Weak-base pH reduction dyeing method using N-acetyl blue and application of weak-base pH reduction dyeing method

By using the weak alkali pH reduction dyeing method of N-acetyl blue in textile dyeing, the problems of environmental pollution and fabric damage in the traditional dyeing process are solved, and the effects of high color depth, high color luster and high color fastness are achieved, satisfying the needs meet the needs of sustainable development.

CN118756508AActive Publication Date: 2024-10-11VERTEXYN (NANJING) BIOWORKS CO LTD

Patent Information

Application Number
CN202410815387.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-11
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

The existing dyeing process of indigo and indigo needs to be carried out under strong alkaline conditions, which leads to environmental pollution and fabric damage. Moreover, traditional chemical synthesis methods are harmful to the environment and cannot meet the needs of sustainable development.

Method used

The weak alkali pH reduction dyeing method of N-acetyl blue is used to dye textiles by adjusting the pH value of the dyeing solution between 7.0 and 8.0 and using less reducing agent and alkali solution to improve the color fastness and color while reducing the environmental pollution.

Benefits of technology

It achieves the effect of textile dyeing under neutral conditions, significantly improves color depth and luster, reduces alkali content, reduces environmental pollution, meets the market's demand for green environmental protection, and improves color fastness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756508A_ABST
    Figure CN118756508A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of dyeing and finishing, in particular to a weak-base pH reduction dyeing method utilizing N-acetyl blue and application of the weak-base pH reduction dyeing method, and it is found that the N-acetyl blue is a novel reduced dye, meets the textile dye safety identification requirement and can be applied to textile dyeing. According to the weak-base pH reduction dyeing method of the N-acetyl blue for the textiles, the color depth of the dyed textiles is remarkably improved, the colors are brighter, the color fastness is good, the national standard for textile dyeing is met, the content of a reducing agent is reduced, and environmental pollution is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of dyeing and finishing, and in particular to a weak-base pH reduction dyeing method using N-acetyl indigo and its application. Background Art

[0002] Blue is one of the common colors in daily life. Indigo has been extracted from plants for a long time and used in textiles, porcelain and other fields. The blue pigment extracted from these plants is an organic pigment, which is more human-friendly and widely loved as a dye for fabrics. With the increase in demand for blue dyes, traditional plant extraction cannot provide enough blue pigments. So in the 19th century, people prepared a large amount of synthetic indigo through chemical synthesis, which gradually replaced natural blue pigment and became the most commonly used blue dye. However, while this chemical synthesis method meets the demand for indigo, it uses a large amount of chemical raw materials, causing damage and pollution to the environment. As a water-insoluble reducing dye, indigo needs to be reduced to a soluble sodium salt of leuco body by adding a reducing agent under strong alkaline conditions before it can be dissolved to dye the fabric. The general dyeing process of indigo in industry is the caustic soda insurance powder method, which requires a large amount of insurance powder (15 times the mass of indigo) and caustic soda (5 times the mass of indigo, pH>13) to prepare the dyeing solution, which will not only cause great pollution to the environment, but also damage the printed and dyed fabrics due to the strong alkalinity of the dyeing solution. In recent years, as society has paid more and more attention to environmental and energy issues, people tend to pursue sustainable and environmentally friendly methods to produce dyes. This synthetic indigo is also in urgent need of being replaced by some other natural blue pigments.

[0003] Common natural blue pigments include gardenia blue (a blue pigment derived from cyclopentane derivatives), phycocyanin, indigo blue, oyster green pigment and anthocyanin, etc., which are mainly extracted from plants and microorganisms. Among them, plant extraction is limited by factors such as slow growth of the plant itself, low pigment content, and complex plant components, and cannot be mass-produced; in contrast, the microbial fermentation cycle is short, and the product is single after strain modification, and a relatively pure product can be obtained through simple post-treatment methods. For example, when microbial fermentation is carried out, L-glutamine is used as a substrate, and two molecules of glutamine are catalyzed by indigo synthase to generate the blue pigment Indigoidine (indigo blue). However, indigo blue still uses a strong alkali reduction dyeing method. Although the dosage is reduced, it still needs to use about 3 times the mass of indigo blue and 3 times the mass of caustic soda, and the required pH is about 11. The strong alkaline conditions required for the indigo blue dyeing solution are still destructive to the environment and textiles.

[0004] Previously, the applicant disclosed that indigo blue synthase and 4'-phosphopantetheinyl transferase were expressed in Escherichia coli, Corynebacterium glutamicum, Saccharomyces cerevisiae, and Streptomyces to catalyze the biosynthesis of N-acetyl indigo blue from glutamine and N-acetylglutamine. Currently, there are no reports on the weak alkaline pH reduction dyeing method of N-acetyl indigo blue. Summary of the invention

[0005] The purpose of the present application is to overcome the deficiencies of the above-mentioned prior art and provide a weak alkali pH reduction dyeing method using N-acetyl indigo and its application. The present application proposes that N-acetyl indigo is a new type of fabric reduction dye. The present application adopts a designed weak alkali pH reduction dyeing method for fabric dyeing. The obtained dyed fabric meets the national standards for fabric dyeing, has significantly improved color depth, brighter color, good color fastness, and reduces the alkali content, thereby reducing environmental pollution.

[0006] To achieve the above purpose, the technical solution adopted by this application is:

[0007] The present application provides a weak-base pH reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0008] S1, weighing N-acetyl indigo blue and dissolving it in water to form an N-acetyl indigo blue solution, adding a reducing agent to the N-acetyl indigo blue solution and stirring to reduce it to obtain a dyeing solution, adjusting the pH of the dyeing solution to 7.0-8.0, and allowing it to be reduced to obtain an N-acetyl indigo blue dyeing solution;

[0009] S2, placing the textile in the N-acetyl indigo dyeing solution obtained in step S1, immersing and dyeing, airing and oxidizing, washing, and drying;

[0010] S3, soaping the textile obtained in step S2, and drying it to obtain a dyed textile.

