Active brazing filler metal for brazing high-thermal-conductivity carbon material and metal and low-temperature direct brazing method

Through Ag-Cu-In-Sn-Ti active solder and low-temperature direct brazing method, the problems of poor wetting and thermal expansion coefficient differences in the interface between high thermal conductivity carbon materials and metals are solved, and efficient welding at low temperature and welding interface bonding are achieved. Compact and low cost.

CN118789162APending Publication Date: 2024-10-18HARBIN INST OF TECH +1
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202410817566.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing connection process between high thermal conductivity carbon materials and metals has problems such as poor interface wetting, interface reactions, stress concentration caused by differences in thermal expansion coefficients, etc., resulting in low bonding strength, high thermal resistance, and prone to defects at the connection interface, making it difficult to realize at low temperatures. Efficient welding.

Method used

Using Ag-Cu-In-Sn-Ti active solder, the active solder is prepared in a vacuum environment by grinding the powder, and mixed with terpineol and cellulose to form a solder paste, and the low-temperature direct brazing method is used in a vacuum brazing furnace. Welding is carried out in the middle, and the welding temperature is controlled between 580°C and 640°C to form a dense TiC layer and Cu2In phase to improve the interface bonding strength and wettability.

Benefits of technology

It achieves defect-free direct brazing of high thermal conductivity carbon materials and metals at low temperatures. The welding interface is tightly combined, reducing the welding temperature and cost, and improving the thermal conductivity and joint performance of the welded structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789162A_ABST
    Figure CN118789162A_ABST
Patent Text Reader

Abstract

The invention provides active brazing filler metal for brazing of a high-thermal-conductivity carbon material and metal and a low-temperature direct brazing method, and belongs to the technical field of low-temperature connection of dissimilar materials. The problem that low-temperature direct brazing and good joint performance cannot be guaranteed at the same time when an existing high-thermal-conductivity carbon material and metal are welded is solved. The active brazing filler metal comprises Ag-Cu powder, In powder, Sn powder and TiH2 powder, the brazing temperature can be reduced by adjusting and controlling the element content, and low-temperature direct brazing of a high-thermal-conductivity carbon material and metal is achieved; the chemical change of the elements at the interface of the carbon material and the metal can improve the wettability of the interface and the bonding strength of the two, and relieve the residual stress at the interface. The low-temperature direct brazing method provided by the invention comprises the following steps: (1) treating a material to be welded; (2) preparation and sealed storage of AgCuSnInTi active brazing filler metal are carried out; (3) assembling the sample by adopting silk-screen printing; and (4) brazing is conducted in a vacuum brazing furnace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of low-temperature connection of dissimilar materials, and particularly relates to an active brazing filler metal for brazing high thermal conductivity carbon material and metal and a low-temperature direct brazing method. Background Art

[0002] As electronic devices develop towards miniaturization, functional integration, compact structure, high power density, and stability and reliability, the heat flux density of the core chips of electronic devices has increased significantly. Faced with ultra-high heat flux density, the thermal control problem of the core chips has become prominent. In order to solve the technical problem of efficient heat dissipation in the development of a new generation of electronic devices, high thermal conductivity composite materials have emerged. Common high thermal conductivity composite materials include diamond / metal composite materials, APG (annealed pyrolytic graphite) / metal composite materials, and graphene / metal composite materials. Since high thermal conductivity composite materials are obtained by connecting high thermal conductivity carbon materials and metals through special methods, the connection process of high thermal conductivity carbon materials and metals is particularly important, which will determine the state and performance of the connection interface, and thus affect the performance of high thermal conductivity composite materials. The main problems at the interface between high thermal conductivity carbon materials and metals are as follows: (1) The wetting of the interface between carbon materials and metals is poor. For example, the contact angle between graphite and aluminum is about 140°, which makes it easy for holes and defects to form at the interface between the two during the preparation process, resulting in low interface bonding strength and large interface thermal resistance. (2) Carbon materials and some metals are prone to interfacial reactions at high temperatures. For example, carbon materials react with metallic aluminum to easily generate brittle and easily hydrolyzed Al4C3 phases, which are seriously detrimental to the mechanical and thermal properties of composite materials. (3) The thermal expansion coefficients between carbon materials and metals are very different, resulting in serious thermal mismatch at the interface. When experiencing thermal cycles or thermal shocks, significant stress concentration will occur, and the interface bonding reliability is low.

