Visible light excited organic long afterglow material as well as preparation method and application thereof

By oxidizing phenothiazine to sulfone, a visible light-excited organic long-afterglow material MOP is formed, which solves the inter-system jump problem in the existing technology that requires external force assistance, and achieves efficient room temperature phosphorescence emission without external force assistance, and is used in biological analysis. Excellent performance in encryption and encryption applications.

CN118852053AInactive Publication Date: 2024-10-29DALIAN NATIONALITIES UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410893801.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing organic long-afterglow materials require external assistance to increase the intersystem jump rate and reduce non-radiative transitions, and are mainly excited by ultraviolet light, which limits their application in fields such as bioanalysis and bioimaging.

Method used

By reacting phenothiazine with potassium tert-butoxide in a tetrahydrofuran solution, a methyl group is introduced and oxidized to a sulfone in the oxidation reaction of dichloromethane and glacial acetic acid to form a visible light-excited organic long-afterglow material MOP, using molecules The interaction between them restricts molecular motion, inhibits the non-radiative transition of triplet excitons, and promotes the intersystem jump rate.

Benefits of technology

It achieves efficient room-temperature phosphorescence emission without external assistance, and expands the application of the material under visible light excitation, especially showing remarkable features in multiple encryption and decryption of data.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852053A_ABST
    Figure CN118852053A_ABST
Patent Text Reader

Abstract

The invention discloses a visible-light-excited organic long-afterglow material and a preparation method and application thereof, and belongs to the technical field of organic long-afterglow luminescent materials.The preparation method comprises the steps that phenothiazine and potassium tert-butoxide are added into a tetrahydrofuran solution and stirred, then methyl iodide is added for a stirring reaction, and a reaction solution is obtained; in the reaction process, hydrogen atoms in phenothiazine molecules are removed, methyl is introduced into the phenothiazine molecular structures, cooling and extraction are carried out, an organic phase is obtained, a solvent in the organic phase is removed, purification is carried out, an intermediate product microcrystal is obtained, the microcrystal is added into a mixed solution of dichloromethane and glacial acetic acid, H2O2 is added, an oxidation reaction is carried out, and phenothiazine is obtained. Sulfur in methylphenothiazine is oxidized into sulfone, and the visible light excited organic long afterglow material MOP capable of realizing fluorescence-room temperature phosphorescence multiple emission is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic long afterglow luminescent materials, and in particular to a visible light excited organic long afterglow material and a preparation method and application thereof. Background Art

[0002] Ultra-long phosphorescence, also known as persistent luminescence or afterglow luminescence, is an amazing optical phenomenon that can continue to glow for seconds, minutes, or even hours after the excitation light source is removed. As early as 1866, an artificial powder with persistent luminescence was obtained. Due to these interesting optical properties, ultra-long phosphorescence has a wide range of applications in various fields such as display, emergency lighting, sensors, bioimaging, and medical diagnosis.

[0003] Although ultralong phosphorescence has a long history, it is mainly limited to inorganic materials doped with transition metals with limited resources. However, these inorganic long-life materials have certain disadvantages, such as expensive metal components, harsh preparation conditions and inherent insulation. Therefore, people's attention has gradually shifted to non-metallic organic phosphorescent materials. Among organic phosphorescent materials, pure organic small molecules are simple to synthesize, low in cost, easy to modify, and functionalized organic light-emitting materials can be obtained through mature excited state theory.

[0004] For small molecule crystal long afterglow materials, on the one hand, it is necessary to introduce some functional groups into the molecules to increase the intersystem crossing rate, such as carbonyl, hydroxyl, carboxylic acid, carboxylate, sulfone, halogen heavy atoms, etc., and use these functional groups to promote spin-orbit coupling and generate more triplet excitons. On the other hand, by constructing a rigid environment to provide a confinement and separation condition for achieving room temperature phosphorescence, such as host-guest doping, polymers, metal-organic frameworks, ionic crystals, etc. Therefore, in order to achieve long afterglow emission of small molecules, an external force is usually required to increase the intersystem crossing process and reduce non-radiative transitions.

