Light emitting diode and preparation method thereof
By adding an oxygen purging step after patterning the epitaxial structure of the light-emitting diode, the surface defects generated after etching are improved, the problems of vacancies and hanging bonds at the dry etching point of the epitaxial structure are solved, and the brightness of the LED is improved.
Patent Information
- Application Number
- CN202410929596.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-26
AI Technical Summary
Existing technologies are prone to surface defects such as vacancies and hanging bonds during the dry etching process of the epitaxial structure of light-emitting diodes, which leads to a decrease in LED brightness.
After the patterning of the epitaxial structure, an oxygen purging step is added. The surface of the epitaxial structure is purged by an oxygen flow to improve the surface defects generated after etching and reduce defects such as cracks, gaps and burrs.
Oxygen purging improves the surface condition of the epitaxial structure, reduces the surface recombination rate, and enhances the brightness of the LED, thus achieving a brightening effect.
Smart Images

Figure CN119029099A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of light-emitting devices, and in particular to a light-emitting diode and a method for preparing the same. Background Art
[0002] Light Emitting Diode (LED) is a semiconductor device that can emit light and is widely used in lighting, display, traffic signal, medical equipment and many other fields. LED is favored for its high energy efficiency, long life and fast response time, and is an important alternative to traditional lighting technology. With the continuous advancement of technology, LED has shown great potential in energy saving and environmental protection, and is gradually becoming the mainstream choice in the field of lighting.
[0003] The related art provides a light emitting diode, the structure of which includes a bonding substrate, a second metal layer, a first metal layer, a dielectric film layer and an epitaxial structure. During the manufacturing process of the light emitting diode with the above structure, the epitaxial structure needs to be dry-etched to form a step structure.
[0004] Related Technology During the process of dry etching an epitaxial structure, surface defects such as vacancies and hanging bonds are easily generated at the dry etching site of the epitaxial structure. Summary of the invention
[0005] The embodiment of the present disclosure provides a light emitting diode and a method for manufacturing the same, which improves surface defects such as vacancies and hanging bonds generated at the dry etching of the epitaxial structure after etching. The technical solution is as follows:
[0006] In one aspect, a method for preparing a light emitting diode is provided, the method comprising:
[0007] fabricating an epitaxial structure on a growth substrate;
[0008] Fabricating a dielectric film layer on the epitaxial structure, wherein the dielectric film layer has a plurality of through holes;
[0009] Growing a first metal layer on the dielectric film layer, wherein the first metal layer is electrically connected to the epitaxial structure through a plurality of the through holes;
[0010] bonding the first metal layer to a bonding substrate via a second metal layer, and removing the growth substrate;
[0011] Performing a patterning process on the epitaxial structure to form a step structure;
[0012] The epitaxial structure is subjected to an oxygen purge treatment.
[0013] Optionally, the epitaxial structure is subjected to an oxygen purge treatment, comprising:
[0014] After the etching is completed, the epitaxial structure is rinsed and the resin is removed;
[0015] Drying the epitaxial structure after water flushing and degumming;
[0016] The epitaxial structure after drying is purged with oxygen.
[0017] Optionally, the step of performing oxygen purge on the epitaxial structure after drying comprises:
[0018] The bonded substrate is placed downward on an electrode plate tray for oxygen purge, and each electrode plate tray is evenly placed with at most 7 chips of the light emitting diode.
[0019] Optionally, the oxygen purge power is 200-400W.
[0020] Optionally, during the oxygen purge, the oxygen flow rate is 100-300 sccm.
[0021] Optionally, the oxygen purge time is 80 to 100 seconds.
[0022] Optionally, the epitaxial structure includes a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence; performing a patterning process on the epitaxial structure to form the step structure; and performing the oxygen purge process on the epitaxial structure, comprising:
[0023] Performing a first patterning process on the epitaxial structure to form a first step structure, wherein a step surface of the first step structure is located in the second semiconductor layer;
[0024] performing the oxygen purge process on the epitaxial structure;
[0025] The epitaxial structure is subjected to a second patterning process to form a second step structure, wherein the step surface of the second step structure is located at the dielectric film layer.
