temperature difference between the target slag temperature and the current slag temperature within the response time to meet the subsequent smelting conditions. When the slag viscosity is stabilized at the target viscosity and the solvent and coal powder are consumed during the smelting process, the amount of coal powder and the amount of each component of the flux in the next stage will be added according to the amount of coal powder and the amount of each component of the flux at the target viscosity.

[0085] The temperature sensor monitors the slag temperature, the analyzer analyzes the composition, the programmable logic controller (PLC) controls and the mechanical gripper executes the closed-loop control to achieve precise control of the slag viscosity.

[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A system for dynamically controlling the viscosity of copper ore matte slag, characterized in that: include: temperature sensors, composition analyzers, robotic grippers, and programmable logic controllers; The temperature sensor is used to collect the slag temperature in real time; The component analyzer detects the slag composition in real time; the mechanical gripper is used to grab the coal powder and flux amount; The programmable logic controller is used to dynamically adjust the slag temperature and flux content in the furnace to adjust the slag properties; The programmable logic controller is connected to the temperature sensor data to obtain temperature data; the composition analyzer is connected to the programmable logic controller data to perform real-time data analysis on the composition of the slag, store it and transmit it to the programmable logic controller; the programmable logic controller is connected to the mechanical gripper data to control the mechanical gripper to adjust the grabbing amount of coal powder and flux.

2. A method for dynamically controlling the viscosity of copper ore matte slag, characterized in that: The steps include: (1) A temperature sensor is installed in the furnace and connected to the programmable logic controller to collect the slag temperature in real time; (2) Connecting the component analyzer to the programmable logic controller, initializing the data, and performing real-time data detection and storage of the slag composition; (3) A mechanical gripper is set up and connected to the programmable logic controller. The programmable logic controller uses the temperature collected by the temperature sensor and the data of the composition analyzer as the basis. According to the relationship between slag viscosity and slag temperature, slag temperature and coal powder dosage, and slag viscosity and slag composition under the target viscosity, the mechanical gripper is controlled to adjust the gripping of coal powder and flux components to achieve the target slag viscosity.

3. The method for dynamically controlling the viscosity of copper ore matte slag according to claim 2, characterized in that: In the step (3), the mechanical gripper is controlled to adjust the coal powder gripping according to the slag viscosity and slag temperature, and the slag temperature and coal powder amount at the target viscosity to achieve the target slag viscosity; when the coal powder amount at the current viscosity is greater than or equal to the coal powder amount at the target viscosity, there is no need to add coal powder; when the coal powder amount at the current viscosity is less than the coal powder amount at the target viscosity, the programmable logic controller controls the mechanical gripper to add coal powder to the smelting furnace in an amount equal to the difference between the coal powder amount at the target viscosity and the coal powder amount at the current viscosity.

4. The method for dynamically controlling the viscosity of copper ore matte slag according to claim 2, characterized in that: The relationship between the slag viscosity and the slag temperature is: η 熔渣 =(-1.055×10 -8 )*T 3 +4.294×10 -5 *T 2 +(-0.05891)*T+27.35 (1); Where η 熔渣 is the slag viscosity, Pa·s; T is the slag temperature, °C.

5. The method for dynamically controlling the viscosity of copper ore matte slag according to claim 2, characterized in that: The relationship between the amount of pulverized coal g and the temperature T is: g=2.53933T-2765.1672 (2); Where g is the amount of pulverized coal used, kg / h.