[0003] Among the existing carbon material / metal connection methods, active brazing is one of the most widely studied and most suitable connection methods. This method has the advantages of strong brazing material designability, little impact on the parent material, large welding area and the ability to achieve complex welding joints. The brazing material system often uses active elements (strong carbide-forming elements such as Ti, Cr, Zr, W, V, etc.) to directly weld high thermal conductivity carbon materials and metals. The active brazing method mainly uses the active elements to react with the carbon material to form a carbide layer to improve the wettability of the carbon material. The welding process is relatively simple. At present, active brazing materials are mainly divided into Ni-based, Cu-based and Ag-Cu-based. The melting temperatures of Ni-based and Cu-based brazing materials are about 1000℃ and 900℃ respectively. The welding temperature is generally high, and large residual stress is easily generated at the joint. Although Ag-Cu-based brazing materials have a relatively low welding temperature (such as the welding temperature of Ag-Cu-Ti is about 800℃), their welding temperature is still high for some low melting point metals. When facing materials such as graphene films and APG with low interlayer bonding strength, stress cracking still exists at the joint.

[0004] Therefore, it is necessary to develop an active solder which not only has a lower melting temperature but also has good joint performance, such as no defects in the weld and high bonding strength. This active solder can be used to successfully weld high thermal conductivity carbon materials and metals to meet the urgent needs of efficient heat dissipation of local heat sources with ultra-high heat flux density in small-volume, high-power electronic devices. Summary of the invention

[0005] The present invention aims to solve the problem that the existing high thermal conductivity carbon materials (applicable to various carbon materials such as graphene, APG, diamond, etc.) and metals (mainly high thermal conductivity metals such as aluminum or copper) cannot obtain a welding structure with excellent joint performance through a low temperature direct brazing method. The present invention provides an active brazing filler metal and a low temperature direct brazing method. The active brazing filler metal has a lower melting point, which can realize direct brazing of high thermal conductivity carbon materials and metals at low temperatures, without obvious defects at the weld, with excellent joint performance, simpler brazing process and lower cost.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] One of the objects of the present invention is to provide an active solder, comprising Ag-Cu powder, In powder, Sn powder and TiH2 powder;

[0008] The Sn content in the active solder is 10wt% to 25wt% of the total mass of the powder, the In content is 15wt% to 25wt% of the total mass of the powder, the Ti content is 3wt% to 6wt% of the total mass of the powder, and the balance is Ag-Cu powder.

[0009] Preferably, the Ag-Cu powder is AgCu28.

[0010] Preferably, the active solder is used for low-temperature direct brazing of high thermal conductivity carbon materials and metals.

[0011] A second object of the present invention is to provide a low temperature direct brazing method, comprising the following steps:

[0012] (1) Processing of materials to be welded: soaking, ultrasonic cleaning, and drying the high thermal conductivity carbon material block and the metal block;

[0013] (2) Preparation of active solder: Ag-Cu powder, In powder, Sn powder and TiH2 powder are taken and ground in a vacuum planetary ball mill to obtain active solder, and the solder powder is sealed and stored;

[0014] (3) Sample assembly: Active solder is mixed with pine alcohol and cellulose to form solder paste, and the solder paste is applied to one side of the high thermal conductivity carbon material by screen printing. After assembling the side with a piece of metal, the solder paste is applied to the other side of the high thermal conductivity carbon material by screen printing again, and another piece of metal is pressed on the high thermal conductivity carbon material to obtain a metal / high thermal conductivity carbon material / metal sandwich welding structure. The sandwich welding structure is placed in a graphite mold, and pressure is applied to the sandwich welding structure;

[0015] (4) Brazing: Place the sandwich welding structure together with the graphite mold into a vacuum brazing furnace and heat it. After keeping it warm for 10 to 30 minutes, cool it to room temperature and the brazing is completed.

