Solar cell and photovoltaic module

By using a composite passivation structure of boron passivation layer, SiOx/SiNx stacked dielectric layer and aluminum backfield in crystalline silicon solar cells, the carrier recombination and cell warping caused by aluminum backfield passivation structure are solved. Problem, improving the photoelectric conversion efficiency and being suitable for industrial production.

CN118919579AInactive Publication Date: 2024-11-08DAS SOLAR CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411405739.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The aluminum back-field passivation structure in existing crystalline silicon solar cells is directly in contact with Si, resulting in serious carrier recombination and high saturation leakage current, which limits the improvement of photoelectric conversion efficiency, and the increase in the thickness of the aluminum layer can easily lead to The battery cell warps and the yield decreases.

Method used

The composite passivation layer structure of P-type silicon substrate is adopted, including the boron passivation layer prepared by low-pressure chemical vapor deposition, the SiOx/SiNx stacked dielectric layer and the aluminum backfield. The built-in field and SiOx/SiNx medium are formed through the boron passivation layer. The layer reduces the carrier recombination rate and increases light reflection. The aluminum backfield realizes local electrical contact through the opening window to avoid the formation of a high composite layer of Al-Si alloy.

Benefits of technology

It effectively reduces the carrier recombination rate, improves the photoelectric conversion efficiency, avoids cell warping, and has low process temperature, which is not easy to cause lattice distortion, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919579A_ABST
    Figure CN118919579A_ABST
Patent Text Reader

Abstract

The invention discloses a solar cell and a photovoltaic module, and relates to the field of photovoltaic technology, the solar cell comprises a P-type silicon substrate, the P-type silicon substrate comprises a front surface and a back surface, the front surface of the P-type silicon substrate is sequentially provided with an N-type doped layer, the N-type doped layer is covered with an antireflection film, the antireflection film is provided with a positive electrode, and the back surface of the P-type silicon substrate is provided with a negative electrode. A composite passivation layer is arranged on the back surface of the P-type silicon substrate and sequentially comprises a boron passivation layer, a SiOx / SiNx laminated dielectric layer and an aluminum back surface field from top to bottom, a back electrode is arranged on the aluminum back surface field, and the boron passivation layer is a boron-doped microcrystalline silicon film prepared in a low-pressure chemical vapor deposition mode. According to the composite passivation layer cell, the recombination rate of carriers on the back surface is greatly reduced, and then the photoelectric conversion efficiency is improved. Meanwhile, the boron passivation layer prepared by adopting the low-pressure chemical vapor deposition method is stable in chemical property, smooth and flat in surface and uniform in grain size.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photovoltaic technology, and in particular relates to a solar cell and a photovoltaic module. Background Art

[0002] Photovoltaic power generation, as a green and renewable energy form, has become an important means to promote the transformation of energy structure and achieve sustainable development. With the continuous innovation of technology and the further reduction of costs, the role of photovoltaic power generation in the global energy system will become increasingly important. Crystalline silicon solar cells are the mainstream products in the photovoltaic industry, and the photoelectric conversion efficiency is its most important performance indicator. Back passivation technology is one of the important means to improve the photoelectric conversion efficiency of crystalline silicon solar cells.

