Colored paint, carbon-ceramic brake disc with colored coating and preparation method of carbon-ceramic brake disc

By applying high-temperature colorants and coating technology on carbon ceramic brake discs, the problem of difficult to determine wear conditions is solved, the combination of safety and ornamentality is achieved, and an intuitive wear determination method is provided.

CN118879152APending Publication Date: 2024-11-01福建康碳防务材料科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411191629.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The wear of existing carbon ceramic brake discs during use is difficult to determine, and there is a lack of intuitive judgment methods, which affects safety.

Method used

Using high-temperature resistant colorants, including components A and components B, colored coatings are prepared through chemical vapor deposition and thermal curing technology. The coating is heat-cured and silicon-permeable on the surface of the carbon ceramic brake disc to form a coating with color changes. The life of the brake disc can be determined as the wear is worn.

Benefits of technology

Through color changes, the wear of the carbon ceramic brake disc is intuitively judged, which improves safety and beautifies the appearance of the brake disc to meet the ornamental needs of some customers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879152A_ABST
    Figure CN118879152A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of carbon-ceramic brake discs, and particularly relates to colored paint, a carbon-ceramic brake disc with a colored coating and a preparation method of the carbon-ceramic brake disc. The high-temperature-resistant pigment provided by the invention comprises a component A and a component B which are independently subpackaged, the component A comprises the following components in percentage by mass: 60-70% of silicon carbide powder, 10-15% of resin powder and 20-30% of pigment; the component B comprises silicon carbide powder and resin powder, and in the component B, the mass ratio of the silicon carbide powder to the resin powder is 9: 1. The high-temperature-resistant pigment provided by the invention has the characteristic of high temperature resistance, and when the high-temperature-resistant pigment provided by the invention is added into the carbon-ceramic brake disc to serve as a coating of the carbon-ceramic brake disc, not only can the appearance of the carbon-ceramic brake disc be beautified, but also the wear condition of the carbon-ceramic brake disc can be confirmed by checking the color change of the disc surface of the carbon-ceramic brake disc; and after the colored coating is completely worn (the color disappears), the service life of the brake disc can be judged to be over, which is more visual and safer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon-ceramic brake discs, and specifically relates to a colored coating, a carbon-ceramic brake disc with a colored coating, and a preparation method thereof. Background Art

[0002] As people pay more and more attention to the safety of automobile driving, the importance of automobile brake discs is highlighted. Traditional brake discs are cast iron discs, but cast iron discs have the disadvantages of being not wear-resistant, high in density, heavy in weight, and easy to soften and heat up. Compared with cast iron discs, carbon ceramic brake discs not only have low loss and long service life, but also have strong mechanical properties and more stable braking performance.

[0003] However, whether it is a cast iron brake disc or a carbon ceramic brake disc, the friction surface will wear out and become scrapped after a period of use. It is currently difficult to define the wear and tear of the brake disc. The only way to judge the braking effect is through the driving of the car, which lacks safety. Summary of the invention

[0004] The purpose of the present invention is to provide a colored coating, a carbon-ceramic brake disc with a colored coating and a preparation method thereof. The colored coating provided by the present invention can beautify the appearance of the carbon-ceramic brake disc, and the wear condition can be confirmed by checking the color of the carbon-ceramic brake disc surface. The carbon-ceramic brake disc with a colored coating provided by the present invention solves the problem that the wear condition of the disc surface is difficult to confirm.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a high temperature resistant colorant, comprising independently packaged component A and component B; the component A comprises the following components in percentage by mass: 60-70% silicon carbide powder, 10-15% resin powder and 20-30% colorant;

[0007] The B component includes silicon carbide powder and resin powder. In the B component, the mass ratio of silicon carbide powder to resin powder is 9:1.

[0008] Preferably, the mass ratio of component A to component B is 1:3.

[0009] Preferably, the colorant includes cobalt blue or vanadium zirconium yellow.