[0005] However, research on simple, easy-to-obtain, efficient and long-lived compounds that do not require any external assistance is still rare. Currently, most organic long-afterglow materials are excited by ultraviolet light, and their applications are mainly anti-counterfeiting, data encryption, sensing, etc. Compared with ultraviolet light, visible light has less phototoxicity, stronger penetration for bioanalysis and bioimaging, lower lethality, and is more convenient for practical applications. Although researchers have made great efforts in this regard, organic long-afterglow emission excited by visible light is still a huge challenge. Summary of the invention

[0006] The present invention provides a visible light excited organic long afterglow material and its preparation method and application, which effectively solves the technical problem of increasing the intersystem crossing process and reducing the non-radiative transition by external force to achieve the long afterglow emission of small molecules. The present invention is based on the structural characteristics of the phenothiazine molecule itself. The MOP molecule interacts with three molecules, including The formation of molecular stacking restricts the movement of molecules, inhibits the non-radiative transition of triplet excitons, and promotes the intersystem crossing rate, thereby achieving efficient room temperature phosphorescence.

[0007] The first object of the present invention is to provide a method for preparing a visible light excited organic long afterglow material, characterized in that it comprises the following steps:

[0008] Phenothiazine and potassium tert-butoxide are added to a tetrahydrofuran solution, stirred at 0°C for 15 to 30 minutes, and then methyl iodide is added and stirred for 12 hours to introduce a methyl group into the molecular structure of phenothiazine. The solution is cooled and extracted to obtain an organic phase, and the solvent in the organic phase is removed and purified to obtain microcrystals. A mixed solution of dichloromethane and glacial acetic acid is added to the microcrystals, and then H2O2 is added to carry out an oxidation reaction to oxidize phenothiazine to sulfone, thereby obtaining a visible light excited organic long afterglow material.

[0009] As a preferred embodiment, the molar ratio of phenothiazine, potassium tert-butoxide, and methyl iodide is 1:1-1.5:1-1.5.

[0010] As a preferred embodiment, the usage ratio of the microcrystals, dichloromethane, glacial acetic acid and H2O2 is 10mmol:90mL:45mL:2-10mL.

[0011] As a preferred embodiment, the usage ratio of phenothiazine to tetrahydrofuran solution is 10 mmol:30 mL.

[0012] As a preferred embodiment, the oxidation reaction temperature is 45-60° C. and the time is 10-15 hours.

[0013] As a preferred embodiment, the organic phase is dried with anhydrous sodium sulfate, the solvent is removed by rotary evaporation, and then separation and purification are performed by column chromatography using petroleum ether to obtain the microcrystalline material.

[0014] As a preferred embodiment, after the oxidation reaction is completed, a crude product is obtained, the crude product is cooled to room temperature, and extracted three times with dichloromethane to obtain a secondary product.

[0015] As a preferred embodiment, the secondary product is separated and purified by column chromatography using dichloromethane and petroleum ether in a volume ratio of 2:1 to obtain a visible light excited organic long afterglow material.

[0016] The second object of the present invention is to provide a visible light excited organic long afterglow material prepared by the above preparation method.

[0017] The third object of the present invention is to provide an application of a visible light excited organic long afterglow material in multiple data encryption and decryption.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention provides a visible light excited organic long afterglow material and its preparation method and application. Phenothiazine and potassium tert-butoxide are added to a tetrahydrofuran solution, stirred at 0°C for 15 to 30 minutes, and then iodomethane is added and stirred for 12 hours. During the reaction, the hydrogen atoms in the phenothiazine molecules are removed and methyl groups are introduced into the phenothiazine molecular structure. The organic phase is cooled and extracted to obtain an organic phase. The solvent in the organic phase is removed and purified to obtain an intermediate product microcrystal. The microcrystal is added to a mixture of dichloromethane and glacial acetic acid, and then H2O2 is added to perform an oxidation reaction to oxidize the sulfur in the methyl phenothiazine to sulfone, thereby obtaining a visible light excited organic long afterglow material MOP that realizes fluorescence-room temperature phosphorescence multiple emission. Crystal analysis found that the MOP molecule interacts through three molecules, including Molecular accumulation is formed, thereby limiting the movement of molecules, inhibiting the non-radiative transition of triplet excitons, and promoting the intersystem crossing rate, thereby achieving effective room temperature phosphorescence. The present invention utilizes the significant characteristics of organic phosphorescence under visible light excitation and successfully realizes the application of multiple encryption and decryption. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The synthetic route of the visible light excited organic long afterglow material MOP of the present invention;