[0011] The present application determines that N-acetyl indigo blue is a green and safe vat dye with a naturalness of 97% through the dye qualitative test, dye safety test, and product naturalness test of the United States Department of Agriculture (USDA) mentioned in ISO 16373-1:2015 (General principles of testing coloured textiles for dyestuff identification).

[0012] N-acetyl indigo is a derivative of indigo, and is the aminoacylation product of L-glutamine during indigo synthesis in microorganisms. The presence of acetyl groups can further reduce the amount of alkali required (the pH of the dyeing solution is closer to neutral), reducing the polarity of N-acetyl indigo, making it less likely to be washed off after dyeing, which helps to increase the color fastness of the dye. N-acetyl indigo, which is also a vat dye, is very different in structure from the traditional vat dye indigo. N-acetyl indigo has more amino groups than indigo, which makes N-acetyl indigo relatively more water-soluble in the leuco state, which is conducive to reducing the amount of reducing agent used during reduction. The presence of aminoacyl groups reduces the polarity, making it less likely to be washed off by water after dyeing on the fabric, which increases the color fastness of the dye.

[0013] The present application applies biosynthesized N-acetyl indigo, a new natural blue pigment, to fabric dyes and establishes a weak alkaline pH reduction dyeing method for N-acetyl indigo for textiles, so as to reduce environmental pollution and lower production costs; the main quality indicators of the obtained N-acetyl indigo dyed textiles, such as color, color depth and color fastness, reach or exceed the quality level of currently available indigo or indigo dyed fabrics.

[0014] The weak-base pH reduction dyeing method of the present application is adopted, and the dyed textiles obtained meet the national standards for fabric dyeing, the color depth of the textiles is improved, the color is brighter, and the color fastness is good. DMSO is used to dissolve the pigment on the textiles, and liquid phase detection proves that the dyed textile pigment is N-acetyl indigo blue.

[0015] As a preferred embodiment of the weak-base pH reduction dyeing method using N-acetyl indigo planta in the present application, in step S1, the mass ratio of the reducing agent to N-acetyl indigo planta indigo planta is (0.5-3):1.

[0016] As a preferred embodiment of the weak-base pH reduction dyeing method using N-acetyl indigo planta in the present application, the mass ratio of the reducing agent to N-acetyl indigo planta indigo planta is (1-2):1.

[0017] The use of the above-mentioned mass ratio of reducing agent and N-acetyl indigo blue can ensure that most of the N-acetyl indigo blue is reduced to a leuco form, and the dyeing effect is obvious; when the mass of N-acetyl indigo blue is too much, the dyeing deepening is not obvious; when the reducing agent is too much, the N-acetyl indigo blue will be over-reduced and not easy to oxidize back, and the pollutants in the dyeing waste liquid will increase.

[0018] As a preferred embodiment of the weak-base pH reduction dyeing method using N-acetyl indigo plant described in the present application, the reducing agent includes one of sodium hydrosulfite, sodium sulfide and bleaching powder;

[0019] Preferably, the reducing agent is sodium hydrosulfite, i.e. sodium dithionite.

[0020] The present application adopts N-acetyl indigo plant blue for weak alkaline pH reduction dyeing, which can reduce the dosage of reducing agents such as hydrosulfite, and at the same time increase the color fastness of dyeing, which is helpful for the dyeing of textiles.

[0021] As a preferred embodiment of the weak-base pH reduction dyeing method using N-acetyl indigo blue described in the present application, in the step S1, an alkali solution or an acid solution is used to adjust the pH of the dyeing solution to 7.0-8.0, preferably pH 7.5;

[0022] The alkali solution includes one of sodium hydroxide, potassium hydroxide, ammonia water, sodium carbonate and sodium bicarbonate; preferably, the alkali solution is sodium hydroxide;

[0023] The acid solution includes one of sulfuric acid, hydrochloric acid, citric acid, acetic acid, and carbonic acid; preferably, the acid solution is citric acid.

[0024] As a preferred embodiment of the weak-base pH reduction dyeing method using N-acetyl indigo described in the present application, in the step S1, the reduction time is 5 to 60 minutes, preferably 10 to 30 minutes.

[0025] If the reduction time is too short, the reduction will be insufficient. If the reduction time is too long, the insurance powder will become ineffective, which will reduce the dyeing rate of N-acetyl indigo.

[0026] As a preferred embodiment of the weak-base pH reduction dyeing method using N-acetyl indigo described in the present application, in the step S2, the dyeing temperature is 20 to 60°C, and the dyeing time is 5 to 20 minutes; the drying and oxidation time is 3 to 10 minutes.

[0027] When the dyeing temperature exceeds 60℃, it will damage N-acetyl indigo. When the temperature is below 20℃, it is not conducive to the penetration of N-acetyl indigo dyeing liquid into the fabric.

[0028] When the drying and oxidation time is less than 3 minutes, washing with water will reduce the amount of color and reduce the color depth of the fabric; when the drying and oxidation time is more than 10 minutes, washing with water will cause color spots on the surface of the fabric that are difficult to wash off, resulting in uneven dyeing.

[0029] As a preferred embodiment of the weak alkaline pH reduction dyeing method using N-acetyl indigo plant described in the present application, in step S2, the mass ratio of N-acetyl indigo plant dyeing solution to textile is (10-100):1.

[0030] As a preferred embodiment of the weak alkaline pH reduction dyeing method using N-acetyl indigo plant described in the present application, in the step S3, the soaping bath ratio of the soaping treatment is 10:1, the soaping temperature is 20 to 60° C., and the soaping time is 5 to 20 minutes.

