Novel ultra-short time T6 process for 6082 aluminum alloy forgings

Through the ultra-short-time T6 new process of 6082 aluminum alloy forgings, including heating, forging, and uniform temperature and aging treatment, the problem of poor uniformity of forging performance is solved, the temperature and tissue uniformity of forgings is achieved, the process time is shortened, and the process time is improved. It has uniform performance and conforms to the concept of green manufacturing.

CN118950909APending Publication Date: 2024-11-15JIANGSU LONGCHENG PREC FORGING CO LTD

Patent Information

Application Number
CN202411305548.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

6082 aluminum alloy forgings have poor performance uniformity after solid solution forging. This is mainly due to the uneven temperature during forging, which leads to different solid solubility in each part, resulting in a decrease in the mechanical properties of the forgings.

Method used

Using the new ultra-short-time T6 process, including step 1: Cut and heat to 545-560℃ to complete solid solution, step 2: Forged immediately in a 200-300℃ mold, step 3: Quickly put it into a 600℃ temperature equalization furnace Insulated for 30-60 seconds, step 4: Cool immediately and stir, step 5: Remove the water stains, cut the edges and incorporate them into the aging furnace, step 6: Aging treatment to room temperature.

Benefits of technology

Through ultra-short-time temperature uniformity treatment, forgings with uniform temperature and tissue are obtained, which significantly shortens the process time, reduces the process flow, improves performance uniformity, and conforms to the green manufacturing concept of energy conservation and emission reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950909A_ABST
    Figure CN118950909A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloy forging and heat treatment, and discloses a 6082 aluminum alloy forge piece ultra-short time T6 new technology which comprises the steps that firstly, 6082 aluminum alloy is blanked, and a blank meeting the design specification and size requirements is obtained; secondly, the blank enters a heating furnace to be heated to 545-560 DEG C, heat preservation is conducted for enough time according to the specific blank thickness so that the solid solution process can be completed, and a solid solution structure is obtained; thirdly, the blank is immediately put into a die to be forged after being discharged out of the furnace; according to the method, an ultra-short temperature equalization process is added after solid solution forging, then water quenching is performed, subsequent conventional aging and short-time temperature equalization are performed, a forge piece with relatively uniform temperature and structure can be obtained, and a product with uniform performance is obtained after quenching; the solid solution state obtained during forging heating is fully utilized, a uniform and fully solid solution structure can be obtained in a very short time, the heating and heat preservation time of the solid solution procedure in T6 treatment is greatly shortened, the process time is shortened, the process flow is shortened, and the energy-saving, emission-reducing and green manufacturing concepts are better met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy forging and heat treatment, in particular to a new ultra-short-time T6 process for 6082 aluminum alloy forgings. Background Art

[0002] Aluminum alloy is the most widely used nonferrous metal structural material in industry, and has been widely used in aviation, aerospace, automobile, machinery manufacturing, shipbuilding and chemical industries. With the rapid development of industrial economy, the demand for aluminum alloy welded structural parts is increasing, which has led to in-depth research on the weldability of aluminum alloy.

[0003] 6082 aluminum alloy is an aluminum alloy material that can be strengthened by heat treatment. It has medium strength, good welding performance and corrosion resistance. It is mainly used in the transportation industry and structural engineering. In recent years, a large number of 6082 aluminum alloys have been used in the process of lightweighting automobiles. The most common problem in the forging of 6082 aluminum alloy is that there are often many coarse grains on the surface of the forging after solid solution + aging. The appearance of coarse grains leads to a decrease in the mechanical properties of the forging, which restricts the use efficiency of 6082 aluminum alloy. For this reason, the solid solution forging technology has been developed. The solid solution process is completed when the forging blank is heated. After the forging is completed, it is directly quenched in water for solid solution, and then conventional aging treatment is performed to obtain forgings with very few coarse grains. Its performance is higher than that of conventional heat-treated forgings.

[0004] However, the forgings of 6082 aluminum alloy have poor performance uniformity in various parts after solid solution forging. This is mainly due to the uneven temperature of various parts during forging and the different solid solubility obtained in various parts after water quenching. Therefore, a new ultra-short time T6 process for 6082 aluminum alloy forgings is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a new ultra-short time T6 process for 6082 aluminum alloy forgings to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a new ultra-short time T6 process for 6082 aluminum alloy forgings, comprising the following steps:

[0007] Step 1: Cut 6082 aluminum alloy to obtain a blank that meets the design specifications and size requirements;

[0008] Step 2: The blank enters the heating furnace and is heated to 545-560°C, and is kept warm for a sufficient time according to the specific thickness of the blank to complete the solid solution process and obtain a solid solution structure;

[0009] Step 3: After the blank is taken out of the furnace, it is immediately put into the mold for forging. The temperature of the forging mold is between 200℃ and 300℃, and the surface of the forging mold is sprayed with lubricant;

[0010] Step 4: After forging, the forging is not trimmed and is quickly placed in a temperature-averaging furnace at 600°C for 30-60 seconds;

[0011] Step 5: After the insulation is completed, take out the forging and immediately immerse it in a cooling water tank with appropriate stirring. The water temperature should not exceed 50°C.