[0016] Preferably, the ultrasonic cleaning time in (1) is 5 to 10 minutes.

[0017] Preferably, the gas atmosphere when the four powders in (2) are ground in a vacuum planetary ball mill is an argon atmosphere.

[0018] Preferably, the speed of the vacuum planetary ball mill in (2) is 100 to 150 r / min, and the grinding time is 4 to 8 h.

[0019] Preferably, the active solder, pineol and cellulose in (3) have a composition ratio of (2:1:1) to (3:1:1).

[0020] Preferably, the pressure applied to the sandwich welding structure in (3) is 0.5 to 3 MPa.

[0021] Preferably, the heating process in (4) is: maintaining a heating rate of 5 to 20°C / min, first heating to 500°C and keeping it for 20 to 40 minutes, and then continuing to heat to 580°C to 640°C.

[0022] Preferably, the cooling rate in (4) is 5 to 10°C / min.

[0023] The beneficial technical effects of the present invention are as follows:

[0024] (1) The active brazing filler metal used in low-temperature direct brazing has a more flexible and controllable composition and a simple preparation method. By regulating the melting point-reducing elements (In, Sn) and active elements (Ti), it can meet the process requirements of different welding structures for welding temperature, wettability, etc.

[0025] (2) The active solder provided by the present invention is obtained by adding In and Sn, two melting point reducing elements, to the traditional AgCuTi solder system. Both elements play a role in reducing the welding temperature of the solder system. In addition, the contents of Sn and In in the active solder are regulated according to the Cu-Sn-In ternary phase diagram, so that the melting point of the AgCuSnInTi active solder is further reduced to 580°C to 640°C compared with the melting point of the traditional AgCuTi solder, which meets the temperature range for directly welding high thermal conductivity carbon materials and metals. However, In and Sn do not only play a role in reducing the melting point. Sn The addition of elements helps to improve the wettability of the solder to the metal side, improve the plasticity and toughness of the solder, and reduce the preparation cost of the solder; the In element can not only improve the thermal conductivity of the solder and reduce the melting point of the solder, but also avoid the formation of Cu6Sn5 brittle compounds. This is because, according to the Cu-In-Sn ternary phase diagram, when Cu, In, and Sn are all present, it is easier to form a Cu2In phase with better plasticity and toughness and a higher melting point, among which the Sn element is dissolved in the Cu2In phase as a solid solution element, thereby preventing the formation of Cu6Sn5 brittle compounds.

[0026] (3) Adding Sn and In to the AgCuTi solder system can achieve direct soldering at low temperature and good joint performance at the same time. Adding Sn or In element alone cannot achieve this effect, because the AgCuSnTi solder with only Sn added cannot reduce the welding temperature to 600℃, while the AgCuInTi solder with only In added generally requires 30-40wt% In addition when the welding temperature is reduced to 600℃. This high addition ratio will cause the In element to precipitate along the grain boundaries on the metal side of the welded joint, reducing the joint performance.

[0027] (4) In the AgCuSnInTi active solder, Ti forms a dense TiC layer on the carbon material side to prevent excessive reaction at the interface. At the same time, when welding metals, the lower Gibbs free energy of reaction between Ti and C can prevent the metal elements from diffusing to the high thermal conductivity carbon material side and reacting with the carbon element to form a harmful phase. In addition, sufficient interfacial reaction between Ti and the high thermal conductivity carbon material is conducive to the formation of a tight interface bonding, which is beneficial to interfacial heat conduction and improves the thermal conductivity of the welding structure. Appropriate Ti content control can make the AgCuSnInTi active solder system fully wet the high thermal conductivity carbon material, solving the problem of simultaneous wetting of the carbon material and metal interface.

[0028] (5) The weld is mainly composed of Al-Cu-In solid solution and fine Ag-metal (Al, Cu, etc.) and Cu-In compounds. The plasticity and toughness of the Al-Cu-In solid solution can effectively relieve the residual stress in the weld. The fine Ag-metal (Al, Cu, etc.) compounds and Cu-In compounds can further improve the weld strength through the second phase strengthening effect.

