Modification method and application of fuel cell catalyst carrier
Surface modification of carbon powder through plasma technology solves the problems of fuel cell catalyst carrier durability and environmental pollution, improves fuel cell performance and achieves green and environmentally friendly production.
Patent Information
- Application Number
- CN202410806854.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-22
AI Technical Summary
The durability of the fuel cell catalyst carrier decreases during use, resulting in a decrease in the long-term operating performance of the fuel cell. Traditional wet processing has problems such as difficulty in control and environmental pollution.
Plasma technology is used to surface modify the carbon powder to increase the specific surface area and active site density, improve the dispersion performance, and achieve uniform loading of platinum particles on the carbon black through plasma treatment.
The durability of the catalyst carrier and the performance of the fuel cell are improved, the cost is reduced, the processing steps are simplified, and green and environmentally friendly industrial production is achieved.
Smart Images

Figure CN118825293A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a modification method of a fuel cell catalyst carrier and application thereof. Background Art
[0002] A fuel cell is a device that converts chemical energy directly into electrical energy. It has the advantages of high efficiency and environmental protection and is widely used in various fields. Catalysts are key components in fuel cells and are of great significance for improving fuel cell performance. However, during use, the durability of catalyst carriers is often reduced due to various factors, affecting the long-term operation of fuel cells. Therefore, how to improve the durability of catalyst carriers is an urgent problem to be solved in the field of fuel cells.
[0003] In recent years, the pretreatment of carbon carriers has received widespread attention as a method to improve catalyst activity. Traditional catalyst carrier materials have some problems in fuel cells, such as poor dispersibility, poor corrosion resistance, and instability. Therefore, finding a new method to improve the performance of catalyst carrier materials is a research hotspot in the current fuel cell field. In traditional methods, carbon black is treated in a solution containing HNO3, H2O2 or NaOH; however, these wet treatments are not easy to control and remove residues from carbon powder, and may cause acidic and alkaline substances to pollute the environment. Plasma is an effective method to adjust the pore size and functionalization of the carbon carrier surface. By changing the plasma gas, various functional groups can be grafted on the carbon surface, thereby modifying the carbon powder surface. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for modifying a fuel cell catalyst carrier and its application, by placing carbon powder in a plasma treatment device and using plasma to modify the surface of the carbon powder, thereby increasing its specific surface area and active site density, improving the dispersion performance of the carbon powder, and then achieving uniform loading of platinum particles on carbon black, thereby improving its performance in fuel cell catalysts.
[0005] The technical solution adopted by the present invention is:
[0006] A method for modifying a fuel cell catalyst carrier, wherein the steps are as follows:
[0007] Step S1. placing the carrier in a cavity of a plasma processing device, evacuating the cavity so that the gas pressure in the plasma processing device is maintained at a first gas pressure, and then introducing a reaction gas into the plasma processing device;
[0008] Step S2: maintaining the first gas pressure, continuing to introduce the reaction gas into the plasma treatment equipment, performing plasma treatment on the carrier, and obtaining a modified catalyst carrier.
[0009] Preferably, in the modification method of the fuel cell catalyst carrier, the plasma treatment equipment in step S1 is selected from one of a normal pressure atmospheric jet plasma equipment, a dielectric barrier plasma equipment and a low pressure vacuum plasma equipment.
[0010] Preferably, in the method for modifying a fuel cell catalyst carrier, the carrier in step S1 is selected from one or more of biomass carbon, graphene, Ketjen black, carbon black, acetylene black, carbon nanotubes, and a mixed carrier of oxide and carbon.
[0011] Preferably, in the method for modifying a fuel cell catalyst carrier, the first gas pressure in step S1 is 1-100 Pa.
[0012] Preferably, in the method for modifying a fuel cell catalyst carrier, the reaction gas in step S1 is selected from one or two of compressed air, N2, H2, O2, and Ar, and the flow rate of the reaction gas is 10 to 200 sccm.
[0013] Preferably, in the method for modifying a fuel cell catalyst carrier, when the carrier is subjected to plasma treatment in step S2, the radio frequency power of the plasma treatment equipment is 50 to 200 W, and the treatment time is 3 to 60 minutes.
