Rapid resin finishing process for pure cotton color lining cloth

By adopting a fast resin finishing process on pure cotton colored lining cloth, combined with ultrasonic treatment and dynamic impregnation technology, the problems of long resin finishing time and uneven distribution in the existing technology are solved, and the wrinkle resistance and color fastness of the lining cloth are improved, and the wrinkle resistance and color fastness of the lining cloth are maintained. The softness of fiber is suitable for efficient and high-quality needs in the high-end clothing and fast fashion industries.

CN119061692APending Publication Date: 2024-12-03NANTONG YIYI INTERLINING
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411330626.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When the existing resin finishing process improves the wrinkle resistance and color fastness of pure cotton color lining cloth, there are problems such as long finishing time, uneven resin distribution, high-temperature treatment, fiber strength damage, and hardening of the hand, making it difficult to take into account the softness of the fiber. , strength and durability.

Method used

A rapid resin finishing process is adopted, including adding polylamine formaldehyde resin, polydimethylsiloxane softener, potassium dihydrogen phosphate catalyst, sodium methylsulfonate anti-wrinkle agent, aziridine crosslinker to the mixing tank and water, high-speed stirring is carried out to form a finishing solution, ultrasonic pretreatment, dynamic immersion, intermediate drying, high-temperature curing, rapid cooling and soft treatment, ensuring uniform distribution of resin and stability of fibers.

Benefits of technology

Improves the overall performance of the lining, avoids local hardening and uneven coloring, enhances wrinkle resistance and color fastness, while maintaining the natural comfort characteristics of pure cotton, suitable for high-efficiency and high-quality needs in high-end clothing and fast fashion industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061692A_ABST
    Figure CN119061692A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of textile processing, in particular to a quick resin finishing process for pure cotton color lining cloth, which comprises the following steps: S1, preparing finishing liquid; s2, fiber pretreatment: carrying out ultrasonic treatment on the pure cotton color lining cloth; s3, the pretreated pure cotton color lining cloth slowly passes through the finishing liquid prepared in the S1 to be subjected to dipping treatment; s4, carrying out intermediate drying on the impregnated lining cloth; s5, carrying out high-temperature curing treatment on the lining cloth subjected to primary resin curing; s6, the lining cloth subjected to high-temperature curing is subjected to rapid cooling treatment immediately, so that a resin structure is locked; s7, carrying out softening treatment on the cooled lining cloth, and then washing with water; and S8, carrying out quality detection on the treated pure cotton color lining cloth. According to the method, by optimizing the chemical treatment and curing steps, the wrinkle resistance and color fastness of the lining cloth are remarkably improved, meanwhile, the softness and comfort of fibers are kept, and the production efficiency and the product quality are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile processing, in particular to a rapid resin finishing process for pure cotton colored lining cloth. Background Art

[0002] Pure cotton colored interlining is widely used in the clothing industry due to its good air permeability, comfort and moisture absorption. However, pure cotton fiber is easy to wrinkle, and its color fastness and appearance quality will be significantly reduced after repeated washing, affecting its appearance and service life. In order to solve these problems, resin finishing process is usually used to enhance the wrinkle resistance and color fastness of pure cotton colored interlining. However, there are some problems with the existing resin finishing process, such as the finishing time is too long, the resin is unevenly distributed in the fiber, resulting in unstable finishing effect. At the same time, due to the damage to the fiber strength caused by high temperature treatment during the finishing process, the feel of the interlining becomes hard, affecting its comfort.

[0003] The existing resin finishing process is still difficult to ensure production efficiency while taking into account the softness, strength and durability of the fiber. The high-temperature curing process often leads to excessive cross-linking reaction between the resin and the fiber, resulting in reduced strength and color changes of the lining cloth. In addition, due to uneven impregnation treatment, the finishing effect in some areas is poor, and the quality of the product is difficult to guarantee. Therefore, an improved rapid resin finishing process is urgently needed to eliminate the above problems. Summary of the invention

[0004] Based on the above purpose, the present invention provides a rapid resin finishing process for pure cotton colored lining cloth.

