Hexagonal boron nitride powder and method for producing same

By heating under a nitrogen atmosphere and reducing nitriding method of wet spray mill crushing, boron nitride powder with the same length diameter and thickness was prepared, and the existing boron nitride powder was solved in terms of sliding, moisturizing and glossiness. The disadvantages of cosmetics achieve high slipperiness, moistness and excellent glossiness.

CN118900821APending Publication Date: 2024-11-05TOKUYAMA CORP
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202380028873.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing boron nitride powders cannot be fully satisfied in terms of having the high slippage, moisture and gloss that cosmetic users expect.

Method used

Hexagonal boron nitride powder is produced by reducing nitriding method heated under a nitrogen atmosphere, and pulverized by a wet spray mill to prepare boron nitride powder with the same length and thickness, which has excellent sliding properties, moisture and Glossiness.

Benefits of technology

The cosmetics have good sliding properties, moisturized and skin-friendly, less rough and excellent glossiness. The prepared boron nitride powder can significantly improve the use and appearance quality of the cosmetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900821A_ABST
    Figure CN118900821A_ABST
Patent Text Reader

Abstract

A hexagonal boron nitride powder having an average major axis (L50) of 3-20 [mu] m, an average thickness (T50) of 0.3-2 [mu] m, (L90-L10) / L50 of 2.0 or less, (T90-T10) / T50 of 2.0 or less, an average aspect ratio of 10-30, a dynamic friction coefficient (MIU) of 0.50 or less, a variation value (MMD) of the dynamic friction coefficient of 0.0050 or less, and a specular reflection intensity of 80 or more as measured by a variable angle photometer at an incident light angle of 60 DEG.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to hexagonal boron nitride powder (hereinafter, sometimes referred to as boron nitride powder or h-BN powder). More specifically, the present invention relates to hexagonal boron nitride powder suitable for use in cosmetics and a method for producing the same. Background Art

[0002] As the extender pigment of cosmetics, inorganic materials such as talc, mica, kaolin, and resin materials such as nylon powder and polyethylene powder have been used. The extender pigment becomes a base for dispersing various components contained in cosmetics such as coloring pigments, and has a great influence on the feel of use such as spreadability (property of being applied smoothly on the skin surface), long-lasting (property of making the state of application on the skin last), and glossiness.

[0003] However, their usability and stability are not necessarily satisfactory. For example, inorganic materials such as talc, mica, and kaolin have catalytic activity, which can cause the deterioration of fragrances and oils, and can be said to be the cause of odor. In addition, resin materials such as nylon powder and polyethylene powder are chemically stable, but have the problem of poor formability.

[0004] Therefore, hexagonal boron nitride, which has a flat shape and superior lubricity to other materials, has come to be used as a white extender pigment for cosmetics.

[0005] Patent Document 1 describes a boron nitride powder which is formed by reacting boric acid, urea and boron carbide at a predetermined ratio of oxygen to carbon to form a plate-like aggregate of stacked flat primary particles having a predetermined average major diameter and thickness.

[0006] Patent Document 2 describes a hexagonal boron nitride powder having a predetermined average particle size, a maximum particle size, a specific surface area, a predetermined graphitization index, an average friction coefficient, and a variation value of the average friction coefficient as a hexagonal boron nitride powder that can improve sliding properties and reduce roughness. Patent Document 2 describes a method for producing hexagonal boron nitride powder by specifying a first sintering condition and a second sintering condition.

[0007] Patent Document 3 found that the "durability" of a cosmetic product, which is a property of maintaining the state of application on the skin, is closely related to the oil absorption of the powder constituting the cosmetic, and proposed a boron nitride powder having a predetermined water penetration rate and oil absorption. The boron nitride powder described in Patent Document 3 is produced by subjecting boric acid, urea, and boron carbide to a two-step heating treatment.

[0008] Patent Document 4 proposes a boron nitride powder which appropriately maintains sliding properties and has an excellent touch such as "wet" and "slippery", and is suitable for cosmetics, wherein the amount of eluted boron, the average particle size, and the content of particles of a specific particle size of the boron nitride powder are below a specified value. Patent Document 4 describes the average friction coefficient and the variation value of the average friction coefficient of the boron nitride powder. In addition, Patent Document 4 describes a method for producing boron nitride powder by two-stage sintering, pulverization, and washing.

[0009] Patent Document 5 proposes a hexagonal boron nitride powder, which is a hexagonal boron nitride powder capable of realizing a resin sheet having high thermal conductivity and high dielectric strength, and the hexagonal boron nitride powder has a predetermined specific surface area, a major diameter of primary particles, and an aspect ratio. Patent Document 5 describes a method for producing hexagonal boron nitride powder by heating boron oxide, an organic compound containing nitrogen, and lithium carbonate at a predetermined weight ratio.

[0010] Patent document 6 describes a method for producing hexagonal boron nitride powder with a low aspect ratio, in which a raw material powder containing hexagonal boron nitride particles having an aspect ratio within a specified range and hexagonal boron nitride particles having an aspect ratio exceeding a specified value is crushed by means substantially without comminuting the primary particles.

[0011] Patent Document 7 states that the brilliance of the boron nitride powder and the brilliance when used in combination with a bright pigment can be improved by increasing the proportion of particles having a structure bent at a specific angle among the boron nitride particles contained in the boron nitride powder. In Patent Document 7, a goniophotometer is used to measure the particles having a structure bent at a specific angle.

[0012] Non-Patent Document 1 describes the flake formation of a two-dimensional nanofiller using a wet jet mill, and hexagonal boron nitride and graphite are used as the two-dimensional nanofiller.

[0013] However, these conventional boron nitride powders cannot fully satisfy both the high feeling during use and the glossiness desired by cosmetic users.

[0014] Prior art literature

[0015] Patent Literature

[0016] Patent Document 1: Japanese Patent Application Publication No. 2012-176910

[0017] Patent Document 2: Japanese Patent Application Publication No. 2018-165241

[0018] Patent Document 3: International Publication No. 2014 / 049956

[0019] Patent Document 4: International Publication No. 2019 / 172440

[0020] Patent Document 5: International Publication No. 2020 / 179662

[0021] Patent Document 6: International Publication No. 2021 / 085223

[0022] Patent Document 7: Japanese Patent No. 6625308

[0023] Non-patent literature

[0024] Non-patent document 1: Effect of medium viscosity on flake formation of two-dimensional nanofillers by wet jet mill, Yusuke Imai, Yuji Horita, J. Soc. Powder Technol., Japan, 54, 442-447 (2017) Summary of the invention

[0025] Problem that the invention aims to solve

[0026] The object of the present invention is to provide a cosmetic comprising hexagonal boron nitride powder, having good sliding properties, good moist feeling (skin-friendly), less roughness, and excellent glossiness, and a hexagonal boron nitride powder for preparing the cosmetic. In addition, the object of the present invention is to provide a method for producing the above-mentioned boron nitride powder.

[0027] Solutions for solving problems

[0028] The present inventors have discovered that when hexagonal boron nitride powder is produced by a reduction nitridation method in which a raw material mixture is heated under a nitrogen atmosphere, if boron nitride powder pulverized by a wet jet mill is present as a seed crystal, a boron nitride powder having a uniform major diameter and thickness can be produced, and cosmetics produced using such a boron nitride powder having a uniform major diameter and thickness have good sliding properties, good moist feeling (skin-friendly), less roughness, and excellent glossiness, thereby completing the present invention.

[0029] That is, the present invention includes the following technical solutions.

[0030] 1. A hexagonal boron nitride powder,

[0031] The average major diameter (L50) is 3 to 20 μm, the average thickness (T50) is 0.3 to 2 μm, (L90-L10) / L50 is less than 2.0, (T90-T10) / T50 is less than 2.0, and the average aspect ratio is 10 to 30.

[0032] The dynamic friction coefficient (MIU) is less than 0.50, and the variation value of the dynamic friction coefficient (MMD) is less than 0.0050.

