Metasurface unit with depth continuously and gradually changed and method

By designing multiple concentric rings in the metasurface structure and adopting specific preparation methods, the problems of complex preparation process and insufficient regulation capabilities of the metasurface structure in the prior art are solved, and the metasurface unit with continuous gradient is realized, which improves the optical Performance and design selectivity.

CN118884579APending Publication Date: 2024-11-01SHANGHAI NORTH OCEAN TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411315827.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing metasurface structure preparation process is complex, with limited dispersion problems and dynamic regulation capabilities, and it is difficult to realize the continuous gradient of multi-structure depth, which limits its application in the fields of optical and optoelectronics.

Method used

By providing a deep continuous gradient metasurface unit, including structures of multiple concentric rings, and using specific preparation methods, including depositing photoresist, etching and planarization, the formation of electrically neutral ionic gases using fluorine-based gases, is carried out by providing a structure of a deep continuous gradient metasurface unit, including structures of multiple concentric rings, and using specific preparation methods, including deposition of photoresist, etching and planarization, the formation of electrically neutral ionic gases using fluorine-based gases. The clusters are etched, and the etching depth and spacing are adjusted to form a functional area with continuous gradient in depth, overcome the overetching phenomenon and improve the etching accuracy.

Benefits of technology

Multi-parameter modulation is realized, which increases the design selectivity and optical performance of the metasurface structure, meets more application scenarios, improves the accuracy and efficiency of the preparation process, and reduces overetching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118884579A_ABST
    Figure CN118884579A_ABST
Patent Text Reader

Abstract

The invention provides a super-surface unit and method with continuously and gradually changed depth, the super-surface unit is provided with a super-surface subunit with continuously and gradually changed depth composed of a plurality of concentric rings, the structures of the super-surface subunits can be the same or different, the diameters of the concentric rings are different, and the line widths and the intervals can be completely the same or partially different. Different parameters of the metasurface subunits are modulated, and more choices are provided for the design of the metasurface structure in the field; by correcting and compensating the etching depths in different functional areas, the etching depths are preferentially adjusted and compensated, so that the functional areas with the depths continuously and gradually changed are formed to perform subsequent etching operation, the etching depths of different positions are adjusted, the over-etching condition in the second material layer is reduced as much as possible, and the etching efficiency is improved. According to the method, the super-surface unit formed by etching is subjected to over-etching at the bottom as less as possible, so that the process steps of the super-surface with the continuously and gradually changed depth are improved, the etching precision is improved, and the optical performance of an optical product is more excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a deep continuous gradient super surface unit and method. Background Art

[0002] Since metasurface structures can achieve precise control of the amplitude, phase, polarization and frequency of light waves in a two-dimensional plane, the design and application of this material is developing rapidly in many fields, such as imaging and reality technology, optical sensing, communication technology, etc. Since it can achieve high-resolution imaging and holographic display, metasurface structures can provide thinner and more efficient near-eye display technology in augmented reality and virtual reality devices; or can be used as an achromatic super lens to achieve high-quality imaging, and have application value in many cutting-edge technology fields.

[0003] With the advancement of materials science and nano-manufacturing technology, metasurfaces are expected to play a more important role in the future fields of optics and optoelectronics. Based on the rapid development of metasurface technology and its broad application prospects, it has become the focus of industry research; however, it still faces some huge challenges, including the complexity of the manufacturing process, dispersion problems, and the limitation of dynamic control capabilities, which makes the preparation process of metasurfaces more difficult. Therefore, it is important for technicians in this field to prepare multi-structured and continuously gradient metasurface unit structures to meet different technical requirements and realize multi-parameter modulation of metasurface units. Summary of the invention

[0004] The present invention intends to provide a deep continuous gradient metasurface unit and method, provide a multi-structure, deep continuous gradient metasurface unit and its related preparation process method, so as to realize multi-parameter modulation of the metasurface unit, improve the existing metasurface preparation process, provide more structural and process options to technical personnel in this field, and increase the scope of application of the metasurface structure.

[0005] The present invention provides a deep continuous gradient super surface unit, which comprises at least a first material layer, wherein any surface of the first material layer comprises at least one functional area, wherein the functional area comprises a plurality of deep continuous gradient super surface sub units, and each of the super surface sub units comprises a plurality of concentric rings.

[0006] Furthermore, it also includes a second material layer, which is formed on a surface of the first material layer away from the functional area.

