Wide-temperature-range polyurethane elastomer and preparation method thereof

By combining flexible segments and metal coordination structures, hydrogen bonding interactions are weakened, the operating temperature range of polyurethane elastomers is broadened, and the problems of cold and heat resistance of polyurethane elastomers in extreme environments are solved, enabling wide-temperature-range applications.

CN118930796AActive Publication Date: 2024-11-12HANGZHOU NORMAL UNIVERSITY

Patent Information

Application Number
CN202411133686.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Existing polyurethane elastomers have limited operating temperature ranges due to hydrogen bonding interactions, making them unsuitable for effective application in extreme environments.

Method used

By introducing flexible segments with low glass transition temperatures and combining them with sterically hindered basic metal ion-ligand coordination structures, hydrogen bond interactions are weakened, thus broadening the operating temperature range.

Benefits of technology

It enables the normal use of polyurethane elastomers within a temperature range of -60℃ to 80℃, improves cold and heat resistance, and maintains good mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930796A_ABST
    Figure CN118930796A_ABST
Patent Text Reader

Abstract

The invention discloses a wide-temperature-range polyurethane elastomer and a preparation method thereof.The wide-temperature-range polyurethane elastomer is obtained through a reaction of a flexible chain segment with a low glass transition temperature, diisocyanate and a large steric hindrance element, and the tail end of the flexible chain segment with the low glass transition temperature is a dihydroxyl-terminated flexible chain segment; the large steric hindrance element is of a metal ion-ligand coordination structure. According to the invention, diisocyanate is utilized to organically combine a flexible chain segment with a low glass transition temperature with a metal coordination structure with a relatively large steric effect, and hydrogen bond interaction between polyurethane chain segments is weakened, so that the use temperature range of the polyurethane elastomer is widened, the cold resistance and heat resistance of the polyurethane elastomer are remarkably improved, and the service life of the polyurethane elastomer is prolonged. The polyurethane elastomer can be normally used in a wide temperature range (-60 DEG C to 80 DEG C), and has very important significance for promoting the application of a polyurethane material in an extreme environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane preparation, and in particular to a wide-temperature range polyurethane elastomer and a preparation method thereof. Background Art

[0002] Polyurethane elastomers play an indispensable role in many application fields due to their unique physical and chemical properties. This type of material has won the favor of the market with its advantages such as high tensile strength, adjustable mechanical properties and toughening effect without additional fillers. In the polymer network structure of polyurethane elastomers, hydrogen bonds between chain segments drive the polymer network to produce a microphase separation structure, which gives polyurethane elastomers excellent mechanical properties and makes them widely used in many industries such as construction, transportation, clothing, and medical treatment.

[0003] In recent years, researchers have focused on how to enhance the mechanical properties of polyurethane elastomers by enhancing hydrogen bond interactions. Patent document CN114773569B discloses a preparation method and application of a self-healing elastomer with a three-dimensional network structure. The invention enhances the self-healing properties of polyurethane by modifying the molecules, introducing multiple hydrogen bond interactions, and forming a large number of hydrogen bond physical crosslinking points.

[0004] Patent document CN115010896B discloses a thermoplastic elastomer with excellent rebound performance and high strength and a preparation method thereof, the preparation method comprising the following steps: placing at least two soft segment monomers in a solvent and then adding a hard segment monomer, reacting under the action of a catalyst to obtain an initial reactant; reacting a chain extender with the initial reactant to obtain a thermoplastic elastomer. This invention significantly enhances the tensile strength and toughness of polyurethane by introducing urea bonds with stronger hydrogen bond interactions into the system.

[0005] However, it is well known that hydrogen bonds are very sensitive to temperature. They can easily induce strong interactions between chain segments under low temperature conditions and can be easily opened under high temperature conditions. Therefore, polyurethane elastomers that rely on hydrogen bonds usually show strong temperature sensitivity, tend to harden under low temperature conditions, and tend to soften under high temperature conditions, which makes their use temperature range very limited, usually only 0℃-60℃. With the continuous development of high-tech industries and my country's continuous exploration of extreme environments, people's requirements for the heat resistance and cold resistance of polyurethane elastomers are increasing. In addition, border defense, polar scientific research and even high-tech fields such as aerospace have always been important directions for the development and application promotion of low-temperature / high-temperature resistant elastomer materials.