[0033] The specular reflection intensity measured by a goniophotometer under the condition of an incident light angle of 60° is 80 or more.

[0034] 2. The hexagonal boron nitride powder according to 1 above, wherein (L90-L10) / L50 is 1.8 or less.

[0035] 3. The hexagonal boron nitride powder according to 1 above, which is used in cosmetics.

[0036] 4. A cosmetic comprising the hexagonal boron nitride powder according to 1 above.

[0037] 5. A method for producing hexagonal boron nitride powder, comprising a reduction nitridation step of heating a raw material mixture under a nitrogen atmosphere, wherein:

[0038] The raw material mixture comprises: an oxygen-containing boron compound, an oxygen-containing alkaline earth metal compound, a carbon source and a seed crystal.

[0039] The seed crystal is a boron nitride powder obtained by treating a raw material boron nitride powder having a graphitization index of 1.7 or less by a wet jet mill. The specific surface area of ​​the seed crystal is 10 m 2 / g or above.

[0040] 6. The method for producing hexagonal boron nitride powder according to the above 5, wherein the concentration of the slurry during the treatment using a wet jet mill is 20 to 100 g / L.

[0041] 7. The method for producing hexagonal boron nitride powder according to the above item 5, wherein the atomic ratio (B / C ratio) of the boron atoms (B) of the oxygen-containing boron compound to the carbon atoms (C) of the carbon source in the raw material mixture is 0.70 to 2.00,

[0042] The aforementioned oxygen-containing alkaline earth metal compound (AO; A is an alkaline earth metal) and the aforementioned oxygen-containing boron compound (B 2 O 3 ) molar ratio (AO / B 2 O 3 Ratio) is 0.01~1.0,

[0043] The boron atoms (B s ) to the carbon atom (C) of the aforementioned carbon source (B s / C ratio) is 0.01~13.

[0044] 8. The method for producing hexagonal boron nitride powder according to the above item 5, wherein the heating is performed at 1700 to 2100°C in the reduction nitriding step.

[0045] Effects of the Invention

[0046] The hexagonal boron nitride powder of the present invention has a sharp and uniform major diameter distribution, and a sharp and uniform thickness distribution, so the cosmetics containing it have good slip, good moist feeling (skin-friendly), less roughness, and excellent glossiness. According to the method for producing the boron nitride powder of the present invention, a hexagonal boron nitride powder having a sharp and uniform major diameter distribution, a sharp and uniform thickness distribution, and a uniform thickness can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 It is a schematic diagram of measuring the specular reflection intensity of the hexagonal boron nitride powder of the present invention using a goniophotometer under the condition of an incident light angle of 60°. DETAILED DESCRIPTION

[0048] <Hexagonal Boron Nitride Powder>

[0049] [About average major diameter, average thickness and average aspect ratio]

[0050] The epoxy resin or the like in which the boron nitride powder is dispersed is cured, and the side of the cured product is milled to form a processed surface. When the processed surface is photographed by SEM, the long side of the boron nitride particles is taken as the major diameter, and the short side is taken as the thickness. When the major diameter and thickness of the boron nitride particles are arranged from the smallest, the values ​​at which the cumulative frequency of the area basis of the boron nitride particles becomes 50% are taken as the average major diameter (L50) and average thickness (T50) of the boron nitride particles.

[0051] The average major diameter (L50) of the boron nitride of the present invention is 3 to 20 μm, preferably 4 to 15 μm, more preferably 5 to 12 μm. The average thickness (T50) of the boron nitride particles is 0.3 to 2 μm, preferably 0.4 to 1.2 μm.

[0052] When the average major diameter (L50) is less than 3 μm, the sliding property becomes insufficient. When the average major diameter (L50) exceeds 20 μm, the sliding property becomes too high, so the touch feeling of the cosmetics such as "wet" and "slippery" is impaired, and the roughness of the appearance of the boron nitride powder becomes stronger, so it becomes unpreferable as a cosmetic raw material. In addition, when the average thickness (T50) is less than 0.3 μm, the hiding power of covering spots and wrinkles becomes insufficient, and when it exceeds 2 μm, the transparency is reduced, and the finished makeup becomes unnatural.

[0053] The content of coarse particles exceeding 2.5 times the average major diameter (L50) is 12 area % or less, preferably 9 area % or less, and more preferably 6 area % or less. The smaller the content of coarse particles, the more "wet" touch can be obtained, and roughness can be suppressed.

[0054] The average aspect ratio is the value obtained by dividing the average major diameter (L50) of the above-mentioned particles by the average thickness (T50) (= L50 / T50). The average aspect ratio is 10 to 30, preferably 12 to 28, and more preferably 14 to 25. If the average aspect ratio exceeds 10, elongation, sliding, and adhesion become particularly excellent. On the other hand, particles with an average aspect ratio exceeding 30 are difficult to manufacture.

[0055] The (L90-L10) / L50 of the boron nitride powder of the present invention is 2.0 or less, preferably 1.9 or less, and more preferably 1.8 or less. It can be said that the smaller the (L90-L10) / L50 is, the sharper the major diameter distribution is and the more consistent the major diameter is. The smaller the value is, the better the sliding property of the cosmetic is, and the more "wet" touch can be obtained. By making the major diameter distribution of the boron nitride powder sharp, the proportion of particles near the preferred range of the average major diameter (L50) increases, and the overall roughness of the boron nitride powder is suppressed. Therefore, when the cosmetic is made, higher sliding property and moist feeling can be obtained. It should be noted that in the present invention, L10, L50 and L90 of the boron nitride powder refer to the cumulative 10% value (L10), the cumulative 50% value (L50), and the cumulative 90% value (L90) of the area basis of the boron nitride particles when the major diameters of the boron nitride particles are sorted from the smallest.

[0056] The (T90-T10) / T50 of the boron nitride powder of the present invention is less than 2.0, preferably less than 1.9, and more preferably less than 1.6. It can be said that the smaller the (T90-T10) / T50 is, the sharper the thickness distribution is, the more consistent the thickness is, and the more glossiness can be obtained, which is an important point in the present invention. By making the thickness distribution sharp, the unevenness of the powder surface of the light incident on the boron nitride powder becomes smaller and becomes close to being basically flat. That is, it becomes less likely to cause diffuse reflection reflected in various directions, and the proportion of light that becomes regular reflection reflected in a certain direction increases, so the glossiness increases. In addition, on the basis of a sharp thickness distribution and a sharp major diameter distribution, the influence of the unevenness of the powder surface is further reduced, so the glossiness is further increased. It should be noted that, in the present invention, T10, T50 and T90 of the boron nitride powder refer to the cumulative 10% value (T10), the cumulative 50% value (T50), and the cumulative 90% value (T90) of the area basis of the boron nitride particles when the thickness of the boron nitride particles is arranged from the smallest.

[0057] [About MIU and MMD]

[0058] As an index that numerically expresses the sliding property, there is MIU (friction coefficient). The smaller the MIU value, the better the sliding property. In addition, as an index that numerically expresses the roughness, there is MMD (variation value of friction coefficient). The smaller the MMD value, the smaller the roughness.

[0059] The boron nitride powder of the present invention has a dynamic friction coefficient (MIU) of 0.50 or less, preferably 0.42 or less, and more preferably 0.40 or less. When the MIU of the boron nitride powder is 0.50 or less, the slip properties of the prepared cosmetic can be further improved.

[0060] The variation value (MMD) of the dynamic friction coefficient of the boron nitride powder of the present invention is 0.0050 or less, preferably 0.0045 or less, and more preferably 0.0040 or less. By making the MMD of the boron nitride powder 0.0050 or less, the roughness of the prepared cosmetics can be suppressed and the feel of the prepared cosmetics can be improved.