[0014] An application of a modified catalyst carrier obtained by a modification method of a fuel cell catalyst carrier, wherein: the modified catalyst carrier is used to synthesize a fuel cell catalyst.
[0015] Preferably, in the application, the synthesis of fuel cell catalyst specifically comprises the following steps:
[0016] (1) dissolving a platinum source in water to obtain a solution A, then adding the modified catalyst support to the solution A, stirring until the mixture is uniformly mixed, and drying to obtain a platinum-carbon precursor;
[0017] (2) Under an inert atmosphere, a platinum-carbon precursor is subjected to plasma treatment to obtain a platinum-carbon catalyst.
[0018] Preferably, in the application, the platinum source in step (1) is selected from one of platinum nitrate, platinum chloride, tetraammineplatinum sulfate, and platinum acetylacetonate, the mass ratio of the platinum source to the modified catalyst carrier is 1-2:1, the drying temperature is 60-80°C, and the drying time is 16-24h.
[0019] Preferably, in the application, the inert gas in step (2) is a mixed gas of H2 and Ar, the gas flow rate ratio of H2 and Ar is 1-2, the discharge frequency during plasma treatment is 12-13KHz, the discharge voltage is 2-30KV, and the discharge time is 5-60min.
[0020] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0021] (1) Compared with the conventional wet treatment of carbon powder, the modification method of the fuel cell catalyst carrier of the present invention introduces specific functional groups or changes the surface morphology through plasma technology, which has low processing cost and is conducive to industrial production; through plasma treatment, the dispersion performance of carbon powder can be improved, and the agglomeration of platinum nanoparticles on the modified carbon powder is reduced.
[0022] (2) The modification method of the fuel cell catalyst carrier of the present invention is that the carrier is subjected to plasma treatment, and the introduced functional groups can effectively inhibit the corrosion of the carbon carrier, so that the durability of the membrane electrode is greatly improved, thereby improving the performance of the fuel cell, reducing costs, and extending the service life.
[0023] (3) The fuel cell catalyst carrier modified by the method of the present invention is used in the synthesis of fuel cell catalysts. The treatment process is green and environmentally friendly, and the treatment steps are simple and efficient, which is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The scanning electron microscope images of the treated carbon powder (a) and the untreated carbon powder (b) of Example 1 of the present invention are shown.
[0025] Figure 2 The XPS full spectrum (a) and O1s element spectrum (b) of the carbon powder treated with plasma by passing compressed air in Example 2 of the present invention and the untreated carbon powder in Comparative Example 1.
[0026] Figure 3 The XRD spectra of the XC-72R carbon black treated with plasma by passing compressed air in Example 3 of the present invention and the untreated XC-72R carbon black in Comparative Example 1.
[0027] Figure 4 Cyclic voltammetry (CV) curves of the platinum-carbon catalyst prepared in Example 4 of the present invention and the platinum-carbon catalyst prepared in Comparative Example 1.
[0028] Figure 5 Polarization curves of the platinum-carbon catalyst prepared in Example 4 of the present invention and the platinum-carbon catalyst prepared in Comparative Example 1.
[0029] Figure 6Transmission electron micrographs of the platinum-carbon catalyst (a) prepared in Example 4 of the present invention and the platinum-carbon catalyst (b) prepared in Comparative Example 1. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific embodiments.
[0031] Example 1
[0032] A method for modifying a fuel cell catalyst carrier, comprising the following steps:
[0033] Step S1. 10 g of XC-72R carbon black is placed in the cavity of a normal pressure atmospheric jet plasma device, and the vacuum is evacuated so that the gas pressure in the plasma treatment device is maintained at 30 Pa, and then the reaction gas N2 is introduced into the plasma treatment device at a gas flow rate of 50 sccm;
[0034] Step S2. Maintain the gas pressure at 30 Pa, continue to introduce the reaction gas into the plasma treatment equipment, perform plasma treatment on the carrier, set the RF power to 50 W, and the treatment time to 3 min to obtain plasma-treated XC-72R carbon black.