[0026] On the other hand, a light emitting diode is provided, the light emitting diode comprising: a bonding substrate, a second metal layer, a first metal layer, a dielectric film layer and an epitaxial structure;
[0027] The first metal layer and the dielectric film layer are stacked in sequence on one side of the epitaxial structure, the dielectric film layer has a plurality of through holes, the first metal layer is electrically connected to the epitaxial structure through the plurality of through holes, the other side of the epitaxial structure is connected to the bonding substrate through the second metal layer, the epitaxial structure is a step structure, and the step surface and step sidewall of the step structure are treated with oxygen purge.
[0028] Optionally, the epitaxial structure may include a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence;
[0029] The step structure includes a first step structure and a second step structure;
[0030] The step surface of the first step structure is located in the second semiconductor layer, and the step surface of the second step structure is located in the dielectric film layer.
[0031] Optionally, the oxygen purge power is 200-400 W, the oxygen flow rate during the oxygen purge is 100-300 sccm, and the oxygen purge time is 80-100 s.
[0032] The technical solution provided by the embodiments of the present disclosure brings the following beneficial effects:
[0033] In the embodiment of the present disclosure, an oxygen purge step is added after the epitaxial structure is patterned. The oxygen purge can improve surface defects such as vacancies and hanging bonds caused by etching at the dry etching of the epitaxial structure after etching, reduce cracks, gaps, burrs, etc. on the surface of the epitaxial structure caused by the above defects, thereby reducing the surface recombination rate of the epitaxial structure and improving the surface state of the epitaxial structure, thereby achieving the purpose of brightening. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0035] Figure 1 is a flow chart of a method for preparing a light emitting diode provided by an embodiment of the present disclosure;
[0036] Figure 2 is a flow chart of another method for preparing a light emitting diode provided by an embodiment of the present disclosure;
[0037] Figure 3 is a structural schematic diagram of a light emitting diode manufacturing process provided by an embodiment of the present disclosure;
[0038] Figure 4 is a structural schematic diagram of a light emitting diode manufacturing process provided by an embodiment of the present disclosure;
[0039] Figure 5 is a structural schematic diagram of a light emitting diode provided by an embodiment of the present disclosure;
[0040] Figure 6 is a schematic structural diagram of another light emitting diode provided by an embodiment of the present disclosure;
[0041] Figure 7This is a brightness comparison chart of the light-emitting diode made according to the embodiment of the present disclosure and the light-emitting diode made according to the related technology.
[0042] The reference numerals are as follows:
[0043] 10: epitaxial structure; 101: first electrode; 102: bonding substrate; 103: second metal layer; 104: first metal layer; 105: dielectric film layer; 106: first semiconductor layer; 107: active layer; 108: second semiconductor layer; 109: second electrode; 110: growth substrate; 111: passivation layer; 201: step surface of the first step structure; 202: step surface of the second step structure; 301: through hole; 401: step structure; 4011: first step structure; 4012: second step structure; 1031: first metal sublayer; 1032: second metal sublayer. DETAILED DESCRIPTION
[0044] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0045] At present, outdoor display LED technology is relatively mature. In order to reduce costs and increase efficiency, the original brightness needs to be maintained while reducing the size of LEDs. More LED chips can be used with the same material, and special brightening methods are required to achieve the same brightness of small-sized LEDs as large-sized LEDs. The light-emitting diode preparation method provided in the present disclosure can achieve brightening benefits for LEDs with a size of less than 7 mil.
[0046] In the related art, after the epitaxial structure is dry-etched by inductively coupled plasma (ICP), surface defects such as vacancies and hanging bonds are easily generated at the dry-etched part, resulting in a decrease in the brightness of the LED. The embodiments of the present disclosure improve the above defects to achieve brightness improvement.
[0047] Figure 1 is a flow chart of a method for preparing a light emitting diode provided by an embodiment of the present disclosure. Figure 1 The method steps include:
[0048] S11. Fabricating an epitaxial structure on a growth substrate.
[0049] In the embodiment of the present disclosure, the growth substrate may be a GaAs substrate.