[0003] For P-type silicon, if the surface passivation film contains a certain amount of fixed negative charge, the electric field induced by the negative charge forms a Coulomb repulsion force on the electrons in the semiconductor, and a Coulomb attraction force on the holes. Then, the semiconductor surface is in an accumulation state under the action of the fixed negative charge, and the surface electron concentration is small, thereby reducing the surface recombination rate. This field effect passivation achieves a good surface passivation effect. Another way to achieve field effect passivation is to form a surface junction (high-low junction or pn junction) by doping. The presence of the space charge region causes the carriers (electrons and holes) to be separated due to the opposite Coulomb force, reducing the surface carrier concentration, thereby reducing the surface recombination rate and achieving a back passivation effect. At present, aluminum back field is widely used as a back passivation method in P-type crystalline silicon solar cells. Aluminum back field can effectively reduce the activity of the back surface of the battery, reduce the surface recombination rate, and improve the photoelectric conversion efficiency. It is the main back surface passivation structure commonly used in commercial crystalline silicon solar cells. The aluminum back field technology has a simple production method and low cost, but the single aluminum back field passivation structure has a high saturation leakage current due to the direct contact of the back metal electrode with Si, the back is fully metal composite, and the carrier recombination is serious, which limits the improvement of the conversion efficiency of crystalline silicon solar cells. In addition, to improve the passivation effect of the aluminum back field, the thickness of the aluminum layer can be increased, but due to the different thermal expansion coefficients of aluminum and silicon, when the thickness of the aluminum layer increases to a certain extent, after high-temperature sintering, the battery cell is prone to warping and deformation, resulting in a decrease in the product yield.

[0004] In view of this, it is necessary to propose a solar cell and a photovoltaic module to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to provide a solar cell to solve the above technical problems existing in the prior art.

[0006] To achieve the above object, the present invention provides the following solutions: A solar cell and a photovoltaic module, comprising a P-type silicon substrate, the P-type silicon substrate having a front surface and a back surface, an N-type doped layer prepared on the front surface of the P-type silicon substrate, an anti-reflection film covered on the N-type doped layer, a positive electrode provided on the anti-reflection film, and a composite passivation layer provided on the back surface of the P-type silicon substrate, which comprises a boron passivation layer, a SiOx / SiNx laminated dielectric layer and an aluminum back field from top to bottom, and a back electrode provided on the aluminum back field. The boron passivation layer is a boron-doped microcrystalline silicon film prepared by low-pressure chemical vapor deposition (LPCVD). The boron-doped microcrystalline silicon film prepared by LPCVD has a smooth surface, fine and uniform grains, and the LPCVD preparation method has a low process temperature, is not easy to cause oxygen deposition inside the silicon wafer, and is not easy to cause lattice distortion.

[0007] Furthermore, the thickness of the boron passivation layer is 100-500 nm, and the boron doping concentration is 10 18 The boron passivation layer makes the boron concentration on the back surface of the battery higher, thus forming a negative charge-rich area on the surface, and the silicon wafer surface presents negative electrical properties. Due to the existence of the boron atom concentration gradient, a built-in field pointing from the inside of the silicon wafer to the surface of the silicon wafer is formed. The built-in field forms a potential barrier on the surface of the silicon wafer, which can block the migration of electrons to the surface of the silicon wafer. At this time, the photogenerated carriers not only diffuse inside the silicon wafer, but are also affected by the built-in field when moving to the surface area of ​​the silicon wafer, which reduces the number of electrons reaching the surface, thereby reducing the probability of recombination between electrons and holes, achieving the effect of back passivation. If the concentration of boron doping is too high, a large number of electrically inactive B-Si, BH-Si and other composite structures will be generated, and the deposition layer will be amorphized, and the number of dangling bonds and defects will increase, limiting the movement of photogenerated carriers. When the boron doping concentration is too low, the concentration gradient of boron atoms is too low to generate a sufficiently strong built-in electric field.

[0008] Furthermore, the boron passivation layer is prepared by using B2H6 and SiH4 as reaction gases, and the gas ratio of doping gas B2H6 to SiH4 is in the range of 1×10 -5 ~5×10 -2 , the reaction temperature is 600-650°C. In the low-pressure chemical vapor deposition process of boron-doped microcrystalline silicon thin film, microcrystals begin to appear when the reaction temperature exceeds 580°C, and the crystallization effect of the film is ideal at 600-650°C.

