Pressurized compact repair mortar and application thereof

By optimizing the composition and process of repair mortar, the weather resistance and fluidity problems of existing repair mortars in harsh environments are solved, and high strength, aesthetics and efficient repair effects are achieved, which are suitable for repairing complex shapes.

CN118955081AActive Publication Date: 2024-11-15CHINA RAILWAY MAJOR BRIDGE ENG GRP CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411064450.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing repair mortar has poor weather resistance in strong ultraviolet rays, high temperatures and high humidity environments, and is prone to yellowing or decomposition failure. It flows, slides down or floats when repairing vertical surfaces, top surfaces or narrow spaces, resulting in difficult control of the thickness of the repaired part and cannot be controlled. Meet the strength and load-bearing capacity required by the design.

Method used

Provide a pressurized compact repair mortar, containing gelling materials, fine aggregates, active stimulation components and tackifying components, water-gluing ratio and glue ratio are optimized, and dry hardness is formed through mechanical stirring and pressurized compaction technology. , repair materials that do not flow, shrink, and have high early strength to ensure consistent color with the repaired concrete components and high bonding strength.

Benefits of technology

It realizes weather resistance and waterproofing effects in harsh environments, ensures high strength and aesthetics of the repair layer, is suitable for repairing vertical surfaces, top surfaces and narrow spaces, reduces the independent flow of repair materials, improves construction efficiency and Overall performance of the patch layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978956910000131
    Figure BDA0004978956910000131
  • Figure BDA0004978956910000141
    Figure BDA0004978956910000141
  • Figure BDA0004978956910000142
    Figure BDA0004978956910000142
Patent Text Reader

Abstract

The invention discloses pressurized dense repair mortar and application thereof, and the pressurized dense repair mortar comprises the following raw materials: a cementing material, the doping amount of which is 25wt%-30wt% of the repair mortar; the mixing amount of the fine aggregate is 65wt%-68wt% of the repairing mortar; the active excitation component is composed of sodium silicate and gypsum, and the doping amount of the active excitation component is 4.4-6.5 wt% of the repairing mortar; the tackifying component is composed of cellulose ether and an amide high-molecular compound, and the doping amount of the tackifying component is 0.4-0.6 wt% of the repairing mortar; the mixing amount of the water reducing agent is 0.5 wt%-1wt% of the binding material; the mixing amount of the water is 17 wt%-20 wt% of the binding material; wherein the ratio of water to glue is 0.17-0.2, and the ratio of glue to bone is 0.37-0.46. The repairing mortar has the working performance of dry hardness and plasticity, and has the advantages of small shrinkage, high early strength, difficulty in cracking, good waterproof effect, high bonding strength with a repaired concrete member, consistent color and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of concrete repair materials and relates to a pressurized dense repair mortar and application thereof. Background Art

[0002] Common repair mortars on the market include polymer repair mortars and epoxy repair mortars. Repair mortars generally have good fluidity and are used to repair concrete surface defects by brushing. However, they generally have the following problems: (1) They shrink relatively large and are prone to secondary cracking in the later stage; (2) They have certain requirements for the construction environment. Under strong ultraviolet rays, high temperature, and high humidity environments, the weather resistance of the product is poor, and the repair mortar is prone to yellowing or even decomposition and failure; (3) Special fast-hardening cements such as sulfoaluminate cement are widely used, which are inconsistent with the color of the repaired building, easily causing color difference and affecting the appearance; (4) When repairing vertical surfaces, top structures, and some narrow spaces such as bridge piers and abutments, the mortar will easily flow, slide, or float up due to gravity, resulting in difficulty in controlling the thickness of the repaired part, uneven repair materials, and failure to achieve the strength and bearing capacity required by the design. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a pressurized compacting repair mortar and its application, which has the advantages of being dry and hard, not flowing, small shrinkage, high early strength, not easy to crack, good waterproof effect, high connection strength with the repaired concrete component, and consistent color.

[0004] The technical solution provided by the present invention is as follows:

[0005] In a first aspect, the present invention provides a pressurized compacting repair mortar, comprising the following raw materials:

[0006] Cementitious material, the dosage of which is 25wt% to 30wt% of the repair mortar;

[0007] Fine aggregate, the amount of which is 65wt% to 68wt% of the repair mortar;

[0008] The active excitation component is composed of sodium silicate and gypsum, and the dosage is 4.4wt% to 6.5wt% of the repair mortar;

[0009] The viscosity-increasing component is composed of cellulose ether and amide polymer compounds, and the dosage is 0.4wt% to 0.6wt% of the repair mortar;

[0010] Water reducing agent, the dosage of which is 0.5wt% to 1wt% of the cementitious material;

[0011] Water, the amount of which is 17wt% to 20wt% of the cementitious material;

[0012] Among them, the water-cement ratio is 0.17-0.2, and the cement-bone ratio is 0.37-0.46.

