Underwater anti-dispersion repairing material for hydraulic structure and preparation method thereof

By using specific proportions of cement, fly ash, microsilica fume, magnesium oxide and other materials in hydraulic building repair materials, and using the combined effect of polyacrylamide and super absorbent resin, we have solved the problem of underwater repair materials. In order to solve the problems of forming and strength in complex environments, it achieves early strength, rapid hardening, anti-dispersion and improved construction performance, and is suitable for repairing underwater concrete defects.

CN118754567APending Publication Date: 2024-10-11WUHAN POLYTECHNIC UNIVERSITY

Patent Information

Application Number
CN202411044590.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Hydraulic structures are prone to damage and cracking in complex environments. Existing cement-based repair materials are difficult to form underwater and have insufficient strength. The addition of commonly used anti-dispersion agents will increase pores and prolong the setting time, affecting construction efficiency and water resistance. Flushing ability.

Method used

Use 30~40 parts of cement, 10~15 parts of fly ash, 5~10 parts of microsilica fume, 15~25 parts of magnesium oxide, 4~7 parts of ammonium dihydrogen phosphate, 0.5~1.5 parts of anti-dispersion agent, 0.5~1 fiber, 0.1~0.5 parts water reduction The ratio of agent, 1 to 2 parts of retarder, and 10 to 15 parts of water, through the combined effect of polyacrylamide and super absorbent resin, achieves early strength and rapid hardening, high strength, strong adhesion, and excellent dispersion resistance. The underwater repair material adopts a self-compacting preparation method.

Benefits of technology

It achieves high strength and anti-dispersion properties of underwater repair materials, can be quickly consolidated to resist erosion by running water, has good construction performance and filling properties, avoids the need for enclosure waterproofing, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an underwater anti-dispersion repair material for a hydraulic structure and a preparation method of the underwater anti-dispersion repair material. The repair material is prepared from the following raw materials in parts by weight: 30-40 parts of cement, 10-15 parts of fly ash, 5-10 parts of micro-silica fume, 15-25 parts of magnesium oxide, 4-7 parts of ammonium dihydrogen phosphate, 0.5-1.5 parts of an anti-dispersion agent, 0.5-1 part of fiber, 0.1-0.5 part of a water reducing agent, 1-2 parts of a retarder and 10-15 parts of water. The underwater anti-dispersion repair material for the hydraulic structure has the characteristics of short setting time, high early strength, good anti-dispersion property, good adhesion between new and old interfaces, good construction performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydraulic structure repair, in particular to a cement-based hydraulic structure underwater anti-dispersion repair material and a preparation method thereof. Background Art

[0002] The environment in which hydraulic structures are located is complex. They are easily damaged and cracked under the influence of dry-wet changes, low-temperature freeze-thaw cycles, ion erosion, etc., which affects the normal use function of the buildings. There are many hydraulic structures in my country, and most of them have defects to varying degrees. In order to avoid the defects from further expanding and affecting the overall safety of the buildings, timely diagnosis and repair are required. However, the underwater environment is complex, and ordinary cement-based repair materials are prone to dispersion and segregation underwater, making them difficult to form and their strength cannot be guaranteed. It is necessary to develop an underwater anti-dispersion repair material for hydraulic structures. However, the commonly used anti-dispersant directly added to cement-based materials will introduce more pores, resulting in low strength. At the same time, the addition of anti-dispersant prolongs the setting time, making it difficult to resist water erosion after pouring, and a setting time that is too short is not conducive to construction. Therefore, it is necessary to develop an underwater anti-dispersion repair material for hydraulic structures with moderate setting time, high strength, strong adhesion between the new and old interfaces, and excellent anti-dispersion properties in response to the needs of hydraulic structure repair. Summary of the Invention

[0003] The present invention aims to provide an underwater anti-dispersion repair material for hydraulic structures, which has the characteristics of early strength and rapid hardening, strong adhesion to old concrete surfaces, good underwater anti-dispersion properties, and ease of construction. To achieve the above-mentioned objectives, the present invention provides, in a first aspect, an underwater repair material for hydraulic structures, comprising: 30-40 parts of cement, 10-15 parts of fly ash, 5-10 parts of microsilica fume, 15-25 parts of magnesium oxide, 4-7 parts of ammonium dihydrogen phosphate, 0.5-1.5 parts of an anti-dispersion agent, 0.5-1 part of fiber, 0.1-0.5 parts of a water reducer, 1-2 parts of a retarder, and 10-15 parts of water.