[0006] Therefore, in view of the above-mentioned deficiencies of the existing technology, finding a new method to prepare polyurethane elastomer materials with a wide temperature range and improve the cold resistance and heat resistance of polyurethane elastomers is of great significance for promoting the application of polyurethane materials in extreme environments. At the same time, it can also help the development of high-end equipment from the direction of materials and promote the advancement of polar scientific research or space exploration. Summary of the invention

[0007] The purpose of the present invention is to provide a wide temperature range polyurethane elastomer and a preparation method thereof. The polyurethane elastomer of the present invention has a wide operating temperature range, excellent cold resistance and heat resistance, and can solve the problem of limited operating temperature range caused by hydrogen bond interaction in existing polyurethane materials.

[0008] The first aspect of the present invention provides a wide temperature range polyurethane elastomer, which is obtained by reacting a flexible chain segment with a low glass transition temperature, a diisocyanate and a large steric hindrance unit, wherein the flexible chain segment with a low glass transition temperature is a flexible chain segment with a dihydroxyl end cap; and the large steric hindrance unit is a metal ion-ligand coordination structure with multiple coordination bonds.

[0009] The present invention organically combines a flexible segment with a low glass transition temperature with a metal coordination structure with a large steric effect by using diisocyanate, effectively weakening the hydrogen bond interaction between polyurethane segments, thereby broadening the use temperature range of the polyurethane elastomer. This design not only reduces the glass transition temperature of the polyurethane elastomer and improves its flexibility in an extremely low temperature environment, but also weakens the hydrogen bond to make it less sensitive to temperature, and also maintains good mechanical properties under high temperature conditions, so that the polyurethane elastomer can be used normally in a wider temperature range (-60°C to 80°C).

[0010] Preferably, the flexible chain segment with a dihydroxyl-terminated terminal includes, but is not limited to, one or more of dihydroxyl-terminated polydimethylsiloxane, dihydroxyl-terminated polybutadiene, or dihydroxyl-terminated perfluoropolyether.

[0011] Preferably, the number average molecular weight of the flexible chain segment terminated with dihydroxy groups is 1000 to 6000 g / mol.

[0012] Preferably, in the metal ion-ligand coordination structure of the multiple coordination bond, the metal ion is a metal cation with a valence of +1 to +6, including but not limited to Eu 3+ 、Zn 2+ , Tb 3+ , Cu 2+ 、Al 3+ 、Ni 2+ , Fe 3+ 、Co 2+ , Mn2+ 、Ag + , Pd 2+ The ligand motif includes, but is not limited to, one or more of 2,6-bis(triazine)pyridine group, 2,6-di(2-pyridyl)pyridine group, 2,2'-bipyridine-4,4'-dicarboxylic acid group, 2,2'-bipyridine group, 2,6-bis(2-benzimidazolyl)pyridine group, pyridine-2,6-dicarboxylic acid group, etc. The complex structure formed by these ligands and metal ions has a large steric hindrance effect, which is conducive to weakening the hydrogen bonds between chains.

[0013] Preferably, the diisocyanate includes but is not limited to one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, naphthalene diisocyanate, tetramethyl meta-xylylene diisocyanate, para-phenylene diisocyanate, norbornane diisocyanate, cyclohexane dimethylene diisocyanate and the like.

[0014] Preferably, the molar ratio of the flexible segment with dihydroxyl end capping, the diisocyanate and the ligand unit in the metal ion-ligand coordination structure with multiple coordination bonds is 1:1.5-2.2:0.5-1.2.

[0015] The second aspect of the present invention provides a method for preparing the above-mentioned wide temperature range polyurethane elastomer, comprising the following steps:

[0016] (1) performing dihydroxy modification on a small molecule containing the above-mentioned ligand motif to obtain a dihydroxy-terminated ligand molecule;

[0017] (2) mixing the above-mentioned flexible chain segment terminated with dihydroxyl groups with diisocyanate, an organic solvent and a catalyst, and performing a prepolymerization reaction to obtain a polyurethane prepolymer;

[0018] (3) adding a dihydroxyl-terminated ligand molecule to the polyurethane prepolymer, stirring to react, and obtaining an uncrosslinked linear polyurethane product;

[0019] (4) adding a metal salt solution to the uncrosslinked linear polyurethane product, stirring to react, and after the reaction is completed, removing the solvent to obtain the wide temperature range polyurethane elastomer.