[0007] Further, any surface of the first material layer includes at least two functional areas.

[0008] Furthermore, in some embodiments, each of the metasurface sub-units includes a plurality of concentric rings, and each of the concentric rings has a different diameter.

[0009] Further, in some other embodiments, the line width of each of the circular rings is the same; or the line widths of at least two of the circular rings are different; the spacing between the circular rings is the same; or the spacing between at least two of the circular rings is different, and the spacing is the distance between adjacent circular rings.

[0010] Furthermore, the structural dimensions of the metasurface subunits range from 0.5 mm to 6 mm; the diameter of any of the concentric rings ranges from 50 nm to 6 mm; the line width W of any of the concentric rings ranges from 20 to 200 nm; and the spacing between adjacent concentric rings ranges from 50 nm to 150 nm.

[0011] At the same time, the present invention provides a method for preparing the depth-continuous gradient supersurface unit described in any of the above embodiments, comprising the following steps:

[0012] (1) providing at least the first material layer and the second material layer, wherein the first material layer is formed on either side of the second material layer;

[0013] (2) forming at least one functional region on a surface of the first material layer away from the second material layer, wherein the depth of the functional region changes continuously and gradually;

[0014] (3) depositing photoresist in the functional area and planarizing the surface thereof;

[0015] (4) patterning the photoresist to form a patterned area;

[0016] (5) Etching the first material layer, exposing and developing it, and obtaining a deep continuous gradient metasurface unit.

[0017] The step (2) also includes first calculating the etching depth of the first material layer at different locations in at least one functional area, and performing depth gradient etching on the first material layer.

[0018] Furthermore, in the functional area, the etching depth of the first material layer at a certain location can be determined by the following formula (1):

[0019] H1=H-[T-(H1 / V1)]*[V1 / K] (1)

[0020] In formula (1), H1 represents the etching depth of the first material layer at a certain point; H represents the target depth; T represents the total etching time, including the etching time of the first material layer and the etching time of the second material layer; V1 represents the etching speed of the first material layer; K represents the etching selectivity of the second material layer to the first material layer.

[0021] Furthermore, in some embodiments, in step (2), at least one functional region is formed on the surface of the first material layer away from the second material layer, and the functional region is etched. Fluorine-based gas is used as etching gas to form electrically neutral ion gas clusters to etch the target region; the target gradient depth is reached and the depth continuity is ensured.

[0022] The depth variation range of the depth-continuous-gradient-supersurface subunit in the supersurface unit is 20nm to 80nm.

[0023] The present invention provides a deep continuous gradient metasurface unit and method, wherein the metasurface unit has a deep continuous gradient metasurface sub-unit composed of a plurality of concentric rings, the structure of each metasurface sub-unit can be the same or different, the diameter of each concentric ring is different, and the line width and distance can be the same or different, so as to modulate different parameters of the metasurface sub-unit, thereby providing more options for the design of metasurface structures in the field.

[0024] On the other hand, by limiting in this method, in step (2), the etching depth in different functional areas is corrected and compensated, and the etching depth is adjusted and compensated first, and the etching depths at different positions are calculated respectively to form functional areas with continuous and gradual depths for subsequent etching operations. Based on such compensation and correction, the etching depths at different positions are adjusted to form functional areas with continuous and gradual depths, so as to overcome the defects of the prior art, reduce the over-etching of the second material layer as much as possible, and make the deep continuous and gradual hypersurface unit formed by etching form as little over-etching as possible at the bottom. In this way, the process steps of the existing deep continuous and gradual hypersurface are improved, the etching accuracy is improved, and the optical performance of the optical product is better to meet more application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 A schematic diagram of the structure of a depth-continuous gradient supersurface unit provided by the present invention;

[0027] Figure 2 A schematic diagram of the structure of a hypersurface subunit of a depth-continuously-gradient hypersurface unit provided by the present invention;

[0028] Figure 3A schematic diagram of the structure of a super surface unit formed by etching a super surface unit with a continuously gradient depth using an etching process provided in the prior art;

[0029] Figure 4 A schematic diagram of the structural changes of a method for preparing a deep continuous gradient supersurface unit provided by the present invention;

[0030] Figure 5 For the present invention Figure 4 A magnified schematic diagram of the local structure of the central functional area;

[0031] Figure 6 A top view of the supersurface subunit structure provided by the present invention. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0033] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0034] The present invention provides a depth-continuous gradient super surface unit 100, such as Figure 1 As shown in the left figure, it includes at least a first material layer 10, and any surface of the first material layer 10 includes at least one functional area, such as Figure 1 As shown by the middle dotted line, the functional area includes several hypersurface sub-units with continuously gradient depths, and each hypersurface sub-unit includes several concentric rings.