[0004] As a preferred embodiment of the present invention, the cement is ordinary Portland cement with a strength grade of 42.5.

[0005] As a preferred embodiment of the present invention, the fly ash is low-calcium fly ash with a particle size of less than 45 μm.

[0006] As a preferred embodiment of the present invention, the SiO2 content in the microsilica fume is 98%, and the specific surface area is 19300m 2 / kg.

[0007] As a preferred embodiment of the present invention, the magnesium oxide is dead-burned magnesium oxide with a fineness of 400 mesh.

[0008] In a preferred embodiment of the present invention, the anti-dispersion agent is one or more of polyacrylamide and a superabsorbent resin. The polyacrylamide has a molecular weight of 10 million and is added in an amount of 0.5% to 1%. The superabsorbent resin is sodium polyacrylate with a molecular weight of 20 million and a particle size of 300 to 500 nm, and is added in an amount of 0.1% to 0.5%.

[0009] As a preferred embodiment of the present invention, the fiber is polyvinyl alcohol fiber with a diameter of 15 μm, a length of 12 mm, and a tensile strength of 1830 MPa.

[0010] As a preferred embodiment of the present invention, the water reducer is a powdered polycarboxylic acid high-efficiency water reducer.

[0011] As a preferred embodiment of the present invention, the retarder is industrial-grade borax with a purity of ≥95% and a fineness of 100-150 mesh.

[0012] A second aspect of the present invention provides a method for preparing the underwater anti-dispersion repair material for hydraulic structures, the method comprising: (1) Heat the tap water to 40 degrees, place the polyacrylamide particles in a beaker, slowly pour in warm water in batches and stir until the polyacrylamide is completely dissolved to obtain the polyacrylamide solution; (2) Place cement, fly ash, microsilica fume, magnesium oxide, ammonium dihydrogen phosphate, super absorbent resin, water reducer, and retarder into a mixer and stir for 3 to 5 minutes to fully mix and obtain a premix; (3) Put the premix and fiber into the blender, stir for 3 minutes, then add the polyacrylamide solution, stir for 2-3 minutes, stop for 30 seconds, and stir for another 2-3 minutes. Repeat 2-3 times to obtain the underwater anti-dispersion repair material for hydraulic structures.

[0013] Compared with traditional underwater repair materials, the present invention has the following main advantages: (1) The present invention has high strength and high anti-dispersion performance, can quickly solidify and resist water erosion, and at the same time has good construction performance and can be used for repairing underwater concrete defects; (2) The present invention can achieve underwater vibration-free, self-compacting, good filling properties, and does not require enclosure for waterproofing, thus saving costs; (3) The present invention uses polyacrylamide and super absorbent resin to work together. On the one hand, polyacrylamide is adsorbed on cement particles through the active functional groups on the long carbon chain, playing a bridging role between cement particles and playing an anti-dispersion role. On the other hand, the physical properties and water retention capacity of the super absorbent resin can not only increase the yield stress and plastic viscosity of the slurry, thereby generating viscosity to achieve the purpose of anti-dispersion, but also promote the hydration of cement and refine the pore structure through the "internal curing effect".

[0014] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0015] The present invention will be further described below with reference to specific embodiments to enable those skilled in the art to more fully understand the present invention, but the present invention is not limited in any way.

[0016] Example 1

[0017] 0.5 parts of polyacrylamide was dissolved in 13 parts of water to obtain a polyacrylamide solution.

[0018] Put 30 parts of cement, 10 parts of fly ash, 5 parts of microsilica fume, 21 parts of magnesium oxide, 7 parts of ammonium dihydrogen phosphate, 0.1 parts of super absorbent resin, 0.5 parts of water reducer and 1 part of retarder into a mixer and stir for 3 to 5 minutes to fully mix and obtain a premix.

[0019] Put the premix and 0.5 parts of fiber into the blender, stir for 3 minutes, then add the polyacrylamide solution, stir for 2-3 minutes, stop for 30 seconds, and then stir for 2-3 minutes. Repeat 2-3 times to obtain the underwater anti-dispersion repair material for hydraulic structures.