[0021] Figure 2 The organic long afterglow material MOP prepared by the present invention under room temperature and excited by visible light is heated in tetrahydrofuran (10 -5 M) UV-visible absorption spectrum (a) and steady-state photoluminescence spectrum (b) in solution;

[0022] Figure 3 It is a fluorescence lifetime decay curve of the organic long afterglow material MOP excited by visible light prepared by the present invention in tetrahydrofuran solution under room temperature;

[0023] Figure 4 Steady-state photoluminescence spectrum of compound MOP in dimethyltetrahydrofuran solution at 77K (Figure a); time-resolved decay curve at 349nm (Figure b); time-resolved decay curve at 384nm and 416nm (Figure c);

[0024] Figure 5 The steady-state photoluminescence spectrum (black line) and phosphorescence spectrum (blue filled part) of the organic long afterglow material MOP of the present invention in the crystalline state; wherein the inset is a luminescence photograph under a 365nm ultraviolet lamp (left) and a luminescence photograph after turning off the ultraviolet lamp (right);

[0025] Figure 6 Steady-state photoluminescence spectrum of compound MOP in the crystalline state (a); time-resolved decay curve at 389 nm (b); time-resolved decay curve at 445 nm and 522 nm (c);

[0026] Figure 7 Steady-state photoluminescence spectrum of compound MOP in the crystalline state at 77K (a); time-resolved decay curve at 380nm (b); time-resolved decay curve at 445nm and 472nm (c);

[0027] Figure 8 The photoluminescence spectrum (a) and the corresponding time-resolved fluorescence decay curve (b) of the film of compound MOP (doped in PMMA at a concentration of 5%) under 330nm excitation at room temperature;

[0028] Fig. 9 The unit cell and stacking structure of compound MOP (a) (b);

[0029] Fig.10 The crystal stacking diagram of compound MOP; the stacking diagram of bc plane (a); the stacking diagram of ac plane (b); the stacking diagram of ab plane (c);

[0030] Fig.11 This is the dimer stacking diagram of compound MOP. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.

[0032] The technical contents of the present invention are analyzed and explained in detail below.

[0033] The first object of the present invention is to provide a method for preparing a visible light excited organic long afterglow material, characterized in that it comprises the following steps:

[0034] Phenothiazine and potassium tert-butoxide are added to a tetrahydrofuran solution, stirred at 0°C for 15 to 30 minutes, and then iodomethane is added and stirred for 12 hours to introduce a methyl group into the molecular structure of phenothiazine. The solution is cooled and extracted to obtain an organic phase, and the solvent in the organic phase is removed and purified to obtain microcrystals. A mixed solution of dichloromethane and glacial acetic acid is added to the microcrystals, and then H2O2 is added to carry out an oxidation reaction to oxidize phenothiazine to sulfone to obtain a visible light excited organic long afterglow material.

[0035] In order to obtain microcrystals with higher purity, the molar ratio of phenothiazine, potassium tert-butoxide and methyl iodide is 1:1-1.5:1-1.5. The molar ratio of phenothiazine, potassium tert-butoxide and methyl iodide is limited to 1:1-1.5:1-1.5, which can ensure that the phenothiazine reacts fully. If the phenothiazine is excessive, there will be by-products and incompletely reacted raw materials in the product. The role of methyl iodide is to provide methyl groups, and excessive methyl iodide is toxic.

[0036] In order to obtain a high-purity visible light-excited organic long afterglow material, the dosage ratio of methyl phenothiazine, dichloromethane, glacial acetic acid and H2O2 is 10mmol:90mL:45mL:2-10mL. The dosage of H2O2 is slightly larger than that of methyl phenothiazine, so that the methyl phenothiazine is fully and completely oxidized. If the dosage of methyl phenothiazine is larger than that of H2O2, by-products and incompletely reacted raw materials will exist in the product.