[0013] In some embodiments of the present invention, the pressurized compacting repair mortar is consistent with the fine aggregate type and gradation and cementitious material composition of the repaired concrete component. Consistent cementitious material composition means that the types of components in the cementitious material and the proportions of the components are consistent.

[0014] In some embodiments of the present invention, the water-to-binder ratio is 0.17-0.18, and the glue-to-bone ratio is 0.46.

[0015] In some embodiments of the present invention, the dosage of cellulose ether is 0.2wt% to 0.4wt% of the repair mortar; the weight average molecular weight of the amide polymer compound is 6 million to 10 million, and the dosage is 0.2wt% to 0.3wt% of the repair mortar; the dosage of sodium silicate is 3wt% to 5wt% of the repair mortar; and the dosage of gypsum is 0.5wt% to 1.5wt% of the repair mortar.

[0016] In some embodiments of the present invention, the amide polymer compound is polyacrylamide or sodium polyacrylate; the cellulose ether is one or more of carboxymethyl cellulose and hydroxypropyl methyl cellulose; the modulus of the sodium silicate is one or more of 2.0 to 2.4; and the gypsum is 120 mesh to 150 mesh.

[0017] In a second aspect, the present invention provides a concrete interface repair method, comprising:

[0018] Prepare the above-mentioned pressurized dense repair mortar;

[0019] Bringing the pressurized dense repair mortar into contact with the repaired interface;

[0020] Compact the pressurized dense repair mortar and allow it to cure naturally.

[0021] In some embodiments of the present invention, the repaired interface is located on one or more of a vertical surface, a top surface, and a narrow space.

[0022] In some embodiments of the present invention, preparing the pressurized compacting repair mortar comprises:

[0023] Pre-dry-mixing the cementitious material and fine aggregate to obtain a solid material;

[0024] Add the water reducing agent and half of the water to the solid material and stir mechanically to obtain a wet mixture;

[0025] Add the modifier and the remaining water to the wet mixture simultaneously and continue stirring for at least 120 seconds.

[0026] In some embodiments of the present invention, bringing the pressurized dense repair mortar into contact with the repaired interface comprises:

[0027] ( i ) Place the repair mortar in a handheld punch and squeeze it out towards the repaired interface; or,

[0028] ( ii ) Gather the repair mortar into a ball and press it onto the surface to be repaired.

[0029] In some embodiments of the present invention, the pressurized strength used for compacting the pressurized dense repair mortar is 10 to 50 MPa.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The repair mortar of the present invention has dry, hard and plastic working properties, and is very suitable for repairing vertical surfaces, top surfaces, narrow spaces and areas where formwork cannot be built.

[0032] 2. The type of fine aggregate and the composition of cementitious materials of the repair mortar of the present invention are consistent with those of the repaired concrete member, which not only ensures that the color of the repair layer is consistent with that of the repaired concrete member, but also allows local materials to be used to prepare the repair mortar of the present invention using the cementitious materials and fine aggregates on site. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range. Similarly, any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.

[0035] It should be noted that, in the description of this article, unless otherwise specified, "above", "below" are inclusive numbers, and the meaning of "multiple" in "one or more" is two or more. Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.

[0036] In the description of this specification, the description with reference to the terms "any embodiment / method", "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.

[0037] The above summary of the invention of the present invention is not intended to describe each disclosed embodiment or each implementation in the present invention. The following description more specifically illustrates exemplary embodiments. These embodiments can be used in various combinations. In each example, the enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0038] Repair mortar

[0039] As described in the background technology, the existing repair mortar has high fluidity and is not suitable for repairing vertical surfaces or top surfaces, as well as narrow spaces. To solve the above problems, the present invention provides a pressurized dense repair mortar, including the following raw materials:

[0040] Cementitious material, the dosage of which is 25wt% to 30wt% of the repair mortar;

[0041] Fine aggregate, the amount of which is 65wt% to 68wt% of the repair mortar;

[0042] The active excitation component is composed of sodium silicate and gypsum, and the dosage is 4.4wt% to 6.5wt% of the repair mortar;

[0043] The viscosity-increasing component is composed of cellulose ether and amide polymer compounds, and the dosage is 0.4wt% to 0.6wt% of the repair mortar;

[0044] Water reducing agent, the dosage of which is 0.5wt% to 1wt% of the cementitious material;

[0045] Water, the amount of which is 17wt% to 20wt% of the cementitious material;

[0046] Among them, the water-cement ratio is 0.17-0.2, and the cement-bone ratio is 0.37-0.46.