[0020] Preferably, in step (1), the small molecules containing the above-mentioned ligand motif include but are not limited to the following structures:

[0021]

[0022] Preferably, in step (2), the molar ratio of the flexible chain segment terminated with dihydroxy groups to diisocyanate is 1:1.5 to 2.2.

[0023] Preferably, in step (2), the organic solvent is a mixture of one or more of dimethyl sulfoxide, tetrahydrofuran, N,N-dimethylformamide, dichloromethane, toluene, n-hexane, petroleum ether and acetone.

[0024] Preferably, in step (2), the catalyst is dibutyltin dilaurate, stannous octoate or N,N-dimethylcyclohexylamine.

[0025] Preferably, in step (2), the amount of the catalyst used is 0.1 to 2% of the molar amount of the flexible chain segment terminated with dihydroxy groups.

[0026] Preferably, in step (2), the temperature of the prepolymerization reaction is 40-80° C., and the reaction time is 2-6 hours.

[0027] Preferably, in step (3), the molar ratio of the dihydroxy-terminated ligand molecule to the dihydroxy-terminated flexible chain segment is 0.5 to 1.2:1.

[0028] Preferably, in step (3), the reaction temperature is 40-80° C., and the reaction time is 6-12 h.

[0029] In step (4), the metal salt solution mainly comprises a metal salt and a solvent. Preferably, the cation in the metal salt is a metal cation with a valence of +1 to +6, such as Eu 3+ 、Zn 2+ , Tb 3+ , Cu 2+ 、Al 3+ 、Ni 2+ , Fe 3+ 、Co 2+ , Mn 2+ 、Ag + , Pd 2+ The anion is a counter anion with a valence of -1 to -3, including one or more of chloride ion, bromide ion, fluoride ion, iodide ion, acetate ion, sulfate ion, trifluoroacetate ion, trifluoromethanesulfonate ion, bistrifluoromethylsulfonyl imide ion, hexafluorophosphate ion, tetrafluoroborate ion, etc.

[0030] Preferably, the amount of the metal salt is determined according to the coordination number between the ligand and the metal ion.

[0031] Preferably, the solvent of the metal salt solution is a mixture of one or more of dimethyl sulfoxide, tetrahydrofuran, N,N-dimethylformamide, dichloromethane, toluene, n-hexane, petroleum ether, acetone, ethanol, and methanol.

[0032] Preferably, in step (4), the reaction temperature is 40-80° C., and the reaction time is 1-4 h.

[0033] Preferably, in step (4), after the reaction is completed, the reaction product is coated on a substrate by a coating process, and the solvent is evaporated to obtain the wide temperature range polyurethane elastomer.

[0034] Preferably, the volatilization temperature is 20 to 80° C., and the volatilization time is 6 to 24 hours.

[0035] Compared with the prior art, the present invention has at least the following beneficial effects:

[0036] The present invention proposes an innovative molecular structure design strategy, which uses diisocyanate to organically combine a flexible segment with a low glass transition temperature with a metal coordination structure with a large steric effect, weakening the hydrogen bond interaction between polyurethane segments, thereby broadening the use temperature range of polyurethane elastomers. The introduction of flexible segments can reduce the glass transition temperature of the material, thereby improving its flexibility at low temperatures; and the addition of large steric hindrance units can weaken the formation of hydrogen bonds at the spatial level, thereby maintaining good mechanical properties at high temperatures, significantly improving the cold resistance and heat resistance of polyurethane elastomers, and enabling polyurethane elastomers to be used normally within a wide temperature range (-60°C to 80°C). BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is the dynamic mechanical analysis temperature scanning curve of the sample in Comparative Example 1.

[0038] Figure 2 This is the dynamic mechanical analysis temperature scanning curve of the sample in Example 1.

[0039] Figure 3 This is the dynamic mechanical analysis temperature scanning curve of the sample in Example 2.

[0040] Figure 4 This is the dynamic mechanical analysis temperature scanning curve of the sample in Example 3.

[0041] Figure 5 It is the mechanical tensile curve of the sample in comparative example 1 at different temperatures.

[0042] Figure 6 1 is the mechanical tensile curve of the sample in Example 1 at different temperatures.