[0031] Soap bath ratio is a term used in textile dyeing and finishing, which refers to the mass ratio of immersion dyed textiles to N-acetyl indigo dyeing solution. In practical applications, the density of the dyeing solution is often treated as 1.

[0032] In the technical solution of the present application, soaping treatment can wash away floating color on the surface of textiles, which is beneficial to increase the color fastness of dyeing.

[0033] The present application provides a method for reducing dyeing with low amount of insurance powder (0.5-3 times the mass of N-acetyl indigo), low amount of alkali (pH 7.0-8.0), and milder weak alkaline pH.

[0034] As a preferred embodiment of the weak alkaline pH reduction dyeing method using N-acetyl indigo described in the present application, the textile comprises at least one of plant fiber, protein fiber, regenerated fiber and chemical fiber;

[0035] Preferably, the plant fiber includes cotton or linen, the protein fiber includes silk or wool, the regenerated fiber includes modal or lyocell, and the chemical fiber includes one of polyester, nylon and acrylic.

[0036] The present application also provides an application of N-acetyl indigo as a dye in fabric dyeing reduction, wherein the molecular formula of the N-acetyl indigo is C 12 H 10 N4O5, the structural formula is shown in formula (I);

[0037]

[0038] N-acetyl blue is a new type of fabric vat dye. The product naturalness of N-acetyl blue is 97%. It is identified as a vat dye and has passed the dye safety test to prove its green safety.

[0039] The present application also includes quality appraisal on dyed textiles. The K / S value is measured and calculated with a colorimeter to characterize the depth of dyed textiles, and the color fastness to rubbing and soap washing of dyed textiles are tested with reference to GB / T 3920-2008 "Textiles - Tests for Color Fastness - Color Fastness to Rubbing" and GB / T 3921-2008 "Textiles - Tests for Color Fastness - Color Fastness to Soaping". Product quality testing shows that the main quality indicators such as color, color depth and color fastness of N-acetyl indigo dyed textiles obtained under the preferred conditions of weak alkaline pH reduction dyeing method reach or exceed the quality level of existing indigo or indigo dyed textiles; while the main quality indicators such as color, color depth and color fastness of indigo or indigo dyed textiles obtained under the preferred conditions of weak alkaline pH reduction dyeing method do not meet the quality standards of dyed textiles.

[0040] On the N-acetyl indigo dyed textile obtained under the preferred conditions of weak alkaline pH reduction dyeing method, a piece of cloth with a diameter of 5 mm was cut out with a hole puncher, and soaked in 1 mL of DMSO to dissolve the pigment on the textile, and then liquid phase analysis and comparison proved that the blue pigment dissolved by soaking was indeed N-acetyl indigo. Small pieces of cloth taken from N-acetyl indigo dyed textile, indigo dyed textile and indigo dyed textile were soaked and dissolved in DMSO respectively, and the obtained solutions were respectively scanned by full wavelength spectrum. The maximum absorption wavelength of the dissolved solution of N-acetyl indigo dyed textile was about 584±2nm, the maximum absorption wavelength of the dissolved solution of indigo dyed textile was about 600±2nm, and the maximum absorption wavelength of the dissolved solution of indigo dyed textile was about 610±2nm, which can be used as an identification method to distinguish the three different dye-dyed textiles.

[0041] Compared with the prior art, this application has the following beneficial effects:

[0042] The present application provides a weak-alkali pH reduction dyeing method of N-acetyl indigo blue and its application. The N-acetyl indigo blue used in the present application can be used as a new type of reduction dye, meets the requirements for textile dye safety identification, and can be applied to textile dyeing. The present application establishes a reduction dyeing method for N-acetyl indigo blue for textiles, and the color depth of the dyed textiles is significantly improved, the color is brighter, the color fastness is good, and it meets the national standards for textile dyeing, and the alkali content is reduced, the environmental pollution is reduced, and the different needs of the market are met. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 The molecular structure diagram of indigo, indigo blue, and N-acetyl indigo blue ( Figure 1 -A is indigo; Figure 1 -B is for viewing blue; Figure 1 -C is N-acetyl (blue);

[0044] Figure 2 This is a picture of the experiment to identify the dye type of N-acetyl blue;

[0045] Figure 3 Certified natural for N-acetyl indigo;

[0046] Figure 4 The dyed cotton cloth of Examples 2-6 and Comparative Examples 1-8 is shown in Figure 1 (1 is an undyed cloth piece, Figure 2-8 is a dyeing diagram of N-acetyl indigo Examples 2-6 and Comparative Examples 1 and 2, Figure 9 and 10 are dyeing diagrams of indigo comparative examples 3 and 4, Figure 11 and 12 are dyeing diagrams of indigo comparative examples 5 and 6, and Figure 13 and 14 are dyeing diagrams of N-acetyl indigo comparative examples 7 and 8);

[0047] Figure 5 The liquid phase spectrum and full-wavelength UV scanning diagram of the three pigments on the DMSO-dissolved cloth sheet ( Figure 5 -A is the liquid phase diagram of N-acetyl blue; Figure 5 -B is a blue liquid phase diagram; Figure 5 -C is the liquid phase diagram of indigo; Figure 5 -D is the full wavelength spectrum scanning diagram corresponding to the three pigments). DETAILED DESCRIPTION

[0048] In order to better illustrate the purpose, technical solutions and advantages of the present application, the present application will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0049] In the following examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0050] The N-acetyl indigo and indigo used in the following examples were obtained by self-developed fermentation by our company (Nanjing Hegu Life Biotechnology Co., Ltd.).