[0050] In the embodiment of the present disclosure, the epitaxial structure may include a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence.
[0051] In the embodiment of the present disclosure, the first semiconductor layer may be an N-type AlGaInP layer, the active layer may be a multi-quantum well layer, and the second semiconductor layer may be a P-type GaP layer.
[0052] Exemplarily, the epitaxial structure is fabricated using a Metal Organic Chemical Vapor Deposition (MOCVD) device.
[0053] S12. Fabricate a dielectric film layer on the epitaxial structure, wherein the dielectric film layer has a plurality of through holes.
[0054] In the embodiment of the present disclosure, the dielectric film layer may be SiO 2 Dielectric film, SiO 2 It has good chemical stability and good dielectric properties, can improve the chemical corrosion resistance of light-emitting diodes, and improve the reliability and durability of light-emitting diodes.
[0055] S13, growing a first metal layer on the dielectric film layer, wherein the first metal layer is electrically connected to the epitaxial structure through a plurality of through holes.
[0056] The dielectric film layer can achieve adhesion between the epitaxial structure and the first metal layer, and the through hole opened in the dielectric film layer can conduct current.
[0057] In the embodiment of the present disclosure, the first metal layer may be a metal mirror layer.
[0058] In one example, the first metal layer may be an Ag or Au layer. In another example, the first metal layer may be a stack of Ag and Au. In yet another example, the first metal layer may be a stack of Ag and TiW. In other examples, the first metal layer may also be a single layer or a stack of other metals or alloys.
[0059] S14, bonding the first metal layer to the bonding substrate through the second metal layer, and removing the growth substrate.
[0060] In the embodiment of the present disclosure, the bonding substrate may be a Si substrate.
[0061] In the embodiment of the present disclosure, the second metal layer may be an Au bonding layer, or a bonding layer formed by a combination of Au and In, or a bonding layer formed by a combination of Ni and Sn.
[0062] In the disclosed embodiment, the second metal layer is bonded under high pressure and high temperature environment, wherein the bonding temperature may be 280-320°C.
[0063] Exemplarily, the bonding temperature is 320°C.
[0064] S15, performing graphic processing on the epitaxial structure to form a step structure.
[0065] In the embodiment of the present disclosure, the epitaxial structure is etched by a dry etching process to form a step structure. Exemplarily, the epitaxial structure is etched by an ICP dry etching process.
[0066] The epitaxial structure after etching is a step structure, and the step surface of the step structure is located in the second semiconductor layer.
[0067] S16, performing oxygen purge treatment on the epitaxial structure.
[0068] The oxygen purge treatment refers to blowing the surface of the epitaxial structure with an oxygen flow, thereby blowing the step surface and step sidewalls of the etched epitaxial structure.
[0069] In the embodiment of the present disclosure, an oxygen purge step is added after the epitaxial structure is patterned. The oxygen purge can improve surface defects such as vacancies and hanging bonds caused by etching at the dry etching of the epitaxial structure after etching, reduce cracks, gaps, burrs, etc. on the surface of the epitaxial structure caused by the above defects, thereby reducing the surface recombination rate of the epitaxial structure and improving the surface state of the epitaxial structure, thereby achieving the purpose of brightening.
[0070] Figure 2 is a flow chart of another method for preparing a light emitting diode provided by an embodiment of the present disclosure. Figure 2 The method steps include:
[0071] S21. Forming a first semiconductor layer, an active layer, and a second semiconductor layer in sequence on a growth substrate, wherein the second semiconductor layer, the active layer, and the first semiconductor layer constitute an epitaxial structure.
[0072] The growth substrate may be a GaAs substrate.
[0073] Exemplarily, step S21 includes:
[0074] The first step is to make the first semiconductor layer.
[0075] In the embodiment of the present disclosure, the first semiconductor layer may be an N-type AlGaInP layer.
[0076] Exemplarily, the N-type AlGaInP layer is manufactured using MOCVD equipment.
[0077] The second step is to make the active layer.
[0078] In the embodiment of the present disclosure, the active layer is a multi-quantum well layer.
[0079] The third step is to make the second semiconductor layer.