[0061] In this specification, "MIU (friction coefficient)" and "MMD (variation value of friction coefficient)" are dimensionless numbers measured by a friction feel measuring instrument (manufactured by KATO TECH CO., LTD., trade name: KES-SE). Specifically, boron nitride powder was placed on artificial leather (manufactured by Idemitsu Technofine Co., Ltd., trade name: SUPPLALE PBZ13001 BK) regarded as skin so as to give a friction coefficient of 0.5 mg / cm 2 The MIU and MMD can be measured by extending the boron nitride powder in a thin layer in a manner of 10 mm square silicon and contacting the sensor part of the friction measuring device (10 mm square silicon). The measurement conditions of the friction measuring device are set as sensitivity: H, test bench moving speed: 1 mm / sec, and static load: 25 gf. The measurement is performed once. Repeat the sample preparation (coating and extension of the boron nitride powder on the artificial leather) and the measurement with the friction measuring device 5 times, and the average value of the 5 measurement results is taken as the MIU and MMD of the boron nitride powder.

[0062] [About specular reflection intensity]

[0063] The specular reflection intensity of the boron nitride powder of the present invention represents the degree of specular reflection measured by a goniophotometer. The larger the value, the stronger the specular reflection, indicating that the glossiness of the boron nitride powder increases. For the boron nitride powder of the present invention, the specular reflection intensity measured under the condition of an incident light angle of 60° is 80 or more, preferably 82 or more, and more preferably 88 or more. If the specular reflection intensity is less than 80, the glossiness becomes weak, and therefore, it is not preferred as a cosmetic raw material.

[0064] Figure 1 This is a schematic diagram of measuring the specular reflection intensity of the hexagonal boron nitride powder 1 of the present invention under the condition of an incident light angle of 60°.

[0065] In the present invention, light with an incident light angle of 60° refers to light (incident light 3) incident from -60° when a straight line perpendicular to the surface (surface formed by the hexagonal boron nitride powder 1) to be irradiated with light is set to 0°. In addition, light specularly reflected by the hexagonal boron nitride powder 1 on the same plane is reflected light 5. Figure 1 In FIG. 1 , light having a reflection light peak at +60° is representatively shown as reflected light 5. In the present invention, the specular reflection intensity refers to a value obtained by measuring the reflected light 5 having the reflection light peak by a goniophotometer.

[0066] <Cosmetics>

[0067] The hexagonal boron nitride powder can be used in cosmetics. The present invention includes cosmetics containing the hexagonal boron nitride powder. By using the hexagonal boron nitride powder of the present invention in cosmetics, the hexagonal boron nitride powder plays a role as a pigment of cosmetics, and the prepared cosmetics have good sliding properties, good moist feeling (skin-friendly), less roughness, and excellent glossiness.

[0068] If an example of cosmetics is given, it can be listed as foundation (powder foundation, liquid foundation, cream foundation), face powder, spot makeup, eye shadow, eyeliner, hand-made nail art, lipstick, blush, and mascara. Among the above cosmetics, the cosmetics disclosed in the present invention are particularly well suited for powder foundation and face powder.

[0069] The content of the boron nitride powder in the cosmetic is, for example, preferably 1 to 70% by mass, more preferably 3 to 40% by mass, and even more preferably 8 to 30% by mass based on the total amount of the cosmetic.

[0070] Other ingredients include pigments such as red iron oxide, yellow iron oxide, black iron oxide, titanium oxide, silicon dioxide, aluminum hydroxide, and mica, esters such as diisostearyl malate and tri-2-ethylhexanoin, and oils such as vaseline. In addition, talc, silicone powder, urethane powder, methyl paraben, sodium dehydroacetate, and the like can be mentioned.

[0071] <Raw material Boron nitride powder>

[0072] The raw material boron nitride powder is a previously produced boron nitride powder that is used as a raw material for obtaining seed crystals (S) by cleaving it with a wet jet mill.

[0073] In the present invention, the raw material boron nitride powder is characterized in that it has a high degree of crystallinity. The degree of crystallinity can be known by measuring the graphitization index (GI) of the boron nitride powder. The smaller the graphitization index, the higher the degree of crystallinity. The graphitization index of the raw material boron nitride powder is 1.7 or less, preferably 1.6 or less. If the degree of crystallinity of the raw material boron nitride powder is high, the crystal will become easy to crack on the (001) plane when it is treated by a wet jet mill. Therefore, the thickness of the treated seed boron nitride powder becomes smaller, and the boron nitride powder obtained by using it as a seed becomes a high aspect ratio, and the thickness distribution becomes sharp. It should be noted that the graphitization index can be measured by applying a known measurement method such as X-ray diffraction to the boron nitride powder.

[0074] The L50 of the raw boron nitride powder is preferably 10.0 μm or less, more preferably 5.0 μm or less. In addition, T50 is preferably 1.5 μm or less, more preferably 0.8 μm or less. If L50 and T50 are too large, the time required for the jet mill treatment to obtain the desired seed crystals will be prolonged, and the manufacturing efficiency will be reduced. If the L50 and T50 of the raw boron nitride powder are too small, it will become difficult to make the graphitization index below 1.7, but such a range is difficult to measure. Therefore, it can be managed by the specific surface area that is correlated with L50 and T50. There is a tendency that the smaller the L50 and T50, the larger the specific surface area of ​​the raw boron nitride powder, preferably 15m 2 / g or less, more preferably 10m 2 / g or less, more preferably 5m 2 / g or less.

[0075] The aspect ratio of the raw material boron nitride powder is preferably 6 to 30, more preferably 7 to 25. If the aspect ratio is too small, the jet mill treatment time to obtain the desired seed crystal becomes long, and the production efficiency decreases. If the aspect ratio exceeds 30, production becomes difficult.

[0076] The raw material boron nitride powder can be used without restriction as long as the graphitization index is below 1.7. The raw material boron nitride powder manufactured by a known manufacturing method such as the melamine method and the reduction nitridation method can also be used. The melamine method is easy to uniformly control the major diameter and thickness, so it is preferred. In addition, commercially available boron nitride powder can also be purchased for use.

[0077] <Seed Crystal(S)>

[0078] Seed crystal (S) is a hexagonal boron nitride powder obtained by treating the raw boron nitride powder with a wet jet mill to crack it and preferably further pulverizing it. As described above, the raw boron nitride powder has a high crystallinity, so the seed crystal (S) has a high aspect ratio and a sharp thickness distribution.

[0079] For the seed crystal (S), the raw material boron nitride powder is cracked and the particles are small, so it is difficult to measure the length and thickness. Therefore, the length and thickness are indirectly managed by measuring the specific surface area which is correlated with L50 and T50. The specific surface area of ​​the seed crystal (S) is 10m 2 / g or more, preferably 11m 2 / g or more, more preferably 12m 2 / g or more. The larger the specific surface area, the thinner the particles are peeled or the smaller they are crushed. In this case, the (L90-L10) / L50 or (T90-T10) / T50 of the seed crystal (S) tends to become smaller. Moreover, when such a seed crystal (S) is used as part of the raw material and the hexagonal boron nitride powder is manufactured by the reduction nitridation method, the major diameter and thickness distribution of the obtained hexagonal boron nitride powder also become sharp.

[0080] The specific surface area (A) of the seed crystal (S) 2 ) and the specific surface area of ​​the raw material boron nitride powder (A 1 ) ratio (A 2 / A 1 ) is preferably 1.6 to 30, more preferably 1.8 to 20. 2 / A 1 If it is greater than 30, the cracking (or crushing) by the wet jet mill is excessive, making the operation difficult. 2 / A 1 If the molecular weight is less than 1.6, the cleavage (or pulverization) by the wet jet mill may be insufficient, and the desired seed crystal (S) may not be produced.

[0081] <Method for producing hexagonal boron nitride powder>

[0082] The method for producing hexagonal boron nitride powder of the present invention is characterized in that the raw material mixture (S) is heated in a nitrogen atmosphere in the presence of seed crystals (S) obtained by treating the raw material boron nitride powder with a wet jet mill to cause it to be cracked, and preferably further pulverized, to carry out reductive nitridation. The production method is described below.