[0047] The repair mortar of the present invention adopts cement-based materials with a small amount of cementitious materials and a large amount of fine aggregates. The ratio of cementitious materials to aggregates (0.46-0.36) of the repair mortar is much lower than that of conventional repair mortars (1.5-0.6). The large amount of fine aggregates plays a role in restraining deformation. Therefore, the shrinkage deformation of the repair mortar during the hardening process is small and it is not easy to crack. In addition, the water-cement ratio of the repair mortar of the present invention is low. Compared with conventional repair mortars, it has poor fluidity, which is actually manifested as a ball when held in the hand, less water evaporation, faster coagulation speed, and less prone to cracking, peeling, etc.

[0048] In some embodiments of the present invention, the water-cement ratio is 0.17-0.18, the cement-bone ratio is 0.46, the strength of the repair layer is higher, and the bonding strength with the repaired concrete component is higher.

[0049] The cementitious material in the pressurized compacted repair mortar of the present invention accounts for 25wt% to 30wt% of the repair mortar. Compared with conventional repair mortars, the cementitious material is greatly reduced. Therefore, the repair mortar has a low shrinkage rate after drying and hardening and is not easy to crack.

[0050] In some embodiments of the present invention, the pressurized dense repair mortar is consistent with the fine aggregate type and cementitious material composition of the repaired concrete component, which can ensure that the color of the pressurized dense repair mortar is consistent with that of the repaired concrete component. In some embodiments of the present invention, the cementitious material is composed of cement, mineral powder, and fly ash. The cementitious material system of common repaired concrete components is generally composed of ordinary Portland cement, fly ash, and mineral powder. The glass structure of mineral admixtures such as mineral powder is mainly composed of calcium, silicon and a small amount of aluminum and magnesium. It can be cracked under alkaline conditions, dissolving different ions to further promote the hydration process.

[0051] The water in the pressurized compacting repair mortar of the present invention is 17wt% to 20wt% of the cementitious material. Compared with conventional repair mortar, the pressurized compacting repair mortar has less water content and a faster coagulation speed, thereby forming a dry and hard material that can be held in a ball.

[0052] The water-cement ratio of the pressurized compacting repair mortar of the present invention is 0.17-0.2. Compared with conventional repair mortar, the water-cement ratio is low, which can improve the flexural strength and compressive strength of the repair layer. When the water-cement ratio is too low, the shrinkage rate of the repair layer after drying and hardening is high, and shrinkage cracks are prone to occur, and the waterproof property is poor; when the water-cement ratio is too high, the strength of the repair layer is low. Note: The water-cement ratio refers to the mass ratio of water to the total mass of the cementitious material.

[0053] The cementitious-aggregate ratio of conventional rapid-hardening cement-based repair mortar or polymer repair mortar is generally higher than 1. The cementitious-aggregate ratio of the pressurized dense repair mortar of the present invention is 0.37-0.46, and the fine aggregate accounts for 65wt%-68wt% of the repair mortar. The purpose is to use the aggregate as the main body to play a role in restraining deformation. When the cementitious-aggregate ratio is too low, the repair layer has insufficient flexural strength due to excessive fine aggregate content; when the cementitious-aggregate ratio is too high, the repair layer has excessive shrinkage due to excessive cementitious material content, and shrinkage cracks are prone to occur. Note: The cementitious-aggregate ratio refers to the mass ratio of the total mass of cementitious material to the fine aggregate. In the embodiment of the present invention, river sand is used as the fine aggregate. Those skilled in the art can replace it with machine-made sand or regenerated sand according to the ease of obtaining the material, and the type and gradation of the aggregate used in the raw materials of the concrete to be repaired can be consistent.

[0054] The water reducing agent of the pressurized compacting repair mortar of the present invention is 0.5wt% to 1wt% of the cementitious material, and this content can ensure that the repair mortar is dry and hard when it leaves the machine, and the aggregate is wrapped by the cementitious material.

[0055] The active activation components of the pressurized compacting repair mortar of the present invention are composed of sodium silicate and gypsum, and the dosage is 4.4wt% to 6.5wt% of the repair mortar. Sodium silicate and gypsum synergistically activate the cementitious materials of the repair material and the repaired concrete component. Mineral admixtures such as cement, mineral powder, fly ash, etc. can maximize their potential activity under the action of sodium silicate and gypsum. Sodium silicate can promote the hydration process, generate a large number of network-like CSH and a small amount of AFt crystals, and form a dense crystal gel structure, which greatly improves the early mechanical strength and water resistance of the repair material, ensures that the repair mortar has higher mechanical properties than the repaired concrete structure, and avoids the problem of weak areas.