[0010] The present invention provides a method for preparing a carbon-ceramic brake disc with a colored coating, comprising the following steps:

[0011] The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns;

[0012] The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric, and needle-punched after laying to obtain a carbon fiber preform;

[0013] Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on the carbon fiber preform to obtain a dense C / C preform;

[0014] Processing the dense C / C preform into a C / C brake disc;

[0015] The surface of the C / C brake disc is coated with the high temperature resistant colorant described in the above technical solution and then heated for thermal curing to obtain a semi-finished product, wherein the coating comprises the following steps: the surface of the C / C brake disc is coated with component B in the high temperature resistant colorant described in the above technical solution and then compacted, and then component A is coated and then compacted;

[0016] The semi-finished product is subjected to siliconizing treatment to obtain the carbon ceramic brake disc with the colored coating.

[0017] Preferably, the coating thickness of the B component is 1 to 2 mm.

[0018] Preferably, the compaction pressure after the B component is coated and the compaction pressure after the A component is coated are independently 1 to 2 MPa.

[0019] Preferably, the thermal curing temperature is 160-180° C., the pressure is 15-30 MPa, and the heat and pressure holding time is 2000-2600 s.

[0020] Preferably, the density of the dense C / C preform is 1.4 g / m 3 ; The auxiliary gas of the chemical vapor deposition is ethane, the reducing gas is hydrogen, the volume ratio of the natural gas and hydrogen is 2:1, the temperature of the chemical vapor deposition is 1100-1200°C, the flow rate of the natural gas is 200SLM, the flow rate of ethane is 30SLM, and the deposition time is ≥160h.

[0021] Preferably, the siliconizing treatment is a molten siliconizing treatment, the temperature of the molten siliconizing treatment is 1400-1550° C., the holding time is 1-3 hours, and the molten siliconizing treatment is carried out in a protective gas atmosphere.

[0022] The present invention provides a carbon-ceramic brake disc with a colored coating prepared by the preparation method described in the above technical solution.

[0023] The present invention provides a high temperature resistant colorant, comprising independently packaged component A and component B; the component A comprises the following components in percentage by mass: 60-70% silicon carbide powder, 10-15% resin powder and 20-30% colorant; the component B comprises silicon carbide powder and resin powder, and in the component B: the mass ratio of silicon carbide powder to resin powder is 9:1. The high temperature resistant colorant provided by the present invention has the characteristic of high temperature resistance. The high temperature resistant colorant provided by the present invention is added to a carbon-ceramic brake disc as a coating of the carbon-ceramic brake disc, which can not only beautify the appearance of the carbon-ceramic brake disc, but also confirm the wear of the carbon-ceramic brake disc by checking the color change of the disc surface of the carbon-ceramic brake disc, which is more intuitive and safe.

[0024] The invention provides a method for preparing a carbon ceramic brake disc with a colored coating, comprising the following steps: preparing a mesh tire using short chopped carbon fiber yarns, and preparing a non-woven fabric using long carbon fiber yarns; laying the mesh tire and the non-woven fabric in a cyclic laying mode of a layer of mesh tire and a layer of non-woven fabric, and performing acupuncture after laying to obtain a carbon fiber preform; using natural gas as a carbon source gas, and adopting a chemical vapor deposition method to perform carbon densification on the carbon fiber preform to obtain a dense C / C preform; processing the dense C / C preform into a C / C brake disc; coating the surface of the C / C brake disc with the high temperature resistant colorant described in the above technical solution, and then heating and heat curing to obtain a semi-finished product, wherein the coating comprises the following steps: coating the surface of the C / C brake disc with the component B in the high temperature resistant colorant described in the above technical solution, and then compacting, and then coating the component A, and then compacting; performing siliconization treatment on the semi-finished product to obtain the carbon ceramic brake disc with the colored coating. In the preparation of the carbon ceramic brake disc of the present invention, before the siliconizing treatment, the high temperature resistant colorant described in the above technical solution is coated on the surface of the C / C brake disc, and cured by hot pressing. The obtained carbon ceramic brake disc has a colored coating. During the braking process of the automobile, the coating is worn away. When the colored coating is completely worn away (the color disappears), it can be determined that the service life of the brake disc has ended. At the same time, the coating surface of the carbon ceramic brake disc prepared by the present invention has color and is ornamental, which can meet the needs of some customers. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a physical photo of the carbon ceramic brake disc prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0026] The present invention provides a high temperature resistant colorant, comprising independently packaged component A and component B; the component A comprises the following components in percentage by mass: 60-70% silicon carbide powder, 10-15% resin powder and 20-30% colorant;

[0027] The B component includes silicon carbide powder and resin powder. In the B component, the mass ratio of silicon carbide powder to resin powder is 9:1.