[0083] <Method for producing raw material boron nitride powder>

[0084] First, a method for producing a raw material boron nitride powder used as a raw material will be described. This raw material boron nitride powder is produced using a melamine method or a reduction nitridation method, so each production method will be described.

[0085] <Manufacturing of raw material boron nitride powder by melamine method>

[0086] The melamine method is a method in which a raw material mixture (M) containing an oxygen-containing boron compound and a nitrogen-containing organic compound is heated under a nitrogen atmosphere.

[0087] <Oxygen-containing boron compounds>

[0088] Examples of the oxygen-containing boron compound include boric acid, boric anhydride (boron oxide), metaboric acid, perboric acid, subboric acid, sodium tetraborate, and sodium perborate.

[0089] <Nitrogen-containing organic compounds>

[0090] Examples of the nitrogen-containing organic compound include melamine, ammeline, dicyandiamide, and urea.

[0091] <Oxygen-containing alkaline earth metal compounds>

[0092] The raw material mixture (M) may also contain an oxygen-containing alkaline earth metal compound. As the oxygen-containing alkaline earth metal compound, magnesium carbonate (MgCO 3 ), calcium carbonate (CaCO 3 ), calcium oxide (CaO), etc. In addition, two or more of the above may be used in combination.

[0093] <Composition ratio in the raw material mixture (M) in the melamine process>

[0094] In the raw material mixture (M) for producing the raw material boron nitride powder, the element ratio of boron / nitrogen (B / N) is preferably 0.2 to 1, more preferably 0.25 to 0.5.

[0095] <Heating process>

[0096] The heating temperature is preferably 500 to 1200° C., more preferably 600 to 1100° C., and further preferably 650 to 1000° C. The higher the heating temperature, the higher the crystallinity of the obtained raw material boron nitride powder.

[0097] The heating time is preferably 5 to 20 hours, more preferably 6 to 15 hours. The longer the heating time, the higher the crystallinity of the obtained raw material boron nitride powder.

[0098] The atmosphere in the heating furnace may be a non-oxidizing gas atmosphere, and nitrogen, ammonia, hydrogen, helium, argon, or the like may be used. Nitrogen is preferred because it is easily available and inexpensive.

[0099] The raw material mixture (M) may be filled into a carbon container, a carbon container coated with boron nitride, a boron nitride sintered body container, or the like, and then placed in a heating furnace.

[0100] In order to efficiently perform the subsequent wet jet mill treatment, it is preferred to reduce the aggregated particles of the raw material boron nitride powder in advance. The reduction of aggregated particles can be performed by crushing or classifying the reaction product.

[0101] <Crushing process>

[0102] In the crushing step, it is preferred to crush the boron nitride particles with a force that does not crush them, and this can be appropriately carried out using a mortar crusher, a roller crusher, etc. On the other hand, if a dry jet mill is used for processing, excessive force will be applied, and there is a concern of crushing.

[0103] <Cleaning process>

[0104] The reaction product obtained in the melamine process contains unreacted raw materials (B 2 O 3 , CaO) and other impurities, so the impurities are removed by cleaning with acid. By removing impurities, the efficiency of wet jet mill processing can be improved.

[0105] The acid cleaning method is not particularly limited, and known methods can be applied without limitation. For example, the reaction product obtained in the melamine method is untied by hand and placed in a container, and 3 to 10 times the amount of dilute hydrochloric acid (5 to 20 mass % HCl) of the reaction product is added, and stirred for 1 to 20 hours.

[0106] After the acid cleaning, pure water is used to remove the acid. From the viewpoint of avoiding secondary mixing of impurities, pure water with an electrical conductivity of 1 mS / m or less can be used. As a cleaning method, the acid used in the acid cleaning is filtered, and then pure water equal to the amount of the acid used is added and filtered again. Furthermore, the cleaning and filtering with pure water are repeated until the filtrate becomes neutral.

[0107] After washing, the slurry may be subjected to wet jet mill treatment without drying, or may be subjected to drying and then a new slurry for wet jet mill treatment may be prepared.

[0108] <Drying process>

[0109] If an example of a drying device that can be used in the drying process of the raw boron nitride powder is shown, it is a shed dryer, a fluidized bed dryer, a spray dryer, a rotary dryer, a belt dryer, a vacuum dryer, a vibration dryer, etc. or a combination thereof. The atmosphere temperature in the dryer is preferably 50 to 300°C, more preferably 100 to 250°C. The drying time is not particularly specified, but it is preferably dried until the moisture content is infinitely close to 0%, and it is generally recommended to dry at the aforementioned temperature for 1 to 48 hours. Cleaning and drying can be performed once each, or the same method or different methods can be combined and performed multiple times.

[0110] <Grading process>

[0111] There is no particular limitation on the method of classification, and known methods can be applied without restriction. Specifically, a vibrating screener, a wet screener, a wind classifier, a cyclone separator, a liquid cyclone separator, etc. can be cited, but from the aspect of being able to be easily performed, it is preferred to use a vibrating screener, a wet screener, etc. for classification. The mesh of the sieve is not particularly limited, and can be appropriately determined according to the purpose. The aperture is preferably set to 25 to 90 μm, and particularly preferably set to 25 to 45 μm. By making the mesh diameter of the sieve the aforementioned range, it becomes easy to efficiently perform wet jet mill treatment. If the mesh diameter is less than 25 μm, time will be consumed in the classification process. It should be noted that classification can be performed in a dry manner before washing and drying, or in a wet manner before drying after washing, or in a dry manner after washing and drying, but since classification can sometimes be easily performed by removing impurities by washing, it is preferably performed before drying after washing, or after washing and drying.

[0112] Regarding the raw material boron nitride powder, it is manufactured by utilizing the melamine method to obtain a boron nitride powder with a relatively consistent long diameter and thickness. In the melamine method, the reaction temperature (boron nitride generation temperature) is as low as 500 to 1200°C, so it is estimated that a boron nitride powder with a relatively consistent long diameter and thickness can be obtained. On the other hand, in the reduction nitridation method, the reaction temperature is a high temperature of more than 1400°C, so the generation of boron nitride and crystal growth are carried out simultaneously, and it is estimated that it is not easy to obtain a raw material boron nitride powder with a consistent long diameter and thickness. When the long diameter and thickness of the raw material boron nitride are consistent, the long diameter and thickness of the boron nitride powder (seed (S)) obtained by processing with a wet jet mill described later are also easy to become more consistent, so the raw material boron nitride powder is preferably manufactured based on the melamine method.

[0113] <Manufacturing of raw material boron nitride powder by reduction nitridation method>

[0114] The reduction nitridation method is a method in which a raw material mixture (R) containing an oxygen-containing boron compound, an oxygen-containing alkaline earth metal compound, and a carbon source is heated under a nitrogen atmosphere to obtain a raw material boron nitride powder.

[0115] <Oxygen-containing boron compounds>

[0116] Examples of the oxygen-containing boron compound include diboron trioxide (boron oxide), diboron dioxide, tetraboron trioxide, tetraboron pentoxide, borax, or anhydrous borax. Among them, diboron trioxide (B 2 O 3 ). Boron trioxide is used as the boron compound, which is industrially beneficial because it uses an inexpensive raw material. It should be noted that two or more boron compounds may be used in combination.

[0117] <Oxygen-containing alkaline earth metal compounds>

[0118] As oxygen-containing alkaline earth metal compounds, oxides or carbonates of alkaline earth metals such as calcium and magnesium can be listed. Specifically, magnesium oxide, calcium oxide, magnesium carbonate, calcium carbonate, magnesium bicarbonate, calcium bicarbonate, magnesium hydroxide, calcium hydroxide, magnesium nitrate, calcium nitrate, magnesium sulfate, calcium sulfate, magnesium phosphate, calcium phosphate, magnesium oxalate, calcium oxalate, etc. can be used. By using carbonates such as magnesium carbonate and calcium carbonate as oxygen-containing alkaline earth metal compounds, carbon dioxide gas is generated in the heating process to generate pores inside the mixed raw material layer, nitrogen gas becomes easy to penetrate into the mixed raw material layer, and the reduction nitridation reaction is easy to efficiently advance. It should be noted that as oxygen-containing alkaline earth metal compounds, two or more types can be used in combination.