[0080] In the embodiment of the present disclosure, the second semiconductor layer may be a P-type GaP layer.
[0081] Exemplarily, the P-type GaP layer is manufactured using MOCVD equipment.
[0082] It should be noted that the introduction of the above epitaxial structure is only an example, and the epitaxial structure may include more film layers, or be composed of other film layers, and the embodiments of the present disclosure are not limited to this.
[0083] In the embodiment of the present disclosure, the growth of the semiconductor layer can be achieved by using Veeco K465i or C4 or RB MOCVD (Metal Organic Chemical Vapor Deposition) equipment or AIXTRON metal organic chemical vapor deposition equipment. 2 (Hydrogen) or high purity N 2 (nitrogen) or high purity H 2 and high purity N 2 A mixed gas of high purity NH 3 As the N source, trimethylgallium (TMGa) and triethylgallium (TEGa) as the gallium source, trimethylindium (TMIn) as the indium source, silane (SiH 4 ) as N-type dopant, trimethylaluminum (TMAl) as aluminum source, bis(cyclopentadienyl)magnesium (CP 2 Mg) as a P-type dopant.
[0084] S22, growing a dielectric film layer on the epitaxial structure, and etching a plurality of through holes on the dielectric film layer.
[0085] Figure 3 Schematic diagram of the structure of the light emitting diode manufacturing process provided by the embodiment of the present disclosure. Figure 3 The first semiconductor layer 106 , the active layer 107 and the second semiconductor layer 108 are sequentially grown on the growth substrate 110 , the dielectric film layer 105 is grown on the second semiconductor layer 108 , and a plurality of through holes 301 are opened on the dielectric film layer 105 .
[0086] In the embodiment of the present disclosure, the dielectric film layer may be SiO 2 Dielectric film, SiO 2 It has good chemical stability and good dielectric properties, can improve the chemical corrosion resistance of light-emitting diodes, and improve the reliability and durability of light-emitting diodes.
[0087] In the embodiment of the present disclosure, a chemical vapor deposition (Plasma Enhanced Chemical Vapor Deposition, PECVD) device is used to grow SiO2 The dielectric film layer is then etched into through holes in the dielectric film layer by photolithography and wet etching.
[0088] S23. Growing a first metal layer on the dielectric film layer.
[0089] In one example, the first metal layer may be an Ag or Au layer. In another example, the first metal layer may be a stack of Ag and Au. In yet another example, the first metal layer may be a stack of Ag and TiW. In other examples, the first metal layer may also be a single layer or a stack of other metals or alloys.
[0090] In the embodiment of the present disclosure, the first metal layer is grown using electron beam evaporation equipment.
[0091] S24, manufacturing a first metal sub-layer on the first metal layer.
[0092] In the embodiment of the present disclosure, the first metal sublayer may be an Au bonding layer, or a bonding layer formed by a combination of Au and In, or a bonding layer formed by a combination of Ni and Sn.
[0093] In the embodiment of the present disclosure, the first metal sub-layer is grown using electron beam evaporation equipment.
[0094] S25. Growing a second metal sublayer on the bonding substrate.
[0095] In the embodiment of the present disclosure, the bonding substrate may be a Si substrate.
[0096] In the embodiment of the present disclosure, the second metal sublayer may be an Au bonding layer, or a bonding layer formed by a combination of Au and In, or a bonding layer formed by a combination of Ni and Sn.
[0097] In the embodiment of the present disclosure, the second metal sub-layer is grown using electron beam evaporation equipment.
[0098] S26, bonding the first metal sublayer on the first metal layer and the second metal sublayer on the bonding substrate into one layer.
[0099] In the disclosed embodiment, the second metal layer is bonded under high pressure and high temperature environment, wherein the bonding temperature is 280-320°C.
[0100] Exemplarily, the bonding temperature is 320°C.
[0101] In the embodiment of the present disclosure, if the bonding temperature is too high, the semiconductor layer will be damaged, and if the bonding temperature is too low, it will be detrimental to the bonding effect. Using the above temperature for bonding can ensure a good bonding effect without damaging the semiconductor layer.