[0043] Figure 7 The mechanical tensile curves of the sample in Example 2 at different temperatures.

[0044] Figure 8 The mechanical tensile curves of the sample in Example 3 at different temperatures. DETAILED DESCRIPTION

[0045] The following will combine the comparative examples and embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] Comparative Example 1: A synthetic route for a polyurethane elastomer used in a conventional temperature range

[0047] (1) Weigh 2.0 g of 2,6-diethynylpyridine and 2.9 g of 2-azidoethanol, add a mixed solvent of 40 mL of deionized water and 40 mL of anhydrous ethanol, then add 0.2 g of copper sulfate pentahydrate and 0.3 g of sodium L-ascorbate, and stir at 30°C for 24 hours. Then purify by column chromatography (methanol: dichloromethane = 3:1), and finally dry in a vacuum oven at 50°C for 10 hours to obtain a dihydroxy-terminated ligand molecule (BTP), the structural formula of which is as follows.

[0048]

[0049] (2) Weigh 20 g of dihydroxy-terminated polybutadiene with a molecular weight of 4000 g / mol, dissolve it in 20 mL of anhydrous tetrahydrofuran, then add 2.2 g of isophorone diisocyanate and 2 drops of catalyst dibutyltin dilaurate, and stir the mixture at 50° C. for 6 hours to obtain a polyurethane prepolymer solution;

[0050] (3) Weigh 1.5 g of dihydroxy-terminated ligand molecule BTP, dissolve it in 2 mL of N,N-dimethylformamide, and add it dropwise to the above prepolymer solution. Stir and react at 50° C. for 12 hours.

[0051] (4) The solution after the reaction was poured into a polytetrafluoroethylene mold, volatilized in a ventilated environment at room temperature for 12 hours, and then dried in a vacuum oven at 60° C. for 12 hours to obtain a polyurethane elastomer film without metal coordination.

[0052] Example 1

[0053] (1) Weigh 2.0 g of 2,6-diethynylpyridine and 2.9 g of 2-azidoethanol, add a mixed solvent of 40 mL of deionized water and 40 mL of anhydrous ethanol, then add 0.2 g of copper sulfate pentahydrate and 0.3 g of sodium L-ascorbate, and stir at 30°C for 24 hours. Then purify by column chromatography (methanol: dichloromethane = 3:1), and finally dry in a vacuum oven at 50°C for 10 hours to obtain a dihydroxy-terminated ligand molecule (BTP), the structural formula of which is as follows.

[0054]

[0055] (2) Weigh 20 g of dihydroxy-terminated polybutadiene with a molecular weight of 4000 g / mol, dissolve it in 20 mL of anhydrous tetrahydrofuran, then add 2.2 g of isophorone diisocyanate and 2 drops of catalyst dibutyltin dilaurate, and stir the mixture at 50° C. for 6 hours to obtain a polyurethane prepolymer solution;

[0056] (3) Weigh 1.5 g of dihydroxy-terminated ligand molecule BTP, dissolve it in 2 mL of N,N-dimethylformamide, and add it dropwise to the above prepolymer solution. Stir and react at 50° C. for 12 hours.

[0057] (4) Weigh 0.9 g of zinc trifluoromethanesulfonate Zn(OTf) 2 , dissolved in 1 mL of organic solvent N,N-dimethylformamide, and added dropwise to the above solution, and stirred at 50°C for 2 hours.

[0058] (5) The solution after the reaction was poured into a polytetrafluoroethylene mold, volatilized in a ventilated environment at room temperature for 12 hours, and then dried in a vacuum oven at 60° C. for 12 hours to obtain a Zn-BTP coordinated cross-linked polyurethane elastomer material with a wide temperature range.

[0059] Example 2

[0060] (1) Weigh 2.0 g of 2,6-diethynylpyridine and 2.9 g of 2-azidoethanol, add a mixed solvent of 40 mL of deionized water and 40 mL of anhydrous ethanol, then add 0.2 g of copper sulfate pentahydrate and 0.3 g of sodium L-ascorbate, and stir at 30°C for 24 hours. Then purify by column chromatography (methanol: dichloromethane = 3:1), and finally dry in a vacuum oven at 50°C for 10 hours to obtain a dihydroxy-terminated ligand molecule (BTP), the structural formula of which is as follows.