[0119] <Carbon source>

[0120] As the carbon source, in addition to amorphous carbon such as carbon black, activated carbon, and carbon fiber, crystalline carbon such as diamond, graphite, and nanocarbon, and pyrolytic carbon obtained by pyrolyzing a monomer or a polymer can be used. Inexpensive carbon black is generally used.

[0121] <Composition ratio of the raw material mixture (R) in the reduction nitridation step>

[0122] The atomic ratio (B / C ratio) of the boron atom (B) of the oxygen-containing boron compound to the carbon atom (C) of the carbon source in the raw material mixture (R) in the reduction nitridation method for producing the raw material boron nitride powder is preferably 0.70 to 2.00, more preferably 0.75 to 1.95. If the B / C ratio is less than the above range, unreacted carbon will remain in the raw material boron nitride powder in the form of black foreign matter, which is not preferred. If the B / C ratio is greater than the above range, unreacted B 2 O 3 If the ratio becomes excessive, the yield of boron nitride relative to the raw material filling amount will be significantly reduced, and the productivity will be reduced.

[0123] The content of the oxygen-containing alkaline earth metal compound in the raw material mixture is the molar ratio of the oxygen-containing alkaline earth metal compound (AO; A is an alkaline earth metal) to the oxygen-containing boron compound in terms of oxide (AO / B 2 O 3 The oxygen-containing alkaline earth metal compound acts as a grain growth promoter for the boron nitride particles. 2 O 3 By blending the oxygen-containing alkaline earth metal compound in such a ratio as to fall within the above range, a raw material boron nitride powder having a graphitization index of 1.7 or less can be obtained.

[0124] <Heating process>

[0125] The reduction nitridation method is a method of heating the raw material mixture (R) under a nitrogen gas flow. Boron oxide (B 2 O 3 ) or after heating and cracking, it will become boron oxide (B 2 O 3 The reaction when boron nitride powder (BN) is generated by heating an oxygen-containing boron compound and carbon (C) or thermal cracked carbon that becomes carbon (C) by heating is shown in the following formula (1).

[0126] B 2 O 3 +3C+N 2 →2BN+3CO (1)

[0127] The reaction starts at about 1400°C or above. The reaction temperature is preferably 1400-1600°C, more preferably 1450-1580°C. If the reaction temperature is low, the reaction time becomes long, and if the reaction temperature is high, the major diameter and thickness of the raw material boron nitride powder are not easy to become uniform. The holding time is preferably 1-10 hours, more preferably 2-8 hours. If the holding time is short, the major diameter and thickness of the raw material boron nitride powder are not easy to become uniform.

[0128] After the reaction, the heating temperature is raised to 1620-2100°C. As the temperature rises, the crystallization of the boron nitride particles advances, the major axis and thickness increase, and the graphitization index decreases. The maximum temperature is more preferably 1700-2000°C, and further preferably 1750-1900°C. If the reaction temperature is low, a raw material boron nitride powder with a graphitization index of less than 1.7 cannot be obtained. If the reaction temperature is high, it will exceed the preferred size of the raw material boron nitride powder and grow excessively, and the processing time in the wet jet mill process needs to be extended. The holding time of the maximum temperature is preferably 0.5-7 hours, and more preferably 1-4 hours. If the holding time is short, the major axis and thickness of the raw material boron nitride powder are not easy to become uniform. If the holding time is long, the productivity decreases.

[0129] Nitrogen is necessary as a nitrogen source in the reduction nitridation reaction, and is preferably supplied by circulating in the heating furnace. The flow path of the nitrogen gas can be designed in such a way that the raw material mixture arranged in the heating furnace is in contact with the circulating nitrogen gas (for example, circulating in the upper space of the raw material mixture layer). Regarding the flow rate of nitrogen gas, it is preferably 0.1 to 20 L / min, more preferably 0.2 to 15 L / min, and further preferably 0.3 to 10 L / min per 1 kg of the mixed raw material. If there is too little nitrogen, the reduction nitridation reaction will not be completed, and unreacted carbon will remain in the reaction product in the form of black foreign matter, which is not preferred. If there is too much nitrogen, the thermal efficiency will decrease, which is not preferred.

[0130] The raw material mixture (R) may be filled into a carbon container, a carbon container coated with boron nitride, a boron nitride sintered body container, etc. and placed in a heating furnace. The shape of the container is preferably a shape that does not prevent the raw material mixture (R) from contacting with the circulating nitrogen gas.

[0131] The raw material mixture (R) is preferably filled into the aforementioned container at a height of 1 to 20 cm. If the filling layer is low, the productivity decreases, and if the filling layer is too high, the reaction of the raw material mixture (R) at the bottom of the container will not proceed, and unreacted carbon will remain, which is not preferred. The height of the filling layer of the raw material mixture (R) is more preferably 2 to 15 cm, and further preferably 3 to 10 cm.

[0132] <Crushing process, cleaning process, drying process and classification process>

[0133] The conditions and means described in the section of the melamine method can be used as is for the crushing method, washing method, drying method and classification method in the reduction nitridation method for producing the raw material boron nitride powder.

[0134] <Production of Seed Crystal (S)>

[0135] Next, the raw material boron nitride powder obtained by the melamine method or the reduction nitridation method is cracked and preferably further pulverized to produce seed crystals (S). In the present invention, it is important to treat the raw material boron nitride powder with a wet jet mill.

[0136] Wet jet mills are more likely to break particles than dry jet mills, so (T90-T10) / T50 becomes smaller, and the thickness distribution can be sharpened. Furthermore, in wet jet mill treatment, if the slurry concentration is set to 20 to 100 g / L to simultaneously produce particle crushing, (L90-L10) / L50 will also become smaller, and the particle size distribution can also be sharpened.

[0137] Regarding the treatment of the wet jet mill, there is no particular limitation as long as the slurry containing the above-mentioned raw material boron nitride powder and the solvent can be treated. It is preferred to adopt conditions that can efficiently crack the particles and easily make (T90-T10) / T50 less than 1.6. Specifically, it is preferred to use pure water, ethanol, isopropanol, N-methylpyrrolidone, N,N-dimethylformamide, polydimethylsiloxane, etc., or those with surfactants added thereto as solvents, so that the slurry concentration is 20 to 100 g / L, the pressure is 100 to 300 MPa, and the slurry supply rate is 0.2 to 1.0 L / min. It should be noted that in the embodiment, Star Burst made by SUGINOMACHINE LIMITED is used, and the nozzle uses an oblique collision chamber, but it is not limited to this device, and a known wet jet mill device that adopts the same pulverization method and can obtain the effect of the present invention can be applied without restriction. When the slurry concentration is low, the collision frequency of particles decreases, and the pulverization effect decreases. Therefore, in order to efficiently make (L90-L10) / L50 less than 2.0, the slurry concentration is preferably 20 g / L or more, and more preferably 40 g / L or more. If the slurry concentration is too high, the high viscosity and efficient wet jet mill treatment sometimes become difficult. Therefore, the slurry concentration is preferably 100 g / L or less, and more preferably 90 g / L or less. In addition, the number of passes in the wet jet mill treatment is not particularly limited, and it can be carried out until the specific surface area reaches the desired value.

[0138] After the wet jet mill treatment, the solvent is removed from the slurry by filtering / drying, etc., so that seed crystals (S) can be obtained. It should be noted that the slurry can be filtered as needed, washed with pure water, and the solvent and surfactant used in the crushing can be removed, and then dried. In addition, before the cleaning based on pure water, the solvent, surfactant, metal impurities, etc. used in the treatment can be removed by cleaning with an organic solvent, acid, etc.