[0020] Example 2

[0021] 0.5 parts of polyacrylamide was dissolved in 13 parts of water to obtain a polyacrylamide solution.

[0022] 30 parts of cement, 10 parts of fly ash, 10 parts of microsilica fume, 24 parts of magnesium oxide, 6 parts of ammonium dihydrogen phosphate, 0.1 parts of super absorbent resin, 0.5 parts of super absorbent resin, 0.5 parts of water reducer and 1.5 parts of retarder are put into a mixer and stirred for 3 to 5 minutes to fully mix and obtain a premix.

[0023] Put the premix and 1 part of fiber into the blender, stir for 3 minutes, then add the polyacrylamide solution, stir for 2-3 minutes, stop for 30 seconds, and then stir for 2-3 minutes. Repeat 2-3 times to obtain the underwater anti-dispersion repair material for hydraulic structures.

[0024] Example 3

[0025] Dissolve 1 part of polyacrylamide in 10 parts of water to obtain a polyacrylamide solution.

[0026] Put 40 parts of cement, 13 parts of fly ash, 6 parts of microsilica fume, 15 parts of magnesium oxide, 5 parts of ammonium dihydrogen phosphate, 0.3 parts of super absorbent resin, 0.3 parts of water reducer and 1.5 parts of retarder into a mixer and stir for 3 to 5 minutes to fully mix and obtain a premix.

[0027] Put the premix and 0.5 parts of fiber into the blender, stir for 3 minutes, then add the polyacrylamide solution, stir for 2-3 minutes, stop for 30 seconds, and then stir for 2-3 minutes. Repeat 2-3 times to obtain the underwater anti-dispersion repair material for hydraulic structures.

[0028] Example 4

[0029] 1 part of polyacrylamide was dissolved in 13 parts of water to obtain a polyacrylamide solution.

[0030] Put 40 parts of cement, 13 parts of fly ash, 8 parts of microsilica fume, 16 parts of magnesium oxide, 4 parts of ammonium dihydrogen phosphate, 0.5 parts of super absorbent resin, 0.3 parts of water reducer and 1 part of retarder into a mixer and stir for 3 to 5 minutes to fully mix and obtain a premix.

[0031] Put the premix and 0.5 parts of fiber into the blender, stir for 3 minutes, then add the polyacrylamide solution, stir for 2-3 minutes, stop for 30 seconds, and then stir for 2-3 minutes. Repeat 2-3 times to obtain the underwater anti-dispersion repair material for hydraulic structures.

[0032] Example 5

[0033] 1 part of polyacrylamide was dissolved in 13 parts of water to obtain a polyacrylamide solution.

[0034] Put 40 parts of cement, 15 parts of fly ash, 8 parts of microsilica fume, 16 parts of magnesium oxide, 4 parts of ammonium dihydrogen phosphate, 0.5 parts of super absorbent resin, 0.5 parts of water reducer and 1 part of retarder into a mixer and stir for 3 to 5 minutes to fully mix and obtain a premix.

[0035] Put the premix and 1 part of fiber into the blender, stir for 3 minutes, then add the polyacrylamide solution, stir for 2-3 minutes, stop for 30 seconds, and then stir for 2-3 minutes. Repeat 2-3 times to obtain the underwater anti-dispersion repair material for hydraulic structures.

[0036] Example 6

[0037] 1 part of polyacrylamide was dissolved in 13 parts of water to obtain a polyacrylamide solution.

[0038] Put 30 parts of cement, 10 parts of fly ash, 5 parts of microsilica fume, 21 parts of magnesium oxide, 7 parts of ammonium dihydrogen phosphate, 0.5 parts of super absorbent resin, 0.5 parts of water reducer and 1 part of retarder into a mixer and stir for 3 to 5 minutes to fully mix and obtain a premix.

[0039] Put the premix and 1 part of fiber into the blender, stir for 3 minutes, then add the polyacrylamide solution, stir for 2-3 minutes, stop for 30 seconds, and then stir for 2-3 minutes. Repeat 2-3 times to obtain the underwater anti-dispersion repair material for hydraulic structures.