[0035] Figure 1 The scanning electron micrographs of the plasma treated carbon powder (a) and the untreated carbon powder (b) are shown. Due to the short treatment time, there is no obvious difference between the treated and untreated carbon powders as seen from the scanning electron micrographs.
[0036] The synthesis of fuel cell catalyst specifically includes the following steps:
[0037] (1) 1.64 g of solid platinum nitrate was dissolved in 50 ml of water to obtain solution A, and then 1 g of plasma-treated XC-72R carbon black was added to solution A and stirred for 20 min until the mixture was uniformly mixed, and then dried at 80 ° C for 18 h to obtain a platinum-carbon precursor;
[0038] (2) In an atmosphere of a mixed gas of H2 and Ar, with a H2 / Ar gas flow rate ratio of 2, the platinum-carbon precursor was subjected to plasma treatment with a discharge frequency of 12.8 kHz, a discharge voltage of 10 KV, and a discharge time of 20 min to obtain a platinum-carbon catalyst.
[0039] Example 2
[0040] The difference between this embodiment and embodiment 1 is that the radio frequency power is 50W, the treatment time is 3min, the gas introduced is compressed air, and the gas flow rate and vacuum degree are the same as those in embodiment 1. Figure 2 After the carrier is treated with air plasma, the characteristic peak of O1s appears in the material, indicating that oxygen-containing functional groups have been added to the surface of the material. Figure 2It can be seen from these data that the oxygen-containing functional groups added are mainly carboxyl groups, which provides evidence that the introduced carboxyl groups effectively anchor the noble metal ion precursors through coordination or electrostatic interactions and disperse the platinum nanoparticles on the carbon black surface in the subsequent reduction reaction.
[0041] The specific steps for synthesizing the fuel cell catalyst are the same as those in Example 1. According to the half-cell performance listed in Table 1, when the treatment time is the same, the half-cell performance of the catalyst synthesized after plasma treatment using compressed air is better than that of the catalyst synthesized after nitrogen plasma treatment.
[0042] Example 3
[0043] The difference between this embodiment and embodiment 2 is that the treatment time is 20 minutes, the type of gas introduced and the RF power setting are the same as those in embodiment 2, and the gas flow rate and vacuum degree are consistent with those in embodiment 1. Figure 3 XRD spectra of untreated XC-72R carbon black and XC-72R carbon black treated with compressed air plasma.
[0044] The specific steps for synthesizing the fuel cell catalyst are the same as those in Example 1. As can be seen from Table 1, the performance of the synthesized catalyst increases as the plasma treatment time increases.
[0045] Example 4
[0046] The difference between this embodiment and embodiment 3 is that the processing time is 30 minutes, the radio frequency power is 100W, the type of gas introduced is the same as that in embodiment 2, and the gas flow rate and vacuum degree are the same as those in embodiment 1.
[0047] The specific steps for synthesizing the fuel cell catalyst are the same as those in Example 1. The prepared catalyst is subjected to a half-cell test using an electrochemical workstation. Figure 4 As shown, the areas of hydrogen desorption peak and hydrogen adsorption peak of the platinum-loaded catalyst sample increased significantly after plasma treatment, indicating an increase in its electrochemical active surface area. The performance of the catalyst half-cell synthesized by platinum-loaded carbon powder after plasma treatment was significantly improved.
[0048] The membrane electrode prepared from the fuel cell catalyst obtained in this example was assembled into a single cell, and its polarization curve (IV characteristic curve) was tested. Figure 5 As shown, the polarization curve of the catalyst sample loaded with platinum after plasma treatment is significantly better than that of the control sample, indicating that the catalyst synthesized by loading platinum on carbon powder after plasma treatment not only improves the half-cell performance but also significantly improves the full-cell performance.
[0049] Example 5
[0050] The difference between this embodiment and embodiment 4 is that the processing time is 60 minutes, the radio frequency power is 200W, the type of gas introduced is the same as that in embodiment 4, and the gas flow rate and vacuum degree are the same as those in embodiment 1.