[0028] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0029] The high temperature resistant colorant provided by the present invention comprises an independently packaged A component. The A component comprises the following components in percentage by mass: 60-70% silicon carbide powder, 10-15% resin powder and 20-30% colorant. In terms of percentage by mass, the A component provided by the present invention comprises 60-70% silicon carbide powder, preferably 60%, 65% or 70%. In terms of percentage by mass, the A component provided by the present invention comprises 10-15% resin powder, preferably 10%, 12% or 15%. The resin powder is preferably phenolic resin powder. In a specific embodiment of the present invention, the phenolic resin powder is purchased from Shandong Shengquan New Materials Co., Ltd., and the product model is PF6291A. In terms of percentage by mass, the A component provided by the present invention comprises 20-30% colorant, preferably 20%, 25% or 30%. The colorant preferably comprises cobalt blue or vanadium zirconium yellow.

[0030] The high temperature resistant colorant provided by the present invention comprises a separately packaged B component. The B component comprises silicon carbide powder and resin powder, wherein the mass ratio of silicon carbide powder to resin powder in the B component is 9:1. In the present invention, the resin powder in the B component is preferably phenolic resin powder. In a specific embodiment of the present invention, the phenolic resin powder is purchased from Shandong Shengquan New Materials Co., Ltd., and the product model is PF6291A.

[0031] In the present invention, the mass ratio of the component A to the component B is preferably 1:3.

[0032] The high temperature resistant colorant provided by the present invention is applied to the preparation of the coating of the carbon-ceramic brake disc. By adding the high temperature resistant colorant described in the above technical solution into the coating of the carbon-ceramic brake disc, the appearance of the brake disc can be beautified, and the wear condition can be confirmed by checking the color of the disc surface. After the colored coating is completely worn out (the color disappears), it can be determined that the service life of the brake disc has ended.

[0033] The present invention provides a method for preparing the high temperature resistant colorant described in the above technical solution, and the preparation method of the A component preferably includes the following steps: silicon carbide powder, resin powder and colorant are first mixed to obtain the A component. The first mixing is preferably carried out in a mixing device, the time of the first mixing is preferably 90 to 120 minutes, the first mixing is preferably carried out under stirring conditions, and the stirring speed during the first mixing is preferably ≥1500RPM. The preparation method of the B component preferably includes the following steps: silicon carbide powder and resin powder are second mixed to obtain the B component. The second mixing is preferably carried out in a mixing device, the time of the second mixing is preferably 90 to 120 minutes, the second mixing is preferably carried out under stirring conditions, and the stirring speed during the second mixing is preferably ≥1500RPM.

[0034] The present invention provides a method for preparing a carbon-ceramic brake disc with a colored coating, comprising the following steps:

[0035] The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns;

[0036] The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric, and needle-punched after laying to obtain a carbon fiber preform;

[0037] Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on the carbon fiber preform to obtain a dense C / C preform;

[0038] Processing the dense C / C preform into a C / C brake disc;

[0039] The surface of the C / C brake disc is coated with the high temperature resistant colorant described in the above technical solution and then heated for thermal curing to obtain a semi-finished product, wherein the coating comprises the following steps: the surface of the C / C brake disc is coated with component B in the high temperature resistant colorant described in the above technical solution and then compacted, and then component A is coated and then compacted;

[0040] The semi-finished product is subjected to siliconizing treatment to obtain the carbon ceramic brake disc with the colored coating.