[0005] A rapid resin finishing process for pure cotton colored lining cloth comprises the following steps:

[0006] S1: adding melamine formaldehyde resin, polydimethylsiloxane softener, potassium dihydrogen phosphate catalyst, sodium methanesulfonate anti-wrinkle agent, aziridine crosslinker and water in a mixing tank according to a predetermined ratio, and stirring at a high speed to form a uniform finishing liquid;

[0007] S2: fiber pretreatment, ultrasonic treatment of pure cotton colored lining fabric;

[0008] S3: slowly passing the pretreated pure cotton colored lining fabric through the finishing liquid prepared in S1 for impregnation treatment;

[0009] S4: intermediate drying of the impregnated lining cloth to remove excess water and perform preliminary resin curing treatment;

[0010] S5: subjecting the lining fabric after the preliminary resin curing to high temperature curing treatment to form a stable wrinkle-resistant network structure;

[0011] S6: The lining cloth is immediately cooled rapidly after high temperature curing to lock the resin structure;

[0012] S7: softening the cooled interlining cloth, and then washing it with water to remove unreacted chemicals and surface residues;

[0013] S8: Carry out quality inspection on the processed pure cotton colored interlining to ensure that each batch of products meets the predetermined quality standards.

[0014] Optionally, the predetermined proportions in S1 are 3%-8% of melamine formaldehyde resin; 1%-4% of polydimethylsiloxane softener; 0.5%-2% of potassium dihydrogen phosphate catalyst; 0.5%-1.5% of sodium methane sulfonate anti-wrinkle agent; 0.1%-0.5% of aziridine cross-linking agent, and the balance is water.

[0015] Optionally, the rotation speed of the high-speed stirring in S1 is 800-1200 rpm, the stirring time is 20-30 minutes, and the stirring temperature is controlled at 30°C-40°C.

[0016] Optionally, the ultrasonic treatment frequency in S2 is 35-45kHz, and the treatment time is 1-3 minutes.

[0017] Optionally, the immersion treatment time in S3 is 2-5 minutes, and the lining cloth moves in the finishing liquid at a speed of 0.3-0.7 m / s.

[0018] Optionally, the intermediate drying temperature in S4 is controlled at 60°C-80°C, and the drying time is 2-4 minutes to remove excess moisture, and after the drying is completed, the temperature is increased to 100°C-120°C, and the initial resin curing treatment time is 30-60 seconds.

[0019] Optionally, the high temperature curing temperature in S5 is controlled at 150° C.-170° C., and the curing time is 1-2 minutes.

[0020] Optionally, the cooling treatment temperature in S6 is controlled at 20° C.-30° C., and the cooling time is 1-3 minutes.

[0021] Optionally, the softener used in the softening treatment in S7 is a cationic softener with a concentration of 0.5%-1.5%, the water washing temperature is 20° C.-30° C., and the water washing time is 2-4 minutes, which is used to remove unreacted chemicals and surface residues.

[0022] Optionally, the quality inspection in S8 includes color fastness inspection, wrinkle resistance inspection, hand feel inspection and strength inspection; in the color fastness inspection, the dry friction color fastness is ≥ level 4, and the wet friction color fastness is ≥ level 3; in the wrinkle resistance test, the wrinkle recovery angle of the lining cloth should be ≥250°; in the hand feel inspection, the softness index of the lining cloth is maintained between 2.0-2.5; in the strength inspection, the warp tensile strength is ≥300N, and the weft tensile strength is ≥200N.

[0023] Beneficial effects of the present invention:

[0024] The present invention ensures uniform distribution of resin and other treatment chemicals on the fiber through pre-ultrasonic treatment and dynamic impregnation technology. This uniform chemical treatment not only improves the overall performance of the lining cloth, but also avoids local hardening or uneven coloring after treatment, thereby greatly enhancing the market competitiveness of the product.

[0025] The present invention effectively reduces the damage that may be caused to the fiber by high temperature by precisely controlling the conditions of the intermediate drying and high-temperature curing steps. The rapid cooling and subsequent softening treatment further ensure the softness and comfort of the treated lining cloth, so that the product can maintain the natural comfort characteristics of pure cotton while improving the wrinkle resistance and color fastness. This improvement in comprehensive performance is not only suitable for the production of high-end clothing materials, but also can meet the needs of the fast fashion industry for high efficiency and high quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 The figure is a schematic diagram of a rapid resin finishing process for pure cotton colored lining cloth according to an embodiment of the present invention. DETAILED DESCRIPTION

[0028] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and the accompanying drawings are only for more specific description of the embodiments, and are not intended to specifically limit the present invention.