6. The method for dynamically controlling the viscosity of copper ore matte slag according to claim 2, characterized in that: The slag components include Al2O3, MgO, SiO2, CaO and FeO. The relationship between the slag viscosity and the content of Al2O3, MgO, SiO2, CaO and FeO in the slag is: The total content of Al2O3, MgO, SiO2, CaO and FeO in the slag is 100%: h+i+u+n+w=100% (3); Al2O3 mass percentage h and viscosity η 熔渣 The calculation relationship is: or 熔渣 =5.634×10 -4 *h 2 +0.007039*h+0.1741 (4); MgO mass percentage i and viscosity η 熔渣 The calculation relationship is: η 熔渣 =-1.219×10 -5 *i 5 +2.059×10 -4 *i 4 +-1.364×10 -3 *i 3 +4.408×10 -3 *i 2 +-6.931×10 -3 *i+0.2043(5); The mass percentage of SiO2 u and viscosity η 熔渣 The calculation relationship is: η 熔渣 =4.379×10 -4 *in 2 +-1.059×10 -2 *u+0.1608 (6); CaO mass percentage n and viscosity η 熔渣 The calculation relationship is: or 熔渣 =-1.162×10 -5 *n 3 +3.621×10 -4 *n 2 +-4.375×10 -3 *n+0.2158 (7); FeO mass percentage w and viscosity η 熔渣 The calculation relationship is: η 熔渣 =-9.177×10 -6 *w 3 +1.607×10 -3 *w 2 +-9.873×10 -2 *w+0.255 (8)。 7. The method for dynamically controlling the viscosity of copper ore matte slag according to claim 6, characterized in that: In step (3), the determination of the amount of flux components to be grasped by the mechanical gripper according to the relationship between the slag viscosity and the slag composition at the target viscosity specifically includes: S1: Set the target viscosity and use a component analyzer to analyze the contents of Al2O3, MgO, SiO2, CaO, and FeO in the slag. Then, calculate the current viscosity of the slag according to formulas (3)-(8). If the current viscosity is not within the target viscosity range, the programmable logic controller analyzes the slag composition and adjusts the dosage. S2: Determine the contents of Al2O3, MgO, SiO2, CaO, and FeO in the slag at the target viscosity according to formulas (3)-(8); calculate the total amount of flux at the target viscosity according to the iron-silicon ratio of the slag at the target viscosity; then multiply the contents of Al2O3, MgO, SiO2, CaO, and FeO in the slag by the total amount of flux to obtain the addition amounts of Al2O3, MgO, SiO2, CaO, and FeO in the flux at the target viscosity; S3: The addition amounts of Al2O3, MgO, SiO2, CaO and FeO in the flux at the current viscosity are compared with the addition amounts of Al2O3, MgO, SiO2, CaO and FeO in the flux at the target viscosity. If the addition amount of one or some components of Al2O3, MgO, SiO2, CaO or FeO in the flux at the current viscosity is less than the addition amount of the corresponding components in the flux at the target viscosity, the programmable logic controller controls the mechanical gripper to add the amount of the component to the melting furnace equal to the difference between the addition amount of the component at the target viscosity and the current viscosity; S4: If the addition amount of one or some components of Al2O3, MgO, SiO2, CaO or FeO in the flux at the current viscosity is greater than or equal to the addition amount of the corresponding components in the flux at the target viscosity, there is no need to add the corresponding components.

8. The method for dynamically controlling the viscosity of copper ore matte slag according to claim 7, characterized in that: The flux includes Al2O3, MgO, SiO2, CaO and FeO.

9. The method for dynamically controlling the viscosity of copper ore matte slag according to claim 7, characterized in that: The relationship between the mass ratio of FeO and SiO2 in the slag and the total amount of flux is: Y=3129.95238X 2 -17150.96429X+22870.7194 (9); Where Y is the total amount of flux, kg / h; X is the mass ratio of FeO and SiO2 in the slag.

Citation Information

Cited By

  • Refractory brick pug temperature real-time detection, regulation and control system and detection, regulation and control method

    CN118963455A

  • Slag rocking smelting control method and system

    CN121349035A

  • Method for predicting viscosity of smelting slag of oxidized-copper sulfide concentrate and application of method

    CN121438992A

  • Oxidized-copper sulfide concentrate smelting furnace slag viscosity prediction method and application thereof

    CN121438992B