[0035] The functional area includes at least two super surface sub-units with continuous depth gradient. Exemplarily, it includes 2 functional areas, 3 functional areas, etc. Those skilled in the art choose to set the number of functional areas according to different technical requirements, etc., all within the scope of protection of this application. The structure of the super surface sub-unit in each functional area can be different or the same, and the different structures mentioned here refer to different structural sizes or shapes.

[0036] The depth continuous gradient defined in the present invention refers to the continuous change of the depth of several super surface sub-units in the functional area, such as the continuous increase of depth, the continuous decrease of depth, or the overlapping setting of two different depths, etc., such as the gradient interval of the depth change difference range of (2% to 5%). And in the functional area, there are multiple super surface sub-units with different depths.

[0037] Further, if Figure 1 As shown in the middle right figure, a second material layer 20 is also included. The second material layer 20 is formed on the surface of the first material layer 20 away from the functional area.

[0038] The first material layer 10 and the second material layer 20 may be silicon, silicon dioxide or the like.

[0039] In some other embodiments, such as Figure 2 As shown, each metasurface subunit includes several concentric rings, each ring has a different diameter, and the line width of each ring can be the same or different. Furthermore, the distance between adjacent rings can be the same or different. The structure of each metasurface subunit can be the same or different, and suitability can be adjusted based on different scene requirements.

[0040] In detail, Figure 6 As shown, a schematic top view of a metasurface subunit structure is shown. Based on different metasurface structure designs, the structural size of the metasurface subunit is limited to a range of 0.5mm to 6mm, which is equivalent to the structural size being the diameter D of the largest circular ring, and the diameter D of the largest circular ring is in the range of 0.5mm to 6mm; the diameter d of any concentric circular ring is in the range of 50nm to 6mm; the line width W of each concentric circular ring is in the range of 20 to 200nm (the line width W refers to the edge width of the concentric circular ring); the spacing L between adjacent concentric circular rings is in the range of 50nm to 150nm; the height of any concentric circular ring is in the range of 50 to 450nm; so as to realize the modulation of different metasurface structures and improve the degree of freedom of regulation.

[0041] like Figure 2 , Figure 6It shows that the diameters d of the multiple concentric rings are different, ranging from 50nm to 6mm, the line widths of adjacent rings are the same or different, the line width W ranges from 20 to 200nm, and the distances L between adjacent rings can be the same or different, ranging from 50nm to 150nm; of course Figure 2 and Figure 6 It is only an example of several concentric rings of a metasurface subunit, and does not represent the number of concentric rings of a specific metasurface structure. Based on different design requirements, it can be limited to include multiple different concentric ring structures. The deep continuous gradient functional area composed of several metasurface subunits can solve the complexity of the manufacturing process of the metasurface unit, dispersion problems, and dynamic control capabilities through the modulation of various process and performance parameters.

[0042] Further, optionally, the depth variation range of the continuous depth gradient supersurface sub-unit in the supersurface unit 100 is 20 nm to 80 nm.

[0043] The present invention limits the structure of each metasurface subunit, and each metasurface subunit is composed of a number of concentric rings. By modulating the diameter, line width, distance and other parameters of each ring, the diameter of each ring, the line width of each ring, and the spacing between adjacent rings can be partially the same or completely different, thereby modulating the amplitude, phase and frequency response of different wavelengths to achieve specific phase delay, control polarization state and other effects, thereby increasing the design freedom of the metasurface structure.

[0044] Specifically, the line width of each ring is the same; or the line width of at least two rings is different; the spacing between the rings is the same; or the spacing between at least two rings is different, and the spacing is the distance between adjacent rings. For example, if there are multiple rings, the spacing between each ring can be the same, or the spacing between each ring can be partially the same or completely different; for example, if there are 6 concentric rings, such as Figure 6 As shown, the spacing L between each ring can be partially the same or completely different to achieve modulation of different spacings. The line width W of the concentric rings can also be partially the same or completely different.

[0045] Furthermore, in order to obtain a depth-continuous gradient metasurface unit 100 of the above embodiment, if a conventional etching process in the prior art is used, the desired etching depth cannot be achieved, and the following problems often occur: Figure 3 The over-etching phenomenon in the process is likely to cause an over-etching depth on the surface of the second material layer 20. In order to improve this phenomenon, the present invention proposes a method for preparing a depth-continuous gradient supersurface unit.