[0012] Step 6. After taking the forging out of the water tank, remove the water stains on the forging and trim it, then put it into the aging furnace at an aging temperature of 170-180°C for 6-10 hours.

[0013] Step 7: After aging treatment, remove from the furnace and air cool to room temperature.

[0014] Preferably, in the above step 2, the thickness of the blank is 60-90 mm.

[0015] Preferably, in the above step 2, the solution holding time is 1.1-1.4h.

[0016] Preferably, in the above step three, the lubricant is a water-based graphite lubricant.

[0017] Preferably, in the above step 3, the forging time of the billet does not exceed 5 seconds, and the time from start forging to final forging does not exceed 15 seconds.

[0018] Preferably, in the above step 5, the cooling time of the forging in the cooling water tank is 2-3 minutes.

[0019] Preferably, in step six, water stains on the surface of the forging are dried using compressed air.

[0020] Preferably, in step six, the time from when the forging emerges from the water to when it enters the aging furnace does not exceed 2-3 hours.

[0021] Compared with the prior art, the present invention adopts the above technical solution and has the following technical effects:

[0022] 1. The present invention adds an ultra-short temperature equalization process after solution forging, then water quenching, and subsequent conventional aging. After a short time of temperature equalization, forgings with relatively uniform temperature and structure can be obtained, and products with uniform performance can be obtained after quenching;

[0023] 2. The present invention makes full use of the solid solution state obtained during forging heating, and can obtain a uniform and fully solid solution structure in a very short time, greatly shortening the heating and insulation time of the solid solution process in the T6 treatment, reducing the process time, shortening the process flow, and being more in line with the green manufacturing concept of energy conservation and emission reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the conditions under which this application can be implemented. Therefore, they have no substantive technical significance. Any structural modification, change in proportional relationship or adjustment of size should still fall within the scope of the technical content disclosed in this application without affecting the effects and purposes that can be achieved by this application.

[0028] Example 1

[0029] See also Figure 1 The present invention provides a technical solution: a new ultra-short-time T6 process for 6082 aluminum alloy forgings, comprising the following steps:

[0030] Step 1: Cut 6082 aluminum alloy to obtain a blank that meets the design specifications and size requirements;

[0031] Step 2: The blank enters the heating furnace and is heated to 545°C. According to the blank thickness of 60 mm, the holding time is 1.1 h to complete the solid solution process and obtain the solid solution structure;

[0032] Step 3: After the billet is taken out of the furnace, it is immediately put into the mold for forging. The forging time does not exceed 5 seconds. The temperature of the forging mold is between 200℃-300℃. The lubricant is sprayed on the surface of the forging mold. The lubricant is a water-based graphite lubricant. In the range of 200℃-300℃, the water-based graphite lubricant can play a better role. The water-based graphite lubricant is relatively cheap and environmentally friendly. However, when the temperature exceeds 300℃, the water-based graphite lubricant will fail, and the time from the start of forging to the final forging shall not exceed 15 seconds.

[0033] Step 4: After forging, the forging is not trimmed and is quickly placed in a temperature-averaging furnace at 600°C for 30-60 seconds;

[0034] Step 5: After the heat preservation is completed, take out the forging and immediately immerse it in the cooling water tank and apply appropriate stirring. The water temperature does not exceed 50°C. The cooling time of the forging in the cooling water tank is 2-3 minutes;

[0035] Step 6. After taking the forging out of the water tank, use compressed air to blow dry the water stains on the surface of the forging, cut the edges, and then put it into the aging furnace. The time from the forging out of the water to entering the aging furnace shall not exceed 2-3 hours, the aging temperature is 170-180℃, and the aging time is 6-10 hours;

[0036] Step 7: After aging treatment, remove from the furnace and air cool to room temperature.

[0037] Example 2

[0038] The difference from Example 1 is that the new ultra-short time T6 process for 6082 aluminum alloy forgings includes the following steps:

[0039] Step 1: Cut 6082 aluminum alloy to obtain a blank that meets the design specifications and size requirements;

[0040] Step 2: The blank enters the heating furnace and is heated to 550°C. According to the blank thickness of 70 mm, the holding time is 1.2 h to complete the solid solution process and obtain the solid solution structure;

[0041] Step 3: After the billet is taken out of the furnace, it is immediately put into the mold for forging. The forging time does not exceed 5 seconds. The temperature of the forging mold is between 200℃-300℃. The lubricant is sprayed on the surface of the forging mold. The lubricant is a water-based graphite lubricant. In the range of 200℃-300℃, the water-based graphite lubricant can play a better role. The water-based graphite lubricant is relatively cheap and environmentally friendly. However, when the temperature exceeds 300℃, the water-based graphite lubricant will fail, and the time from the start of forging to the final forging shall not exceed 15 seconds.