[0056] However, gypsum is difficult to dissolve in water. If it is added alone to the repair mortar with a low water-binder ratio, it may not react fully and fail to play the expected retarding effect, which greatly shortens the construction time of workers. Sodium silicate (Na2SiO3) and gypsum (CaSO4·2H2O) will react chemically to produce sodium sulfate (Na2SO4) and calcium silicate (CaSiO3). The reaction equation is:

[0057] Na2SiO3+CaSO4·2H2O→Na2SO4+CaSiO3+2H2O

[0058] The product sodium sulfate has a certain solubility and can dissociate into sodium ions (Na + ) and sulfate ions (SO4 2- ). Sulfate ions can promote the secondary hydration of cement, mineral powder and other mineral admixtures, stimulate activity, improve early strength, and react chemically with cement and mineral powder to generate products with a certain viscosity, which once again improves the bonding performance.

[0059] That is, sodium silicate is an alkaline activator, and the silicon in sodium silicate will combine with the calcium ions in cement to form CSH gel products. As the calcium ions are continuously consumed, the vitreous body of the mineral powder is forced to continue to decompose and consume the alkali in the system. Adding an appropriate amount of gypsum for regulation can promote the formation of calcium sulfonate. The alkaline excitation reaction occurs simultaneously inside the repair mortar and at the interface of the repaired concrete component. A reaction occurs between the repaired concrete component and the repair mortar, and the hydration products generated at the interface play a bonding role, enhancing the integrity.

[0060] The viscosity-increasing component of the present invention is composed of cellulose ether and amide polymer compounds, and the dosage is 0.4wt% to 0.6wt% of the repair mortar, which can increase the consistency of the mortar and enhance the interfacial bonding strength. Cellulose ether and amide polymer compounds are polymers, and have good compatibility with cement-based materials. They will be deposited or condensed on the surface of hydrated cement and aggregates to form a thin film, and this film will form an interpenetrating network structure with the cement hydration product. Because the dosage is low, this network structure with a certain flexibility mainly affects the fluidity of the repair mortar, has a water-retaining effect, and increases the consistency of the newly mixed repair mortar. The newly mixed repair mortar does not have the characteristics of autonomous flow, and is a loose slurry-coated sand particle with a slump of less than 10mm, which has the effect of being held in a ball by hand.

[0061] In some embodiments of the present invention, the amount of cellulose ether is 0.2wt% to 0.4wt% of the repair mortar; the weight average molecular weight of the amide polymer compound is 6 million to 10 million, and the amount of cellulose ether is 0.2wt% to 0.3wt% of the repair mortar; the amount of sodium silicate is 3wt% to 5wt% of the repair mortar; the amount of gypsum is 0.5wt% to 1.5wt% of the repair mortar. The amide polymer compound is polyacrylamide or sodium polyacrylate; the cellulose ether is one or more of carboxymethyl cellulose and hydroxypropyl methyl cellulose; the modulus of sodium silicate is one or more of 2.0 to 2.4; the gypsum is 120 mesh to 150 mesh.

[0062] In summary, under the combined effect of low glue-bone ratio and cellulose ether and amide polymer compounds, the pressurized compacting repair mortar of the present invention has the characteristics of dryness and hardness. During construction, it is compacted by supporting mechanical equipment. The handheld punch can press the loose repair mortar particles into a whole, filling the local peeling, flaking, cracks, honeycomb and other defects of the repaired substrate, and the pressurized strength is about 10 to 50 MPa. In the early stage, when the mortar is not completely dry, it has a high bonding strength and density. It can ensure the good water penetration resistance of the repair mortar and effectively inhibit the erosion of corrosive ions such as chloride ions on concrete under external environment.

[0063] application

[0064] The pressurized compacted repair mortar of the present invention has the characteristic of being able to be formed into a ball by hand, and can be applied by manual plastering and pressurized compaction to give the repair material early strong adhesion, and with the slow hydration of the cementitious material, the mechanical properties and bonding properties of the repair mortar are greatly improved after drying and hardening.

[0065] The cementitious material of the pressurized dense repair mortar of the present invention is consistent with the type and gradation of the fine aggregate and the composition of the cementitious material of the repaired concrete component. Therefore, the repair layer formed by the pressurized dense repair mortar is consistent with the color of the repaired concrete component and has no color difference. It can be used to fill the defective positions of honeycomb, rough surface, cracks, exposed reinforcement, etc. in the repaired concrete component, ensuring the integrity and beauty of the appearance of the concrete structure.

[0066] The pressurized dense repair mortar of the present invention has strong alkalinity and acts as an active stimulant to promote the secondary hydration of cementitious materials in the repaired concrete components, improve the strength of key parts of the concrete, form a new whole, and effectively prevent secondary cracking. Therefore, the pressurized dense repair mortar can be used for interface repairs with higher bonding strength requirements.

[0067] The pressurized compacting repair mortar of the present invention has excellent water-repellent effect and self-cleaning property after hardening. Water is difficult to penetrate into the building surface, and the waterproof effect is good. The surface dirt can be washed away by water. Therefore, the pressurized compacting repair mortar can be used to repair concrete components that need to be waterproof or difficult to clean, for example, surface repair of concrete projects such as cooling towers and sewage treatment tanks.