[0009] Furthermore, in the SiOx / SiNx laminated dielectric layer, the thickness of the SiOx dielectric layer is 10 to 30 nm, and the thickness of the SiNx dielectric layer is 10 to 60 nm. Due to the presence of a large number of dangling bonds on the surface of the silicon wafer, surface states are formed, causing band bending on the surface and interface of the silicon wafer, affecting the diffusion of carriers. After preparing SiOx / SiNx on the back surface, the dielectric layer effectively saturates the dangling bonds, improves the surface state of the back surface, reduces the recombination rate of carriers, and increases the open circuit voltage. In addition, compared with the aluminum layer, the dielectric layer has a higher reflectivity, which can effectively increase the back reflection of long-wave light, thereby increasing the number of photogenerated carriers, improving the quantum efficiency of the long-wave part, and increasing the open circuit voltage.

[0010] Furthermore, an opening window is provided on the SiOx / SiNx laminated dielectric layer, and the aluminum back field realizes point contact with the boron passivation layer through the opening window. Since SiOx / SiNx are both dielectric insulating layers, local openings are required in the dielectric layer to realize electrical contact, and the aluminum back field realizes electrical contact with the silicon wafer through the opening window. The local Al-Si alloy contact can reduce the recombination rate of the back surface of the battery, improve the quantum efficiency of the long-wave part, increase the open circuit voltage, and thus improve the photoelectric conversion efficiency.

[0011] Furthermore, the opening window adopts a local laser opening method, using laser to drill holes or grooves on the back of the silicon wafer, partially penetrating the SiOx / SiNx stacked dielectric layer to expose the silicon substrate, and the aluminum back field achieves electrical contact with the silicon substrate through the holes or grooves on the film.

[0012] Furthermore, the opening window is opened by etching slurry, and the etching slurry is transferred to the opening position by screen printing technology, and the etching slurry is removed after the etching is completed.

[0013] Furthermore, the anti-reflection film is a SiNx film deposited by plasma enhanced chemical vapor deposition (PECVD) method, the thickness of the film layer is 75-85nm, and the refractive index is 2.0-2.1. The SiNx film has good insulation, compactness, stability and shielding ability for impurity ions. By adjusting the film thickness and refractive index of the SiNx film, the reflectivity of the 500-700nm band where the peak of the solar spectrum is located can be greatly reduced. In addition, when PECVD deposits SiNx, SiNx:H will be generated because the reaction gas contains hydrogen. During the high temperature process, the hydrogen in SiNx:H combines with the dangling bonds of the silicon-air interface, thereby reducing the surface recombination rate and achieving a back passivation effect.

[0014] A solar cell assembly comprises the crystalline silicon solar cell with the composite passivation layer structure.

[0015] The present invention discloses the following technical effects: The present invention provides a solar cell and a photovoltaic module. The back surface of the solar cell with a P-type silicon substrate is provided with a boron passivation layer, a SiOx / SiNx laminated dielectric layer and an aluminum back field in sequence. The boron passivation layer makes the boron concentration on the back surface of the battery higher, forms a potential barrier on the surface of the silicon wafer, reduces the recombination probability of electrons and holes, and achieves the effect of back passivation. The SiOx / SiNx laminated dielectric layer can effectively saturate dangling bonds, improve the surface state of the back surface, reduce the recombination rate of carriers, and increase the open circuit voltage. The SiOx / SiNx laminated dielectric layer also has a high reflectivity, which can effectively increase the back reflection of long-wave light, thereby increasing the number of photogenerated carriers, improving the quantum efficiency of the long-wave part, and increasing the open circuit voltage. The aluminum back field can effectively reduce the activity of the back surface of the battery, reduce the recombination rate of the surface, and increase the open circuit voltage. The battery structure of this composite passivation layer avoids the formation of a high composite layer of Al-Si alloy, greatly reduces the recombination rate of carriers, and at the same time improves the back passivation effect, thereby improving the photoelectric conversion efficiency. At the same time, the boron-doped microcrystalline silicon film prepared by LPCVD has a smooth surface and small and uniform grains. The LPCVD preparation method has a low process temperature, is not easy to cause oxygen deposition inside the silicon wafer, is not easy to cause lattice distortion, and the process operation is simple, making it suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 It is a schematic structural diagram of a solar cell of the present invention; In the figure: 1. P-type silicon substrate; 2. N-type doping layer; 3. anti-reflection film; 4. positive electrode; 5. boron passivation layer; 6. SiOx / SiNx stacked dielectric layer; 61. SiOx dielectric layer; 62. SiNx dielectric layer; 7. aluminum back field; 8. back electrode; 9. opening window. DETAILED DESCRIPTION