[0139] After the wet jet mill treatment, classification can also be performed. By performing classification, it becomes easy to adjust (L90-L10) / L50 and (T90-T10) / T50 to less than 2.0. The classification method is not particularly limited. From the viewpoint of continuously performing after pulverization by a wet jet mill, wet classification is preferred. As long as the coarse particles of the seed crystal (S) can be removed by classification, it becomes easy to obtain a boron nitride powder with small (L90-L10) / L50 and (T90-T10) / T50.

[0140] <Manufacturing of hexagonal boron nitride powder>

[0141] In the present invention, a raw material mixture (S) including an oxygen-containing boron compound, an oxygen-containing alkaline earth metal compound, a carbon source and a seed crystal (S) is heated in a nitrogen atmosphere to produce hexagonal boron nitride powder by a reduction nitridation method.

[0142] <Raw material mixture (S)>

[0143] As the oxygen-containing boron compound, oxygen-containing alkaline earth metal compound and carbon source used as the reaction raw materials, the compounds described in the section of the production method of the raw material boron nitride powder by the reduction nitridation method can be used without limitation.

[0144] <Composition ratio of raw material mixture (S) in reduction nitridation method>

[0145] In the reduction nitridation method, although the reaction proceeds as shown in formula (1), the seed crystal (S) present only participates in the control of the length and thickness of the boron nitride powder to be generated, and does not participate in the reduction nitridation (stoichiometric) reaction itself. Therefore, the atomic ratio (B / C ratio) of the boron atom (B) of the oxygen-containing boron compound to the carbon atom (C) of the carbon source, and the molar ratio (AO / B ratio) of the oxygen-containing alkaline earth metal compound (AO; A is an alkaline earth metal) to the oxygen-containing boron compound in terms of oxide conversion are determined. 2 O 3 The quantitative ratio described in the item of the method for producing the raw material boron nitride powder can be used as it is.

[0146] By mixing the carbon source in such a way that the B / C ratio is within the above range, a boron nitride powder having a uniform length and thickness can be obtained. If the carbon source is too little, the length and thickness are not easy to be consistent. If the carbon source is too much, unreacted carbon will remain in the boron nitride powder in the form of black foreign matter, which is not preferred. 2 O 3 By blending the oxygen-containing alkaline earth metal compound in such a ratio as to fall within the above range, a boron nitride powder having a desired major axis and thickness, good sliding properties, little roughness, and excellent glossiness can be obtained.

[0147] The amount of the seed crystal (S) is based on the boron atoms (B S ) to the carbon atom (C) of the carbon source (B S The ratio of B / C is preferably in the range of 0.01 to 13, more preferably in the range of 0.1 to 10, and still more preferably in the range of 0.5 to 8. S By mixing the seed crystal (S) so that the ratio of A to C falls within the above range, a boron nitride powder having a uniform major axis and thickness can be obtained. If the seed crystal (S) is too little, the effect as a seed crystal cannot be obtained, and if the seed crystal (S) is too much, it becomes disadvantageous in terms of productivity.

[0148] <Heating process>

[0149] In the reduction nitridation method, the reaction is carried out according to the above formula (1). The reaction starts at about 1400°C or above. The reaction temperature is preferably 1400-1600°C, more preferably 1450-1580°C. If the reaction temperature is low, the reaction time becomes long, and if the reaction temperature is high, the major axis and thickness of the boron nitride powder are not easy to become uniform. The holding time is preferably 1-10 hours, more preferably 2-8 hours. If the holding time is short, the major axis and thickness of the boron nitride powder are not easy to become uniform.

[0150] After the reaction, the heating temperature is raised to 1700-2100°C. As the temperature rises, the crystallization of the boron nitride particles advances, and the major axis and thickness become larger. The maximum temperature is more preferably 1730-2000°C, and further preferably 1750-1950°C. If the reaction temperature is low, the boron nitride powder will not grow to a size preferred as a cosmetic. If the reaction temperature is high, it will grow excessively beyond the size preferred as a cosmetic. The holding time of the maximum temperature is preferably 0.5-7 hours, and more preferably 1-4 hours. If the holding time is short, the major axis and thickness of the boron nitride powder are not easy to become uniform. If the holding time is long, the productivity decreases.

[0151] <Nitrogen usage conditions, reaction vessel, and raw material filling method>

[0152] In the present reduction nitriding method, the nitrogen use conditions, the reaction container, and the method of filling the raw material can adopt the conditions and means described in the section of the reduction nitriding method of the raw material boron nitride powder as they are.

[0153] <Crushing process>

[0154] In order to reduce the aggregated particles in the reaction product obtained in the reduction nitridation step, it is preferable to crush the particles. The crushing method can directly adopt the conditions and means described in the section of the method for producing the raw material boron nitride powder.

[0155] <Grading process>

[0156] In order to reduce the coarse particles in the reaction product obtained in the reduction nitridation step, it is preferred to perform classification. The classification method can directly adopt the conditions and means described in the item of the method for preparing the raw material boron nitride powder. It should be noted that the reason why the mesh size is preferably in the above range is that it becomes easy to adjust the MMD of the hexagonal boron nitride powder to a lower level.

[0157] <Cleaning process>

[0158] The reaction product obtained in the reduction nitridation step contains unreacted raw materials (B 2 O 3, CaO) and other impurities other than hexagonal boron nitride, so by using acid cleaning to remove impurities, etc., it is possible to obtain a high-purity hexagonal boron nitride powder suitable for cosmetic use. The cleaning method can directly adopt the conditions and means described in the item of the method for preparing the raw material boron nitride powder.

[0159] It should be noted that when hexagonal boron nitride powder is used in cosmetics, it is expected to comply with the Quasi-drug Raw Material Standards 2021, which sets standards such as purity of 95% or more, pH 5.0-8.0, and eluted boron amount of 20 ppm or less. Therefore, it is necessary to wash in a manner that satisfies these standards.

[0160] <Drying process>

[0161] The drying method can directly adopt the conditions and means described in the item of the method for preparing the raw material boron nitride powder. However, in the drying process, the boron nitride powder is hydrolyzed, and the amount of dissolved boron sometimes exceeds 20ppm. Therefore, as a drying method for the boron nitride powder in the manufacture of hexagonal boron nitride powder, vacuum drying that can suppress hydrolysis is preferred.

[0162] Example

[0163] The present invention will be described in detail below by way of examples, but the present invention is not limited to these examples. In addition, the combination of features described in the examples is not necessarily all necessary for the solution of the present invention.

[0164] In the following examples, the boron nitride powder before the jet mill treatment is recorded as the raw material boron nitride powder (or raw material h-BN powder), the boron nitride powder after the jet mill treatment is recorded as the seed crystal, the boron nitride powder obtained in the reduction nitridation step using the seed crystal is recorded as the nitrided powder, and the boron nitride powder after washing / drying is recorded as the hexagonal boron nitride powder (or h-BN powder). In addition, the powder for the seed crystal is marked as (S) as needed.

[0165] The raw material h-BN powder is prepared according to the melamine method or the reduction nitridation method.

[0166] <Preparation of raw material h-BN powder (M1) by melamine method>

[0167] Boron oxide (B 2 O 3 ) 30 g and 50 g of melamine as an organic compound containing nitrogen were mixed in a ball mill to prepare a raw material mixture (S). In the prepared raw material mixture (S), B / N was 0.36.

[0168] The prepared raw material mixture (S) was subjected to a batch sintering furnace, and in the heating process, the temperature was raised at 15°C / min under nitrogen flow, and heated at a temperature of 1800°C for 6 hours to prepare a nitrided powder (M1). The prepared nitrided powder (M1) was crushed with a mortar crusher, and then acid-washed with a 5% hydrochloric acid aqueous solution, and then filtered, washed with water and dried, and then further classified using a vibrating screen with an aperture of 45 μm to obtain a raw material h-BN powder (M1).