[0102] Figure 4FIG. 1 is a schematic diagram of the structure of the light emitting diode manufacturing process provided by the embodiment of the present disclosure. Figure 4 As shown, a first metal layer 104 is grown on the surface of the dielectric film layer 105 , and a first metal sublayer 1031 on the first metal layer 104 and a second metal sublayer 1032 on the bonding substrate 102 are bonded to form a second metal layer 103 .
[0103] S27. Remove the growth substrate.
[0104] In the disclosed embodiment, the growth substrate is removed by wet etching.
[0105] S28. Fabricate a first electrode on the first semiconductor layer, and fabricate a second electrode on a side of the bonding substrate away from the epitaxial structure.
[0106] In the embodiment of the present disclosure, the first electrode and the second electrode may be TiAu electrodes or Au / AuGeNi / Au / Pt / Au electrodes.
[0107] In the embodiment of the present disclosure, the first electrode may be an N-electrode, and the second electrode may be a P-electrode.
[0108] It is worth noting that in the embodiment of the present disclosure, the second electrode provided on the bonding substrate may be used only for testing, and in actual application, the second metal layer may be used as the second electrode.
[0109] S29, performing a first patterning process on the epitaxial structure to form a first step structure, wherein a step surface of the first step structure is located in the second semiconductor layer.
[0110] Exemplarily, a patterned mask layer is formed on the surface of the first semiconductor layer; under the protection of the mask layer, the epitaxial structure is etched to form a step structure extending to the second semiconductor layer.
[0111] In the embodiment of the present disclosure, the first step structure is etched so that the current can be better extended vertically on the epitaxial structure, thereby ensuring composite luminescence.
[0112] S30, performing oxygen purge treatment on the epitaxial structure.
[0113] The oxygen purge treatment refers to blowing the surface of the epitaxial structure with an oxygen flow, thereby blowing the step surface and step sidewalls of the etched epitaxial structure.
[0114] Exemplarily, step S30 may include:
[0115] The first step is to rinse and remove the glue from the epitaxial structure after etching.
[0116] In the disclosed embodiment, the epitaxial structure after etching is rinsed and debonded using a debonding solution.
[0117] The second step is to spin dry the epitaxial structure after water-washing and degumming.
[0118] The third step is to purge the epitaxial structure after drying with oxygen.
[0119] In the disclosed embodiment, when oxygen purging is performed, the light-emitting diode chips are placed on the electrode plate tray with the bonding substrate facing downward, and each electrode plate tray is evenly placed with a maximum of 7 light-emitting diode chips.
[0120] Among them, the electrode plate tray is an aluminum alloy tray.
[0121] Exemplarily, six LED chips are evenly placed on each electrode plate tray to avoid problems such as too many chips causing insufficient area on the electrode plate tray, making it difficult to take and place chips.
[0122] In the disclosed embodiment, the oxygen purge power can be 200-400W. Too much power will affect the sidewall of the epitaxial structure and increase the probability of wafer leakage, while too little power will not achieve the oxygen purge effect. The above power can ensure the oxygen purge effect while avoiding wafer leakage.
[0123] Exemplarily, the oxygen purge power may be 300W.
[0124] In the disclosed embodiment, the oxygen flow rate can be 100-300 sccm. If the flow rate is too small, the oxygen purge effect cannot be achieved, and if the flow rate is too large, oxygen waste will be caused. The above flow rate can ensure the oxygen purge effect while avoiding oxygen waste.
[0125] Exemplarily, the oxygen flow rate may be 200 sccm.
[0126] In the disclosed embodiment, the oxygen purge time may be 80 to 100 seconds. If the time is too short, the oxygen purge effect cannot be achieved, and if the time is too long, the efficiency will be low. The above flow rate can ensure the oxygen purge effect while ensuring the efficiency.
[0127] Exemplarily, the oxygen purge time may be 90 seconds.
[0128] S31, forming a passivation layer on the first semiconductor layer.
[0129] Exemplarily, step S31 includes:
[0130] The first step is to perform roughening treatment on the first semiconductor layer.
[0131] For example, the surface of the first semiconductor layer is processed by photolithography and etching to form a roughened surface.