[0051] The specific steps of synthesizing the fuel cell catalyst are the same as those in Example 1. As can be seen from Table 1, the performance does not continue to increase after long-term treatment, indicating that long-term treatment may have an impact on the carbon powder, thereby causing the performance of the synthesized catalyst to deteriorate.
[0052] Comparative Example 1
[0053] The difference between this comparative example and Example 4 is that the XC-72R carbon black is not subjected to plasma treatment, and the specific steps for synthesizing the fuel cell catalyst are the same as those in Example 1. Figure 6 From the transmission electron microscope, it can be seen that the platinum particles grow more evenly on the surface of the treated XC-72R carbon black, while the platinum particles in the platinum-carbon catalyst synthesized from the untreated XC-72R carbon black have obvious agglomeration. Comparing the performance in Table 1, it can be seen that the mass activity and electrochemical activity of the synthesized catalyst are lower than the half-cell performance after plasma treatment without the plasma treatment of the carbon powder.
[0054] The half-cell performances of Examples 1-5 of the present invention and Comparative Example 1 are shown in Table 1.
[0055] Table 1
[0056]
[0057] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for modifying a fuel cell catalyst carrier, characterized in that: Here are the steps: Step S1. placing the carrier in a cavity of a plasma processing device, evacuating the cavity so that the gas pressure in the plasma processing device is maintained at a first gas pressure, and then introducing a reaction gas into the plasma processing device; Step S2: maintaining the first gas pressure, continuing to introduce the reaction gas into the plasma treatment equipment, performing plasma treatment on the carrier, and obtaining a modified catalyst carrier.
2. The method for modifying a fuel cell catalyst carrier according to claim 1, characterized in that: In step S1, the plasma processing equipment is selected from one of a normal pressure atmospheric jet plasma equipment, a dielectric barrier plasma equipment, and a low pressure vacuum plasma equipment.
3. The method for modifying a fuel cell catalyst carrier according to claim 1, characterized in that: In step S1, the carrier is selected from one or more of biomass carbon, graphene, Ketjen black, carbon black, acetylene black, carbon nanotubes, and a mixed carrier of oxide and carbon.
4. The method for modifying a fuel cell catalyst carrier according to claim 1, characterized in that: In step S1, the first gas pressure is 1-100 Pa.
5. The method for modifying a fuel cell catalyst carrier according to claim 1, characterized in that: In step S1, the reaction gas is selected from one or two of compressed air, N2, H2, O2, and Ar, and the flow rate of the reaction gas is 10-200 sccm.
6. The method for modifying a fuel cell catalyst carrier according to claim 1, characterized in that: When the carrier is subjected to plasma treatment in step S2, the radio frequency power of the plasma treatment equipment is 50-200 W, and the treatment time is 3-60 min.
7. An application of a modified catalyst carrier obtained by the modification method of a fuel cell catalyst carrier according to any one of claims 1 to 6, characterized in that: The modified catalyst carrier is used for synthesizing fuel cell catalysts.
8. The use according to claim 7, characterized in that: The synthesis of fuel cell catalyst specifically includes the following steps: (1) dissolving a platinum source in water to obtain a solution A, then adding a modified catalyst support to the solution A, stirring until the mixture is uniformly mixed, and drying to obtain a platinum-carbon precursor; (2) Under an inert atmosphere, the platinum-carbon precursor is plasma treated to obtain a platinum-carbon catalyst.
9. The use according to claim 8, characterized in that: In step (1), the platinum source is selected from one of platinum nitrate, platinum chloride, tetraammineplatinum sulfate, and platinum acetylacetonate, the mass ratio of the platinum source to the modified catalyst carrier is 1-2:1, the drying temperature is 60-80°C, and the drying time is 16-24 h.
10. The use according to claim 8, characterized in that: In step (2), the inert gas is a mixture of H2 and Ar, the gas flow rate ratio of H2 to Ar is 1-2, the discharge frequency during plasma treatment is 12-13 KHz, the discharge voltage is 2~30KV, and the discharge time is 5~60 min.
Citation Information
Cited By
Modification method of catalyst particles, catalyst particles and application of catalyst particles
CN119764468A
Fuel cell catalyst for improving durability of carrier and preparation method of fuel cell catalyst