[0068] The pressurized dense repair mortar of the present invention does not have autonomous fluidity, therefore, it can be used for the repair of vertical surfaces, top surfaces, locations where molds are not easy to install, and narrow spaces. For example, stress concentrations such as the connection between the pier and the beam body, expansion joints, and chamfers of box beams in bridge concrete, special-shaped structures, and large-volume parts are prone to cracks. When repair and reinforcement are required, workers can shape the dry hard mortar according to the actual cross-sectional shape and size required to achieve precise filling, improve the fit of the repair mortar and the integrity of the structure. The repair process does not require the construction of templates, or the use of auxiliary tools and equipment such as pumping equipment to control the flow of materials, which saves repair time, improves overall construction efficiency, and realizes rapid repair of irregular bridge structures. The pressurized dense repair mortar of the present invention is fully infiltrated into the pores of the repaired base by mechanical pressurization, reducing the tiny gaps and loose areas existing in the bonding interface. Moisture is less likely to invade the bonding interface, thereby extending the service life of the bridge after repair and reinforcement.

[0069] Repair method

[0070] The present invention provides a concrete interface repair method, comprising:

[0071] Prepare the above-mentioned pressurized dense repair mortar;

[0072] Bringing the pressurized dense repair mortar into contact with the repaired interface;

[0073] Compact the pressurized dense repair mortar and allow it to cure naturally.

[0074] In some embodiments of the present invention, the repaired interface is located on one or more of a vertical surface, a top surface, and a narrow space.

[0075] In some embodiments of the present invention, preparing the above-mentioned pressurized dense repair mortar includes: pre-dry mixing the cementitious material and fine aggregate to obtain a solid material; adding a water reducer and half of the water to the solid material, mechanically stirring, to obtain a wet mixture; adding a modifier and the remaining water to the wet mixture at the same time and continuing to stir for no less than 120 seconds.

[0076] In some embodiments of the present invention, bringing the pressurized dense repair mortar into contact with the repaired interface comprises:

[0077] (i) Place the repair mortar in a handheld punch and squeeze it out towards the repaired interface; or,

[0078] ( ii ) Gather the repair mortar into a ball and press it onto the surface to be repaired.

[0079] In some embodiments of the present invention, the pressurized strength used for compacting the pressurized dense repair mortar is 10 to 50 MPa.

[0080] The concrete interface repair method can be applied to the aforementioned application scenarios.

[0081] Example

[0082] The technical scheme of the present invention is described in detail by way of examples below. If the manufacturer's brand or preparation method is not specified, the raw materials, equipment or solvents used are all common raw materials, equipment or solvents on the market. Unless otherwise specified, the raw materials of the same name used in the following examples and comparative examples are all the same raw materials.

[0083] The cement used in the following examples is ordinary Portland cement - P·O52.5 grade cement, with a specific surface area of ​​350m 2 / kg; the fly ash used is Grade I fly ash, with a water requirement ratio of 94.2% and a 45μm sieve residue of 11.4%; the mineral powder used is Grade S95 slag powder with a specific surface area of ​​421m 2 / kg, its particle size is mainly distributed between 1-13μm, and D50 is 3-5μm. The modulus of sodium silicate is between 2.0 and 2.4; gypsum uses commercially available common anhydrite, the main chemical component of which is CaSO4, and the particle size is 120 mesh to 150 mesh. Cellulose ether uses methyl hydroxypropyl cellulose, and amide polymer compound uses polyacrylamide.

[0084] Example 1

[0085] The repair mortar provided in this embodiment is composed of the following raw materials:

[0086] 19.5 parts by weight of cement, 6 parts by weight of mineral powder, 4.5 parts by weight of fly ash, 3.9 parts by weight of sodium silicate, 0.5 parts by weight of gypsum, 0.35 parts by weight of methyl hydroxypropyl cellulose, 0.25 parts by weight of polyacrylamide, 65 parts by weight of river sand, 5.1 parts by weight of water, and 0.27 parts by weight of water reducer.

[0087] The preparation method of the repair mortar provided in this embodiment comprises the following steps:

[0088] Pre-dry mix cement, mineral powder, fly ash and river sand to obtain solid materials; then add water reducer and half of the water and stir mechanically for about 60 seconds to obtain a wet mixture; then add sodium silicate, gypsum, methyl hydroxypropyl cellulose, polyacrylamide and water at the same time and continue stirring for no less than 120 seconds. If the slurry is not uniform or too dry and hard at the end of stirring, the stirring time can be extended to 180 seconds and the amount of water reducer can be adjusted; repair mortar is obtained after stirring is completed.