[0132] The second step is to form a passivation layer on the first semiconductor layer. The passivation layer is arranged around the first electrode and covers the surface of the first semiconductor layer, the sidewall of the first step structure and the step surface of the first step structure.
[0133] In the embodiment of the present disclosure, the passivation layer is a SiN passivation layer grown by PECVD, and the passivation layer is patterned to form a passivation layer pattern.
[0134] S32, performing a second patterning process on the epitaxial structure to form a second step structure, wherein a step surface of the second step structure is located in the dielectric film layer.
[0135] In the embodiment of the present disclosure, the second semiconductor layer is etched by a photolithography process to reduce light absorption by the second semiconductor layer, thereby achieving a brightening effect.
[0136] Exemplarily, a patterned mask layer is formed on the step surface of the first step structure; under the protection of the mask layer, the epitaxial structure is etched to form a second step structure extending to the dielectric film layer, with the step surface on the dielectric film layer.
[0137] In the embodiment of the present disclosure, the above solution can improve the brightness by 3-5%.
[0138] Optionally, the method may further include: grinding and cutting the chip to complete the product.
[0139] Figure 5 is a schematic diagram of the structure of a light emitting diode provided by an embodiment of the present disclosure. Figure 5 The light emitting diode includes: a bonding substrate 102 , a second metal layer 103 , a first metal layer 104 , a dielectric film layer 105 and an epitaxial structure 10 .
[0140] The first metal layer 104 and the dielectric film layer 105 are stacked in sequence on one side of the epitaxial structure 10. The dielectric film layer 105 has a plurality of through holes 301. The first metal layer 104 is electrically connected to the epitaxial structure 10 through the plurality of through holes 301. The other side of the epitaxial structure 10 is connected to the bonding substrate 102 through the second metal layer 103. The epitaxial structure 10 presents a step structure 401. The step surface and step sidewall of the step structure 401 are treated by oxygen purge.
[0141] In the disclosed embodiment, the step surface and step side walls of the step structure are treated with oxygen purging. Oxygen purging can improve surface defects such as vacancies and hanging bonds caused by etching at the dry etching of the epitaxial structure after etching, reduce cracks, gaps, burrs, etc. on the surface of the epitaxial structure caused by the above defects, thereby reducing the surface recombination rate of the epitaxial structure and improving the surface state of the epitaxial structure, thereby achieving the purpose of brightening.
[0142] In the embodiment of the present disclosure, the bonding substrate 102 may be a Si substrate.
[0143] In the embodiment of the present disclosure, the second metal layer 103 may be an Au bonding layer, or a bonding layer formed by a combination of Au and In, or a bonding layer formed by a combination of Ni and Sn.
[0144] In one example, the first metal layer 104 may be an Ag or Au layer. In another example, the first metal layer 104 may be a stack of Ag and Au. In yet another example, the first metal layer 104 may be a stack of Ag and TiW. In other examples, the first metal layer 104 may also be a single layer or a stack of other metals or alloys.
[0145] In the embodiment of the present disclosure, the dielectric film layer 105 may be SiO 2 Dielectric film layer 105, SiO 2 It has good chemical stability and good dielectric properties, can improve the chemical corrosion resistance of light-emitting diodes, and improve the reliability and durability of light-emitting diodes.
[0146] In the embodiment of the present disclosure, the epitaxial structure 10 may include a first semiconductor layer 106 , an active layer 107 , and a second semiconductor layer 108 which are sequentially stacked.
[0147] In the embodiment of the present disclosure, the first semiconductor layer 106 may be an N-type AlGaInP layer, the active layer 107 may be a multi-quantum well layer, and the second semiconductor layer 108 may be a P-type GaP layer.
[0148] Figure 6 is a schematic diagram of the structure of another light emitting diode provided by an embodiment of the present disclosure. Figure 6 The light emitting diode further includes: a first electrode 101 , a second electrode 109 and a passivation layer 111 .
[0149] The first electrode 101 is located on the first semiconductor layer 106, and the second electrode 109 is located on a side of the bonding substrate 102 away from the epitaxial structure 10. The passivation layer 111 is located on the first semiconductor layer 106 and surrounds the first electrode 101, and covers the surface of the first semiconductor layer 106, the sidewall of the first step structure 4011, and the step surface 201 of the first step structure.