[0046] In more detail, a method for preparing a deep continuous gradient super surface unit as described in the above embodiment can be referred to Figure 4 , including the following steps:

[0047] (1) providing at least a first material layer 10 and a second material layer 20, wherein the first material layer 10 is formed on any one side surface of the second material layer 20;

[0048] (2) forming at least one functional region on the surface of the first material layer 10 away from the second material layer 20, wherein the depth of the functional region changes continuously and gradually;

[0049] (3) depositing photoresist in the functional area and planarizing the surface thereof;

[0050] (4) patterning the photoresist to form a patterned area;

[0051] (5) Etching the first material layer 10, exposing and developing, and obtaining a depth-continuous gradient metasurface unit.

[0052] In detail, in step (1), the second material layer 20 is used as an etching substrate material, and materials such as Si, SiO2, TiO2, SiC, LiNbO3, germanium, gallium arsenide, etc. can be selected as the substrate; the first material layer 10 is deposited on any surface of the second material layer 20, and the first material layer can be selected from materials such as SiO2, TiO2, SiC, LiNbO3, etc. The thickness of the first material layer 10 and the second material layer 20 is 10 to 200 nm.

[0053] In step (2), in detail, it also includes: first calculating the etching depth of the first material layer at different locations in at least one functional area, and performing depth gradient etching on the first material layer; thereby obtaining a functional area with a continuous gradient depth.

[0054] Specifically, in a certain functional area, the etching depth H1 of the first material layer at a certain location can be determined by the following formula:

[0055] H1=H-[T-(H1 / V1)]*[V1 / K] (1)

[0056] In formula (1), H1 represents the etching depth of the first material layer at a certain location; H represents the target depth; T represents the total etching time, including the etching time of the first material layer and the etching time of the second material layer; V1 represents the etching speed of the first material layer, ranging from 0.5 to 3 nm / s; K represents the etching selectivity of the second material layer to the first material layer, ranging from 4 to 9;

[0057] To further explain, Figure 5 As shown, Figure 4In the enlarged view of the local structure of step 2, assuming that the etching depth H1 of the first material layer at a certain position, the gradient etching depth of the depth-continuous gradient functional area at a certain position can be determined by formula (1), thereby determining the gradient etching depth at different positions, and obtaining a series of different first material layer etching depths, such as H 11 , H 12 , H 13 ... and so on. Based on this, a functional area with a continuous gradient in depth can be formed through the etching process. Of course, Figures 1 to 5 Only one functional area is shown. For those skilled in the art, there are also two functional areas, three functional areas and other multiple functional areas. The present invention does not impose any quantitative limitation on this.

[0058] In this step, by etching different functional areas or different positions of functional areas at different depths, in the present invention, the time for the first material layer to be exposed to the gas ion cluster beam is limited, and the moving speed of the first material layer is controlled, so that etching at different depths in different functional areas can be achieved, and the following is obtained: Figure 4 The continuous gradient functional area shown in step (2) in FIG.

[0059] Furthermore, in step (2), the present invention reversely calculates the etching depth of the first material layer with continuous depth gradient at different positions based on the etching selectivity ratio between the first material layer and the second material layer, thereby realizing the modulation of the continuous depth gradient and preparing for the subsequent etching process, which is important for the preparation of the deep continuous gradient metasurface unit of the present invention and is substantially different from the prior art.

[0060] In more detail, for the first material layer and the second material layer, the etching depths of different functional areas are calculated based on formula (1), as shown in Table 1 below:

[0061]

[0062] In the table, T1 represents the etching time of the first material layer; T2 represents the etching time of the second material layer; T represents the total etching time; V1 represents the etching rate of the first material layer; V2 represents the etching rate of the second material layer; and H represents the total depth change.

[0063] From the formula (1): H1=H-[T-(H1 / V1)]*[V1 / K], after transformation, H1=(KH-TV1) / (K-1) is obtained; H1 represents the etching depth of the first material layer at a certain location.