[0029] (6) Compared with other high thermal conductivity carbon material / metal brazing methods, the low temperature direct brazing method provided by the present invention can directly weld high thermal conductivity carbon material and metal at a lower welding temperature. The welding interface is tightly bonded, the microstructure distribution in the weld is uniform, and there are no obvious defects. In addition, compared with the two-step method (low temperature brazing method after graphene modification), the low temperature direct brazing method has the advantages of mature and simple welding process and lower cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The wetting conditions of the AgCuSnInTi active solder obtained in Example 1 on the graphene surface at different temperatures;

[0031] Figure 2 This is a microstructure picture of the aluminum / graphene / aluminum sandwich welded structure joint obtained in Example 1;

[0032] Figure 3 This is a microstructure picture of the aluminum / graphene / aluminum sandwich welded structure joint obtained in Comparative Example 1;

[0033] Figure 4 This is a microstructure picture of the aluminum / graphene / aluminum sandwich welded structure joint obtained in Comparative Example 2;

[0034] Figure 5 This is a microstructure picture of the aluminum / graphene / aluminum sandwich welded structure joint obtained in Comparative Example 3;

[0035] Figure 6 This is a microstructure picture of the aluminum / graphene / aluminum sandwich welded structure joint obtained in Comparative Example 4;

[0036] Figure 7 (a) is a microstructure picture of the copper / diamond / copper sandwich welded structure joint obtained in Example 2. Figure 7 (b) Figure 7 (a) A partial enlarged view. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. The following embodiments are only used to more clearly illustrate the technical solutions of the present invention, and cannot be used to limit the protection scope of the present invention.

[0038] Unless otherwise specified, the experimental materials, reagents, methods and instruments used in the following embodiments and comparative examples are conventional materials, reagents, methods and instruments in the art and can be obtained through commercial channels by those skilled in the art.

[0039] Example 1

[0040] Wettability experiment: In powder, Sn powder, TiH2 powder and AgCu28 powder were weighed according to a certain proportion, wherein the contents of Sn, In and Ti were 10wt%, 20wt% and 4wt% of the total mass of the powder respectively, and the balance was AgCu28 powder. The four powders were placed in the ball mill jar of a vacuum planetary ball mill. The gas atmosphere in the jar was argon atmosphere. The ball mill speed was 120r / min and the grinding time was 6h to obtain AgCuSnInTi active solder. The vacuum dynamic wetting angle equipment was used to observe the wetting state of the active solder on the graphene surface in real time. The heating rate was 5℃ / min, and the temperature was raised to 800℃ to ensure that the highest experimental temperature was higher than the melting point of the active solder. After the observation, the temperature was cooled with the furnace.

[0041] Figure 1 Figure 3 is the wetting of active solder on the graphene surface at different temperatures. It can be seen that the wettability of AgCuSnInTi active solder with graphene is poor at 550℃ and 570℃. As the temperature increases to 610℃, 630℃ and 690℃, the wetting angle gradually decreases. However, at 610℃ or 630℃, the wettability of the active solder with graphene is sufficient for brazing. This indicates that AgCuSnInTi active solder has a low melting point and can be used to weld high thermal conductivity carbon materials and metals at low temperatures.

[0042] Brazing:

[0043] (1) Processing of materials to be welded: soak the graphene block and the metal aluminum block in alcohol, put them in an ultrasonic cleaning machine for cleaning for 5 to 10 minutes, take them out and dry them;

[0044] (2) Preparation of active solder: AgCuSnInTi active solder was prepared according to the steps in the wettability test method. The contents of Sn, In and Ti were the same as those in the active solder used in the wettability test, which were 10wt%, 20wt% and 4wt% of the total mass of the powder, respectively. The balance was Ag-Cu28 powder. The prepared solder powder was transferred into a centrifuge tube and sealed, and then stored in a vacuum glove box to prevent oxidation of the solder powder.