[0169] <Preparation of raw material h-BN powder (M2) by melamine method>

[0170] A raw material h-BN powder (M2) was produced in the same manner as in the production of the raw material h-BN powder M1 except that the heating temperature and the heating time were changed as shown in Table 1.

[0171] <Preparation of raw material h-BN powder (M3) by melamine method>

[0172] A raw material h-BN powder (M3) was produced in the same manner as in the production of the raw material h-BN powder M1 except that the heating temperature and the heating time were changed as shown in Table 1.

[0173] <Preparation of raw material h-BN powder (M4) by melamine method>

[0174] A raw material h-BN powder (M4) was produced in the same manner as in the production of the raw material h-BN powder M2, except that classification using a vibrating screen having an aperture of 45 μm was not performed.

[0175] <Preparation of raw material h-BN powder (R1) by reduction nitridation method>

[0176] Boron oxide (B 2 O 3 ) 70g, carbon black 30g, and calcium carbonate 10g are mixed in a ball mill. The mixture is heated to 1500°C at 15°C / min in a nitrogen atmosphere using a graphite Tamm furnace, and maintained at 1500°C for 6 hours. After maintaining at 1500°C, the temperature is increased to 1750°C at 15°C / min, and maintained at 1750°C for 2 hours to prepare a nitrided powder (R1). The prepared nitrided powder (R1) is crushed with a mortar crusher, acid-washed with a 5% hydrochloric acid aqueous solution, and then filtered, washed with water and dried, and then further classified using a vibrating screen with an aperture of 45μm to obtain a raw material h-BN powder (R1).

[0177] <Graphitization Index>

[0178] The raw material h-BN powder was pressed at 10 tons to obtain The h-BN pellets of about 1000 Å were used as test pieces, and their X-ray diffraction spectra were measured using an X-ray diffraction device (D2 PHASER, BRUKER). The X-ray diffraction spectra were analyzed to calculate the graphitization index.

[0179] The analysis of the X-ray diffraction spectrum was performed by using the analysis software attached to the X-ray diffraction device to obtain the peak areas of the (100), (101), and (102) planes of h-BN. The peaks appearing near 2θ=41.5°, 44°, and 50° were regarded as the peaks corresponding to the (100), (101), and (102) planes, respectively.

[0180] The graphitization index is calculated according to the following formula: Wherein, Area (10X) represents the peak area of ​​the (10X) plane.

[0181] Graphitization index

[0182] =(Area(100)+Area(101)) / Area(102) Formula (2)

[0183] It should be noted that, when the crystallinity of h-BN is too low, there are cases where the peaks of (100) and (101) overlap, and there is no peak of (102). In the former case, if (100) and (101) are analyzed as one broad peak, and the obtained peak area is used for the numerator of formula (2), the graphitization index can be calculated (usually a graphitization index exceeding 1.7). In the latter case, the graphitization index cannot be calculated, and therefore, it is considered that the graphitization index exceeds 1.7.

[0184] <Specific surface area>

[0185] The specific surface area was determined by the BET method (nitrogen adsorption single point method) using a specific surface area measuring apparatus (Flowsorb 2-2300, manufactured by Shimadzu Corporation).

[0186] <Average major diameter, average thickness, aspect ratio>

[0187] The h-BN powder was treated with an ultrasonic homogenizer to break up the aggregated particles and make them monodisperse, and then dried, and the obtained material was used for the measurement sample. Specifically, 2 g of h-BN powder was mixed with 25 mL of ion exchange water to make a slurry, and then ultrasonically treated with an ultrasonic homogenizer made by BRANSON: SONIFIRE (model SFX250, chip: 20kHz microchip 1 / 4 inch) at an amplitude of 40% and a treatment time of 20 minutes, and then filtered and dried.

[0188] Next, 1 g of h-BN powder was added to 9 g of epoxy resin (EA E-30CL manufactured by Henkel), stirred and degassed using Mazerustar manufactured by KURABO, and poured into a 10 mm square, 1 mm thick mold frame, and heated and cured at a temperature of 70° C. After cooling, the cured resin composition was pulled out of the mold frame, and a cross-section milling process was performed on one side thereof, and SEM images with a magnification of 1000 were taken in multiple fields of view.

[0189] Then, the obtained SEM image was analyzed using an image analyzer (Asahi Kasei Engineering Corporation: A-image) to measure the major axis and thickness of the h-BN particles. The analysis mode of A-image was set to needle-shaped analysis. Ignoring particles that were difficult to accurately measure due to the overlap of multiple particles, all particles contained in the SEM image of one field of view were measured, and the same was repeated for multiple fields of view and measured, thereby measuring the major axis and thickness of more than 1,000 particles.

[0190] Next, the area-based L50, T50, etc. are analyzed using spreadsheet software (Microsoft: Excel). The planar shape of the h-BN particles is regarded as a circle, and the major axis is further regarded as the diameter of the circle, and the area of ​​each h-BN particle (the amount of a single surface in the two planes) is calculated. When the major axis and thickness are sorted from the smallest, the values ​​at which the area of ​​the h-BN powder accumulates to 50% are respectively used as the average major axis (L50) and average thickness (T50) of the h-BN powder. In addition, the value obtained by dividing the average major axis by the average thickness is used as the aspect ratio (average major axis (L50) / average thickness (T50)).

[0191] In addition, (L90-L10) / L50 was calculated using the area-based cumulative 10% value (L10), cumulative 50% value (L50), and cumulative 90% value (L90) when the major diameters of the h-BN powders were sorted from the smallest. Similarly, (T90-T10) / T50 was calculated using the area-based cumulative 10% value (T10), cumulative 50% value (T50), and cumulative 90% value (T90) of the boron nitride particles when the thickness of the raw material h-BN powders was sorted from the smallest.

[0192] <MIU and MMD>

[0193] MIU (friction coefficient) and MMD (variation value of friction coefficient) are dimensionless numbers measured by a friction feel measuring instrument (manufactured by KATO TECH CO., LTD., trade name: KES-SE). Specifically, h-BN powder was placed on artificial leather (manufactured by Idemitsu Technofine Co., Ltd., trade name: SUPPLALE PBZ13001 BK) which was regarded as skin, and the concentration of h-BN powder was 0.5 mg / cm 2 The MIU and MMD can be measured by extending the sample in a thin layer in a manner of , and contacting the sensor part of the friction meter (10 mm square silicon) on it. The measurement conditions of the friction meter are set as sensitivity: H, test bench moving speed: 1 mm / sec, and static load: 25 gf. The measurement is performed once. Repeat the sample preparation (coating and extending the raw material h-BN powder on the artificial leather) and the measurement with the friction meter 5 times, and the average value of the 5 measurement results is taken as the MIU and MMD of the h-BN powder.

[0194] <Specular reflection intensity>

[0195] Double-sided tape was pasted on black matte velvet thick paper, and h-BN powder was seamlessly attached to the double-sided tape using a makeup brush. Excess powder was then gently blown off with an air dust collector. The test piece was used as a test piece. When the reflected light intensity from -90° to +90° relative to incident light at -60° was measured using a goniophotometer (Murakami Color Laboratory Co., Ltd., trade name GP-200), the intensity of the reflected light peak that appeared near +60° was used as the mirror reflection intensity.

[0196] The production methods, production conditions and measurement results of the raw material h-BN powders (M1) to (M4) and (R1) are shown in Table 1. Since the particles of the raw material h-BN powder (M3) were too small, the distribution of the major axis and thickness could not be measured.

[0197] [Table 1]

[0198]

[0199] <Example 1>

[0200] <Preparation of seed crystal>

[0201] 65 g of the obtained raw material boron nitride powder (M1) was mixed with 1 L of N,N-dimethylformamide, and stirred thoroughly to form a slurry, and the slurry was treated with a wet jet mill device (manufactured by SUGINO MACHINE LIMITED: Star Burst). The treatment conditions were set as nozzle: oblique collision chamber, pressure: 200 MPa, slurry supply rate 0.5 L / min, and number of passes 5 times. The slurry after the wet jet mill treatment was filtered out by suction, washed with pure water, filtered out by suction, and then vacuum dried at 200°C to obtain seed crystals (S) (M1).