[0041] The present invention uses short-cut carbon fiber filaments to prepare the mesh tire, and uses long carbon fiber filaments to prepare the non-woven fabric; in the present invention, the short-cut carbon fiber filaments are preferably short-cut T400-24K carbon fiber filaments. The present invention has no special requirements for the specific preparation method of the mesh tire. The surface density of the mesh tire is preferably 140g / cm 2 The long carbon fiber yarn is preferably T400-24K carbon fiber yarn. The present invention has no special requirements on the specific preparation method of the non-woven fabric. The area of ​​the non-woven fabric is preferably 380g / cm 2 .

[0042] After obtaining the mesh tire and the non-woven fabric, the present invention lays the mesh tire and the non-woven fabric in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric, and then performs acupuncture after laying to obtain a carbon fiber preform. In the present invention, during the laying, the non-woven fabric is preferably used alternately in three directions of 0°, 60° and 90°. The laying is preferably laid to a thickness of 40 mm and then acupuncture is performed. The density of the acupuncture is preferably 20 to 26 needles / cm 2 The depth of the needle punching is preferably 8 to 10 mm. After the needle punching, a carbon fiber preform is obtained.

[0043] After obtaining the carbon fiber preform, the present invention uses natural gas as a carbon source gas and adopts a chemical vapor deposition (CVD) method to perform carbon densification on the carbon fiber preform to obtain a dense C / C preform.

[0044] In the present invention, the deposition temperature of the chemical vapor deposition is 1100-1200°C, the natural gas flow rate is preferably 200SLM, the auxiliary gas is preferably ethane, the auxiliary gas flow rate is preferably 30SLM, the reducing gas is preferably hydrogen, the volume ratio of natural gas to hydrogen is preferably 2:1, and the deposition time is preferably 160h. In the present invention, the density of the obtained dense C / C preform is preferably ≥1.4g / cm 3 .

[0045] After obtaining the dense C / C preform, the present invention processes the dense C / C preform into a C / C brake disc. The present invention has no special requirements for the specific implementation of the processing. The shape of the C / C brake disc is preferably annular. In a specific embodiment of the present invention, the outer diameter of the annular C / C brake disc is preferably 370 mm, and the inner diameter is preferably 170 mm.

[0046] After obtaining the C / C brake disc, the present invention applies the high temperature resistant colorant described in the above technical solution on the surface of the C / C brake disc, and then heats and heats to obtain a semi-finished product. The coating includes the following steps: applying the B component in the high temperature resistant colorant described in the above technical solution on the surface of the C / C brake disc, and then compacting it, and then applying the A component and compacting it. The present invention preferably applies the high temperature resistant colorant described in the above technical solution on one surface of the C / C brake disc, and then heats and heats it; then applies the high temperature resistant colorant described in the above technical solution on the other surface of the C / C brake disc, and then heats and heats it to obtain a semi-finished product. The present invention has the same operating parameters for coating the high temperature resistant colorant and heat curing treatment on the two surfaces of the C / C brake disc. When the high temperature resistant colorant described in the above technical solution is applied to any surface of the C / C brake disc, the coating thickness of the B component is preferably 1 to 2 mm. The mass ratio of the A component to the B component is preferably 1:3. The compaction after the B component is applied and the compaction after the A component is applied are preferably performed using appropriate tooling, respectively. The compaction pressure after coating component B is preferably 1-2MPa. The compaction pressure after coating component A is preferably 1-2MPa. In the present invention, after coating component B, compacting component B, coating component A and compacting component A on any surface of the C / C brake disc in sequence, the compacted sample is subjected to the thermal curing. The thermal curing temperature is preferably 160-180°C, the pressure is preferably 15-30MPa, and the heat preservation and pressure holding time is preferably 2000-2600s. The thermal curing is preferably carried out in a hot pressing setting. In the present invention, after coating component B, compacting component B, coating component A, compacting component A and thermal curing on any surface of the C / C brake disc in sequence, the present invention preferably performs surface grinding on the thermally cured product, and the surface grinding is preferably carried out in a machining workshop. In the present invention, the surface after thermal curing is preferably ground flat by the grinding.