[0089] Example 2

[0090] The repair mortar provided in this embodiment is composed of the following raw materials:

[0091] 19.5 parts by weight of cement, 6 parts by weight of mineral powder, 4.5 parts by weight of fly ash, 3.0 parts by weight of sodium silicate, 1.5 parts by weight of gypsum, 0.2 parts by weight of methyl hydroxypropyl cellulose, 0.3 parts by weight of polyacrylamide, 65 parts by weight of river sand, 5.4 parts by weight of water, and 0.25 parts by weight of water reducer.

[0092] The preparation method of the repair mortar provided in this embodiment is the same as that in Embodiment 1.

[0093] Example 3

[0094] The repair mortar provided in this embodiment is composed of the following raw materials:

[0095] 16.9 parts by weight of cement, 5.2 parts by weight of mineral powder, 3.9 parts by weight of fly ash, 4.9 parts by weight of sodium silicate, 1.5 parts by weight of gypsum, 0.4 parts by weight of methyl hydroxypropyl cellulose, 0.2 parts by weight of polyacrylamide, 67 parts by weight of river sand, 4.9 parts by weight of water, and 0.22 parts by weight of water reducer.

[0096] The preparation method of the repair mortar provided in this embodiment is the same as that in Embodiment 1.

[0097] Example 4

[0098] The repair mortar provided in this embodiment is composed of the following raw materials:

[0099] 16.25 parts by weight of cement, 5 parts by weight of mineral powder, 3.75 parts by weight of fly ash, 5.0 parts by weight of sodium silicate, 1.5 parts by weight of gypsum, 0.3 parts by weight of methyl hydroxypropyl cellulose, 0.2 parts by weight of polyacrylamide, 68 parts by weight of river sand, 5.0 parts by weight of water, and 0.25 parts by weight of water reducer.

[0100] The preparation method of the repair mortar provided in this embodiment is the same as that in Embodiment 1.

[0101] Table 1 Raw material composition in each embodiment

[0102]

[0103]

[0104] Table 2 Performance of the repair mortar provided in each embodiment

[0105]

[0106] Comparative Example 1

[0107] The repair mortar provided in this comparative example is composed of the following raw materials:

[0108] 19.5 parts by weight of cement, 6 parts by weight of mineral powder, 4.5 parts by weight of fly ash, 0.35 parts by weight of methyl hydroxypropyl cellulose, 0.25 parts by weight of polyacrylamide, 65 parts by weight of river sand, 5.1 parts by weight of water, and 0.27 parts by weight of water reducer.

[0109] The preparation method of the repair mortar provided in this comparative example is the same as that of Example 1.

[0110] Comparative Example 2

[0111] The repair mortar provided in this comparative example is composed of the following raw materials:

[0112] 19.5 parts by weight of cement, 6 parts by weight of mineral powder, 4.5 parts by weight of fly ash, 3.9 parts by weight of sodium silicate, 0.5 parts by weight of gypsum, 65 parts by weight of river sand, 5.1 parts by weight of water, and 0.27 parts by weight of water reducer.

[0113] The preparation method of the repair mortar provided in this comparative example is the same as that of Example 1.

[0114] Comparative Example 3

[0115] The repair mortar provided in this comparative example is composed of the following raw materials:

[0116] 32.5 parts by weight of cement, 10 parts by weight of mineral powder, 7.5 parts by weight of fly ash, 3.9 parts by weight of sodium silicate, 0.5 parts by weight of gypsum, 0.35 parts by weight of methyl hydroxypropyl cellulose, 0.25 parts by weight of polyacrylamide, 50 parts by weight of river sand, 8.5 parts by weight of water, and 0.25 parts by weight of water reducer.

[0117] The preparation method of the repair mortar provided in this comparative example is the same as that of Example 1.

[0118] Comparative Example 4

[0119] The repair mortar provided in this comparative example is composed of the following raw materials:

[0120] 19.5 parts by weight of cement, 6 parts by weight of mineral powder, 4.5 parts by weight of fly ash, 5 parts by weight of sodium silicate, 0.35 parts by weight of methyl hydroxypropyl cellulose, 0.25 parts by weight of polyacrylamide, 64.4 parts by weight of river sand, 5.1 parts by weight of water, and 0.27 parts by weight of water reducer.

[0121] The preparation method of the repair mortar provided in this comparative example is the same as that of Example 1.

[0122] Comparative Example 5

[0123] The repair mortar provided in this comparative example is composed of the following raw materials:

[0124] 19.5 parts by weight of cement, 6 parts by weight of mineral powder, 4.5 parts by weight of fly ash, 1.4 parts by weight of gypsum, 0.35 parts by weight of methyl hydroxypropyl cellulose, 0.25 parts by weight of polyacrylamide, 68 parts by weight of river sand, 5.1 parts by weight of water, and 0.27 parts by weight of water reducer.