[0042] Step 4: After forging, the forging is not trimmed and is quickly placed in a temperature-averaging furnace at 600°C for 30-60 seconds;

[0043] Step 5: After the heat preservation is completed, take out the forging and immediately immerse it in the cooling water tank and apply appropriate stirring. The water temperature does not exceed 50°C. The cooling time of the forging in the cooling water tank is 2-3 minutes;

[0044] Step 6. After taking the forging out of the water tank, use compressed air to blow dry the water stains on the surface of the forging, cut the edges, and then put it into the aging furnace. The time from the forging out of the water to entering the aging furnace shall not exceed 2-3 hours, the aging temperature is 170-180℃, and the aging time is 6-10 hours;

[0045] Step 7: After aging treatment, remove from the furnace and air cool to room temperature.

[0046] Example 3

[0047] The difference from Examples 1 and 2 is that the new ultra-short time T6 process for 6082 aluminum alloy forgings comprises the following steps:

[0048] Step 1: Cut 6082 aluminum alloy to obtain a blank that meets the design specifications and size requirements;

[0049] Step 2: The blank enters the heating furnace and is heated to 555°C. According to the blank thickness of 80 mm, the holding time is 1.3 h to complete the solid solution process and obtain the solid solution structure;

[0050] Step 3: After the billet is taken out of the furnace, it is immediately put into the mold for forging. The forging time does not exceed 5 seconds. The temperature of the forging mold is between 200℃-300℃. The lubricant is sprayed on the surface of the forging mold. The lubricant is a water-based graphite lubricant. In the range of 200℃-300℃, the water-based graphite lubricant can play a better role. The water-based graphite lubricant is relatively cheap and environmentally friendly. However, when the temperature exceeds 300℃, the water-based graphite lubricant will fail, and the time from the start of forging to the final forging shall not exceed 15 seconds.

[0051] Step 4: After forging, the forging is not trimmed and is quickly placed in a temperature-averaging furnace at 600°C for 30-60 seconds;

[0052] Step 5: After the heat preservation is completed, take out the forging and immediately immerse it in the cooling water tank and apply appropriate stirring. The water temperature does not exceed 50°C. The cooling time of the forging in the cooling water tank is 2-3 minutes;

[0053] Step 6. After taking the forging out of the water tank, use compressed air to blow dry the water stains on the surface of the forging, cut the edges, and then put it into the aging furnace. The time from the forging out of the water to entering the aging furnace shall not exceed 2-3 hours, the aging temperature is 170-180℃, and the aging time is 6-10 hours;

[0054] Step 7: After aging treatment, remove from the furnace and air cool to room temperature.

[0055] Example 4

[0056] The difference from Examples 1, 2 and 3 is that the new ultra-short time T6 process for 6082 aluminum alloy forgings comprises the following steps:

[0057] Step 1: Cut 6082 aluminum alloy to obtain a blank that meets the design specifications and size requirements;

[0058] Step 2: The blank enters the heating furnace and is heated to 560°C. According to the blank thickness of 90 mm, the holding time is 1.4 h to complete the solid solution process and obtain the solid solution structure;

[0059] Step 3: After the billet is taken out of the furnace, it is immediately put into the mold for forging. The forging time does not exceed 5 seconds. The temperature of the forging mold is between 200℃-300℃. The lubricant is sprayed on the surface of the forging mold. The lubricant is a water-based graphite lubricant. In the range of 200℃-300℃, the water-based graphite lubricant can play a better role. The water-based graphite lubricant is relatively cheap and environmentally friendly. However, when the temperature exceeds 300℃, the water-based graphite lubricant will fail, and the time from the start of forging to the final forging shall not exceed 15 seconds.

[0060] Step 4: After forging, the forging is not trimmed and is quickly placed in a temperature-averaging furnace at 600°C for 30-60 seconds;

[0061] Step 5: After the heat preservation is completed, take out the forging and immediately immerse it in the cooling water tank and apply appropriate stirring. The water temperature does not exceed 50°C. The cooling time of the forging in the cooling water tank is 2-3 minutes;

[0062] Step 6. After taking the forging out of the water tank, use compressed air to blow dry the water stains on the surface of the forging, cut the edges, and then put it into the aging furnace. The time from the forging out of the water to entering the aging furnace shall not exceed 2-3 hours, the aging temperature is 170-180℃, and the aging time is 6-10 hours;

[0063] Step 7: After aging treatment, remove from the furnace and air cool to room temperature.