[0047] After obtaining the semi-finished product, the present invention preferably performs a molding process on the semi-finished product before performing the siliconizing treatment. The molding process preferably includes: opening ventilation grooves in the semi-finished product. The molding process is preferably performed in a machining center.

[0048] After the forming process, the present invention performs siliconizing treatment on the semi-finished product after the forming process to obtain the carbon ceramic brake disc with the colored coating. In the present invention, the raw material used for the siliconizing treatment is preferably silicon powder, and the siliconizing treatment is preferably carried out in a siliconizing furnace. The present invention preferably places the silicon powder in a crucible with BN coated on the surface, and then places the semi-finished product on the silicon powder, and then places it in a siliconizing furnace for siliconizing treatment. In the present invention, the siliconizing treatment is preferably a molten siliconizing treatment, and the temperature of the molten siliconizing treatment is preferably 1400-1550°C, the holding time is preferably 1-3h, and the heating time from room temperature to the temperature of the siliconizing treatment is preferably 25-30h. The molten siliconizing treatment is carried out in a protective gas atmosphere. The present invention preferably fills the siliconizing furnace with a protective gas when the temperature of the siliconizing furnace is raised from room temperature to 800°C. The protective gas is preferably nitrogen, and the pressure of the protective gas is preferably 70-85kPa.

[0049] In the present invention, after the siliconizing treatment, the present invention preferably performs surface grinding on the siliconized brake disc to obtain the carbon ceramic brake disc with the colored coating. In the present invention, the surface grinding is preferably performed in a machining workshop. The present invention preferably performs surface grinding on the siliconized brake disc to remove excess silicon material on the surface, and grinds until ceramic cracks appear.

[0050] The present invention provides a carbon-ceramic brake disc with a colored coating prepared by the preparation method described in the above technical solution.

[0051] The coating of the carbon ceramic brake disc with colored coating provided by the present invention has a special color. During the braking process of the automobile, the coating is worn away. When the colored coating is completely worn away (the color disappears), it can be determined that the service life of the brake disc has ended.

[0052] The coating surface of the colored-coated carbon-ceramic brake disc provided by the present invention has a special color and is ornamental, thereby meeting the needs of some customers.

[0053] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0054] Example 1

[0055] This embodiment provides a high temperature resistant colorant, including independently packaged component A and component B; wherein component A includes the following components in percentage by mass: 60% silicon carbide powder, 10% phenolic resin powder and 30% cobalt blue; wherein the percentage by mass of each raw material in component A is shown in Table 1. Component B includes silicon carbide powder and phenolic resin powder, and in component B: the mass ratio of silicon carbide powder to phenolic resin powder is 9:1.

[0056] The preparation method of the high temperature resistant colorant provided in this embodiment comprises the following steps:

[0057] The preparation method of component A is as follows: silicon carbide powder, phenolic resin powder and cobalt blue are poured into a mixing device with a rotation speed of 1500RPM according to mass percentage and mixed evenly for 120 minutes, and then taken out after mixing to obtain component A;

[0058] The preparation method of component B is as follows: silicon carbide powder and phenolic resin powder are poured into a mixing device with a rotation speed of 1500 RPM at a mass ratio of 9:1 and mixed evenly for 120 minutes to obtain component B.

[0059] This embodiment provides a method for preparing a carbon ceramic brake disc with a colored coating, comprising the following steps:

[0060] (1) Preparation of C / C brake disc: A non-woven fabric was prepared using 1400 cm long T400-24K carbon fiber yarn, and a mesh was prepared using 7 cm long chopped T400-24K carbon fiber yarn. A cyclic laying method of one layer of mesh and one layer of non-woven fabric was adopted, wherein the non-woven fabric was alternately used in three directions of 0°, 60° and 90°, and the thickness was laid to 40 mm. Finally, acupuncture was performed, and the acupuncture density was 26 needles / cm 2 The needle-punching depth is 10 mm, forming a carbon fiber preform with a needle-punched structure. The carbon fiber preform is then treated with CVD (chemical vapor deposition), with a deposition temperature of 1200°C, a natural gas flow rate of 200 SLM, ethane as the auxiliary gas, a flow rate of 30 SLM as the auxiliary gas, hydrogen as the reducing gas, a volume ratio of natural gas to hydrogen of 2:1, and a deposition time of 160 h, so that the preform density reaches 1.4 g / cm 3 The preform with the density reaching the standard after deposition is then processed into a ring-shaped C / C brake disc with an outer diameter of 370 mm and an inner diameter of 170 mm.