[0125] The preparation method of the repair mortar provided in this comparative example is the same as that of Example 1.

[0126] Comparative Example 6

[0127] The repair mortar provided in this comparative example is composed of the following raw materials:

[0128] 19.5 parts by weight of cement, 6 parts by weight of mineral powder, 4.5 parts by weight of fly ash, 3.9 parts by weight of sodium silicate, 0.5 parts by weight of gypsum, 0.6 parts by weight of methyl hydroxypropyl cellulose, 65 parts by weight of river sand, 5.1 parts by weight of water, and 0.27 parts by weight of water reducer.

[0129] The preparation method of the repair mortar provided in this comparative example is the same as that of Example 1.

[0130] Comparative Example 7

[0131] The repair mortar provided in this comparative example is composed of the following raw materials:

[0132] 19.5 parts by weight of cement, 6 parts by weight of mineral powder, 4.5 parts by weight of fly ash, 3.9 parts by weight of sodium silicate, 0.5 parts by weight of gypsum, 0.6 parts by weight of polyacrylamide, 65 parts by weight of river sand, 5.1 parts by weight of water, and 0.27 parts by weight of water reducer.

[0133] The preparation method of the repair mortar provided in this comparative example is the same as that of Example 1.

[0134] Table 3 Composition of raw materials in Example 1 and Comparative Example

[0135]

[0136]

[0137] Table 4 shows the physical property test results of the repair mortars of Example 1 and each comparative example and the test pieces made therefrom. The inspection method is in accordance with the "JG / T 336-2011 Technical Requirements for Polymer Cement Mortar for Repair of Concrete Structures", Type A index detection.

[0138] The 1d and 28d compressive and flexural strength tests were carried out in accordance with the "Test Method for Cement Mortar Strength (ISO Method)" (GB / T 17671-1999). The specimen size was 40mm×40mm×160mm and was prepared according to the raw material composition in Table 1. The freshly mixed dry hard material was compacted in the mortar mold by a punching machine to ensure that the mass of a single specimen was between 0.7 and 0.75kg.

[0139] Similarly, the 56d shrinkage test refers to the contact method in the Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete (GB / T50082-2009). The specimen size is 100mm×100mm×400mm and is prepared according to the raw material composition in Table 1. The freshly mixed cement mortar is compacted in a steel mold by a punch press to ensure that the mass of each specimen is between 10.8 and 11.5kg.

[0140] Table 4

[0141]

[0142]

[0143] As shown in Example 1, the test piece obtained from the repair mortar of the present invention has higher compressive and flexural strengths, smaller 56d shrinkage rate, and the repair mortar has higher 28d bonding strength with the concrete to be repaired and better impermeability.

[0144] As shown in Comparative Example 1, after sodium silicate and gypsum are omitted in the present invention relative to Example 1, the strength of the test piece itself decreases significantly, and the 28d bonding strength between the repair layer and the repaired concrete component also decreases seriously, but the 56d shrinkage rate decreases. This is because without the active excitation component, the cementitious material in the repair mortar is not completely hydrated, and the early strength decreases significantly. In addition, compared with Comparative Example 1, the mortar does not generate Na2SO4, and the product generated after the chemical reaction with cement and mineral powder has a certain viscosity, which once again improves the bonding performance.

[0145] As shown in Comparative Example 2, although the strength of the specimen itself is improved after omitting methyl hydroxypropyl cellulose and polyacrylamide relative to Example 1, the 28d bonding strength between the repair layer and the repaired concrete component decreases significantly, the 56d shrinkage rate also increases, and water seepage is prone to occur. This is because the two types of polymer particles, methyl hydroxypropyl cellulose and polyacrylamide, have good compatibility with cement-based materials and will be deposited or condensed on the surface of hydrated cement and aggregate to form a thin film. This film will form an interpenetrating network structure with the cement hydration product. Although this film will slightly hinder the hydration of cement particles and reduce the mechanical properties of the mortar, it will give the mortar a water-retaining effect and increase the consistency of the freshly mixed mortar. Without this component, the mortar does not have a flexible network structure and does not have obvious dry and hard characteristics, and the mechanical properties are enhanced, but the fluidity becomes larger and the bonding strength of the slurry is smaller.

[0146] As shown in Comparative Example 3, the present invention significantly increases the 56d shrinkage rate after increasing the ratio of glue to bone to 1 under the condition of unchanged water-binder ratio relative to Example 1. This is because, on the one hand, the decrease in the amount of aggregate will lead to a decrease in its effect of constraining deformation; on the other hand, the increase in the amount of glue will increase the corresponding amount of hydration reaction, resulting in more water consumption, smaller volume of hydration products, and more obvious drying shrinkage. The 28d bonding strength between the repair layer and the repaired concrete component also decreases slightly, because the increase in mortar shrinkage also has an adverse effect on the bonding strength.