[0150] In the embodiment of the present disclosure, the first electrode 101 and the second electrode 109 may be TiAu electrodes or Au / AuGeNi / Au / Pt / Au electrodes.
[0151] In the embodiment of the present disclosure, the first electrode 101 may be an N-electrode, and the second electrode 109 may be a P-electrode.
[0152] It is worth noting that, in the embodiment of the present disclosure, the second electrode 109 disposed on the bonding substrate 102 may be used only for testing, and in actual application, the second metal layer 103 may be used as the second electrode.
[0153] In the embodiment of the present disclosure, the passivation layer 111 is a SiN passivation layer grown by PECVD, and the passivation layer 111 is patterned to form a passivation layer pattern.
[0154] In the embodiment of the present disclosure, the step structure 401 may include a first step structure 4011 and a second step structure 4012 .
[0155] The step surface 201 of the first step structure 4011 is located in the second semiconductor layer 108. By etching the first step structure 4011, the current can be better vertically extended on the epitaxial structure, thereby ensuring composite light emission.
[0156] The step surface 202 of the second step structure 4012 is located at the dielectric film layer 105. The second semiconductor layer 108 is etched by a photolithography process to form the second step structure 4012, thereby reducing light absorption of the second semiconductor layer 108 and achieving a brightening effect.
[0157] In other embodiments, the step structure 401 may also include only the first step structure 4011 .
[0158] In the embodiment of the present disclosure, when oxygen purging is performed, the LED chips are placed on the electrode plate tray with the bonding substrate 102 facing downward, and each electrode plate tray is evenly placed with at most 7 LED chips.
[0159] Among them, the electrode plate tray is an aluminum alloy tray.
[0160] Exemplarily, six LED chips are evenly placed on each electrode plate tray to avoid problems such as too many chips causing insufficient area on the electrode plate tray, making it difficult to take and place chips.
[0161] In the disclosed embodiment, the oxygen purge power can be 200-400W. Too much power will affect the sidewall of the epitaxial structure and increase the probability of wafer leakage, while too little power will not achieve the oxygen purge effect. The above power can ensure the oxygen purge effect while avoiding wafer leakage.
[0162] Exemplarily, the oxygen purge power may be 300W.
[0163] In the disclosed embodiment, the oxygen flow rate can be 100-300 sccm. If the flow rate is too small, the oxygen purge effect cannot be achieved, and if the flow rate is too large, oxygen waste will be caused. The above flow rate can ensure the oxygen purge effect while avoiding oxygen waste.
[0164] Exemplarily, the oxygen flow rate may be 200 sccm.
[0165] In the disclosed embodiment, the oxygen purge time may be 80 to 100 seconds. If the time is too short, the oxygen purge effect cannot be achieved, and if the time is too long, the efficiency will be low. The above flow rate can ensure the oxygen purge effect while ensuring the efficiency.
[0166] Exemplarily, the oxygen purge time may be 90 seconds.
[0167] It is worth noting that in the embodiments of the present disclosure, structures may be selectively increased or decreased based on the structure of the above-mentioned light emitting diode, and the present disclosure does not impose any limitation on this.
[0168] Figure 7 is a brightness comparison diagram of the light emitting diode produced by the embodiment of the present disclosure and the light emitting diode produced by the related technology. Figure 7 , the horizontal axis is the number of wafers (4-inch wafer: piece). The vertical axis is the brightness (unit: MCD). Figure 7 In the figure, dark triangles represent light-emitting diodes made in the embodiment of the present disclosure, and light circles represent light-emitting diodes made in related technologies. Figure 7 It can be seen that the brightness center line after oxygen purge (embodiment of the present disclosure) is higher than the brightness without oxygen purge (related technology), which means that the brightness of the LED is significantly improved after oxygen purge.
[0169] Table 1 below is a comparison of brightness data of a light-emitting diode made by an embodiment of the present disclosure and a light-emitting diode made by a related technology before and after 3 months.