[0051] The safety report of N-acetyl indigo blue in this application was issued by Shaoxing Quality and Technical Supervision Inspection Institute, and the dye type was qualitatively determined by the inventor according to the method provided by the international standard ISO 16373-1:2015, and passed the product naturalness certification of the United States Department of Agriculture (USDA BIOPREFERRED Biological Priority Program).

[0052] From Example 2 to Example 7, different conditions were selected for dyeing test with N-acetyl indigo; Comparative Example 1 and Comparative Example 2 were dyeing tests for indigo; Comparative Example 3 and Comparative Example 4 were dyeing tests for indigo. Example 8 Quality inspection was performed on the dyed cloth pieces of Examples 2-7 and Comparative Examples 1-4, and the K / S value was used to characterize the depth of the cotton cloth after dyeing, and the color fastness to rubbing and the color fastness to soaping of the cotton cloth were tested with reference to GB / T3920-2008 "Textiles - Tests for Color Fastness - Color Fastness to Rubbing" and GB / T 3921-2008 "Textiles - Tests for Color Fastness - Color Fastness to Soaping". Example 9 The dyed cloth pieces in Example 2, Comparative Example 1 and Comparative Example 3 were soaked in DMSO to dissolve the pigment, and the solution was subjected to full wavelength spectrum scanning to compare the maximum absorption wavelengths of the three blue pigments.

[0053] The molecular structures of indigo, indigo blue, and N-acetyl indigo blue mentioned in the following examples and comparative examples are shown in FIG. Figure 1 As shown ( Figure 1 -A is indigo; Figure 1 -B is for viewing blue; Figure 1 -C is N-acetyl (blue).

[0054] Example 1: Identification of Type, Safety and Naturalness of N-Acetyl Blue Dye

[0055] The dye type of N-acetyl indigo was determined by the dye qualitative detection method mentioned in ISO 16373-1:2015 (General principles of testing coloured textiles for dyestuff identification). Then the obtained pure N-acetyl indigo was sent to Shaoxing Quality and Technical Supervision Inspection Institute for dye safety testing, mainly to test whether N-acetyl indigo contains harmful aromatic amines, heavy metal content, harmful solvents, etc. In addition, the pure N-acetyl indigo was sent to the United States Department of Agriculture (USDA) to test the naturalness of the product.

[0056] Specifically:

[0057] Since N-acetyl blue appears dark blue in solution, the applicant identified the dye type of N-acetyl blue according to the method provided by the international standard ISO 16373-1:2015. The specific experimental steps are shown in (AF) below. The experimental results are as follows: Figure 2 ( Figure 2 -A to Figure 2 -F) as shown.

[0058] A. Put 0.2g of N-acetyl indigo blue sample into 10mL boiling 1% ammonia solution for 1 minute. After centrifugation at 13000r / min for 5min, a light purple color is generated in the solution and a blue precipitate is generated at the bottom of the test tube, indicating that N-acetyl indigo blue is not dissolved in 1% ammonia water, so indigo blue is not an acid dye.

[0059] B. Put 0.2g of N-acetyl indigo blue sample into boiling 5% acetic acid for 1 minute. The color of the solution did not change significantly. After centrifugation, a large amount of indigo blue precipitate was produced, and the supernatant did not change in color. Therefore, N-acetyl indigo blue is not an alkaline dye.

[0060] C. Add 0.2g of N-acetyl indigo blue sample directly into 5% sodium hydroxide, and then centrifuge at 13000r / min for 5min. Because N-acetyl indigo blue will change when pH>12, the supernatant of the solution is light brown, but there is still precipitation. N-acetyl indigo blue is basically insoluble in 5% sodium hydroxide, so N-acetyl indigo blue is neither a direct dye nor a reactive dye.

[0061] D. Since N-acetyl indigo blue will change when pH>12, the N-acetyl indigo blue sample was treated with a pH 11 aqueous solution instead of a 20% sodium hydroxide solution. Water and sodium dithionite were then added and the test tube was shaken. The solution turned gray and then oxidized to blue. Cold diluted sodium hypochlorite solution was added and the solution color did not change. Therefore, N-acetyl indigo blue is a reducing dye.

[0062] E. Treat 0.2g of N-acetyl indigo blue with 16% hydrochloric acid, heat and cool, then add magnesium ribbon. The color of N-acetyl indigo blue changes in 16% hydrochloric acid, but it does not turn black after testing with lead acetate paper, and no gas with the odor of hydrogen sulfide is produced, so N-acetyl indigo blue is not a sulfur dye.

[0063] F. Heat a small amount of N-acetyl blue sample with concentrated sulfuric acid for a few seconds and pour it into cold water. The solution color is blue at this time, and no dark green color is produced, so N-acetyl blue is not aniline black dye.

[0064] In summary, the identification result shows that the new substance N-acetyl indigo is a vat dye. At present, the most commonly used blue vat dye is synthetic indigo, which is synthesized by chemical methods. The raw materials and intermediates contain a large amount of phenylacetic acid, toluene, β-aniline, anthranilic acid and other substances, which will cause environmental pollution to a large extent. The safety of N-acetyl indigo, a vat dye, was tested, and the test results issued by the Shaoxing Quality and Technical Supervision Inspection Institute are shown in Table 1. Since N-acetyl indigo is fermented by microorganisms, no harmful aromatic amines, harmful solvents, etc. are used in the cultivation process, so the final test results also show that N-acetyl indigo does not contain such substances.

[0065] Table 1

[0066]

[0067]

[0068] In addition, the N-acetyl indigo produced by the applicant has been certified by the BioPreferred Program managed by the US Department of Agriculture (USDA), and the product's naturalness has reached 97% ( Figure 3 ). Therefore, N-acetyl indigo has the characteristics of being more natural, environmentally friendly, green and safe.