[0040] The test results of the materials described in the above examples are shown in Table 1.

[0041] Table 1 Test results of underwater anti-dispersion repair materials for hydraulic structures

[0042] The above is a further detailed description of the present invention in conjunction with specific preferred embodiments, and the specific implementation of the present invention should not be considered to be limited to these descriptions. For those skilled in the art of the present invention, without departing from the concept of the present invention, several simple deductions or substitutions can be made, which should be considered to fall within the scope of protection of the present invention.

Claims

1. An underwater anti-dispersion repair material for hydraulic structures, characterized in that: The repair material is composed of the following raw materials in parts by weight: 30-40 parts of cement, 10-15 parts of fly ash, 5-10 parts of microsilica fume, 15-25 parts of magnesium oxide, 4-7 parts of ammonium dihydrogen phosphate, 0.5-1.5 parts of anti-dispersant, 0.5-1 part of fiber, 0.1-0.5 part of water reducer, 1-2 parts of retarder and 10-15 parts of water.

2. The underwater anti-dispersion repair material for hydraulic structures according to claim 1, characterized in that: The cement is ordinary Portland cement with strength grade 42.

5.

3. The underwater anti-dispersion repair material for hydraulic structures according to claim 1, characterized in that: The fly ash is low-calcium fly ash with a particle size of less than 45μm.

4. The underwater anti-dispersion repair material for hydraulic structures according to claim 1, characterized in that: The SiO2 content in microsilica ash is ≥98%, and the specific surface area is 19300m 2 / kg.

5. The underwater anti-dispersion repair material for hydraulic structures according to claim 1, characterized in that: The magnesium oxide is dead-burned magnesium oxide with a fineness of 400 mesh.

6. The underwater anti-dispersion repair material for hydraulic structures according to claim 1 is characterized by: The anti-dispersant is one or more of polyacrylamide and super absorbent resin. The molecular weight of polyacrylamide is 10 million, and the dosage is 0.5%~1%; the super absorbent resin is sodium polyacrylate with a molecular weight of 20 million, a particle size of 300~500nm, and a dosage of 0.1%~0.5%.

7. The underwater anti-dispersion repair material for hydraulic structures according to claim 1, characterized in that: The fiber is polyvinyl alcohol fiber with a diameter of 15 μm, a length of 12 mm and a tensile strength of 1830 MPa.

8. The underwater anti-dispersion repair material for hydraulic structures according to claim 1, characterized in that: The water reducing agent is a powdered polycarboxylic acid type high efficiency water reducing agent.

9. The underwater anti-dispersion repair material for hydraulic structures according to claim 1, characterized in that: The retarder is industrial grade borax with a purity of ≥95% and a fineness of 100~150 mesh.

10. An underwater anti-dispersion repair material for hydraulic structures, the preparation process of which is as follows: (1) Heat the tap water to 40 degrees, place the polyacrylamide particles in a beaker, slowly pour in warm water in portions and stir until the polyacrylamide is completely dissolved to obtain a polyacrylamide solution; (2) Put cement, fly ash, microsilica fume, magnesium oxide, diammonium phosphate, super absorbent resin, water reducer and retarder into a mixer and stir for 3 to 5 minutes to fully mix and obtain a premix; (3) Put the premix and fiber into a blender, stir for 3 minutes, then add the polyacrylamide solution, stir for 2-3 minutes, stop for 30 seconds, and stir for another 2-3 minutes. Repeat 2-3 times to obtain the underwater anti-dispersion repair material for hydraulic structures.

Citation Information

Patent Citations

  • Manufactured sand underwater dispersion resistant concrete and preparation method thereof

    CN103102125A

  • Grouting material and local fractured formation inclined shaft inverse well guide hole drilling technology using the same

    CN107311574A

  • Underwater anti-dispersion mortar and preparation method thereof

    CN113004003A

  • High-strength solid-waste-based magnesium phosphate grouting slurry and preparation method thereof

    CN118026639A

Cited By

  • Viscosity time-varying grouting material with controllable dynamic water dispersion and condensation resistance and preparation method thereof

    CN119797865A

  • Preparation method of underwater anti-dispersion grouting material easy to prepare on construction site

    CN122212587A