[0064] Based on different embodiments of Table 1, based on the total etching time of different etching targets and the etching rate V1 of the first material layer and the etching selectivity, it can be simplified based on the total depth change value requirement determined in Table 1 to obtain H1=(KH-80) / (K-1). In Table 1, based on the design to determine the total depth change value of the continuous gradient depth, such as 20nm, 22nm, 25nm...80nm, combined with the etching selectivity of the first material layer and the second material layer, the etching depth H1 at different positions in the depth continuous gradient functional area can be calculated respectively to carry out the next etching process. By calculating the etching depth H1 of the first material layer in step (2), the compensation is corrected as follows: Figure 3 The over-etching phenomenon in the process makes it different from the conventional etching process. The present invention first corrects and compensates the etched part to reduce the subsequent over-etching, so that the structure formed after etching is as follows Figure 2 shown.

[0065] In the embodiment of the above table, based on the design requirements, the depth variation range of the depth continuous gradient super surface unit is limited to 20nm to 80nm. Of course, based on different design requirements, the depth variation range of the super surface unit is limited to other ranges, such as 20nm to 300nm, 200nm to 300nm, 20nm to 100nm, 100nm to 150nm, 100nm to 200nm, etc. parameter ranges, and the present invention does not limit the specific variation value.

[0066] In this step, during etching, SF6 is conventionally used as the core etching gas, C4F8, CHF3, etc. are used as auxiliary etching gases, and then a high-density plasma is formed for etching; while in step (2) of the present method, the present invention uses fluorine-based gas to form electrically neutral ion gas clusters for etching, and the etching efficiency is relatively high; in more detail, the etching process of the present invention uses fluorine-based gas as the etching gas to form electrically neutral ion gas clusters, and etches the target structure area to achieve the target gradient depth.

[0067] In more detail, in order to achieve continuous and gradual modulation of depth, in step (5), the etching gas fluorine-based gas flow range is limited to 10-125sccm; the Ar flow range is 10-500sccm; the acceleration voltage Accel voltage range is: 10-60Kv; and the ion bias current range is 10-200mA.

[0068] The etching process of step (2), that is, under a high vacuum state, the etching gas is ionized to form charged ion gas clusters, which are accelerated under the action of an accelerating voltage and then neutralized by Ar ionization, so that the entire ion group is electrically neutral. After the electrically neutral ion gas clusters reach the surface of the substrate, chemical and physical reactions occur on the surface to achieve the purpose of etching.

[0069] Through the etching process using fluorine-based gas as etching gas, on the one hand, the morphology of the gradient structure of the metasurface, such as surface roughness, is modified by ionized gas clusters of fluorine-based gas to achieve high-precision etching with continuous gradient in depth; on the other hand, the depth continuity between different metasurface sub-units is ensured, especially the boundary line problem between different metasurface depths, and the visualization problem of the boundary lines between different sub-units is blurred or optimized as much as possible, reducing the influence of the boundary lines of different metasurface sub-unit depth changes on the appearance of the metasurface structure, so as to improve the appearance of the metasurface unit.

[0070] Further, in step (3), based on at least one depth-continuous gradient functional region formed by etching in the previous step, a certain thickness of photoresist is deposited in the functional region, such as Figure 4 As shown in step (3), the surface of the photoresist is planarized to make it flush with the surface of the first material layer.

[0071] In this step, the deposited photoresist is used to completely fill the different positions of the depth-continuous gradient functional area, and the surface is planarized to prevent the photoresist from not completely filling the functional area, in preparation for the next step.

[0072] Further, in step (4), the photoresist is patterned based on the pre-screened pattern to form a patterned area.

[0073] In this step, based on the designed metasurface unit structure, especially various parameters such as the diameter of each of the several concentric rings and the line width of each ring, the corresponding photoresist is patterned.

[0074] In step (5), the first material layer 10 is etched, exposed and developed to obtain a depth-continuous gradient metasurface unit.

[0075] In this step, the process parameters for etching the first material layer 10 are defined as follows:

[0076] Chamber pressure (mTorr): 2.0~6.0;

[0077] Beam current (uA): 200~800;

[0078] Beam current(V): 300~1000;

[0079] Ar(sccm): 0~5;

[0080] O2(sccm): 1~10;

[0081] Etching rate of the first material layer (nm / s): 0.5-3.

[0082] Based on the above etching process, the first material layer is etched to form the required metasurface unit structure; during the etching process, different etching parameters are adjusted.