[0069] Example 2

[0070] This embodiment provides a weak-base pH reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0071] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 1 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain an N-acetyl indigo blue solution. Weigh 0.5 g of sodium hydrosulfite (sodium dithionite) and add it to the N-acetyl indigo blue and stir it thoroughly to reduce it. Then adjust the pH of the dyeing solution to 7.0 with an alkali solution (sodium hydroxide). Seal it and place it to reduce it for 5 minutes to obtain a 1 g / L N-acetyl indigo blue dyeing solution.

[0072] (2) Dyeing of textiles: Take 50 mL of the N-acetyl indigo dyeing solution from (1) above, soak cotton cloth in a bath ratio of 10:1 (weight of N-acetyl indigo dyeing solution: weight of dyed cotton cloth), dye at 20°C for 5 min, take out, dry in the sun for oxidation for 3 min, then wash with water and dry;

[0073] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 20°C, and a soaping time of 5 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 Middle 2, Figure 4 (1 is the undyed cloth piece for control).

[0074] Example 3

[0075] This embodiment provides a weak-base pH reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0076] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 2 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain N-acetyl indigo blue solution, weigh 2 g of sodium hydrosulfite (sodium dithionite) and add it to N-acetyl indigo blue and stir thoroughly to reduce, then adjust the pH of the dyeing solution to 7.5 with alkali solution (sodium hydroxide), seal and place it to reduce for 15 minutes, and then obtain 2 g / L N-acetyl indigo blue dyeing solution;

[0077] (2) Dyeing of textiles: Take 50 mL of the N-acetyl indigo dyeing solution from (1) above, soak cotton cloth in a bath ratio of 10:1 (weight of N-acetyl indigo dyeing solution: weight of dyed cotton cloth), dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0078] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (3).

[0079] Example 4

[0080] This embodiment provides a weak-base pH reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0081] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 5 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain N-acetyl indigo blue solution, weigh 15 g of sodium hydrosulfite (sodium dithionite) and add it to N-acetyl indigo blue and stir thoroughly to reduce, then adjust the pH of the dyeing solution to 8.0 with alkali solution (sodium hydroxide), seal and place it to reduce for 60 minutes, and then obtain 5 g / L N-acetyl indigo blue dyeing solution;

[0082] (2) Dyeing of textiles: Take 250 mL of the N-acetyl indigo dyeing solution from the above (1), soak cotton cloth in a bath ratio of 50:1 (weight of N-acetyl indigo dyeing solution: weight of dyed cotton cloth), dye at 45°C for 20 min, take out, dry in the sun for 10 min, then wash with water and dry;

[0083] (3) Soaping process: The dyed cotton cloth in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 45°C, and a soaping time of 20 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (4).

[0084] Example 5

[0085] This embodiment provides a weak-base pH reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0086] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 1 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain an N-acetyl indigo blue solution. Weigh 2 g of sodium hydrosulfite (sodium dithionite) and add it to the N-acetyl indigo blue and stir it thoroughly to reduce it. Then adjust the pH of the dyeing solution to 7.5 with an alkali solution (sodium hydroxide). Seal it and place it to reduce for 30 minutes to obtain a 2 g / L N-acetyl indigo blue dyeing solution.

[0087] (2) Dyeing of textiles: Take 50 mL of the N-acetyl indigo dyeing solution from (1) above, soak cotton cloth in a bath ratio of 10:1 (weight of N-acetyl indigo dyeing solution: weight of dyed cotton cloth), dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0088] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (5).

[0089] Example 6

[0090] This embodiment provides a weak-base pH reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0091] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 2 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain an N-acetyl indigo blue solution. Weigh 2 g of sodium hydrosulfite (sodium dithionite) and add it to the N-acetyl indigo blue and stir it thoroughly to reduce it. Then adjust the pH of the dyeing solution to 7.5 with an alkali solution (sodium hydroxide). Seal it and place it to reduce it for 10 minutes to obtain a 2 g / L N-acetyl indigo blue dyeing solution.

[0092] (2) Dyeing of textiles: Take 50 mL of the N-acetyl indigo dyeing solution from (1) above, soak cotton cloth in a bath ratio of 10:1 (weight of N-acetyl indigo dyeing solution: weight of dyed cotton cloth), dye at 60°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0093] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 60°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (6).

[0094] Comparative Example 1

[0095] This comparative example uses the optimal conditions of the indigo blue strong base reduction dyeing method to reduce and dye N-acetyl indigo blue.

[0096] This comparative example provides a strong alkali reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0097] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 2 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain an N-acetyl indigo blue solution. Weigh 4 g of sodium hydrosulfite (sodium dithionite) and add it to the N-acetyl indigo blue and stir it thoroughly to reduce it. Then adjust the pH of the dyeing solution to 10.0 with an alkali solution (sodium hydroxide). Seal it and place it to reduce for 15 minutes to obtain a 2 g / L N-acetyl indigo blue dyeing solution.

[0098] (2) Dyeing of textiles: Take 50 mL of the N-acetyl indigo dyeing solution from (1) above, soak cotton cloth in a bath ratio of 10:1 (weight of N-acetyl indigo dyeing solution: weight of dyed cotton cloth), dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0099] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (7).

[0100] Comparative Example 2

[0101] This comparative example uses the general strong alkali reduction method of indigo dyeing to carry out N-acetyl indigo reduction dyeing.

[0102] This comparative example provides a strong alkali reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0103] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 2 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain an N-acetyl indigo blue solution. Weigh 30 g of sodium hydrosulfite (sodium dithionite) and add it to the N-acetyl indigo blue solution and stir it thoroughly to reduce it. Then add 10 g of caustic soda. At this time, the pH value is about 12.8. Seal and place it to reduce for 20 minutes to obtain 2 g / L N-acetyl indigo blue dyeing solution.