[0037] In order to make the reaction fully complete, the temperature of the oxidation reaction is 45-60°C and the time is 10-15h. If the reaction temperature is lower than 45°C, the reaction progress will be slow and the reaction will be incomplete; if the reaction temperature is higher than 60°C, the excessively high reaction temperature will cause the rapid evaporation of dichloromethane and glacial acetic acid, thereby limiting the continuation of the reaction and inevitably affecting the yield of the product. If it is lower than 10h, although a part of the organic long afterglow material will be obtained, the reaction is not complete, and the product must be a mixture of raw materials and target products; when the reaction is continued for 15h, the maximum yield of the organic long afterglow material is obtained, so there is no need to react for a longer time.

[0038] In order to purify the organic phase efficiently, the organic phase is dried with anhydrous sodium sulfate, the solvent is removed by rotary evaporation, and then column chromatography with petroleum ether is used for separation and purification to obtain the microcrystalline substance.

[0039] In order to efficiently separate and purify the product after the oxidation reaction, after the oxidation reaction is completed, a crude product is obtained, the crude product is cooled to room temperature, and extracted three times with dichloromethane to obtain a secondary product; the secondary product is separated and purified by column chromatography using dichloromethane and petroleum ether in a volume ratio of 2:1 to obtain a visible light excited organic long afterglow material.

[0040] The effects are described below in conjunction with specific embodiments.

[0041] Example 1

[0042] A method for preparing a visible light excited organic long afterglow material comprises the following steps:

[0043] S1, add phenothiazine (2.00 g, 10 mmol) and potassium tert-butoxide (1.69 g, 15 mmol) to a tetrahydrofuran (30 mL) solution, stir at 0°C for 15 min, then add iodomethane (0.93 mL, 15 mmol) and stir for 12 h. After the reaction is completed, cool to room temperature, extract three times with dichloromethane, dry the collected organic phase with anhydrous sodium sulfate, remove the solvent by rotary evaporation, and finally purify the obtained product by column chromatography with petroleum ether as the eluent to obtain white microcrystals.

[0044] S2, add the white microcrystals to dichloromethane (90mL) and glacial acetic acid (45mL), slowly add H2O2 (2mL), stir at 60°C for 24h, cool to room temperature, extract three times with dichloromethane, and then separate and purify by column chromatography (dichloromethane: petroleum ether = 2:1) to obtain a white solid with a yield of 71%. After multiple recrystallizations, colorless crystals, namely compound MOP, are obtained. The synthetic route of compound MOP is as follows Figure 1 shown.

[0045] 1 HNMR (500MHz, CDCl3, δ [ppm]): 8.08 (d, J = 7.5Hz, 2H), 7.59 (t, J = 7.5Hz, 2H), 7.23-7.28 (m, 4H), 3.65 (s, 3H).

[0046] 13 CNMR(125MHz, CDCl3, δ[ppm]):142.07,133.22,124.41,123.41,121.89,115.66,35.79.MS[m / z]:CalcdforC 13 H 11 NO2S:245.05,Found268.0393[M+Na]+.Anal.CalcdforC 13 H 11 NO2S: C, 63.65; H, 4.52; N, 5.71. Found: C, 63.59; H, 4.55; N, 5.78.

[0047] The performance of the visible light excited organic long afterglow material prepared above was tested, and the specific process and results are as follows:

[0048] 1. Study on Photophysical Properties

[0049] The absorption spectra, steady-state photoluminescence spectra, excitation spectra and time-resolved emission spectra of the compounds prepared in the embodiments of the present invention in solution and crystal state were systematically studied. - 5 M) UV-visible absorption spectrum in solution Figure 2 As shown in Figure a. It can be seen from this figure that the absorption peaks of MOP are at 270nm, 300nm, and 333nm. In addition, the steady-state photoluminescence spectrum of compound MOP is shown in Figure 2 As shown in Figure b, under room temperature conditions, we also tested the fluorescence lifetime decay curve of MOP in solution. The luminescence lifetime of MOP at 355nm is 1.27ns, and the luminescence lifetime is in the nanosecond range, which is a typical monomer fluorescence emission.