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0020] Reference Figure 1 As shown, the present invention provides a solar cell, including a P-type silicon substrate 1, the P-type silicon substrate 1 includes a front surface and a back surface, the front surface is prepared with an N-type doping layer 2, the N-type doping layer 2 is covered with an anti-reflection film 3, and the anti-reflection film 3 is provided with a positive electrode 4; the back surface is provided with a boron passivation layer 5, a SiOx / SiNx stacked dielectric layer 6 and an aluminum back surface field 7 in sequence, and the aluminum back surface field 7 is provided with a back electrode 8.

[0021] In the solar cell of the above structure, the boron passivation layer 5 is a boron-doped microcrystalline silicon film prepared by low-pressure chemical vapor deposition. The gas pressure of the deposition system is 420Pa, SiH4 and B2H6 are the reaction gases, the gas flow rate is 90sccm, the concentrations of SiH4 and B2H6 are 10% and 1% respectively, and the reaction temperature is 600°C. In the low-pressure chemical vapor deposition process of boron-doped microcrystalline silicon film, microcrystals begin to appear when the reaction temperature exceeds 580°C, and the crystallization effect of the film is ideal at 600-650°C. The grain size of the microcrystalline structure is 25-40nm.

[0022] Further optimization scheme, the thickness of the boron passivation layer 5 is 100-500nm, and the boron doping concentration is 10 18 The boron passivation layer 5 makes the boron concentration on the back surface of the battery higher, so that a negative charge-rich area is formed on the surface, and the surface of the silicon wafer presents negative electrical properties. Due to the existence of the boron atom concentration gradient, a built-in field pointing from the inside of the silicon wafer to the surface of the silicon wafer is formed. The built-in field forms a potential barrier on the surface of the silicon wafer, which can block the migration of electrons to the surface of the silicon wafer. At this time, the photogenerated carriers not only diffuse inside the silicon wafer, but are also affected by the built-in field when moving to the surface area of ​​the silicon wafer, which reduces the number of electrons reaching the surface, thereby reducing the probability of recombination between electrons and holes, achieving the effect of back passivation. If the concentration of boron doping is too high, a large number of electrically inactive B-Si, BH-Si and other composite structures will be produced, and the deposition layer will be amorphized, resulting in an increase in dangling bonds and defects, which will limit the movement of photogenerated carriers. When the boron doping concentration is too low, the concentration gradient of boron atoms is too small, and a sufficiently strong built-in field cannot be generated, and the passivation effect is weakened. Experiments have shown that when the thickness is 100-500nm and the boron doping concentration is 10 18 For example, the thickness is 150nm and the doping concentration is 4×10 18 cm -3 When the boron passivation layer 5 has an excellent passivation effect.

[0023] Further optimization scheme, in the SiOx / SiNx laminated dielectric layer 6, the thickness of the SiOx dielectric layer 61 is 10-30nm, and the thickness of the SiNx dielectric layer 62 is 10-60nm. The hydrogen in the SiNx dielectric layer 62 can saturate the dangling bonds on the surface of the silicon wafer, thereby reducing the surface recombination rate and increasing the carrier lifetime, but the defect density of the SiNx / Si interface is high, while the defect density of the SiOx / Si interface is low, but the field effect passivation effect is not as good as SiNx. Therefore, the use of the SiOx / SiNx laminated dielectric layer 6 can not only use SiOx to reduce the interface state density, but also use the positive charge in SiNx to form a good field effect passivation. In addition, the dielectric layer also plays the role of a back reflector, which can reflect more long-wavelength light back to the battery, thereby improving the long-wave response of the battery.