[0170] Wherein, LOP is the light output performance, the unit is MCD; AVG is the mean value.
[0171] The following data is the average brightness of a 4-inch single wafer. Comparing the 3-month data using oxygen purge brightening technology with that without oxygen purge brightening technology, the average brightness increased by 4%.
[0172] Table 1
[0173]
[0174] The above description is only an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A method for preparing a light emitting diode, It is characterized in that The light emitting diode preparation method comprises: Fabricating an epitaxial structure (10) on a growth substrate (110); Manufacturing a dielectric film layer (105) on the epitaxial structure (10), wherein the dielectric film layer (105) has a plurality of through holes (301); Growing a first metal layer (104) on the dielectric film layer (105), wherein the first metal layer (104) is electrically connected to the epitaxial structure (10) through a plurality of through holes (301); Bonding the first metal layer (104) to a bonding substrate (102) via a second metal layer (103), and removing the growth substrate (110); Performing a patterning process on the epitaxial structure (10) to form a step structure (401); The epitaxial structure (10) is subjected to an oxygen purge treatment.
2. The method for preparing a light emitting diode according to claim 1, It is characterized in that The epitaxial structure (10) is subjected to an oxygen purge treatment, comprising: After the etching is completed, the epitaxial structure (10) is rinsed with water to remove the glue; After the water flushing and degumming, the epitaxial structure (10) is subjected to a spin-drying treatment; The epitaxial structure (10) after being spun dry is purged with oxygen.
3. The method for preparing a light emitting diode according to claim 2, It is characterized in that The step of performing oxygen purge on the epitaxial structure (10) after drying comprises: The bonding substrate (102) is placed downward on an electrode plate tray for oxygen purge, and each electrode plate tray is evenly placed with at most 7 chips of the light emitting diode.
4. The method for preparing a light emitting diode according to any one of claims 1 to 3, It is characterized in that The oxygen purge power is 200-400W.
5. The method for preparing a light emitting diode according to any one of claims 1 to 3, It is characterized in that The oxygen flow rate during the oxygen purge is 100-300 sccm.
6. The method for preparing a light emitting diode according to any one of claims 1 to 3, It is characterized in that The oxygen purge time is 80 to 100 seconds.
7. The method for preparing a light emitting diode according to any one of claims 1 to 3, It is characterized in that The epitaxial structure (10) comprises a first semiconductor layer (106), an active layer (107) and a second semiconductor layer (108) which are stacked in sequence; Performing a patterning process on the epitaxial structure (10) to form a step structure (401); The epitaxial structure (10) is subjected to the oxygen purge treatment, comprising: Performing a first patterning process on the epitaxial structure (10) to form a first stepped structure (4011), wherein a step surface (201) of the first stepped structure (4011) is located on the second semiconductor layer (108); Performing the oxygen purge treatment on the epitaxial structure (10); The epitaxial structure (10) is subjected to a second patterning process to form a second step structure (4012), wherein the step surface (202) of the second step structure (4012) is located on the dielectric film layer (105).
8. A light emitting diode, It is characterized in that The light emitting diode comprises: a bonding substrate (102), a second metal layer (103), a first metal layer (104), a dielectric film layer (105) and an epitaxial structure (10); The first metal layer (104) and the dielectric film layer (105) are sequentially stacked on one side of the epitaxial structure (10); the dielectric film layer (105) has a plurality of through holes (301); the first metal layer (104) is electrically connected to the epitaxial structure (10) through the plurality of through holes (301); the other side of the epitaxial structure (10) is connected to the bonding substrate (102) through the second metal layer (103); the epitaxial structure (10) is a step structure (401); and the step surface and step side wall of the step structure (401) are subjected to oxygen purging treatment.
9. The light emitting diode according to claim 8, It is characterized in that The epitaxial structure (10) comprises a first semiconductor layer (106), an active layer (107) and a second semiconductor layer (108) which are stacked in sequence; The step structure (401) includes a first step structure (4011) and a second step structure (4012); The step surface (201) of the first step structure (4011) is located on the second semiconductor layer (108), and the step surface (202) of the second step structure (4012) is located on the dielectric film layer (105).