[0061] (2) Hot pressing: Take a C / C brake disc with an outer diameter / inner diameter of 370×170mm to be pressed and place it in a mold. Weigh 300g of component B and spread it evenly on the surface of the brake disc. Use appropriate tooling to compact it. The coating thickness of component B is 1.3mm and the compaction pressure is 2MPa. Then weigh 100g of component A and spread it evenly on the mixture B. Use appropriate tooling to compact component A at a compaction pressure of 2MPa. Then press the pressure head on component A and transfer it to the hot pressing hot preparation for pressing; control the pressure to 30MPa, the temperature to 180℃, and the pressing and curing time to 2600s.

[0062] (4) Machining and grinding: The product pressed in step (2) is sent to a machining workshop for surface grinding to make the surface smooth.

[0063] (5) Hot pressing: Turn the disc that has been ground flat in step (4) over for coating pressing. Place the disc that has been ground flat in step (4) in a mold. Weigh 300g of component B and spread it evenly on the surface of the brake disc. Use appropriate tooling to compact it. The coating thickness of component B is 1.3mm and the compaction pressure is 2MPa. Then weigh 100g of component A and spread it evenly on mixed material B. Use appropriate tooling to compact component A at a compaction pressure of 2MPa. Then press the pressure head on component A and transfer it to hot pressing and hot preparation for pressing. Control the pressure to 30MPa, the temperature to 180°C, and the pressing and curing time to 2600s.

[0064] (6) Machining and grinding: The product pressed in step (5) is sent to a machining workshop for surface grinding to make the surface smooth.

[0065] (7) Forming processing: The disc body after (6) grinding is transferred to the machining center for a series of forming processing such as opening ventilation grooves.

[0066] (8) Siliconizing: Place silicon powder in a crucible coated with BN, place the C / C brake disc to be siliconized obtained in step (7) on the silicon powder, and then transfer the crucible to a siliconizing furnace for melt siliconizing treatment, wherein the maximum temperature of the melt siliconizing treatment is 1550°C, the heating time from room temperature to the maximum temperature of the melt siliconizing treatment is 30 hours, and the maximum temperature holding time is 3 hours. During the heating process, when the room temperature reaches 800°C, nitrogen is filled into the siliconizing furnace, and the nitrogen pressure is 85 kPa.

[0067] (9) Finishing: The brake disc after siliconizing in step (8) is transferred to a machining workshop for surface grinding to remove excess silicon material on the surface, and is ground until ceramic cracks appear.

[0068] Example 2

[0069] The high temperature resistant pigment provided in this embodiment is basically the same as the high temperature resistant pigment provided in Example 1, and the only difference is that the mass percentage of each raw material in component A of the high temperature resistant pigment provided in this embodiment is as shown in Table 1.

[0070] The preparation method of the high temperature resistant colorant provided in this embodiment is the same as that in embodiment 1.

[0071] The method for preparing the colored coated carbon ceramic brake disc provided in this embodiment is basically the same as that in Embodiment 1, except that the high temperature resistant colorant in this embodiment is used for preparation.

[0072] The actual picture of the carbon ceramic brake disc with colored coating prepared in Example 2 is as follows Figure 1 shown.

[0073] Example 3

[0074] The high temperature resistant pigment provided in this embodiment is basically the same as the high temperature resistant pigment provided in Example 1, and the only difference is that the mass percentage of each raw material in component A of the high temperature resistant pigment provided in this embodiment is as shown in Table 1.