[0029] It should be noted that the references to "one embodiment", "an embodiment", "an exemplary embodiment", "some embodiments" and the like in the specification indicate that the embodiments described may include specific features, structures or characteristics, but not every embodiment may include the specific features, structures or characteristics. In addition, when a specific feature, structure or characteristic is described in conjunction with an embodiment, it should be within the knowledge of a person skilled in the art to implement such feature, structure or characteristic in conjunction with other embodiments (whether or not explicitly described).

[0030] In general, a term can be understood, at least in part, from its use in context. For example, depending, at least in part, on the context, the term "one or more" as used herein can be used to describe any feature, structure, or characteristic in the singular sense, or can be used to describe a combination of features, structures, or characteristics in the plural sense. Additionally, the term "based on" can be understood as not necessarily intended to convey an exclusive set of factors, but can instead, depending, at least in part, on the context, allow for the presence of other factors that are not necessarily explicitly described.

[0031] Example 1

[0032] like Figure 1 As shown, a rapid resin finishing process for pure cotton colored interlining fabric comprises the following steps:

[0033] S1: adding melamine formaldehyde resin, polydimethylsiloxane softener, potassium dihydrogen phosphate catalyst, sodium methanesulfonate anti-wrinkle agent, aziridine crosslinker and water in a mixing tank according to a predetermined ratio, and stirring at a high speed to form a uniform finishing liquid;

[0034] S2: Fiber pretreatment, ultrasonic treatment of pure cotton interlining to open the surface structure of cotton fibers and enhance the permeability and adsorption capacity of finishing liquid;

[0035] S3: slowly passing the pretreated pure cotton colored lining fabric through the finishing liquid prepared in S1 for impregnation treatment to ensure uniform distribution and absorption of the finishing liquid;

[0036] S4: The impregnated lining cloth is intermediately dried to remove excess moisture and undergo a preliminary resin curing treatment to enhance its adhesion to the fiber and prepare for the next step of high-temperature curing;

[0037] S5: subjecting the lining fabric after the preliminary resin curing to high temperature curing treatment to form a stable wrinkle-resistant network structure;

[0038] S6: The lining cloth is immediately cooled rapidly after high temperature curing to lock the resin structure and prevent the shape from recovering under high temperature;

[0039] S7: softening the cooled interlining cloth, and then washing it with water to remove unreacted chemicals and surface residues;

[0040] S8: Carry out quality inspection on the processed pure cotton colored interlining fabric, including color fastness, wrinkle resistance, feel and strength inspection, to ensure that each batch of products meets the predetermined quality standards.

[0041] The predetermined proportions in S1 are 5% of melamine formaldehyde resin, 2% of polydimethylsiloxane softener, 1% of potassium dihydrogen phosphate catalyst, 1% of sodium methane sulfonate anti-wrinkle agent, 0.3% of aziridine cross-linking agent, and the balance of water.

[0042] The speed of the high-speed stirring in S1 is 1000 rpm, the stirring time is 25 minutes, and the stirring temperature is controlled at 35° C. to ensure that the components of the finishing liquid are fully mixed.

[0043] The ultrasonic treatment frequency in S2 was 40 kHz and the treatment time was 2 min to open the surface structure of the pure cotton fiber and enhance the permeability of the finishing liquid.

[0044] The immersion treatment time in S3 was 3 minutes, and the lining cloth moved in the finishing liquid at a speed of 0.5 m / s to ensure uniform distribution and absorption of the finishing liquid in the fibers.

[0045] The intermediate drying temperature in S4 is controlled at 70°C for 3 minutes to remove excess moisture, and the temperature is raised to 110°C after the drying is completed. The initial resin curing treatment time is 45 seconds to ensure that the resin is partially cross-linked on the fiber surface to enhance its adhesion and prepare for subsequent high-temperature curing.

[0046] The S5 high temperature curing temperature is controlled at 160°C and the curing time is 1.5 minutes. The resin is efficiently cured by infrared heating technology.

[0047] In S6, the cooling treatment temperature is controlled at 25° C. and the cooling time is 2 minutes to ensure the stability of the resin after curing.

[0048] The softener used in the softening treatment in S7 is a cationic softener with a concentration of 1%, the water washing temperature is 25° C., and the water washing time is 3 minutes, which is used to remove unreacted chemicals and surface residues.

[0049] The quality inspections carried out in S8 include color fastness inspection, wrinkle resistance inspection, hand feel inspection and strength inspection; in the color fastness inspection, the dry friction color fastness is level 6, and the wet friction color fastness is level 5; in the wrinkle resistance test, the wrinkle recovery angle of the lining cloth is 270°; in the hand feel inspection, the softness index of the lining cloth is 2.5; in the strength inspection, the warp tensile strength is 320N, and the weft tensile strength is 220N.