[0050] In order to further understand the photophysical properties of compound MOP, we studied the steady-state photoluminescence spectrum and time-resolved decay curve of MOP under low temperature conditions, such as Figure 3 and Figure 4 As shown, the photophysical data of the compound MOP in the crystal state at room temperature were detected, as shown in Table 1. Under 77K conditions, due to the suppression of the non-radiative transition process of triplet excitons, the phosphorescence intensity is greatly enhanced in the steady-state photoluminescence spectrum in the solution, while the fluorescence intensity is very weak. For MOP, there are two main emission bands, one at about 348nm with a lifetime of 1.31ns in the nanosecond level; the other at 384 and 416nm with lifetimes of 382 and 383ms, respectively. It can be inferred that under 77K conditions, the molecules are fixed, and when the molecules are close to a certain extent, the orbits of adjacent molecules will overlap and redistribute, which may lead to the activation of high-energy triplet states, thereby stabilizing the excitons.

[0051] Table 1 Photophysical data of compound MOP in the crystalline state at room temperature

[0052]

[0053] λ F : fluorescence emission peak; τ F : fluorescence lifetime; λ P : phosphorescence emission peak; τ P : Phosphorescence lifetime; Φ P : Phosphorescence quantum efficiency; k isc : intersystem crossing rate from singlet to triplet; k r : Phosphorescence radiation rate; k nr : non-radiative transition rate; k isc =Φ Phos / τ Fluo ;k r Phos =Φ Phos / τ Phos ;k nr Phos =(1-Φ Phos ) / τ Phos

[0054] In the crystalline state, Figure 5 As shown in Figure 1, MOP exhibits blue luminescence under 365nm excitation, and a blue-green afterglow appears after the excitation light source is turned off. Figure 6 It can be seen that, unlike the emission spectrum at low temperature, the compound MOP crystal has only one emission peak at 389nm, and the corresponding lifetime is 2.03ns.

[0055] The present invention further tests the steady-state photoluminescence spectra and corresponding time-resolved decay curves of these compound crystals at 77K, such as Figure 7 As shown. At low temperatures, these compounds are fixed, reducing the free movement of molecules, greatly suppressing luminescence quenching and non-radiative transitions, so the phosphorescence intensity in these spectra is greatly enhanced, and they all show three obvious emission bands. The short-lived emission peak of compound MOP is at 380nm with a lifetime of 2.32ns, and the long-lived emission peak is at 445,472nm with a lifetime of 258,285ms.

[0056] In order to understand the effect of aggregation on organic afterglow luminescence, we conducted a set of control experiments by doping 5% of the compound MOP into polymethyl methacrylate (PMMA). Figure 8 As shown, at room temperature, the doped films of these compounds only have a broad blue light emission band at about 366nm, with a lifetime of nanoseconds, and no phosphorescence peak. These results prove that the organic long afterglow of compound MOP comes from aggregated molecules with strong intermolecular connections rather than single molecules.

[0057] 2. Crystal Analysis

[0058] The single crystal data and intermolecular forces of the compound MOP prepared by the present invention are shown in Tables 2 and 3.

[0059] Table 2 Single crystal data of compound MOP

[0060]

[0061]

[0062] a R1=Σ||F o |-|Fc || / Σ|F o |. b wR2=|Σw(|F o | 2 -|F c | 2 )| / Σ|w(F o 2 ) 2 | 1 / 2 .

[0063] Table 3 Intermolecular forces of compound MOP

[0064]

[0065] Since these compounds have similar electronic structures, their different luminescence behaviors may be attributed to different stacking modes, so we have conducted a detailed analysis of their single crystal structures. Table 2 provides the single crystal data of MOP, and Table 3 provides the interaction forces between the molecules of compound MOP. The unit cell and stacking structure of the compound are shown in Fig. 9 As shown. Each unit cell of MOP also has four molecules (Z=4). In the compound MOP, the four molecules are arranged in a parallelogram. From the overall stacking point of view, the MOP molecules are stacked more loosely. This is because for the MOP crystal, the introduction of methyl groups not only destroys the hydrogen bonds between molecules but also forms a certain steric effect, which disperses the molecules, so the overall stacking is looser.

[0066] Fig.10 The stacking diagrams of MOP in the bc plane, ac plane, and ab plane are shown. In MOP, due to the introduction of methyl groups, there are no hydrogen bonds between molecules, and there are only three interactions between molecules, including It can be seen that there are fewer types of intermolecular connections in MOP, but since these three intermolecular connections are relatively short, they are all smaller than Therefore, the molecules accumulate, and the triplet excitons are lost through non-radiative transitions or quenched by oxygen and moisture in the surrounding environment. As a result, the phosphorescence lifetime of MOP is shorter and the efficiency is lower.