[0075] The preparation method of the high temperature resistant colorant provided in this embodiment is the same as that in embodiment 1.

[0076] The method for preparing the colored coated carbon ceramic brake disc provided in this embodiment is basically the same as that in Embodiment 1, except that the high temperature resistant colorant in this embodiment is used for preparation.

[0077] Table 1 Composition of component A in the high temperature resistant colorant provided in Examples 1 to 3

[0078]

[0079] Conclusion: Too much pigment is used in the coating of Example 1, resulting in a reduction in the silicon carbide content of the coating and insufficient bonding strength of the coating, because the pigment and silicon cannot react to form a silicon carbide ceramic surface.

[0080] From the above examples, it can be seen that the carbon ceramic brake disc with colored coating provided by the present invention has the following advantages compared with cast iron brake discs or carbon ceramic brake discs with ordinary coatings: the coating of the carbon ceramic brake disc with colored coating provided by the present invention has a special color, and during the braking process of the vehicle, the coating wears away. When the colored coating is completely worn away (the color disappears), it can be determined that the service life of the brake disc has ended. The coating surface of the carbon ceramic brake disc with colored coating provided by the present invention has a special color and is ornamental, which can meet the needs of some customers.

[0081] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A high temperature resistant colorant, characterized in that: It comprises independently packaged component A and component B; the component A comprises the following components in percentage by mass: 60-70% silicon carbide powder, 10-15% resin powder and 20-30% colorant; The B component includes silicon carbide powder and resin powder. In the B component, the mass ratio of silicon carbide powder to resin powder is 9:

1.

2. The high temperature resistant colorant according to claim 1, characterized in that: The mass ratio of the A component to the B component is 1:

3.

3. The high temperature resistant colorant according to claim 1 or 2, characterized in that: The colorant includes cobalt blue or vanadium zirconium yellow.

4. A method for preparing a carbon ceramic brake disc with a colored coating, characterized in that: The following steps are involved: The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns; The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric, and needle-punched after laying to obtain a carbon fiber preform; Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on the carbon fiber preform to obtain a dense C / C preform; Processing the dense C / C preform into a C / C brake disc; The surface of the C / C brake disc is coated with the high temperature resistant colorant according to any one of claims 1 to 3, and then heated and heat cured to obtain a semi-finished product, wherein the coating comprises the following steps: the surface of the C / C brake disc is coated with component B in the high temperature resistant colorant according to any one of claims 1 to 3, and then compacted, and then component A is coated and compacted; The semi-finished product is subjected to siliconizing treatment to obtain the carbon ceramic brake disc with the colored coating.

5. The preparation method according to claim 4, characterized in that: The coating thickness of the B component is 1 to 2 mm.

6. The preparation method according to claim 4 or 5, characterized in that: The compaction pressure after the B component is applied and the compaction pressure after the A component is applied are independently 1 to 2 MPa.

7. The preparation method according to claim 4, characterized in that: The thermal curing temperature is 160-180° C., the pressure is 15-30 MPa, and the heat preservation and pressure holding time is 2000-2600 seconds.

8. The preparation method according to claim 4, characterized in that: The density of the dense C / C preform is ≥1.4 g / m 3 ; The auxiliary gas of the chemical vapor deposition is ethane, the reducing gas is hydrogen, the volume ratio of the natural gas and hydrogen is 2:1, the temperature of the chemical vapor deposition is 1100-1200°C, the flow rate of the natural gas is 200SLM, the flow rate of ethane is 30SLM, and the deposition time is ≥160h.

9. The preparation method according to claim 4, characterized in that: The siliconizing treatment is a molten siliconizing treatment, the temperature of the molten siliconizing treatment is 1400-1550° C., the heat preservation time is 1-3 hours, and the molten siliconizing treatment is carried out in a protective gas atmosphere.

10. A carbon-ceramic brake disc with a colored coating prepared by the preparation method according to any one of claims 4 to 9.

Citation Information

Cited By

  • Silicon carbide composite powder, preparation method thereof, surface modified coating and application

    CN122255767A