[0064] Working principle: first, the blank is cut according to the process requirements, and the blank is placed in the forging heating furnace for heating. The solid solution parameters of 6082 aluminum alloy are used for heating, so that the forging blank obtains the solid solution structure after heating. Secondly, after the blank is heated, it is taken out of the furnace and enters the forging process. Considering the temperature drop requirements, the time interval from the furnace to the forging is shortened as much as possible. The forging die temperature should be between 200-300℃. Too low a temperature is not conducive to reducing the coarse grain structure. After forging, the forging with flash is obtained. At this time, the edge is not trimmed first, so as to avoid the forging drastically cooling down during edge trimming, which is not conducive to the subsequent process implementation. The forging with flash is directly placed in the temperature of 600 The temperature of the forging is averaged in an average temperature furnace at about ℃ for 30-60 seconds; because the temperature of the forging has dropped to about 500℃ at this time, it can be heated to 530-540℃ at most within 30-60 seconds, and due to the high thermal conductivity of aluminum alloy, the temperature of various parts of the forging will tend to be consistent during this period of time; after the forging is taken out of the furnace, it is immediately quenched in water to obtain a solid solution structure, and this time interval is as short as possible to ensure the solid solution effect; after the solid solution is completed, the water stains are blown dry and the edges are trimmed. After the trimming, the forgings are placed in an aging furnace for aging, and this time interval does not exceed 2-3h; after the aging is completed, qualified products with less coarse grains and uniform performance can be obtained.

[0065] It will be appreciated by those skilled in the art that the features described in the various embodiments and / or claims of the present invention may be combined and / or combined in various ways, even if such combinations and / or combinations are not explicitly described in the present invention. In particular, the features described in the various embodiments and / or claims of the present invention may be combined and / or combined in various ways without departing from the spirit and teachings of the present invention. All of these combinations and / or combinations fall within the scope of the present invention.

Claims

1. 6082 aluminum alloy forging ultra-short time T6 new process, characterized by: The following steps are involved: Step 1: Cut 6082 aluminum alloy to obtain a blank that meets the design specifications and size requirements; Step 2: The blank enters the heating furnace and is heated to 545-560°C, and is kept warm for a sufficient time according to the specific thickness of the blank to complete the solid solution process and obtain a solid solution structure; Step 3: After the blank is taken out of the furnace, it is immediately put into the mold for forging. The temperature of the forging mold is between 200℃ and 300℃, and the surface of the forging mold is sprayed with lubricant; Step 4: After forging, the forging is not trimmed and is quickly placed in a temperature-averaging furnace at 600°C for 30-60 seconds; Step 5: After the insulation is completed, take out the forging and immediately immerse it in a cooling water tank with appropriate stirring. The water temperature should not exceed 50°C. Step 6. After taking the forging out of the water tank, remove the water stains on the forging and trim it, then put it into the aging furnace at an aging temperature of 170-180°C for 6-10 hours. Step 7: After aging treatment, remove from the furnace and air cool to room temperature.

2. The new ultra-short time T6 process for 6082 aluminum alloy forgings according to claim 1 is characterized in that: In step 2, the thickness of the blank is 60-90 mm.

3. The new ultra-short time T6 process for 6082 aluminum alloy forgings according to claim 1 is characterized in that: In step 2, the solution holding time is 1.1-1.4h.

4. The new ultra-short time T6 process for 6082 aluminum alloy forgings according to claim 1 is characterized in that: In step three, the lubricant is a water-based graphite lubricant.

5. The new ultra-short time T6 process for 6082 aluminum alloy forgings according to claim 1 is characterized in that: In step three, the forging time of the billet does not exceed 5 seconds, and the time from start forging to final forging does not exceed 15 seconds.

6. The new ultra-short time T6 process for 6082 aluminum alloy forgings according to claim 1 is characterized in that: In step five, the forging is cooled in the cooling water tank for 2-3 minutes.

7. The new ultra-short time T6 process for 6082 aluminum alloy forgings according to claim 1 is characterized in that: In step six, compressed air is used to blow water stains off the surface of the forging.

8. The new ultra-short time T6 process for 6082 aluminum alloy forgings according to claim 1 is characterized in that: In step six, the time from when the forgings exit the water to when they enter the aging furnace does not exceed 2-3 hours.

Citation Information

Patent Citations

  • Waste heat hardening and tempering process of motorcycle crank forged piece

    CN101524813A

  • Solid solution forging process for aluminum alloy part

    CN114346143A

  • High-performance aluminum alloy component coarse grain elimination forging process

    CN117086248A

  • Production method of aluminum alloy forging for automobile suspension

    US20210156016A1

  • Forging process for an aluminum alloy part

    US20230398597A1

Cited By

  • Preparation method of welding crack resistant 6082 aluminum alloy forge piece

    CN121004235A