[0024] In some embodiments, the SiOx dielectric layer 61 is prepared by chemical vapor deposition, using SiH4 and N2O as reaction gases. This preparation method has a short process time, but the density of the film layer is poor.

[0025] In some embodiments, the SiOx dielectric layer 61 can also be prepared by thermal oxidation, using the reaction of silicon wafers with O2 under high temperature conditions to generate SiOx. This preparation method has a long process time, but the density of the film layer is higher than the deposition preparation method, and the quality of the film is good.

[0026] Furthermore, an opening window 9 is provided on the SiOx / SiNx stacked dielectric layer 6. Since SiOx / SiNx are both dielectric insulating films, local openings are required in the dielectric layer to achieve electrical contact. Point contact is achieved between the aluminum back surface field 7 and the silicon wafer through the opening window 9. Local Al-Si alloy contact can reduce the recombination rate of the back surface of the battery, improve the quantum efficiency of the long-wave part, increase the open circuit voltage, and thereby improve the photoelectric conversion efficiency.

[0027] Furthermore, the opening window 9 adopts a local laser opening method, using laser to ablate part of the SiOx / SiNx laminated dielectric layer 6 on the back surface to expose the silicon substrate, and then complete the slurry printing on the back of the silicon wafer and perform high-temperature sintering. Since there is no obstruction of the SiOx / SiNx laminated dielectric layer 6 in the laser grooved area, the aluminum back field 7 is in contact with the silicon substrate through the holes or grooves on the film, and under high-temperature sintering conditions, it forms an aluminum-silicon alloy with the silicon substrate, thereby reducing the series resistance and smoothly extracting the current. The laser conditions are: wavelength of 532nm, power of 30W, frequency of 2.0MHz, pulse width of 5ns / ps, and the damage to the silicon wafer is small under these parameters. The shape of the opening is a discontinuous groove. Theoretically, on the one hand, the increase in the width of the groove will increase the effective ohmic contact between the aluminum back surface field 7 and the silicon wafer, and improve the transport performance of the carriers on the surface of the cell, but at the same time increase the high recombination area of ​​the Al-Si alloy. The smaller the area of ​​the laser groove area, the less damage to the passivation layer, the higher the minority carrier lifetime, and the higher the open circuit voltage. But at the same time, the area of ​​the laser groove area cannot be too small. If the area of ​​the groove area is too small, during the high-temperature sintering process, the aluminum paste cannot completely penetrate the laser groove area, that is, the groove area cannot be filled, forming a void. The void area cannot form a good aluminum-silicon contact, which will affect the series resistance and fill factor, and then affect the conversion efficiency of the battery. Therefore, a balance is made between the ohmic contact and the high recombination area. Experiments have shown that when the groove line width is 35 to 40 μm, for example, at 37 μm, it has better battery conversion efficiency.

[0028] Furthermore, the opening window 9 is opened by etching slurry, and the silicon nitride etching paste of Merck is transferred to the opening position by screen printing technology. The etching paste has low fluoride components, does not require organic detergent, has a fast etching speed, and the etching slurry is removed after the etching is completed. This opening method avoids laser damage caused by laser opening, but increases the process links.

[0029] Furthermore, the anti-reflection film 3 is a SiNx film deposited by plasma enhanced chemical vapor deposition (PECVD) method, the thickness of the film layer is 75-85nm, and the refractive index is 2.0-2.1. The SiNx film has good insulation, compactness, stability and shielding ability for impurity ions. By adjusting the film thickness and refractive index of the SiNx film, the reflectivity of the 500-700nm band where the peak of the solar spectrum is located can be greatly reduced. In addition, when PECVD deposits SiNx, SiNx:H will be generated because the reaction gas contains hydrogen. During the high temperature process, the hydrogen in SiNx:H combines with the dangling bonds of the silicon-air interface, thereby reducing the surface recombination rate and achieving a back passivation effect.