[0050] Example 2

[0051] S1: Add 3% of melamine formaldehyde resin, 1% of polydimethylsiloxane softener, 0.5% of potassium dihydrogen phosphate catalyst, 0.5% of sodium methanesulfonate anti-wrinkle agent, 0.1% of aziridine crosslinker and the balance of water into a mixing tank, mix, and stir at a speed of 800 rpm for 20 minutes, and control the temperature at 30° C. to form a uniform finishing solution;

[0052] S2: The pure cotton colored interlining fabric is subjected to ultrasonic treatment at a frequency of 35kHz for 1 minute;

[0053] S3: The pretreated lining cloth is slowly passed through the finishing liquid at a speed of 0.3 m / s, and the immersion treatment time is 2 minutes;

[0054] S4: drying the impregnated lining cloth at 60°C for 2 minutes to remove excess moisture, and then heating to 100°C for 30 seconds for preliminary resin curing treatment;

[0055] S5: high temperature curing the lining cloth at 150°C for 1 minute to form a stable anti-wrinkle network structure;

[0056] S6: Immediately cool the high temperature cured lining at 20°C for 1 minute to lock the resin structure;

[0057] S7: softening the cooled interlining cloth by using a cationic softener with a concentration of 0.5%, controlling the washing temperature at 20°C and the washing time for 2 minutes to remove unreacted chemicals;

[0058] S8: The treated lining fabric was subjected to quality inspection. The color fastness test results showed that the dry friction color fastness was level 5 and the wet friction color fastness was level 4. The wrinkle recovery angle in the wrinkle resistance test was 260°. The softness index in the hand feel test was 2.3. The warp tensile strength in the strength test was 310N and the weft tensile strength was 210N.

[0059] Example 3

[0060] S1: Add 8% of melamine formaldehyde resin, 4% of polydimethylsiloxane softener, 2% of potassium dihydrogen phosphate catalyst, 1.5% of sodium methanesulfonate anti-wrinkle agent, 0.5% of aziridine cross-linking agent and the balance of water into a mixing tank, mix, and stir at a speed of 1200 rpm for 30 minutes, and control the temperature at 40° C. to form a uniform finishing solution;

[0061] S2: The pure cotton colored interlining is subjected to ultrasonic treatment at a frequency of 45kHz for 3 minutes;

[0062] S3: The pretreated lining cloth is slowly passed through the finishing liquid at a speed of 0.7 m / s, and the immersion treatment time is 5 minutes;

[0063] S4: drying the impregnated lining cloth at 80°C for 4 minutes to remove excess moisture, and then heating to 120°C for 60 seconds for preliminary resin curing;

[0064] S5: high temperature curing the lining cloth at 170°C for 2 minutes to form a stable anti-wrinkle network structure;

[0065] S6: Immediately cool the high temperature cured lining cloth at 30°C for 3 minutes to lock the resin structure;

[0066] S7: softening the cooled interlining cloth by using a 1.5% cationic softener, washing at a temperature of 30°C for 4 minutes to remove unreacted chemicals;

[0067] S8: The treated lining fabric was subjected to quality inspection. The color fastness test results showed that the dry friction color fastness was level 4 and the wet friction color fastness was level 3. The wrinkle recovery angle in the wrinkle resistance test was 250°. The softness index in the hand feel test was 2.0. The warp tensile strength in the strength test was 300N and the weft tensile strength was 200N.

[0068] Table 1 Comparison of performance parameters of finished pure cotton colored interlining fabrics

[0069] Compare Projects Example 1 Example 2 Example 3 Dry rubbing color fastness (grade) 6 5 4 Wet rubbing color fastness (grade) 5 4 3 Wrinkle recovery angle (°) 270 260 250 Softness Index 2.5 2.3 2 Warp tensile strength (N) 320 310 300 Weft tensile strength (N) 220 210 200

[0070] As can be seen from Table 1 above, the dry rubbing color fastness of Example 1 is level 6, and the wet rubbing color fastness is level 5, both higher than the other two groups, indicating that Example 1 has better performance in color fastness, especially higher stability under wet rubbing conditions; the wrinkle recovery angle of Example 1 reaches 270°, showing that it has excellent wrinkle resistance, which is significantly better than Example 2 and Example 3, thanks to the better ratio of resin and anti-wrinkle agent; the softness index of Example 1 is 2.5, while ensuring good wrinkle resistance, it also maintains a high softness of hand feel; the warp tensile strength of Example 1 is 320N, and the weft tensile strength is 220N. These two strength indicators show that it has better durability in actual use. In general, the overall effect of Example 1 is more balanced, suitable for application scenarios with high requirements for color fastness, wrinkle resistance and hand feel.