[0104] (2) Dyeing of textiles: Take 50 mL of the dyeing solution from (1) above, soak cotton cloth in a bath ratio (mass of dyeing solution: mass of dyed cloth) of 10:1, dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0105] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (8).

[0106] Comparative Example 3

[0107] This comparative example uses Guanlan as a comparison. Guanlan (existing) is also obtained by self-developed fermentation of our company (Nanjing Hegu Life Biotechnology Co., Ltd.) and can be purchased from the company's official website. At present, the best condition for Guanlan dyeing is 2 times the reduction of insurance powder and dyeing at pH 10.0, which is a strong alkaline reduction dyeing method.

[0108] (1) Preparation of indigo blue dyeing solution: Weigh 2 g of indigo blue powder and dissolve it in 1 L of pure water to obtain indigo blue solution, weigh 4 g of sodium hydrosulfite (sodium dithionite) and add it to the indigo blue and stir thoroughly to reduce, then adjust the pH of the dyeing solution to 10.0 with alkali solution (sodium hydroxide), seal it and place it to reduce for 15 minutes, and then obtain 2 g / L indigo blue dyeing solution;

[0109] (2) Dyeing of cotton cloth: Take 50 mL of the indigo dyeing solution from (1) above, soak the cloth in a bath ratio of 10:1 (mass of indigo dyeing solution: mass of dyed cloth), dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0110] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (9).

[0111] Comparative Example 4

[0112] In this embodiment, indigo blue is selected as a comparison. Indigo blue (existing) is also obtained by self-developed fermentation of the company (Nanjing Hegu Life Biotechnology Co., Ltd.) and can be purchased from the company's official website. The dyeing method is carried out according to the optimized conditions of Example 3 of the above-mentioned N-acetyl indigo blue weak alkaline pH reduction dyeing method.

[0113] (1) Preparation of indigo blue dyeing solution: Weigh 2 g of indigo blue powder and dissolve it in 1 L of pure water to obtain indigo blue solution, weigh 2 g of sodium hydrosulfite (sodium dithionite) and add it to the indigo blue and stir thoroughly to reduce, then adjust the pH of the dyeing solution to 7.5 with alkali solution (sodium hydroxide), seal and place it to reduce for 15 minutes, and then obtain 2 g / L indigo blue dyeing solution;

[0114] (2) Dyeing of cotton cloth: Take 50 mL of the indigo dyeing solution from (1) above, soak the cloth in a bath ratio of 10:1 (mass of indigo dyeing solution: mass of dyed cloth), dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0115] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (10).

[0116] Comparative Example 5

[0117] This comparative example uses commercial indigo as a comparison. The commercial indigo is purchased from Roan's Reagent. The dyeing method is carried out according to the general strong alkali reduction dyeing method of indigo, that is, reduction dyeing with 15 times the mass of indigo and 5 times the mass of indigo using caustic soda.

[0118] (1) Preparation of indigo dyeing solution: Weigh 2 g of indigo powder and dissolve it in 1 L of pure water to obtain an indigo solution. Weigh 30 g of sodium hydrosulfite (sodium dithionite) and add it to the indigo solution and stir it thoroughly to reduce it. Then add 10 g of caustic soda. At this time, the pH value is about 13.2. Seal it and place it to reduce it for 20 minutes to obtain 2 g / L indigo dyeing solution.

[0119] (2) Dyeing of cotton cloth: Take 50 mL of the dyeing solution from (1) above, soak the cotton cloth in a bath ratio (mass of dyeing solution: mass of dyed cloth) of 10:1, dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0120] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (11).

[0121] Comparative Example 6

[0122] This comparative example uses commercial indigo as a comparison. The commercial indigo is purchased from Ron's reagent, and the dyeing method is carried out according to the above-mentioned N-acetyl indigo weak base pH reduction dyeing method optimization condition Example 3.

[0123] (1) Preparation of indigo dyeing solution: Weigh 2 g of indigo powder and dissolve it in 1 L of pure water to obtain an indigo solution. Weigh 2 g of sodium hydrosulfite (sodium dithionite) and add it to the indigo solution and stir it thoroughly to reduce it. Then adjust the pH of the dyeing solution to 7.5 with alkali solution (sodium hydroxide). Seal it and let it reduce for 15 minutes to obtain 2 g / L indigo dyeing solution.

[0124] (2) Dyeing of cotton cloth: Take 50 mL of the dyeing solution from (1) above, soak the cloth in a bath ratio (mass of dyeing solution: mass of dyed cloth) of 10:1, dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0125] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (12).

[0126] Comparative Example 7

[0127] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 2 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain N-acetyl indigo blue solution, weigh 2 g of sodium hydrosulfite (sodium dithionite) and add it to N-acetyl indigo blue and stir thoroughly to reduce, then adjust the pH of the dyeing solution to 6 with acid solution (citric acid), seal and place it to reduce for 15 minutes, and then obtain 2 g / L N-acetyl indigo blue dyeing solution;

[0128] (2) Dyeing of textiles: Take 50 mL of the N-acetyl indigo dyeing solution from (1) above, soak cotton cloth in a bath ratio of 10:1 (weight of N-acetyl indigo dyeing solution: weight of dyed cotton cloth), dye at 25°C for 10 min, take out, dry in the sun for oxidation for 5 min, then wash with water and dry;

[0129] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (13).

[0130] The difference from Example 3 is that the pH is adjusted by different acid solution.