[0202] <Raw material mixture>

[0203] Boron oxide (B 2 O 3 ) 50g, calcium carbonate (CaCO 3 )8g, 24g of carbon black (C) as a carbon source and 40g of seed crystals (S) (M1) were mixed in a ball mill to obtain a raw material mixture (S). In the prepared raw material mixture, B / C (atomic ratio) was 0.72, CaO / B 2 O 3 (molar ratio) is 0.11, B s / C (atomic ratio) is 0.81.

[0204] <Reduction nitriding process>

[0205] The prepared raw material mixture (S) was heated at 1870° C. for 2 hours in a nitrogen flow using a batch type sintering furnace to produce a nitrided powder (S).

[0206] <Purification process>

[0207] The prepared nitrided powder (S) was acid-cleaned with a 5% hydrochloric acid aqueous solution, filtered out, washed with water, and then vacuum-dried at 200° C. to obtain h-BN powder (M1).

[0208] <Grading process>

[0209] The obtained h-BN powder was classified using a vibrating sieve with a pore size of 45 μm.

[0210] <Various measurements>

[0211] The h-BN powder after classification was measured in the same manner as the raw material h-BN for the measurement items shown in Tables 3 to 5. The ratio of coarse particles exceeding 2.5 times the average major diameter (L50) was determined according to the following formula.

[0212] Ratio of coarse particles exceeding 2.5 times the average major diameter (L50) (area %)

[0213] = 100 - (the cumulative value of the area basis corresponding to the value of L50 multiplied by 2.5)

[0214] <Sensory Evaluation>

[0215] The obtained h-BN powder (M1) was mixed with the following cosmetic ingredients to prepare cosmetics (powdered foundation). The prepared cosmetics were used by 20 panelists specializing in cosmetic evaluation and were evaluated for their slip, roughness, moistness, and glossiness. The case where less than 30% of the evaluators felt good was marked as ×, the case where more than 30% and less than 60% was marked as △, the case where more than 60% and less than 80% was marked as ○, and the case where more than 80% was marked as ◎.

[0216] Powder foundation ingredients and blending amounts (mass %)

[0217] Hexagonal boron nitride powder (h-BN powder) 20.0

[0218] ·Mica 15.0

[0219] Synthetic Phlogopite 12.0

[0220] ·Ethylhexyl methoxycinnamate 8.0

[0221] ·(Vinyl Dimethicone / Methicone Silsesquioxane) Crosspolymer 8.0

[0222] (Diphenyl Dimethicone / Vinyl Diphenyl Dimethicone / Silsesquioxane) Crosspolymer 8.0

[0223] Nylon 12, 3.0

[0224] ·Silica 3.0

[0225] Talc 3.0

[0226] ·Acrylic acid cross-linked polymer 3.0

[0227] ·Perfluorooctyltriethoxysilane 3.0

[0228] Zinc oxide 3.0

[0229] Polymethacrylate polymer 3.0

[0230] Silicone treated red iron oxide (iron red) 1.0

[0231] Silicone treated yellow iron oxide 0.6

[0232] Silicone treated black iron oxide 0.4

[0233] Silicone treated titanium oxide 6.0

[0234] <Examples 2 to 11, Comparative Examples 1 to 5>

[0235] The type of raw material h-BN powder, the treatment method of the jet mill, the slurry concentration, the number of passes, the B / C atomic ratio of the raw material mixture and the CaO / B 2 O 3 Molar ratio, B s / C atomic ratio and calcination temperature, boron nitride powders of Examples 2 to 11 and Comparative Examples 1 to 5 were prepared. In addition, using the boron nitride powders, cosmetics were prepared in the same manner as in Example 1. The production conditions and evaluation results of each boron nitride are shown in Tables 2 to 4. It should be noted that Comparative Example 5 is an example in which a seed crystal is not used for production.

[0236] [Table 2]

[0237]

[0238] [Table 3]

[0239]

[0240] [Table 4]

[0241]

[0242] As shown in Tables 2 to 4, by using the hexagonal boron nitride powder of the present invention in cosmetics, high evaluations were obtained in terms of slip, roughness, moist feeling, and glossiness.

[0243] Comparative Example 1 is an example in which the specific surface area of ​​the seed crystal was reduced, and the glossiness was extremely poor.

[0244] Comparative Example 2 is an example in which the raw material boron nitride was processed by a dry jet mill, and the glossiness was poor.

[0245] Comparative Example 3 is an example in which the raw material boron nitride was not subjected to a pulverization treatment such as a jet mill, and the moist feeling and glossiness were extremely poor.

[0246] Comparative Example 4 is an example using a raw material h-BN powder (M3) produced under low heating temperature conditions in the melamine process. (L90-L10) / L50, (T90-T10) / T50 and average aspect ratio are not satisfied, and the moist feeling and glossiness become extremely poor.

[0247] Comparative Example 5 is a case where a boron nitride powder obtained by a reduction nitridation method without the presence of seed crystals was used. All physical properties were poor and a satisfactory powder foundation was not obtained.

[0248] Description of Reference Numerals

[0249] 1 Hexagonal Boron Nitride Powder

[0250] 3 Incident light

[0251] 5. Reflected Light

Claims

1. A hexagonal boron nitride powder, The average major diameter (L50) is 3 to 20 μm, the average thickness (T50) is 0.3 to 2 μm, (L90-L10) / L50 is less than 2.0, (T90-T10) / T50 is less than 2.0, and the average aspect ratio is 10 to 30. The dynamic friction coefficient (MIU) is less than 0.50, and the variation value of the dynamic friction coefficient (MMD) is less than 0.0050. The specular reflection intensity measured by a goniophotometer under the condition of an incident light angle of 60° is 80 or more.

2. The hexagonal boron nitride powder according to claim 1, wherein (L90-L10) / L50 is 1.8 or less. The hexagonal boron nitride powder according to claim 1 , which is used in cosmetics.

4. A cosmetic comprising the hexagonal boron nitride powder according to claim 1.

5. A method for producing hexagonal boron nitride powder, comprising a reduction nitridation step of heating a raw material mixture under a nitrogen atmosphere, wherein: The raw material mixture comprises: an oxygen-containing boron compound, an oxygen-containing alkaline earth metal compound, a carbon source and a seed crystal, The seed crystal is a boron nitride powder obtained by treating a raw material boron nitride powder having a graphitization index of less than 1.7 using a wet jet mill. The specific surface area of ​​the seed crystal is 10 m 2 / g or above.

6. The method for producing hexagonal boron nitride powder according to claim 5, wherein: The slurry concentration during the treatment with a wet jet mill is 20 to 100 g / L.

7. The method for producing hexagonal boron nitride powder according to claim 5, wherein: The atomic ratio (B / C ratio) of the boron atoms (B) of the oxygen-containing boron compound to the carbon atoms (C) of the carbon source in the raw material mixture is 0.70 to 2.00, The molar ratio of the oxygen-containing alkaline earth metal compound (AO; A is an alkaline earth metal) to the oxygen-containing boron compound (B2O3) (AO / B2O3 ratio) is 0.01 to 1.0 in terms of oxide conversion, The boron atoms (B s ) to the carbon atoms (C) of the carbon source (B s / C ratio) is 0.01~13.

8. The method for producing hexagonal boron nitride powder according to claim 5, wherein: In the reduction nitridation step, heating is performed at 1700 to 2100°C.

Citation Information

Cited By

  • High-strength and high-deformability hexagonal boron nitride ceramic and preparation method thereof

    CN118771892A

  • High-strength high-deformation hexagonal boron nitride ceramic and method for preparing the same

    CN118771892B

  • A low-irritation hexagonal boron nitride powder suitable for sensitive skin cosmetics, and a preparation method and application thereof

    CN121823492A