[0061]

[0062] (2) Weigh 20 g of dihydroxy-terminated polybutadiene with a molecular weight of 4000 g / mol, dissolve it in 20 mL of anhydrous tetrahydrofuran, then add 2.2 g of isophorone diisocyanate and 2 drops of catalyst dibutyltin dilaurate, and stir the mixture at 50° C. for 6 hours to obtain a polyurethane prepolymer solution;

[0063] (3) Weigh 1.5 g of dihydroxy-terminated ligand molecule BTP, dissolve it in 2 mL of N,N-dimethylformamide, and add it dropwise to the above prepolymer solution. Stir and react at 50° C. for 12 hours.

[0064] (4) Weigh 1.0 g of europium trifluoromethanesulfonate Eu(OTf) 3 , dissolved in 1 mL of organic solvent N,N-dimethylformamide, and added dropwise to the above solution, and stirred at 50°C for 2 hours.

[0065] (5) The solution after the reaction was poured into a polytetrafluoroethylene mold, volatilized in a ventilated environment at room temperature for 12 hours, and then dried in a vacuum oven at 60° C. for 12 hours to obtain a Eu-BTP coordinated cross-linked polyurethane elastomer material with a wide temperature range.

[0066] Example 3

[0067] (1) Weigh 2.3 g of [2,2′-bipyridine]-5,5′-diacetonitrile, 1.0 g of anhydrous ethanol, and 0.2 g of cuprous iodide catalyst, add them to 10 mL of deionized water, then add dilute hydrochloric acid solution to the water to adjust the pH to 3, stir and react at 30°C for 12 hours, then add sodium bicarbonate solution to adjust the pH to 7, then add 20 mL of poor solvent n-hexane for recrystallization to obtain an intermediate product. After drying the intermediate product, add 10 mL of ultra-dry tetrahydrofuran to dissolve it in an anhydrous and oxygen-free environment, then add 1.0 g of reducing agent lithium aluminum hydride, and stir and react at 60°C for 5 hours. Then purify it by column chromatography, and finally dry it in a vacuum oven at 60°C for 5 hours to obtain a 2,2′-bipyridine group [2,2′-bipyridine]-5,5′-diethanol ligand small molecule (BPy), the structural formula of which is as follows.

[0068]

[0069] (2) Weigh 20 g of dihydroxy-terminated polybutadiene with a molecular weight of 4000 g / mol, dissolve it in 20 mL of anhydrous tetrahydrofuran, then add 2.2 g of isophorone diisocyanate and 2 drops of catalyst dibutyltin dilaurate, and stir the mixture at 50° C. for 6 hours to obtain a polyurethane prepolymer solution;

[0070] (3) Then, 1.2 g of ligand molecule BPy was weighed, dissolved in 2 mL of N,N-dimethylformamide, and added dropwise to the prepolymer solution, and stirred at 50 °C for 12 h.

[0071] (4) Next, weigh 0.6 g of zinc trifluoromethanesulfonate Zn(OTf) 2 , dissolved in 1 mL of organic solvent N,N-dimethylformamide, and added dropwise to the above solution, and stirred at 50°C for 2 hours.

[0072] (5) The solution after the reaction was poured into a polytetrafluoroethylene mold, volatilized in a ventilated environment at room temperature for 12 hours, and then dried in a vacuum oven at 60° C. for 12 hours to obtain a Zn-BPy coordinated cross-linked wide temperature range polyurethane elastomer material.

[0073] In order to evaluate the cold resistance and heat resistance of the wide temperature range polyurethane elastomer of the present invention, dynamic mechanical analysis (DMA) test and mechanical property test under high and low temperature were carried out on each polyurethane elastomer. Figure 1-8 As shown. From the DMA temperature scanning spectrum, it can be seen that ( Figure 1-Figure 4 ), the typical rubber platform range of the comparative sample is narrow, and the storage modulus is relatively stable only between 0 and 50°C; while the rubber platform range of the samples of Examples 1-3 is wide, and the storage modulus is basically stable between -60°C and 120°C, reflecting that the examples have a wide operating temperature range. It can be seen from the stretching under high and low temperatures ( Figure 5-Figure 8 ), the strength of the comparative sample at 80°C is very low, only 0.5MPa; while the samples of Examples 1-3 show good tensile strength at both high and low temperatures, and even at 80°C, they still maintain a tensile strength of more than 3MPa. According to the above two tests, the results show that the polyurethane elastomer based on flexible segments and metal coordination crosslinking has a wide operating temperature range and has good cold resistance and heat resistance.