[0131] Comparative Example 8

[0132] This embodiment provides a reduction dyeing method using N-acetyl indigo, comprising the following steps:

[0133] (1) Preparation of N-acetyl indigo blue dyeing solution: Weigh 2 g of N-acetyl indigo blue powder and dissolve it in 1 L of pure water to obtain an N-acetyl indigo blue solution. Weigh 30 g of sodium hydrosulfite (sodium dithionite) and add it to the N-acetyl indigo blue and stir it thoroughly to reduce it. Then adjust the pH of the dyeing solution to 7.5 with an alkali solution (sodium hydroxide). Seal it and place it to reduce it for 15 minutes to obtain a 2 g / L N-acetyl indigo blue dyeing solution.

[0134] (2) Dyeing of textiles: Take 50 mL of the N-acetyl blue dyeing solution from (1) above, soak cotton cloth in a bath ratio (dyeing solution mass: dyed cloth mass) of 10:1, dye at 25°C for 10 min, then take out, air-dry and oxidize for 5 min, then wash with water and dry;

[0135] (3) Soaping process: The cotton cloth dyed in the above (2) is subjected to soaping treatment, with a soaping bath ratio of 10:1, a soaping temperature of 25°C, and a soaping time of 10 min. After being taken out and air-dried, the dyed cotton cloth ( Figure 4 (14).

[0136] The difference from Example 3 is that the quality of the hydrosulfite is different.

[0137] Test Example 1

[0138] The above-mentioned Examples 2-6 and Comparative Examples 1-8 were dyed multiple times, and the color depth (K / S) and color fastness of the fabrics were measured. The color fastness test was carried out with reference to GB / T 3920-2008 "Textiles - Tests for Color Fastness - Color Fastness to Rubbing" and GB / T 3921-2008 "Textiles - Tests for Color Fastness - Color Fastness to Soaping". At least 3 pieces of fabric were taken from each group for testing, and the average result was calculated. The specific results are shown in Table 2 below. The dyed fabric pieces are shown as follows: Figure 4 shown.

[0139] Table 2

[0140]

[0141]

[0142] From Table 2, we can see that:

[0143] Embodiment 2-7 is the quality detection of N-acetyl blue dyeing cloth pieces under different conditions. The weakly alkaline pH (7.0-8.0) dyeing condition average color depth K / S of the scope of the present application is greater than 11.5 to 15.1, and the color depth K / S of the optimized condition at pH7.5 reaches 15.1, and the average color depth K / S of the optimal dyeing condition (Comparative Example 1) of blue dyeing is 10.4, the average color depth K / S of the traditional dyeing condition (Comparative Example 2) of indigo is 3.6, the average color depth K / S of the acid dyeing condition (Comparative Example 7) is 9.9, and the average color depth K / S of the high insurance powder dyeing condition (Comparative Example 8) is 10.1. The cloth pieces dyed by the weakly alkaline pH reduction dyeing method of the present application have obtained higher color depth. And the color fastness of the optimal condition (Example 3) of the present application is better, compared with Comparative Examples 1-2 and Comparative Examples 7-8, which also shows that the traditional strong alkali reduction dyeing method of blue or indigo is not suitable for N-acetyl blue dyeing.

[0144] Comparative Examples 3 and 4 are respectively dyeing under the optimal conditions for viewing blue and dyeing using the present application N-acetyl viewing blue dyeing optimization pH condition method, and Comparative Examples 5 and 6 are respectively dyeing by the traditional method of indigo and dyeing using the present application N-acetyl viewing blue dyeing optimization pH condition method. It can be seen that the optimal pH for viewing blue dyeing is 10.0 (Comparative Example 3), and the average color depth K / S of the dyed cloth piece is 13.6. When the average color depth K / S of dyeing is 8.8 at neutral pH (Comparative Example 4), it is greatly reduced, and the color fastness is equivalent to both, which are 4 levels of color fastness to dry friction, 3-4 levels of color fastness to wet friction, and 3-4 levels of color fastness to soaping. And the amount of alkali required for indigo is more (pH>12), and a large amount of insurance powder is also needed for reduction (Comparative Example 5). At this time, the average color depth K / S=14.0, 4 levels of color fastness to dry friction, 4 levels of color fastness to wet friction, and 4 levels of color fastness to soaping. When the low amount of insurance powder and low amount of alkali solution under the optimized conditions of N-acetyl indigo dyeing are used (Comparative Example 6), the indigo dyed cotton cloth has a low color amount and an average color depth K / S=8.3, and the color fastness is reduced, with a dry friction color fastness of 3-4, a wet friction color fastness of 3, and a soap washing color fastness of 3. This also shows that the weak alkaline pH reduction dyeing method of the present application is not suitable for indigo or indigo.

[0145] Test Example 2

[0146] Take about 4cm x 4cm pieces of the dyed fabrics of Example 2, Comparative Example 3 and Comparative Example 5, put them into 10mL centrifuge tubes, and then add 5mL of DMSO to soak the pieces to dissolve the pigment. The obtained N-acetyl indigo and indigo DMSO solutions were subjected to liquid phase detection ( Figure 5 -A, Figure 5-B): Chromatographic column: Shim-pack GIS 5μm C18 4.6×250mm (HSS), wavelength 600nm, flow rate 1.0ml / min, sample solution DMSO, injection volume 10μL, column temperature 35℃, running time 18min. The peak time of about 9.9min is N-acetyl indigo, and the peak time of about 8.8min is indigo. The obtained indigo DMSO solution was subjected to liquid phase detection ( Figure 5 -C): Chromatographic column: Galasil○ R EF-C18M 4.6mm id×250mm L, wavelength 600nm, flow rate 1.0ml / min, sample solution DMSO, injection volume 10μL, column temperature 35℃, running time 22min. The elution time of indigo is 14.3min.