[0071] The present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention. In order to make the public have a thorough understanding of the present invention, specific details are described in detail in the following preferred embodiments of the present invention, but those skilled in the art can fully understand the present invention without the description of these details. In addition, in order to avoid unnecessary confusion about the essence of the present invention, well-known methods, processes, procedures, components and circuits are not described in detail.

[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A rapid resin finishing process for pure cotton colored lining cloth, characterized in that: The following steps are involved: S1: adding melamine formaldehyde resin, polydimethylsiloxane softener, potassium dihydrogen phosphate catalyst, sodium methanesulfonate anti-wrinkle agent, aziridine crosslinker and water in a mixing tank according to a predetermined ratio, and stirring at a high speed to form a uniform finishing liquid; S2: fiber pretreatment, ultrasonic treatment of pure cotton colored lining fabric; S3: slowly passing the pretreated pure cotton colored lining fabric through the finishing liquid prepared in S1 for impregnation treatment; S4: intermediate drying of the impregnated lining cloth to remove excess water and perform preliminary resin curing treatment; S5: subjecting the lining fabric after the preliminary resin curing to high temperature curing treatment to form a stable wrinkle-resistant network structure; S6: The lining cloth is immediately cooled rapidly after high temperature curing to lock the resin structure; S7: softening the cooled interlining cloth, and then washing it with water to remove unreacted chemicals and surface residues; S8: Carry out quality inspection on the processed pure cotton colored interlining to ensure that each batch of products meets the predetermined quality standards.

2. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The predetermined proportions in S1 are 3%-8% of melamine formaldehyde resin, 1%-4% of polydimethylsiloxane softener, 0.5%-2% of potassium dihydrogen phosphate catalyst, 0.5%-1.5% of sodium methane sulfonate anti-wrinkle agent, 0.1%-0.5% of aziridine cross-linking agent, and the balance is water.

3. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The speed of the high-speed stirring in S1 is 800-1200 rpm, the stirring time is 20-30 minutes, and the stirring temperature is controlled at 30°C-40°C.

4. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The ultrasonic treatment frequency in S2 is 35-45kHz, and the treatment time is 1-3 minutes.

5. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The immersion treatment time in S3 is 2-5 minutes, and the lining cloth moves in the finishing liquid at a speed of 0.3-0.7 m / s.

6. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The intermediate drying temperature in S4 is controlled at 60°C-80°C for 2-4 minutes to remove excess moisture, and after the drying is completed, the temperature is raised to 100°C-120°C, and the initial resin curing treatment time is 30-60 seconds.

7. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The high temperature curing temperature in S5 is controlled at 150° C.-170° C., and the curing time is 1-2 minutes.

8. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The cooling treatment temperature in S6 is controlled at 20° C.-30° C., and the cooling time is 1-3 minutes.

9. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The softener used in the softening treatment in S7 is a cationic softener with a concentration of 0.5%-1.5%, the water washing temperature is 20° C.-30° C., and the water washing time is 2-4 minutes, which is used to remove unreacted chemical substances and surface residues.

10. The rapid resin finishing process for pure cotton colored interlining cloth according to claim 1, characterized in that: The quality inspection in S8 includes color fastness inspection, wrinkle resistance inspection, hand feel inspection and strength inspection; in the color fastness inspection, the dry friction color fastness is ≥ level 4, and the wet friction color fastness is ≥ level 3; in the wrinkle resistance test, the wrinkle recovery angle of the lining cloth should be ≥250°; in the hand feel inspection, the softness index of the lining cloth is maintained between 2.0-2.5; in the strength inspection, the warp tensile strength is ≥300N, and the weft tensile strength is ≥200N.

Citation Information

Cited By

  • Anti-wrinkle composite treatment device for four-way stretch fabric and treatment method of anti-wrinkle composite treatment device

    CN122013467A

  • A device for preventing wrinkles of elastic cloth and a method for processing the device

    CN122013467B