[0045] (3) Sample assembly: Active solder powder is mixed with pine alcohol and cellulose to make solder paste in a mass ratio of 3:1:1. The solder paste is evenly applied to one side of the graphene by screen printing. After assembling this side with an aluminum block, the solder paste is again applied to the other side of the graphene by screen printing. Then, another aluminum block is pressed on top of the graphene to obtain an aluminum / graphene / aluminum sandwich welding structure. The structure is placed in a graphite mold, the bottom of the graphite mold is fixed, and a pressure of 0.5 MPa is applied to the sandwich welding structure from the top.

[0046] (4) Low temperature direct brazing: Place the sandwich welded structure together with the graphite mold in a vacuum chamber with a degree of vacuum below 10 -4Pa vacuum brazing furnace with a heating rate of 15°C / min. The temperature was first raised to 500°C and kept for 30 min, then continued to rise to 600°C and kept for 20 min. After the insulation, the temperature was cooled to room temperature at a cooling rate of 5°C / min to obtain the aluminum / graphene / aluminum sandwich structure after brazing.

[0047] The aluminum / graphene / aluminum sandwich welded structure joint obtained in this example was characterized, and the SEM results are as follows: Figure 2 As shown, the joint weld is uniform and has no defects, and the brazing angle climbing effect is obvious, indicating that the active brazing material has good wettability to graphene. The average shear strength of the welded joint obtained in this embodiment is 38±6MPa.

[0048] Comparative Example 1

[0049] The difference between this comparative example and Example 1 is that the contents of Sn, In and Ti in the active solder are 15wt%, 25wt% and 6wt% of the total mass of the powder respectively, and the balance is Ag-Cu28 powder. The other brazing process steps and parameter settings are the same as those in Example 1.

[0050] The aluminum / graphene / aluminum sandwich welded structure joint obtained in this comparative example was characterized, and the SEM results are as follows: Figure 3 As shown, it can be seen that there are many holes in the welded structure. On the one hand, the high Sn content leads to the precipitation of a large number of flaky Cu-Sn compounds. The compounds have high brittleness, resulting in crack defects in the weld. During the metallographic treatment of SEM characterization, large pieces of Cu-Sn compounds fell off. On the other hand, the high In content leads to the diffusion of a large amount of In elements into Al metal, weakening the properties of the welded metal. In addition, the increase in Ti content does not improve the wetting effect of the graphene surface, but instead forms too many Ag-Ti and Al-Ti compounds, which also weakens the joint performance.

[0051] Comparative Example 2

[0052] The difference between this comparative example and Example 1 is that the brazing temperature is 560° C., and the other brazing process steps and parameter settings are the same as those in Example 1.

[0053] The aluminum / graphene / aluminum sandwich welded structure joint obtained in this comparative example was characterized, and the SEM results are as follows: Figure 4 As shown, it can be seen that due to the low temperature at 560℃, there are unwelded defects in the weld.

[0054] Comparative Example 3

[0055] The difference between this comparative example and Example 1 is that the brazing temperature is 580° C., and the other brazing process steps and parameter settings are the same as those in Example 1.

[0056] The aluminum / graphene / aluminum sandwich welded structure joint obtained in this comparative example was characterized, and the SEM results are as follows: Figure 5 As shown in the figure, the unwelded defects at the joints were significantly eliminated at 580°C.

[0057] Comparative Example 4

[0058] The difference between this comparative example and Example 1 is that the brazing temperature is 640° C., and the other brazing process steps and parameter settings are the same as those in Example 1.

[0059] The aluminum / graphene / aluminum sandwich welded structure joint obtained in this comparative example was characterized, and the SEM results are as follows: Figure 6 As shown in the figure, the content of brittle compounds such as Ag-Al in the weld increases significantly, and the large amount of brittle compounds is not conducive to the strength of the joint. The strength test of the aluminum / graphene / aluminum sandwich welded joint brazed at 640°C showed that the shear strength was only 15MPa, which was about 20MPa lower than that of the joint brazed at 600°C. This shows that the higher the brazing temperature, the better. When the temperature rises to 640°C, the brittle compounds such as Ag-Al in the weld increase significantly. At the same time, due to the large difference in thermal expansion coefficient between high thermal conductivity carbon materials and metals, the joint is more affected by thermal stress as the welding temperature rises, so the joint strength decreases.