[0067] In addition, we also studied the π-π interactions of their dimers. Fig.11 As shown, the intermolecular distance of MOP is Therefore, MOP has a certain phosphorescence lifetime. All these crystal data are consistent with the photophysical data we tested, proving that the tighter the crystal stacking, the more conducive to the generation of room temperature phosphorescence. In the system of the present invention, the molecules form a stacked three-dimensional network structure through intermolecular interactions, which not only limits the non-radiative loss of triplet excitons to inhibit luminescence quenching, but also promotes the intersystem crossing rate, which plays a vital role in achieving efficient and long-life room temperature phosphorescence.

[0068] In summary, the present invention adds phenothiazine and potassium tert-butoxide to a tetrahydrofuran solution, then adds iodomethane to stir and react, removes hydrogen atoms from the phenothiazine molecule during the reaction and introduces methyl groups into the phenothiazine molecular structure, cools and extracts to obtain an organic phase, removes the solvent from the organic phase, purifies to obtain an intermediate product microcrystal, adds a mixed solution of dichloromethane and glacial acetic acid to the microcrystal, then adds H2O2 to carry out an oxidation reaction, oxidizes sulfur in methyl phenothiazine to sulfone, and obtains a visible light excited organic long afterglow material MOP that realizes fluorescence-room temperature phosphorescence multiple emission. Crystal analysis found that the MOP molecule interacts with three molecules, including Molecular accumulation is formed, thereby limiting the movement of molecules, inhibiting the non-radiative transition of triplet excitons, and promoting the intersystem crossing rate, thereby achieving effective room temperature phosphorescence. The present invention utilizes the significant characteristics of organic phosphorescence under visible light excitation and successfully realizes the application of multiple encryption and decryption.

[0069] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a visible light excited organic long afterglow material, characterized in that: The following steps are involved: Phenothiazine and potassium tert-butoxide are added to a tetrahydrofuran solution to dissolve, and then iodomethane is added to remove hydrogen atoms in the phenothiazine molecule with potassium tert-butoxide, and at the same time, a methyl group is introduced into the phenothiazine molecular structure, and then the solution is cooled to obtain an organic phase, which is purified to obtain methyl phenothiazine. The methyl phenothiazine is added to a mixed solution of dichloromethane and glacial acetic acid, and then H2O2 is added to carry out an oxidation reaction to oxidize the sulfur atom of the methyl phenothiazine into sulfone, thereby obtaining a visible light excited organic long afterglow material.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the phenothiazine, potassium tert-butoxide and methyl iodide is 1:1-1.5:1-1.

5.

3. The preparation method according to claim 1, characterized in that: The dosage ratio of the methyl phenothiazine, dichloromethane, glacial acetic acid and H2O2 is 10mmol:90mL:45mL:2-10mL.

4. The preparation method according to claim 1, characterized in that: The usage ratio of the phenothiazine to the tetrahydrofuran solution is 10 mmol:30 mL.

5. The preparation method according to claim 1, characterized in that: The temperature of the oxidation reaction is 45-60° C. and the time is 10-15 hours.

6. The preparation method according to claim 1, characterized in that: The organic phase is dried with anhydrous sodium sulfate, the solvent is removed by rotary evaporation, and then separation and purification are performed by column chromatography using petroleum ether to obtain the microcrystals.

7. The preparation method according to claim 1, characterized in that: After the oxidation reaction is completed, a crude product is obtained. The crude product is cooled to room temperature and extracted with dichloromethane to obtain a secondary product.

8. The preparation method according to claim 7, characterized in that: The secondary product is separated and purified by column chromatography using dichloromethane and petroleum ether to obtain a visible light excited organic long afterglow material.

9. A visible light excited organic long afterglow material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the visible light excited organic long afterglow material according to claim 9 in multiple data encryption and decryption.

Citation Information

Patent Citations

  • Room temperature phosphorescence molecule based on phenothiazine derivative, preparation method and application thereof

    CN109206384A

  • Phenothiazine derivative as well as preparation method and application thereof

    CN115611826A

  • Force-response pure organic multiple luminescent material based on 5, 5-phenothiazine dioxide and preparation method of force-response pure organic multiple luminescent material

    CN116239546A