[0083] In step (5), combine Figure 2 and Figure 3 As can be seen from the comparative embodiment, when the first material layer is etched based on the conventional etching process, it is easy to form Figure 3 The over-etching situation shown in the figure makes the conventional etching process produce an over-etching depth on the surface of the second material layer 20, which is something that the technicians in this field do not want to see during etching, because such etching results have a great influence on the optical properties of the super surface structure. Since the refractive index and material of the two material layers are different, their optical properties are different, which makes it difficult to meet the design requirements. In the present invention, through the method of the present invention, in step (2), by correcting and compensating the etching depths at different positions of the functional area, a functional area with a continuous gradient in depth is formed for subsequent etching operations, and etching is performed in a continuous gradient structure. Based on this compensation and correction, the defects of the prior art can be overcome, the over-etching of the second material layer can be reduced as much as possible, so that the deep continuous gradient super surface unit formed by etching forms as little over-etching phenomenon as possible at the bottom, such as Figure 2 As shown, the process steps of the existing deep continuous gradient metasurface are improved, so that the optical performance of the optical product is better, and at the same time, more metasurface unit structure options are given to technical personnel in the field, with a higher degree of freedom.

[0084] The structure of the deep continuous gradient hypersurface unit proposed in the present invention is different from that in the prior art, and the method for preparing the deep continuous gradient hypersurface unit proposed in the present invention is different from that in the prior art. Based on this, compared with the prior art, it has outstanding substantial characteristics and significant progress.

[0085] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A deep continuous gradient hypersurface unit, characterized in that: It at least comprises a first material layer, wherein any surface of the first material layer comprises at least one functional region, wherein the functional region comprises a plurality of super surface sub-units with continuously gradient depths, and each of the super surface sub-units comprises a plurality of concentric rings.

2. A depth-continuously-gradient hypersurface unit according to claim 1, characterized in that: It also includes a second material layer, which is formed on a surface of the first material layer away from the functional area.

3. A depth-continuously-gradient supersurface unit according to any one of claims 1 to 2, characterized in that: Each of the metasurface subunits includes a plurality of concentric rings, and each of the concentric rings has a different diameter.

4. A depth-continuously-gradient hypersurface unit according to claim 3, characterized in that: The line width of each of the circular rings is the same; or the line widths of at least two of the circular rings are different; the spacing between the circular rings is the same; or the spacing between at least two of the circular rings is different, and the spacing is the distance between adjacent circular rings.

5. A depth-continuously-gradient supersurface unit according to claim 1 or 4, characterized in that: The structural dimensions of the metasurface subunits range from 0.5 mm to 6 mm; the diameter of any of the concentric rings ranges from 50 nm to 6 mm; the line width of any of the concentric rings ranges from 20 to 200 nm; and the spacing between adjacent concentric rings ranges from 50 nm to 150 nm.

6. A method for preparing the deep continuous gradient supersurface unit according to any one of claims 1 to 5, characterized in that: The steps include: (1) providing at least a first material layer and a second material layer, wherein the first material layer is formed on either side surface of the second material layer; (2) forming at least one functional region on a surface of the first material layer away from the second material layer, wherein the depth of the functional region changes continuously and gradually; (3) depositing photoresist in the functional area and planarizing the surface thereof; (4) patterning the photoresist to form a patterned area; (5) Etching the first material layer, exposing and developing it, and obtaining a deep continuous gradient metasurface unit.

7. The method according to claim 6, characterized in that The step (2) also includes first calculating the etching depth of the first material layer at different locations in at least one of the functional areas, and performing depth gradient etching on the first material layer.

8. The method according to claim 7, characterized in that In the functional area, the etching depth of the first material layer at a certain location can be determined by the following formula (1): H1=H-[T-(H1 / V1)]*[V1 / K] (1) In formula (1), H1 represents the etching depth of the first material layer at a certain location; H represents the target depth; T represents the total etching time, including the etching time of the first material layer and the etching time of the second material layer; V1 represents the etching speed of the first material layer; K represents the etching selectivity ratio of the second material layer to the first material layer.

9. The method according to any one of claims 6 or 8, characterized in that: In the step (2), at least one functional area is formed on the surface of the first material layer away from the second material layer, and the functional area is etched. Fluorine-based gas is used as etching gas to form electrically neutral ion gas clusters to etch the target area; the target gradient depth is reached and the depth continuity is ensured.

10. The method according to claim 9, characterized in that The depth variation range of the depth-continuous-gradient-supersurface subunit in the supersurface unit is 20nm to 80nm.

Citation Information

Cited By

  • Grating structure with continuous gradually-changed depth based on silicon carbide substrate and preparation method of grating structure

    CN121276675A