[0030] It should be understood that, in practical applications, the crystalline silicon cell can be a polycrystalline P-type silicon wafer or a multicrystalline P-type silicon wafer.

[0031] The embodiment of the present invention further provides a solar cell assembly, comprising a plurality of solar cell sheets arrayed in a packaging material, wherein the solar cell sheets are the solar cells described in the embodiment of the present invention.

[0032] Compared with the prior art, a solar cell and a photovoltaic module according to an embodiment of the present invention at least disclose the following beneficial effects: The battery structure of the composite passivation layer avoids the formation of a high composite layer of Al-Si alloy, greatly reduces the recombination rate of carriers, and at the same time improves the back passivation effect, thereby improving the photoelectric conversion efficiency.

[0033] The boron-doped microcrystalline silicon film prepared by LPCVD has a smooth surface and small and uniform grains. The LPCVD preparation method has a low process temperature, is not easy to cause oxygen deposition inside the silicon wafer, is not easy to cause lattice distortion, and has simple process operation, making it suitable for industrial production.

[0034] The details not disclosed in the present invention are conventional technical means well known to those skilled in the art.

[0035] In the description of the present invention, it should be understood that the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0036] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A solar cell, It is characterized in that The invention comprises a P-type silicon substrate (1), wherein an N-type doping layer (2) is prepared on the front surface of the P-type silicon substrate (1), an anti-reflection film (3) is covered on the N-type doping layer (2), and a positive electrode (4) is arranged on the anti-reflection film (3); a composite passivation layer is provided on the back surface of the P-type silicon substrate (1), wherein the composite passivation layer comprises, from top to bottom, a boron passivation layer (5), a SiOx / SiNx stacked dielectric layer (6) and an aluminum back field (7), and a back electrode (8) is arranged on the aluminum back field (7), and the boron passivation layer (5) is a boron-doped microcrystalline silicon thin film prepared by low-pressure chemical vapor deposition.

2. A solar cell according to claim 1, It is characterized in that The thickness of the boron passivation layer (5) is 100 to 500 nm, and the boron doping concentration is 10 18 Magnitude.

3. A solar cell according to claim 2, It is characterized in that The boron passivation layer (5) is prepared by using B 2 H 6 and SiH 4 is the reaction gas, doping gas B 2 H 6 With SiH 4 The ratio range is 1×10 -5 ~5×10 -2 , the reaction temperature is 600-650℃.

4. A solar cell according to claim 1, It is characterized in that In the SiOx / SiNx stacked dielectric layer (6), the thickness of the SiOx dielectric layer (61) is 10 to 30 nm, and the thickness of the SiNx dielectric layer (62) is 10 to 60 nm.

5. A solar cell according to claim 4, It is characterized in that An opening window (9) is provided on the SiOx / SiNx stacked dielectric layer (6), and the aluminum back surface field (7) is point-contacted with the boron passivation layer (5) through the opening window (9).

6. A solar cell according to claim 5, It is characterized in that The opening window (9) is formed by local laser opening.

7. A solar cell according to claim 5, It is characterized in that The opening window (9) is opened by etching slurry.

8. A solar cell according to claim 1, It is characterized in that The anti-reflection film (3) is a SiNx film deposited by a plasma enhanced chemical vapor deposition (PECVD) method, the thickness of the film layer is 75 to 85 nm, and the refractive index is 2.0 to 2.

1.

9. A photovoltaic module comprising a plurality of solar cells arrayed in an encapsulation material, It is characterized in that The solar cell sheet is the solar cell according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Solar cell subjected to back passivation and preparation method thereof

    CN104362189A

  • Structure of TOP Con crystalline silicon / perovskite laminated solar cell and preparation method thereof

    CN117337065A

  • Preparation process of semiconductor silicon wafer for preparing back contact solar cell

    CN118380515A

  • Solar cell and fabrication thereof

    JP1994310740A

  • Method for manufacturing solar cell

    KR101870326B1