[0060] Example 2

[0061] The difference between this embodiment and embodiment 1 is that the high thermal conductivity carbon material is diamond, the metal is oxygen-free copper, and the remaining brazing process steps and parameter settings are the same as those in embodiment 1.

[0062] The copper / diamond / copper sandwich welded structure joint obtained in this example was characterized, and the SEM results are as follows: Figure 7 As shown, the active brazing filler metal has excellent solderability for diamond and can achieve heterogeneous connection with Cu material.

Claims

1. An active solder, characterized in that: Including Ag-Cu powder, In powder, Sn powder and TiH2 powder; The active solder contains 10wt% to 25wt% of the total mass of the powder of Sn, 15wt% to 25wt% of the total mass of the powder of In, 3wt% to 6wt% of the total mass of the powder of Ti, and the remainder is Ag-Cu powder.

2. The active solder according to claim 1, characterized in that: The Ag-Cu powder is AgCu28.

3. Use of the active solder according to any one of claims 1 to 2, characterized in that: Used for low temperature direct brazing of high thermal conductivity carbon materials and metals.

4. The use of the active solder according to claim 3, characterized in that: The application method comprises the following steps: (1) Processing of materials to be welded: soaking, ultrasonic cleaning, and drying the high thermal conductivity carbon material block and the metal block; (2) Preparation of active solder: Ag-Cu powder, In powder, Sn powder and TiH2 powder are taken and ground in a vacuum planetary ball mill to obtain active solder, and the solder powder is sealed and stored; (3) Sample assembly: Active solder is mixed with pine alcohol and cellulose to form solder paste, and the solder paste is applied to one side of the high thermal conductivity carbon material by screen printing. After assembling the side with a piece of metal, the solder paste is applied to the other side of the high thermal conductivity carbon material by screen printing again, and another piece of metal is pressed on the high thermal conductivity carbon material to obtain a metal / high thermal conductivity carbon material / metal sandwich welding structure. The sandwich welding structure is placed in a graphite mold, and pressure is applied to the sandwich welding structure; (4) Brazing: Place the sandwich welding structure together with the graphite mold into a vacuum brazing furnace and heat it. After keeping it warm for 10 to 30 minutes, cool it to room temperature and the brazing is completed.

5. The use of the active solder according to claim 4, characterized in that: The ultrasonic cleaning time in (1) is 5 to 10 minutes.

6. The use of the active solder according to claim 4, characterized in that: The gas atmosphere when the four powders in (2) are ground in the vacuum planetary ball mill is argon atmosphere.

7. The use of the active solder according to claim 4, characterized in that: The rotation speed of the vacuum planetary ball mill in (2) is 100-150 r / min, and the grinding time is 4-8 h.

8. The use of the active solder according to claim 4, characterized in that: The mass ratio of the active solder, pineol and cellulose in (3) is (2:1:1) to (3:1:1).

9. The use of the active solder according to claim 4, characterized in that: In the above (3), the pressure applied to the sandwich welding structure is 0.5-3Mpa.

10. The use of the active solder according to claim 4, characterized in that: The heating process in (4) is as follows: maintaining a heating rate of 5 to 20°C / min, first heating to 500°C and keeping the temperature for 20 to 40 minutes, and then continuing to heat to 560 to 640°C.

Citation Information

Cited By

  • Method for brazing graphite / copper dissimilar material by using diamond particle reinforced AgCuInTi composite brazing filler metal

    CN119566623A

  • Graphene aluminum vapor chamber and preparation method thereof

    CN119653739A

  • Ag-Cu-Ti-based composite brazing filler metal and preparation method and application thereof

    CN120828232A

  • Copper alloy and preparation method and application thereof

    CN122564328A

  • A copper alloy, a method for preparing the same, and an application thereof

    CN122564328B