[0147] The obtained DMSO solutions of N-acetyl indigo, indigo and indigo dyed fabrics were subjected to full wavelength spectral scanning. The results are as follows: Figure 5 -D. The maximum absorption wavelength of the DMSO solution of N-acetyl cyanine dyed fabric is 582nm, the maximum absorption wavelength of the DMSO solution of cyanine dyed fabric is 601nm, and the maximum absorption wavelength of the DMSO solution of indigo dyed fabric is 609nm, which are consistent with the maximum absorption wavelength values ​​of the DMSO solutions prepared with N-acetyl cyanine (584±2nm), cyanine (600±2nm) and indigo (610±2nm) dyes, respectively (as shown in Figure 2). Figure 5 ).

[0148] In summary, the present application proposes for the first time the application of N-acetyl indigo in fabric dyeing, and proposes a weakly alkaline pH reduction dyeing method suitable for N-acetyl indigo. The method (Example 3) is compared with the dyeing methods of indigo and indigo (Comparative Examples 3 and 5), which is more gentle and environmentally friendly. The K / S value and color fastness of the N-acetyl indigo dyed cloth piece are comparable to or even improved with the traditional dyeing of indigo and indigo, but the pH and the amount of insurance powder used are reduced by more than 1 times, which effectively solves the problems of difficult coloring, poor color fastness, damage to fabrics, difficult degradation of wastewater, and difficult treatment in the indigo dyeing and finishing industry.

[0149] The dyeing method of the present application is a dyeing method specifically suitable for N-acetyl indigo blue, which reduces pollution and saves costs from both the material selection and dyeing process, and highlights the concept of green environmental protection. At the same time, the identification of the dye in Example 1 shows that the quality of the cloth pieces dyed using the method of the present application meets the national standards and is safe. Furthermore, the present application also provides a method for identifying and distinguishing N-acetyl indigo blue, indigo blue and indigo blue to prevent chemically synthesized commercial indigo blue from impersonating N-acetyl indigo blue with a higher degree of naturalness.

[0150] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.

Claims

1. A weak base pH reduction dyeing method using N-acetyl indigo, characterized in that: The following steps are involved: S1, weighing N-acetyl indigo blue and dissolving it in water to form an N-acetyl indigo blue solution, adding a reducing agent to the N-acetyl indigo blue solution and stirring to reduce it to obtain a dyeing solution, adjusting the pH of the dyeing solution to 7.0-8.0, and allowing it to be reduced to obtain an N-acetyl indigo blue dyeing solution; S2, placing the textile in the N-acetyl indigo dyeing solution obtained in step S1, immersing and dyeing, airing and oxidizing, washing, and drying; S3, soaping the textile obtained in step S2, and drying it to obtain a dyed textile.

2. The weakly alkaline pH reduction dyeing method as claimed in claim 1, wherein In the step S1, the mass ratio of the reducing agent to N-acetyl indigo is (0.5-3):

1.

3. The weakly alkaline pH reduction dyeing method as claimed in claim 1, wherein The mass ratio of the reducing agent to N-acetyl indigo is (1-2):

1.

4. The weakly alkaline pH reduction dyeing method as claimed in claim 1, wherein The reducing agent includes one of sodium hydrosulfite, sodium sulfide and bleaching powder; Preferably, the reducing agent is hydrosulfur powder.

5. The weakly alkaline pH reduction dyeing method as claimed in claim 1, characterized in that, In the step S1, an alkali solution or an acid solution is used to adjust the pH of the dyeing solution to 7.0-8.0, preferably pH 7.5; The alkali solution includes one of sodium hydroxide, potassium hydroxide, ammonia water, sodium carbonate and sodium bicarbonate; preferably, the alkali solution is sodium hydroxide; The acid solution includes one of sulfuric acid, hydrochloric acid, citric acid, acetic acid, and carbonic acid; preferably, the acid solution is citric acid.

6. The reduction dyeing method according to claim 1, wherein In step S1, the reduction time is 5 to 60 minutes, preferably 10 to 30 minutes.

7. The reduction dyeing method according to claim 1, wherein In the step S2, the dyeing temperature is 20-60°C, and the dyeing time is 5-20 minutes; the drying and oxidation time is 3-10 minutes.

8. The reduction dyeing method according to claim 1, wherein In the step S3, the soaping bath ratio of the soaping treatment is 10:1, the soaping temperature is 20 to 60° C., and the soaping time is 5 to 20 minutes.

9. The reduction dyeing method according to claim 1, wherein The textile comprises at least one of plant fiber, protein fiber, regenerated fiber and chemical fiber; Preferably, the plant fiber includes cotton or linen, the protein fiber includes silk or wool, the regenerated fiber includes modal or lyocell, and the chemical fiber includes one of polyester, nylon and acrylic.

10. A use of N-acetyl indigo as a dye in fabric dyeing reduction, characterized in that: The molecular formula of the N-acetyl indigo plant is C 12 H 10 N4O5, the structural formula is shown in formula (I);

Citation Information

Patent Citations

  • Blue staining solution as well as preparation method and application thereof

    CN117925920A

  • Dyeing method of silk fabric

    CN118007448A

  • Dyeing method of linen fabric

    CN118147931A

  • Double-stage fermentation production process of N-acetyl blue

    CN118562910A

  • Method for identifying indigo blue, observation blue and N-acetyl observation blue

    CN118731011A

Cited By

  • 5-substituted amino-5 '-acetamido-3, 3'-dipyridyl derivative as well as preparation method and application thereof

    CN119798151A

  • N-hydroxyamino-N '-acetyl ornamental blue as well as fermentation method and application thereof

    CN120058602A

  • An N-hydroxyamino-N'-acetyl indigo carmine and its fermentation method and application

    CN120058602B

  • Biological blue dye, staining solution and preparation method and application thereof

    CN121160112A

  • Preparation method of N-acetyl blue and application of prepared N-acetyl blue in fabric dyeing

    CN121990989A