Claims

1. A wide temperature range polyurethane elastomer, characterized in that: The wide temperature range polyurethane elastomer is obtained by reacting a flexible chain segment with a low glass transition temperature, a diisocyanate and a large steric hindrance unit, wherein the flexible chain segment with a low glass transition temperature is a flexible chain segment with a dihydroxyl end capping; and the large steric hindrance unit is a metal ion-ligand coordination structure.

2. The wide temperature range polyurethane elastomer according to claim 1, characterized in that: The flexible chain segment with a dihydroxyl-terminated terminal includes one or more of dihydroxyl-terminated polydimethylsiloxane, dihydroxyl-terminated polybutadiene, and dihydroxyl-terminated perfluoropolyether.

3. The wide temperature range polyurethane elastomer according to claim 2, characterized in that: The number average molecular weight of the flexible chain segment with double hydroxyl end-capping is 1000-6000 g / mol.

4. The wide temperature range polyurethane elastomer according to claim 1, characterized in that: In the metal ion-ligand coordination structure, the metal ion is one or more metal cations with valences from +1 to +6; the ligand motifs include one or more of a 2,6-bis(triazine)pyridine group, a 2,6-di(2-pyridyl)pyridine group, a 2,2'-bipyridine-4,4'-dicarboxylic acid group, a 2,2'-bipyridine group, a 2,6-bis(2-benzimidazolyl)pyridine group, and a pyridine-2,6-dicarboxylic acid group.

5. The wide temperature range polyurethane elastomer according to claim 4, characterized in that: The molar ratio of the flexible chain segment with dihydroxyl end capping, diisocyanate and ligand unit in the metal ion-ligand coordination structure is 1:1.5-2.2:0.5-1.

2.

6. The method for preparing a wide temperature range polyurethane elastomer according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) performing dihydroxy modification on a small molecule containing a ligand motif to obtain a dihydroxy-terminated ligand molecule; (2) mixing the flexible chain segment having a dihydroxyl end cap with a diisocyanate, an organic solvent and a catalyst, and performing a prepolymerization reaction to obtain a polyurethane prepolymer; (3) adding a dihydroxyl-terminated ligand molecule to the polyurethane prepolymer, stirring to react, and obtaining an uncrosslinked linear polyurethane product; (4) Adding a metal salt solution to the uncrosslinked linear polyurethane product and stirring to react, thereby obtaining the wide temperature range polyurethane elastomer.

7. The preparation method according to claim 6, characterized in that: In step (1), the small molecules containing ligand motifs include the following structures:

8. The preparation method according to claim 6, characterized in that: In step (2), the molar ratio of the flexible chain segment terminated with dihydroxyl groups to diisocyanate is 1:1.5-2.2; the temperature of the prepolymerization reaction is 40-80°C, and the reaction time is 2-6h.

9. The preparation method according to claim 6, characterized in that: In step (3), the molar ratio of the dihydroxy-terminated ligand molecule to the dihydroxy-terminated flexible chain segment is 0.5-1.2:1; the reaction temperature is 40-80° C., and the reaction time is 6-12 hours.

10. The preparation method according to claim 6, characterized in that: In step (4), the cations in the metal salt are one or more metal cations with valences of +1 to +6; the anions are one or more counter anions with valences of -1 to -3; the reaction temperature is 40 to 80°C, and the reaction time is 1 to 4 hours.

Citation Information

Patent Citations

  • Metal coordination self-healing polyurethane elastomer and preparation method thereof

    CN111217985A

  • Polysiloxane supramolecular elastomer with high mechanical properties and self-repairing function as well as preparation method and application thereof

    CN112063153A

  • Conductive self-repairing polyurethane elastomer based on dynamic coordination bond and preparation method thereof

    CN114752209A

  • Polyurethane material and preparation method thereof

    CN116496466A

  • Dipyrazole-based metal coordination self-repairing polyurethane elastomer and preparation method thereof

    CN117843913A

Cited By

  • Responsive dendritic polyamino acid modified polyurethane as well as preparation method and application thereof

    CN120737307A