[0147] As shown in Comparative Examples 4 to 7, when any one of sodium silicate, gypsum, methyl hydroxypropyl cellulose, and polyacrylamide is missing in the modifier, the 28d bonding strength between the repair layer and the repaired concrete member will decrease. In addition, the compressive strength and flexural strength of the specimen itself will also decrease.

[0148] When either sodium silicate or gypsum is missing in the active activation component of the modifier, the compressive and flexural strengths of the repair mortar will also decrease; and when either methyl hydroxypropyl cellulose or polyacrylamide is missing in the viscosity-enhancing component, the synergistic effect is lost, resulting in a significant decrease in the 28d bonding strength between the repair material and the repaired concrete component.

[0149] When the repair mortar prepared by the present invention is used to repair concrete components, there is no need to perform chemical treatment on the repaired interface. After cleaning the repaired interface, the repair mortar is applied to the area that needs to be repaired, compacted by manual pressure equipment, and the surface of the repair mortar is smoothed and cured to a specified age before it can be put into use.

[0150] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A pressurized dense repair mortar, characterized in that: Including the following ingredients: Cementitious material, the dosage of which is 25wt% to 30wt% of the repair mortar; Fine aggregate, the amount of which is 65wt% to 68wt% of the repair mortar; The active excitation component is composed of sodium silicate and gypsum, and the dosage is 4.4wt% to 6.5wt% of the repair mortar; The viscosity-increasing component is composed of cellulose ether and amide polymer compounds, and the dosage is 0.4wt% to 0.6wt% of the repair mortar; Water reducing agent, the dosage of which is 0.5wt% to 1wt% of the cementitious material; Water, the amount of which is 17wt% to 20wt% of the cementitious material; Among them, the water-cement ratio is 0.17-0.2, and the cement-bone ratio is 0.37-0.

46.

2. The pressurized dense repair mortar according to claim 1, characterized in that: The pressurized dense repair mortar is consistent with the fine aggregate type and cementitious material composition of the repaired concrete component.

3. The pressurized dense repair mortar according to claim 1, characterized in that: The water-to-binder ratio is 0.17-0.18, and the glue-to-bone ratio is 0.

46.

4. The pressurized dense repair mortar according to claim 1, characterized in that: The dosage of cellulose ether is 0.2wt% to 0.4wt% of the repair mortar; The weight average molecular weight of the amide polymer compound is 6 million to 10 million, and the dosage is 0.2wt% to 0.3wt% of the repair mortar; The dosage of sodium silicate is 3wt% to 5wt% of the repair mortar; The dosage of gypsum is 0.5wt% to 1.5wt% of the repair mortar.

5. The pressurized dense repair mortar according to claim 1 or 4, characterized in that: The amide polymer compound is polyacrylamide or sodium polyacrylate; the cellulose ether is one or more of carboxymethyl cellulose and hydroxypropyl methyl cellulose; the modulus of the sodium silicate is one or more of 2.0 to 2.4; and the gypsum is 120 mesh to 150 mesh.

6. A method for repairing a concrete interface, characterized in that: include: Preparing the pressurized dense repair mortar according to any one of claims 1 to 5; Bringing the pressurized dense repair mortar into contact with the repaired interface; Compact the pressurized dense repair mortar and allow it to cure naturally.

7. The concrete interface repair method according to claim 6, characterized in that: The repaired interface is located at one or more of a vertical surface, a top surface, and a narrow space.

8. The concrete interface repair method according to claim 6, characterized in that: Preparing the pressurized dense repair mortar according to any one of claims 1 to 5 comprises: Pre-dry-mixing the cementitious material and fine aggregate to obtain a solid material; Add the water reducing agent and half of the water to the solid material and stir mechanically to obtain a wet mixture; Add the modifier and the remaining water to the wet mixture simultaneously and continue stirring for at least 120 seconds.

9. The concrete interface repair method according to claim 6, characterized in that: Bringing the pressurized dense repair mortar into contact with the repaired interface comprises: ( i ) Place the repair mortar in a handheld punch and squeeze it out towards the repaired interface; or, ( ii ) Gather the repair mortar into a ball and press it onto the surface to be repaired.

10. The concrete interface repair method according to claim 6, characterized in that: The pressurized strength used for compacting the pressurized dense repair mortar is 10 to 50 MPa.

Citation Information

Patent Citations

  • Repair method of concrete surface layer defects

    CN106760603A

  • Method for repairing surface of assembly-type building prefabricated component

    CN109400085A

  • Fast hardening early strength type composite repair mortar

    CN109437759A

  • Squeezing type anti-crack mortar, preparation method and use method thereof

    CN110723941A

  • Premixed colored pervious concrete

    CN112897961A